Preparation method of silver nanoparticle surface enhanced Raman substrate
By performing plasma pretreatment on the silicon substrate and coating silver nanoparticles, the problem of insufficient signal uniformity and sensitivity of the surface enhancement of Raman substrate in the prior art is solved, and uniform deposition and significant signal enhancement of silver nanoparticles are achieved , improves the detection effect.
Patent Information
- Application Number
- CN202411001338.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
The signal uniformity and sensitivity of existing double-conical and cube silver nanoparticles surface enhancement of Raman substrates still need to be improved, resulting in uneven Raman signal strength and affecting the detection effect.
By plasma pretreating the silicon substrate and coating the dispersion of triangular double-cone silver nanoparticles and cube silver nanoparticles, a uniform and dense SERS substrate was prepared by solvothermal reaction and spin coating technology to improve the deposition of silver nanoparticles. Uniformity and signal enhancement effects.
The signal uniformity and sensitivity of the SERS substrate are significantly improved, and the excellent performance of triangular biconical silver nanoparticles is confirmed by the calculation of Raman enhancement factor, which enhances the detection sensitivity and signal strength.
Smart Images

Figure CN118937301A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of surface enhanced Raman substrates, and in particular to a method for preparing a silver nanoparticle surface enhanced Raman substrate. Background Art
[0002] Raman spectroscopy is a convenient and efficient testing and analysis method. It is widely used in food safety, biomedicine and environmental monitoring due to its advantages such as high sensitivity, non-destructive to samples and no interference from water. However, the Raman signal intensity of the sample being tested is usually very weak. Therefore, the application and development of Raman spectroscopy depends to a certain extent on the research and preparation of Raman scattering enhancement (SERS) substrates. In terms of materials used to prepare SERS substrates, noble metal nanoparticles are generally used because they have excellent localized plasma resonance effect (LSPR), that is, excellent Raman enhancement effect, and are easier to prepare. Among them, the preparation method of silver nanomaterials is relatively simpler and the preparation cost is low, so it is the most commonly used SERS material. The SERS performance of the material is related to its morphology. At present, the silver nanoparticles used to prepare SERS substrates include nanowires (rods), nanosheets, cubes, bipyramids, spheres, dodecahedrons, etc. Among them, cubic and bipyramid types have large specific surface areas, more sharp edges and corners, and excellent surface plasma resonance effects, which are more conducive to the preparation of SERS substrates with excellent performance.
[0003] At present, the SERS performance research method of bipyramidal and cubic silver nanoparticles is generally to prepare the particles into a SERS substrate, add a standard substance to the surface, perform a Raman test, obtain the Raman spectrum of the standard substance, and calculate the corresponding Raman enhancement factor (EF). For example, Tan et al. (Tavakkoli Yaraki, M.; Daqiqeh Rezaei, S.; Middha, E.; Tan, YN Synthesis and Simulation Study of Right Silver Bipyramids via Seed-Mediated Growth Cum Selective Oxidative Etching Approach. Part. Part. Syst. Charact. 2020, 37, 1–9.) used 1, 4-benzenedithiol (1, 4-BDT) as a Raman standard substance under a 532nm excitation light source to study the SERS performance of 87nm right bipyramidal silver nanoparticles. Xia et al. (McLellan, JM; Siekkinen, A.; Chen, J.; Xia, Y. Comparison of the Surface-Enhanced Raman Scattering on Sharp and Truncated Silver Nanocubes. Chem. Phys. Lett. 2006, 427, 122–126.) used 1,4-benzenedithiol as a Raman standard test substance to measure and compare the SERS performance of cubic silver nanoparticles with sharp edges and broken corners of 60 nm, 90 nm, and 100 nm in size, and obtained a maximum Raman enhancement factor of 3.56×10 under 785 nm excitation light source. 5 The same research group (Zhang, Q.; Li, W.; Moran, C.; Zeng, J.; Chen, J.; Wen, LP; Xia, Y. Seed-Mediated Synthesis of Ag Nanocubes with Controllable Edge Lengths in the Range of 30-200 nm and Comparison of Their Optical Properties. Journal of the American Chemical Society. 2010, 132, 11372–11378.) also measured and compared the SERS performance of cubic silver nanoparticles with sizes of 57 nm, 82 nm, 125 nm, and 170 nm, and obtained a maximum Raman enhancement factor of 4.1×10-1 at an excitation light source of 514 nm.6 However, the signal uniformity and sensitivity of the surface-enhanced Raman substrate prepared by it still need to be improved. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a silver nanoparticle surface enhanced Raman substrate. The surface enhanced Raman substrate prepared by the preparation method has good signal uniformity and high sensitivity, and the SERS substrate signal enhancement effect is significant.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a silver nanoparticle surface enhanced Raman substrate, comprising the following steps:
[0007] After the surface of the silicon substrate is subjected to plasma pretreatment, a silver nanoparticle dispersion is coated to obtain the surface enhanced Raman substrate;
[0008] The silver nanoparticles in the silver nanoparticle dispersion include right trigonal bipyramidal silver nanoparticles and / or cubic silver nanoparticles.
[0009] Preferably, the frequency of the plasma pretreatment is 9KHz to 14MHz, the power is 10 to 1200W, and the time is 5 to 600s;
[0010] The plasma pretreatment is carried out under the condition of air flow, and the air flow rate is 50-500 mL / min.
[0011] Preferably, the solvent in the silver nanoparticle dispersion includes one or more of ethanol, methanol and isopropanol;
[0012] The concentration of the silver nanoparticle dispersion is 0.5-20 mg / mL.
[0013] Preferably, the coating amount of the silver nanoparticle dispersion is (10-1000) μL / (1-2) cm 2 .
[0014] Preferably, the method for preparing cubic silver nanoparticles in the silver nanoparticle dispersion comprises the following steps:
[0015] The quinone compound, poly (N-vinyl pyrrolidone), a silver source, an additive and a polyol compound are mixed and then subjected to a solvothermal reaction to obtain the cubic silver nanoparticles;
[0016] The amount ratio of the silver source, quinone compound, poly N-vinyl pyrrolidone, additive and polyol compound is (8.83×10 -4 ~1.18×10 -2)mol:(1.80×10 -3 ~2.41×10 -2 )mol:(1.80×10 -3 ~1.80×10 -2 )mol:(2.22×10 -4 ~5.55×10 -3 )mol:1L.
[0017] Preferably, the silver source is a soluble silver salt;
[0018] The additive includes one or more of sodium chloride, potassium chloride, ferric chloride, copper chloride, hexadecyltrimethylammonium chloride, sodium bromide, potassium bromide and hexadecyltrimethylammonium bromide.
[0019] Preferably, the quinone compound includes one or more of camphorquinone, benzoquinone, naphthoquinone, anthraquinone and phenanthrenequinone;
[0020] The polyol compound includes one or more of ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, neopentyl glycol, diethylene glycol and glycerol.
[0021] Preferably, the coating method is spin coating, and the number of spin coating is ≥1 times.
[0022] Preferably, the spin coating is performed 6 times.
[0023] Preferably, the rotation speed of each spin coating is 1400-3600 rpm, and the time is 5-120 s.
[0024] The present invention provides a method for preparing a silver nanoparticle surface enhanced Raman substrate, comprising the following steps: after plasma pretreatment of the surface of a silicon substrate, coating a silver nanoparticle dispersion to obtain the surface enhanced Raman substrate; the silver nanoparticles in the silver nanoparticle dispersion include right triangular bipyramid silver nanoparticles and / or cubic silver nanoparticles. The right triangular bipyramid silver nanoparticles and / or cubic silver nanoparticles used in the present invention can enhance the Raman signal intensity and improve the detection sensitivity due to their sharp edges, and the uniform deposition of particles leads to the signal intensity obtained by testing at different points on the SERS substrate being equivalent. Therefore, by plasma pretreatment of the silicon substrate, a SERS substrate with uniform and dense deposition of silver nanoparticles can be prepared, and finally a SERS substrate with good signal uniformity and high sensitivity is obtained. The calculation and quantitative characterization of the Raman enhancement factor confirms that the SERS substrate prepared by the right triangular bipyramid silver nanoparticles and the cubic silver nanoparticles has a significant signal enhancement effect, and at the same time, in terms of the enhancement effect of the SERS substrate performance, the right triangular bipyramid silver nanoparticles are superior to the cubic silver nanoparticles. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The SEM image, particle size distribution image and UV-visible spectrum image of the cubic silver nanoparticles described in Example 1;
[0026] Figure 2 The SEM image, particle size distribution diagram and UV-visible spectrum diagram of the right triangular bipyramidal silver nanoparticles described in Example 2;
[0027] Figure 3 The top observation diagram and the side observation diagram of the deposition behavior of silver nanoparticles on the surface of the silicon substrate after plasma pretreatment in Comparative Example 1, and the SEM diagram of the right triangular bipyramid silver nanoparticles on the surface of the surface enhanced Raman substrate of the right triangular bipyramid silver nanoparticles in Comparative Example 1;
[0028] Figure 4 The SEM image (A) and Raman scan image (B) of the right triangular bipyramid silver nanoparticles on the surface of the right triangular bipyramid silver nanoparticle surface enhanced Raman substrate described in Example 2;
[0029] Figure 5 The SEM image of the right triangular bipyramid silver nanoparticles on the surface of the right triangular bipyramid silver nanoparticle surface enhanced Raman substrate described in Example 2 (A) and the SERS spectrum of the standard substance on the right triangular bipyramid silver nanoparticles under a 532nm excitation light source when the right triangular bipyramid silver nanoparticle surface enhanced Raman substrate is immersed in standard substances of different concentrations (B);
[0030] Figure 6 The SEM image of the cubic silver nanoparticles on the surface of the cubic silver nanoparticle surface enhanced Raman substrate described in Example 1 (A) and the SERS spectrum of the standard substance on the cubic silver nanoparticles under a 532nm excitation light source when the cubic silver nanoparticle surface enhanced Raman substrate is immersed in standard substances of different concentrations (B);
[0031] Figure 7 For R6G(10 -6 M, 20 μL) on the right trigonal bipyramidal silver nanoparticle surface enhanced Raman substrate described in Example 2 and the cubic silver nanoparticle surface enhanced Raman substrate described in Example 1, and the Raman spectrum of R6G (0.025 M, 20 μL) on a bare silicon substrate;
[0032] Figure 8 The top observation image and the side observation image of the deposition behavior of the silver nanoparticles on the surface of the silicon substrate of Comparative Example 2 and the SEM image of 10 microliters of the silver nanoparticle dispersion (4.7 mg / mL) dropped on the surface of the silicon substrate;
[0033] Fig. 9 The SEM images of the right triangular bipyramidal silver nanoparticle surface enhanced Raman substrates described in Comparative Examples 3 to 6;
[0034] Fig.10 For R6G(10 -6 M, 20 μL) Raman surface scanning images of the right trigonal bipyramidal silver nanoparticle surface enhanced Raman substrate described in Comparative Examples 4 and 5. DETAILED DESCRIPTION
[0035] The present invention provides a method for preparing a silver nanoparticle surface enhanced Raman substrate, comprising the following steps:
[0036] After the surface of the silicon substrate is subjected to plasma pretreatment, a silver nanoparticle dispersion is coated to obtain the surface enhanced Raman substrate;
[0037] The silver nanoparticles in the silver nanoparticle dispersion include right trigonal bipyramidal silver nanoparticles and / or cubic silver nanoparticles.
[0038] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.
[0039] In the present invention, since the right triangular bipyramidal silver nanoparticles and / or cubic silver nanoparticles have a larger specific surface area and more sharp edges and corners, they have an excellent surface plasmon resonance effect and can be more conducive to preparing a SERS substrate with excellent performance.
[0040] The present invention has no special limitation on the silicon substrate, and any type well known to those skilled in the art may be used.
[0041] In the present invention, the frequency of the plasma pretreatment is preferably 9KHz to 14MHz, more preferably 40KHz to 10MHz, and most preferably 40KHz to 100KHz; the power is preferably 10 to 1200W, more preferably 50 to 1000W, and most preferably 180 to 500W; the time is preferably 5 to 600s, more preferably 50 to 100s, and most preferably 60 to 80s; the plasma pretreatment is preferably carried out under air-passing conditions, and the air-passing rate is preferably 50 to 500mL / min, more preferably 200 to 400mL / min, and most preferably 250 to 300mL / min. In the present invention, the plasma pretreatment is preferably carried out in a vacuum plasma cleaning machine.
[0042] In the present invention, the plasma pretreatment is used to increase the surface energy and hydrophilicity of the silicon substrate so that the dispersion of silver nanoparticles can be evenly spread on the silicon substrate, thereby improving the deposition uniformity of the silver nanoparticles.
[0043] In the present invention, when the silver nanoparticles in the silver nanoparticle dispersion include right trigonal bipyramidal silver nanoparticles and cubic silver nanoparticles, the present invention has no special limitation on the ratio of the right trigonal bipyramidal silver nanoparticles and the cubic silver nanoparticles.
[0044] In the present invention, the solvent in the silver nanoparticle dispersion includes one or more of ethanol, methanol and isopropanol. When the solvent is two or more of the above specific selections, the present invention has no special restrictions on the ratio of the above specific substances, and they can be mixed in any ratio. In the present invention, the concentration of the silver nanoparticle dispersion is preferably 0.5 to 20 mg / mL, more preferably 4 to 10 mg / mL, and most preferably 4.7 to 6 mg / mL.
[0045] In the present invention, the method for preparing cubic silver nanoparticles in the silver nanoparticle dispersion preferably comprises the following steps:
[0046] The quinone compound, poly (N-vinyl pyrrolidone), a silver source, an additive and a polyol compound are mixed and then subjected to a solvothermal reaction to obtain the cubic silver nanoparticles;
[0047] The amount ratio of the silver source, quinone compound, poly N-vinyl pyrrolidone, additive and polyol compound is (8.83×10 -4 ~1.18×10 -2 )mol:(1.80×10 -3 ~2.41×10 -2 )mol:(1.80×10 -3 ~1.80×10 -2 )mol:(2.22×10 -4 ~5.55×10 -3 )mol:1L.
[0048] In the present invention, the quinone compound preferably includes one or more of camphorquinone, benzoquinone, naphthoquinone, anthraquinone and phenanthrenequinone, and more preferably camphorquinone; when the quinone compound is two or more of the above-mentioned specific selections, the present invention has no special limitation on the ratio of the above-mentioned specific substances, and they can be mixed in any ratio.
[0049] In the present invention, the silver source is preferably a soluble silver salt, more preferably one or more of silver nitrate, silver acetate, silver oxalate, silver hexafluorophosphate and silver hexafluoroantimonate, more preferably silver nitrate; when the silver source is two or more of the above-mentioned specific selections, the present invention has no special limitation on the ratio of the above-mentioned specific substances, and they can be mixed in any ratio.
[0050] In the present invention, the additive preferably includes one or more of sodium chloride, potassium chloride, ferric chloride, cupric chloride, hexadecyltrimethylammonium chloride, sodium bromide, potassium bromide and hexadecyltrimethylammonium bromide, more preferably ferric chloride; when the additive is two or more of the above specific selections, the present invention has no special limitation on the ratio of the above specific substances, and they can be mixed in any ratio.
[0051] In the present invention, the polyol compound preferably includes one or more of ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, neopentyl glycol, diethylene glycol and glycerol, and ethylene glycol is more preferred; when the polyol compound is two or more of the above-mentioned specific selections, the present invention has no special limitation on the ratio of the above-mentioned specific substances, and they can be mixed in any ratio.
[0052] In the present invention, the usage ratio of the silver source, quinone compound, poly N-vinyl pyrrolidone, additive and polyol compound is (0.15-2.0) g: (0.3-4.0) g: (0.2-2.0) g: (0.06-1.5) mg: 100 mL, preferably (0.5-1.5) g: (1.0-3.0) g: (0.8-1.3) g: (0.33-1.3) mg: 100 mL, and more preferably 1.0 g: 1.9 g: 1.0 g: 0.65 mg: 100 mL.
[0053] In the present invention, the role of controlling the usage ratio of the silver source, quinone compound, poly (N-vinyl pyrrolidone), additive and polyol compound within the above range is to regulate the reduction rate of the silver source, selectively change the crystal structure of the silver nanoparticles and the growth rate of different crystal faces, achieve control of the product morphology, and obtain silver nanoparticles with the morphology of right triangular bipyramid and cube.
[0054] In the present invention, the mixing is preferably performed by sequentially adding a quinone compound and poly (N-vinyl pyrrolidone) to the polyol compound, and then sequentially adding a silver source and an additive to dissolve them.
[0055] In the present invention, the temperature of the solvothermal reaction is preferably 110-130° C., more preferably 115-125° C., most preferably 120° C.; the time is preferably 2.5-4 h, more preferably 3-3.5 h.
[0056] After the solvothermal reaction is completed, the present invention also preferably includes sequential washing and centrifugation; the washing is preferably performed using ethanol; the rotation speed of the centrifugation is preferably 8000 rpm, and the number of times is preferably ≥1.
[0057] In the present invention, the coating amount of the silver nanoparticle dispersion is preferably (350-1000) μL / (1-2) cm 2, more preferably (450-800) μL / (1-2) cm 2 , the most preferred range is (600-750) μL / (1-2) cm 2 .
[0058] In the present invention, the coating method is preferably spin coating, and the number of spin coating is preferably ≥ 1 time, and more preferably 6 times. In the present invention, the rotation speed of each spin coating is preferably 1400-3600 rpm, more preferably 1800-2800 rpm, and most preferably 2000-2300 rpm; the time is preferably 5-120 s, more preferably 10-80 s, and most preferably 10-40 s.
[0059] In the present invention, each spin coating process is preferably performed by dropping a drop of the silver nanoparticle dispersion on the surface of the plasma pretreated silicon substrate, and then using a coating machine for coating. After each spin coating is completed, it is also preferably included in the process of drying, and the present invention has no special limitation on the drying process.
[0060] The right triangular bipyramid silver nanoparticles and / or cubic silver nanoparticles used in the present invention can enhance the Raman signal intensity and improve the detection sensitivity because of their sharp edges. The uniform deposition of particles leads to the signal intensity obtained by testing at different points on the SERS substrate being equivalent. Therefore, a SERS substrate with uniform and dense deposition of silver nanoparticles can be prepared by plasma pretreatment of a silicon substrate, and finally a SERS substrate with good signal uniformity and high sensitivity is obtained. The calculation and quantitative characterization of the Raman enhancement factor confirms that the SERS substrate signal enhancement effect prepared by the right triangular bipyramid silver nanoparticles and the cubic silver nanoparticles is significant. At the same time, in terms of the enhancement effect of the SERS substrate performance, the right triangular bipyramid silver nanoparticles are superior to the cubic silver nanoparticles.
[0061] The preparation method of the silver nanoparticle surface enhanced Raman substrate provided by the present invention is described in detail below in conjunction with the examples, but they should not be construed as limiting the scope of protection of the present invention.
[0062] Example 1
[0063] 0.289 g of camphorquinone (CQ) and 0.155 g of polyvinyl pyrrolidone (PVP) were added to 15 mL of ethylene glycol (EG). After complete dissolution, 0.150 g of AgNO3 was added to the solution and dissolved. Then, 1.1 mL of EG solution of iron (III) chloride hexahydrate with a concentration of 600 μM was added and stirred at 900 rpm for 4 minutes, at which time the concentration of FeCl3 in the reaction solution was 0.04 mM (mmol / L millimoles per liter). The reaction solution was then heated at 120°C and stirred at 300 rpm (revolutions per minute) for 3 hours. After the reaction, the resulting product was washed with ethanol, and after centrifugation at 8000 rpm for several times, the particle precipitation product (cubic silver nanoparticles mainly cubic and right trigonal bipyramidal silver nanoparticles) was redispersed and stored in ethanol;
[0064] Figure 1 The SEM images, particle size distribution images and UV-visible spectra of the cubic silver nanoparticles are shown in Figure 1, wherein A is the SEM image of the cubic silver nanoparticles at an enlargement factor of 12,000, B is the SEM image of the cubic silver nanoparticles at an enlargement factor of 20,000, C is the particle size distribution image of the cubic silver nanoparticles, and D is the UV-visible spectra of the cubic silver nanoparticles. As can be seen from A to B, when the FeCl3 concentration is 0.04 mM, the product has cubic silver nanoparticles with sharp corners and a small amount of right triangular bipyramidal silver nanoparticles. A mixture of rice particles, at this time, the yield of cubic silver nanoparticles is significantly higher than that of bipyramidal silver nanoparticles, and is the main product (the yield of the cubic silver nanoparticles is 70% calculated according to the average of the picture counting); from C, it can be seen that the size of the cubic silver nanoparticles is mainly distributed in 110-140nm, with an average size of 120nm; from D, it can be seen that the peak positions of the four LSPR peaks are consistent with the LSPR peak positions of cubic silver nanoparticles with the same size in the previous studies (Pan, ZY; Zhou, J.; Zou, HY; Li, YF; Gao, PF; Huang, CZ In Situ Investigating the Size-Dependent Scattering Signatures and Sensing Sensitivity of Single Silver Nanocube through a Multi-Model Approach. J. Colloid Interface Sci. 2021, 584, 253-262.), and the results prove that the camphorquinone-mediated polyol synthesis method is effective in preparing cubic silver nanoparticles;
[0065] The silicon substrate was plasma pretreated (180 W, 60 s) by passing air atmosphere (passing rate of 250 mL / min) using a vacuum plasma cleaning machine (40 KHz) to obtain a pretreated silicon substrate;
[0066] dispersing the cubic silver nanoparticles in ethanol to obtain a silver nanoparticle dispersion having a concentration of 4.7 mg / mL;
[0067] A drop of the silver nanoparticle dispersion (10 μl) was dropped onto the pretreated silicon substrate surface (1 cm×1 cm), and then the pretreated silicon substrate was rotated at a speed of 2000 rpm for 10 seconds using a coating machine to evenly disperse and coat the cubic silver nanoparticle dispersion on the silicon substrate surface, and then blow-dried to ensure that the volatilization of ethanol can be accelerated at a faster air flow rate, thereby accelerating the deposition and drying of the cubic silver nanoparticles on the silicon substrate surface; the spin coating and blow-drying process was repeated 5 times to obtain a cubic silver nanoparticle surface enhanced Raman substrate;
[0068] Figure 6 The SEM image (A) of the cubic silver nanoparticles on the surface of the cubic silver nanoparticle surface enhanced Raman substrate and the SERS spectrum (B) of the standard substance on the cubic silver nanoparticles under a 532nm excitation light source when the cubic silver nanoparticle surface enhanced Raman substrate is immersed in different concentrations of standard substances, wherein (A) is the SEM image of the cubic silver nanoparticles at a magnification of 12000, and (B) is the SERS spectrum measured at room temperature using a 532nm wavelength and an intensity of 0.5mW incident laser. As shown in A, the cubic silver nanoparticles are evenly distributed on the SERS substrate before the test. As shown in B, the SERS spectrum shows the R6G spectral line characteristics of the standard substance, and when the R6G concentration is as low as 10 -12 The Raman spectra with distinguishable characteristic peaks can also be seen below M. This shows that the synthesized cubic silver nanoparticles can effectively enhance the Raman signal of the sample under test and are suitable for SERS enhancement.
[0069] Example 2
[0070] 0.289 g of camphorquinone (CQ) and 0.155 g of polyvinyl pyrrolidone (PVP) were added to 15 mL of ethylene glycol (EG). After complete dissolution, 0.150 g of AgNO3 was added to the solution and dissolved. Then, 3.1 mL of iron (III) chloride hexahydrate (600 μM in EG solution) was added and stirred vigorously for 4 minutes, at which time the FeCl3 concentration in the reaction solution was 0.11 mM (mmol / L millimoles per liter). The reaction solution was then heated at 120°C and stirred at 300 rpm (revolutions per minute) for 3 hours. After the reaction, the resulting product was washed with ethanol, and after centrifugation at 8000 rpm for several times, the particle precipitation product (right trigonal bipyramidal silver nanoparticles) was redispersed and stored in ethanol;
[0071] Figure 2 The SEM image, particle size distribution image and UV-visible spectrum image of the right triangular bipyramid silver nanoparticles are shown in Figure 1, wherein A is the SEM image of the right triangular bipyramid silver nanoparticles at an enlargement factor of 12,000, B is the SEM image of the right triangular bipyramid silver nanoparticles at an enlargement factor of 20,000, C is the particle size distribution image of the right triangular bipyramid silver nanoparticles, and D is the UV-visible spectrum image of the right triangular bipyramid silver nanoparticles. It can be seen from A to B that when the FeCl3 concentration is 0.11 mM, the product is a mixture of right triangular bipyramid silver nanoparticles and cubic silver nanoparticles. Among them, right trigonal bipyramidal silver nanoparticles are the main product (the yield of the cubic silver nanoparticles is 80% calculated based on the average calculation of the image counting); from C, it can be seen that the size of the right trigonal bipyramidal silver nanoparticles is mainly distributed in 160-190nm, with an average size of 170nm; from D, it can be seen that the peak position of its LSPR peak is consistent with the results of existing studies on right bipyramidal silver nanoparticles of similar sizes (Wiley, BJ; Im, SH; Li, ZY; McLellan, J.; Siekkinen, A.; Xia, Y. Maneuvering the Surface Plasmon Resonance of Silver Nanostructures through Shape-Controlled Synthesis. J. Phys. Chem. B 2006, 110, 15666-15675.). Comparison with the results of Example 1 proves that the morphology of the main reaction product can be changed from a cube to a right trigonal bipyramid simply by changing the concentration of ferric chloride in the reaction solution, indicating that the camphorquinone-mediated polyol synthesis method is simple and efficient in preparing right trigonal bipyramid silver nanoparticles.
[0072] The silicon substrate was plasma pretreated (180 W, 60 s) by passing air atmosphere (passing rate of 250 mL / min) using a vacuum plasma cleaning machine (40 KHz) to obtain a pretreated silicon substrate;
[0073] Dispersing the right triangular bipyramidal silver nanoparticles in ethanol to obtain a silver nanoparticle dispersion with a concentration of 4.7 mg / mL;
[0074] A drop of the silver nanoparticle dispersion (10 μl) was dropped on the surface of the pretreated silicon substrate (1 cm×1 cm), and then the pretreated silicon substrate was rotated at a speed of 2000 rpm for 10 seconds using a coating machine to evenly disperse and coat the right triangular bipyramid silver nanoparticle dispersion on the surface of the silicon substrate, and then blow-dried to ensure that the volatilization of ethanol can be accelerated at a faster air flow rate, thereby accelerating the deposition and drying of the right triangular bipyramid silver nanoparticles on the surface of the silicon substrate; the spin coating and blowing process were repeated 59 times to obtain a right triangular bipyramid silver nanoparticle surface enhanced Raman substrate.
[0075] Figure 4 The SEM image (A) and Raman scanning image (B) of the right triangular bipyramid silver nanoparticles on the surface of the right triangular bipyramid silver nanoparticle surface enhanced Raman substrate. From A, it can be seen that the amount of silver nanoparticle dispersion added is sufficient, and almost the entire surface of the silicon substrate is evenly covered with silver particles. In order to test the signal uniformity of the prepared SERS substrate, the substrate was immersed in a concentration of 10 -6 SERS analysis was performed on the standard material R6G of M. The surface enhanced Raman substrate of right trigonal bipyramidal silver nanoparticles was used in 20×20μm 2 Raman scanning is performed on an area of Figure 4 As shown in B, the uniformity of the Raman signal has been significantly improved, with 1649 cm -1 The relative standard deviation (RSD) of the peak intensity at 11% was as low as 11%. The entire deposition process of 600 μL of silver nanoparticle dispersion in preparing the SERS substrate only took 600 seconds, indicating that a simple deposition method can effectively prepare a silver nanoparticle SERS substrate with good signal uniformity.
[0076] In order to detect the enhancement effect of the prepared right triangular bipyramidal silver nanoparticle surface enhanced Raman substrate, the Raman test was performed using the standard test object R6G: the SERS substrate prepared by right triangular bipyramidal silver nanoparticles and cubic silver nanoparticles was immersed in 10 mL of different molar concentrations (10 -2 ~10 -6 M) in an ethanol solution of R6G for 2 h and then dried at room temperature. Figure 5 The SEM image (A) of the right triangular bipyramid silver nanoparticles on the surface of the right triangular bipyramid silver nanoparticle surface enhanced Raman substrate and the SERS spectrum (B) of the standard substance on the right triangular bipyramid silver nanoparticles under a 532nm excitation light source when the right triangular bipyramid silver nanoparticle surface enhanced Raman substrate is immersed in different concentrations of standard substances. Figure 5From A in the figure, we can see that the right triangular bipyramidal silver nanoparticles are evenly distributed on the SERS substrate before the test. Figure 5 From the B in the figure, we can see that it is located at 1364cm -1 、1509cm -1 、1649cm -1 The peak at 1574 cm is believed to be derived from CC stretching vibration; -1 The peak at 1181cm is derived from the C=O bond; -1 The peak at 1310 cm is due to the bending vibration of CN and NH, while the peak at 1310 cm -1 、1275cm -1 、1127cm -1 、774cm -1 and 612cm -1 The black line at the bottom of B is the exposed silicon substrate immersed for 10 -4 The Raman spectrum of the R6G after 10 -4 At a higher concentration of R6G, there is still no Raman signal. However, the SERS substrate prepared by adding right triangular bipyramidal silver nanoparticles has a Raman signal even at a lower concentration of 10 -12 The Raman spectrum with distinguishable characteristic peaks can also be seen under R6G of M. This shows that the synthesized right bipyramidal silver nanoparticles can effectively enhance the Raman signal of the sample under test and are suitable for the preparation of SERS enhanced substrates.
[0077] Test Case
[0078] The concentration is 10 -6 20 μL of R6G with a concentration of 0.025 M was added to the cubic silver nanoparticle surface enhanced Raman substrate described in Example 1 and the right triangular bipyramidal silver nanoparticle surface enhanced Raman substrate described in Example 2, respectively. 20 μL of R6G with a concentration of 0.025 M was added to the bare Si substrate treated with plasma to obtain the corresponding parameters to calculate the enhancement factor (EF) of the silver nanoparticle SERS substrate. The calculation formula is shown in Formula 1:
[0079] EF=(I SERS / I Si )×(N Si / N SERS ) Formula 1;
[0080] In formula 1, I SERS Refers to the 1649 cm in the SERS spectrum of R6G -1 The signal intensity at the peak, I Si Refers to the 1649 cm-1 in the Raman spectrum of R6G on a bare silicon substrate.-1 The peak signal intensity at N SERS and N Si They refer to the molecular weight of R6G irradiated by laser on the SERS substrate and the bare silicon substrate during Raman testing. SERS and T Si represents the molecular weight of R6G added to the surface of the SERS substrate and the bare silicon substrate, respectively. The surface of the SERS substrate prepared in Examples 1 and 2 is uniformly covered with silver nanoparticles. Assuming that the detected substance R6G is also uniformly deposited on the SERS substrate and the bare silicon substrate treated with plasma, it can be considered that N Si / N SERS Equal to T Si / T SERS When 20μL 10 -6 When 20 μL of 0.025 M R6G and 20 μL of 0.025 M R6G were dropped on the SERS substrate and the bare silicon substrate, respectively, T SERS and T Si 2×10 -11 and 5×10 -7 The I of the SERS substrate of right bipyramidal silver nanoparticles and cubic silver nanoparticles was measured. SERS They are 3820 and 2912 respectively, such as Figure 7 (R6G(10 -6 The Raman spectra of R6G (0.025 M, 20 μL) on right triangular bipyramidal silver nanoparticle surface-enhanced Raman substrate and cubic silver nanoparticle surface-enhanced Raman substrate and the Raman spectra of R6G (0.025 M, 20 μL) on a bare silicon substrate are shown in Figure 1. Si is 3061. Therefore, it can be calculated that the SERS substrate of right triangular bipyramidal silver nanoparticles and cubic silver nanoparticles is 1649 cm -1 The enhancement factors (EF) at 4 and 2.37×10 4 The Raman enhancement factor of both silver nanoparticles can reach 10 4According to existing studies (Zhang, Q.; Li, W.; Moran, C.; Zeng, J.; Chen, J.; Wen, LP; Xia, Y. Seed-Mediated Synthesis of Ag Nanocubes with Controllable Edge Lengths in the Range of 30-200 nm and 31 Comparison of Their Optical Properties. Journal of the American Chemical Society. 2010, 132, 11372-11378.), silver nanoparticles with a size close to 125 nm have stronger Raman enhancement ability than other sizes, but in this patent, the Raman enhancement factor of the SERS substrate prepared by cubic silver nanoparticles with an average size of 120 nm is 24% lower than that of the SERS substrate prepared by right bipyramidal silver nanoparticles with an average size of 170 nm, indicating that right triangular bipyramidal silver nanoparticles have a stronger Raman enhancement effect than cubic silver nanoparticles.
[0081] Comparative Example 1
[0082] Referring to Example 2, the difference is that the right triangular bipyramid silver nanoparticles are directly added once to the surface of the silicon substrate without coating (spin coating), so as to obtain a right triangular bipyramid silver nanoparticle surface enhanced Raman substrate;
[0083] Figure 3 A in the figure is a top view and a side view of the deposition behavior of silver nanoparticles on the surface of a silicon substrate after plasma pretreatment (wherein, (1) is a side view before the droplet drips, (2) is a side and top view of the liquid just dripping on the substrate surface, (3) is a side view after the droplet is completely spread, (4) is a side and top view of multiple small droplets formed during the liquid drying process, and (5) is a side and top view after the droplet is completely dried), and B is a SEM image of the right triangular bipyramid silver nanoparticles on the surface of the right triangular bipyramid silver nanoparticle surface enhanced Raman substrate. By Figure 3 It can be seen that since plasma treatment can effectively improve the surface energy and hydrophilicity of the silicon substrate, the silver nanoparticles can be evenly diffused and distributed on the surface of the silicon substrate, thereby effectively improving the deposition process and greatly improving the uniformity of the silver nanoparticle deposition. However, there are still many places on the surface of the silicon substrate where no silver nanoparticles are deposited.
[0084] Comparative Example 2
[0085] Referring to Example 2, 0.289 g of camphorquinone (CQ) and 0.155 g of polyvinyl pyrrolidone (PVP) were added to 15 mL of ethylene glycol (EG). After complete dissolution, 0.150 g of AgNO3 was added to the solution and dissolved. Then, 3.1 mL of iron (III) chloride hexahydrate (600 μM in EG solution) was added and stirred vigorously for 4 minutes, at which time the FeCl3 concentration in the reaction solution was 0.11 mM (mmol / L millimoles per liter). The reaction solution was then heated at 120°C and stirred at 300 rpm (revolutions per minute) for 3 hours. After the reaction, the resulting product was washed with ethanol, and after centrifugation at 8000 rpm for several times, the particle precipitation product (right trigonal bipyramidal silver nanoparticles) was redispersed and stored in ethanol;
[0086] Dispersing the right triangular bipyramidal silver nanoparticles in ethanol to obtain a silver nanoparticle dispersion with a concentration of 4.7 mg / mL;
[0087] A drop of the silver nanoparticle dispersion (10 μl) was dropped on the surface (1 cm×1 cm) of the pretreated silicon substrate (the pretreated silicon substrate described in Reference Example 2), and blown dry to ensure that the volatilization of ethanol can be accelerated at a faster air flow rate, thereby accelerating the deposition and drying of right-trigonal bipyramid silver nanoparticles on the surface of the silicon substrate; and a right-trigonal bipyramid silver nanoparticle surface-enhanced Raman substrate was obtained.
[0088] Figure 8 A in the figure is a top view and a side view of the deposition behavior of silver nanoparticles on the surface of the silicon substrate (wherein (1) is a side view before the droplet drips, (2) is a side and top view of the liquid just dripping on the substrate surface, (3) is a side view after the droplet is completely spread, (4) is a side and top view of the liquid forming multiple small droplets during the drying process, and (5) is a side and top view after the droplet is completely dried). Figure 8 B in FIG. 1 is a SEM image of 10 microliters of silver nanoparticle dispersion (4.7 mg / mL) added dropwise to the surface of the silicon substrate. Figure 8 It can be seen that when the silicon substrate used to deposit the right trigonal bipyramidal silver nanoparticle dispersion has not been plasma treated, when the silver nanoparticle dispersion is added to the substrate surface, the liquid cannot diffuse quickly on the substrate surface, resulting in uneven particle aggregation after the solvent evaporates; this is not conducive to preparing a SERS substrate with uniform test signals.
[0089] Comparative Example 3
[0090] Refer to Comparative Example 2, the difference is that after taking a drop of the silver nanoparticle dispersion (10 μl) and dropping it on the pretreated silicon substrate surface (1 cm×1 cm) described in Reference Example 2, a spin coating process is also included. The spin coating conditions are to use a coating machine to rotate the pretreated silicon substrate at a speed of 2000 rpm for 10 seconds to obtain a right trigonal bipyramidal silver nanoparticle surface enhanced Raman substrate.
[0091] Comparative Example 4
[0092] Refer to Comparative Example 3, the difference is that after the spin coating and blow drying are completed, the process of dripping, spin coating and blow drying is repeated 9 times to obtain a right trigonal bipyramidal silver nanoparticle surface enhanced Raman substrate.
[0093] Comparative Example 5
[0094] Refer to Comparative Example 4, the difference is that the number of repetitions is 29 times, and a right trigonal bipyramidal silver nanoparticle surface enhanced Raman substrate is obtained.
[0095] Comparative Example 6
[0096] Refer to Comparative Example 4, the difference is that the number of repetitions is 49 times, and a right trigonal bipyramidal silver nanoparticle surface enhanced Raman substrate is obtained.
[0097] Fig. 9 The SEM images of the right triangular bipyramidal silver nanoparticle surface enhanced Raman substrates described in Comparative Examples 3 to 6, wherein A is Comparative Example 3, B is Comparative Example 4, C is Comparative Example 5, and D is Comparative Example 6. Fig. 9 It can be seen that the sample with a smaller amount of silver nanoparticle dispersion added has loose particle distribution and more exposed track plate areas;
[0098] Fig.10 For R6G(10 -6 M, 20 μL) Raman surface scanning image of the surface enhanced Raman substrate of the right triangular bipyramidal silver nanoparticles described in Comparative Examples 4 and 5 (selected Raman spectrum 1649 cm -1 The peak intensity is used to draw a heat map, and the Raman scan is selected to be 20×20μm 2 ), wherein A is comparative example 4, and B is comparative example 5; Fig.10 It can be seen that the relative standard deviations of the signals of the particle dispersions used were 79% and 26% respectively when the particle dispersions were used in amounts of 100 μL and 300 μL, both lower than the 11% shown in the more optimal condition (600 μL in Example 2). Therefore, in order to prepare a dense and uniform particle-enhanced SERS substrate, the particle dispersion used in an amount higher than 500 μL (4.7 mg / mL) has a more excellent signal uniformity.
[0099] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a silver nanoparticle surface enhanced Raman substrate, characterized in that: The following steps are involved: After the surface of the silicon substrate is subjected to plasma pretreatment, a silver nanoparticle dispersion is coated to obtain the surface enhanced Raman substrate; The silver nanoparticles in the silver nanoparticle dispersion include right trigonal bipyramidal silver nanoparticles and / or cubic silver nanoparticles.
2. The preparation method according to claim 1, characterized in that The frequency of the plasma pretreatment is 9KHz to 14MHz, the power is 10 to 1200W, and the time is 5 to 600s; The plasma pretreatment is carried out under the condition of air flow, and the air flow rate is 50-500 mL / min.
3. The preparation method according to claim 1, characterized in that: The solvent in the silver nanoparticle dispersion includes one or more of ethanol, methanol and isopropanol; The concentration of the silver nanoparticle dispersion is 0.5-20 mg / mL.
4. The preparation method according to claim 1 or 3, characterized in that: The coating amount of the silver nanoparticle dispersion is (10-1000) μL / (1-2) cm 2 .
5. The preparation method according to claim 4, characterized in that: The method for preparing cubic silver nanoparticles in the silver nanoparticle dispersion comprises the following steps: The quinone compound, poly (N-vinyl pyrrolidone), a silver source, an additive and a polyol compound are mixed and then subjected to a solvothermal reaction to obtain the cubic silver nanoparticles; The amount ratio of the silver source, quinone compound, poly N-vinyl pyrrolidone, additive and polyol compound is (8.83×10 -4 ~1.18×10 -2 )mol:(1.80×10 -3 ~2.41×10 -2 )mol:(1.80×10 -3 ~1.80×10 -2 )mol:(2.22×10 -4 ~5.55×10 -3 )mol:1L.
6. The preparation method according to claim 5, characterized in that: The silver source is a soluble silver salt; The additive includes one or more of sodium chloride, potassium chloride, ferric chloride, copper chloride, hexadecyltrimethylammonium chloride, sodium bromide, potassium bromide and hexadecyltrimethylammonium bromide.
7. The preparation scheme according to claim 5, characterized in that: The quinone compound includes one or more of camphorquinone, benzoquinone, naphthoquinone, anthraquinone and phenanthrenequinone; The polyol compound includes one or more of ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, neopentyl glycol, diethylene glycol and glycerol.
8. The preparation method according to claim 1, characterized in that: The coating method is spin coating, and the number of spin coating is ≥1 times.
9. The preparation method according to claim 8, characterized in that: The spin coating was performed 6 times.
10. The preparation method according to claim 8 or 9, characterized in that: The rotation speed of each spin coating is 1400-3600 rpm, and the time is 5-120 s.