Method for detecting two-dimensional material defects
By depositing rare earth quantum dots on the surface of two-dimensional materials and performing photoluminescence spectral surface scanning, the complex sample preparation, low spatial resolution and irreversible damage of two-dimensional material defect detection in the prior art is solved, and fast and lossless Large-scale defect detection significantly improves detection speed and sample integrity.
Patent Information
- Application Number
- CN202310531514.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-12
AI Technical Summary
The existing two-dimensional material defect characterization methods have the problems of complex sample preparation, low spatial resolution, or irreversible damage, making it difficult to achieve fast and lossless large-scale defect detection.
By placing rare earth compound powder and two-dimensional material samples in a tube furnace, evaporate to form rare earth quantum dots, and photoluminescence spectroscopy surface sweep test is performed using a microfluorescence spectrometer to qualitatively determine the defect position and density, and remove the quantum dots after annealing to recover the sample.
It realizes fast and lossless large-area two-dimensional material defect characterization, with a detection speed of 1,000,000 times, is easy to operate, and the samples are lossless, and is suitable for various two-dimensional materials.
Smart Images

Figure CN118937354A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of materials. Specifically, the present invention relates to a method for detecting defects in two-dimensional materials. Background Art
[0002] In the process of preparing, doping, and transferring two-dimensional materials, some defects are inevitably introduced into the material lattice, such as point defects such as atomic vacancies, or line defects such as grain boundaries and dislocations. The existence of these defects greatly affects the physical properties of two-dimensional materials: on the one hand, lattice defects increase electron and phonon scattering, reduce intrinsic properties such as carrier mobility and tensile strength, and hinder the application of material devices; on the other hand, defect engineering can effectively regulate the band gap, thermal conductivity, electrical transmission and other properties of two-dimensional materials, thereby expanding the device application prospects of two-dimensional materials. Therefore, defect characterization of two-dimensional materials is crucial for the development of high-end two-dimensional device applications.
[0003] At present, commonly used methods for characterizing defects in two-dimensional materials include scanning transmission electron microscopy (STEM), Raman and photoluminescence spectroscopy (PL), chemical etching, etc.
[0004] STEM can obtain atomic-level resolution images, but it has problems such as complex sample preparation process and small observation area, and cannot realize the characterization of large-size samples.
[0005] Spectroscopic methods are simple to operate, but their spatial resolution is usually on the micrometer level, not the nanometer level, which results in very low accuracy and makes it difficult to characterize isolated point defects.
[0006] Chemical etching such as oxygen and water vapor can visualize point defects, but it will cause irreversible damage to the sample and reduce sample performance.
[0007] In view of this, there is an urgent need to develop a simple, fast, large-scale and non-destructive method for characterizing defects in two-dimensional materials to promote the application of two-dimensional material devices. Summary of the invention
[0008] The object of the present invention is to provide a method for detecting defects in two-dimensional materials, which is simple, fast and non-destructive to the two-dimensional materials.
[0009] The above-mentioned object of the present invention is achieved through the following technical solutions.
[0010] The present invention provides a method for detecting defects in two-dimensional materials, which comprises the following steps:
[0011] (1) placing a two-dimensional material sample to be tested and a rare earth compound powder in a tube furnace, wherein the rare earth compound powder is located in an upstream area of the tube furnace, and the two-dimensional material sample is located in a downstream area of the tube furnace;
[0012] (2) introducing a protective gas to control the pressure in the tube furnace, and controlling the temperature of the tube furnace so that the rare earth compound powder evaporates and diffuses, so as to deposit rare earth quantum dots on the two-dimensional material sample;
[0013] (3) After the rare earth quantum dots are formed, a photoluminescence spectrum scanning (PL mapping) test is performed on the surface of the two-dimensional material sample using a microfluorescence spectrometer;
[0014] (4) Determine the defect position on the surface of the two-dimensional material sample based on the position and signal intensity of the bright spot in the photoluminescence spectrum scanning image, and qualitatively determine the defect density;
[0015] (5) Optionally, the rare earth quantum dots adsorbed on the surface of the two-dimensional material sample are removed by annealing.
[0016] The inventors of the present application have found that the luminescence signal can be enhanced by adsorbing rare earth compounds on the surface of two-dimensional materials. Without wishing to be bound by theory, the present invention uses PLmapping images after the selective adsorption of rare earth quantum dots on the surface of two-dimensional materials to visualize the defect positions and defect densities on the surface of two-dimensional materials. Compared with the perfect lattice, the defects have higher adsorption energy and are more likely to adsorb rare earth quantum dots. Therefore, the position of sample defects can be characterized by the position of the luminescent bright spots in the PL mapping image. At the same time, the higher the sample defect density, the more rare earth quantum dots are adsorbed per unit area. Therefore, the number of defects per unit area can be obtained by the luminescence intensity of the bright spots in the PL mapping image, thereby qualitatively determining the defect density of the sample. In the present invention, the imaging basis of PL mapping is the signal intensity of the characteristic luminescence peak of the rare earth quantum dots.
[0017] The inventors of this application have also found that after characterization, the rare earth quantum dots adsorbed on the surface of the two-dimensional material can be evaporated and removed by annealing, restoring the sample with a clean surface, which can then be further used for other characterizations or device manufacturing. The method proposed in this invention can quickly and non-destructively characterize the defect position and defect density of large-area two-dimensional materials through very simple operations.
[0018] Preferably, in the method of the present invention, the rare earth compound is selected from one or more of rare earth oxides and rare earth chlorides.
[0019] Preferably, in the method of the present invention, the rare earth compound is selected from ErCl 3 、TbCl 3 , GdCl 3 , DyCl 3 、Eu 2 O 3 and CeO 2One or more of the .
[0020] Preferably, in the method described in the present invention, the two-dimensional material sample is selected from graphene, hexagonal boron nitride (hBN) or transition metal dichalcogenides (TMDCs).
[0021] Preferably, in the method described in the present invention, the amount of the rare earth compound and the two-dimensional material sample in step (1) is 0.5-50 mg of the rare earth compound per square centimeter of the two-dimensional material sample.
[0022] Preferably, in the method of the present invention, the protective gas is selected from H 2 , one or more of argon, nitrogen, helium and neon.
[0023] Preferably, in the method of the present invention, the pressure in step (2) is 0.1-10 5 Pa.
[0024] Preferably, in the method of the present invention, the temperature of the tube furnace in step (2) is controlled under the following conditions: the temperature of the upstream zone of the tube furnace is controlled to 600-900°C, and the temperature of the downstream zone is controlled to 20-600°C.
[0025] Preferably, in the method of the present invention, the deposition time for forming rare earth quantum dots in step (2) is 10-500 minutes.
[0026] Preferably, in the method described in the present invention, the laser of the microfluorescence spectrometer is a common commercial laser with a wavelength below 700 nm (including 375, 405, 445, 460, 488, 514, 532, 577, 633, 656 nm), the laser power is 0.5-50 mW, the single-point integration time is 0.1-30 s, and the moving step length of the photoluminescence spectrum scan is 0.1-2 μm.
[0027] Preferably, in the method of the present invention, the annealing treatment in step (5) is performed at 600-900° C. for 1-10 h.
[0028] In a specific embodiment of the present invention, the rare earth compound powder may be 15-30 mg ErCl 3 powder.
[0029] In a specific embodiment of the present invention, 5 sccm H is introduced into the tube furnace. 2 and 40 sccm Ar gas.
[0030] The present invention has the following beneficial effects:
[0031] 1. The present invention is a method for quickly characterizing the defect position and defect density of two-dimensional materials by optical detection means;
[0032] 2. The present invention utilizes a CVD tube furnace to perform rare earth quantum dot evaporation treatment on the sample to be tested, which is easy to operate.
[0033] 3. The present invention can simply and quickly characterize large-scale defects under a microscopic fluorescence spectrometer. For example, a scanning transmission electron microscope (STEM) in the prior art can detect an area of 10×10 nm every 40 seconds. 2 In contrast, the detection method of the present invention can detect an area of 10×10μm every 40 seconds. 2 The detection speed of 2D materials is 1,000,000 times that of STEM detection methods.
[0034] 4. The present invention can remove the rare earth quantum dots adsorbed on the sample surface through annealing treatment, restore the clean surface of the sample, and achieve non-destructive characterization.
[0035] 5. The operations involved in the present invention are relatively simple, and the required instruments (high-temperature tube furnace, microscopic fluorescence spectrometer) are relatively common, saving time and effort. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The embodiments of the present invention are described in detail below with reference to the accompanying drawings, wherein:
[0037] Figure 1 It is a light microscope photo of the graphene sample of Example 1 of the present invention and the corresponding PL mapping result after the graphene sample is deposited with Er quantum dots; wherein Figure 1 a is a light microscope photo of the graphene sample; Figure 1 b is the corresponding PL mapping result after Er quantum dots were deposited on the graphene sample. The imaging is based on the PL characteristic peak of Er (672nm).
[0038] Figure 2 The PL mapping results of the graphene sample deposited with Er quantum dots after annealing in Example 1 of the present invention and the Raman spectrum curve comparison of the graphene sample before and after annealing are shown; Figure 2 a is the PL mapping result of the graphene sample deposited with Er quantum dots after annealing, and the imaging is based on the PL characteristic peak of Er (672nm); Figure 2 b is the comparison of Raman spectrum curves of graphene samples before and after annealing.
[0039] Figure 3 The optical microscope photo of the hBN sample of Example 2 of the present invention and the corresponding PL mapping result after Er quantum dots were deposited on the hBN sample; wherein Figure 3a is a light microscope photo of the hBN sample; Figure 3 b is the corresponding PL mapping result after Er quantum dots were deposited on the hBN sample. The imaging is based on the PL characteristic peak of Er (672nm).
[0040] Figure 4 The optical microscope photo of the graphene sample of Example 3 of the present invention and the corresponding PL mapping results after the graphene sample is deposited with Dy quantum dots and after annealing to remove the Dy quantum dots; wherein Figure 4 a is a light microscope photo of the graphene sample; Figure 4 b is the corresponding PL mapping result after the graphene sample is deposited with Dy quantum dots. The imaging is based on the PL characteristic peak of Dy (480nm); Figure 4 c is the PL mapping result of the graphene sample deposited with Dy quantum dots after annealing, and the imaging is based on the PL characteristic peak of Dy (480nm).
[0041] Figure 5 WS of Embodiment 4 of the present invention 2 Light microscopy photos of samples and WS 2 The corresponding PL mapping results of the sample after Tb quantum dots were deposited and after annealing to remove Tb quantum dots; Figure 5 a is WS 2 Light microscopic photograph of the sample; Figure 5 b is WS 2 The corresponding PL mapping results after the sample was deposited with Tb quantum dots. The imaging was based on the PL characteristic peak of Tb (489nm). Figure 5 c is WS with Tb quantum dots deposited 2 PL mapping results after sample annealing. The imaging is based on the PL characteristic peak of Tb (489nm).
[0042] Figure 6 The Raman mapping results and PL mapping results of the graphene sample of Example 1 of the present invention before the deposition of Er quantum dots are shown; Figure 6 a is the Raman mapping result of the graphene sample before the deposition of Er quantum dots. The imaging is based on the Raman defect peak of graphene (1345cm -1 ); Figure 6 b is the PLmapping result of the graphene sample before depositing Er quantum dots. The imaging is based on the PL characteristic peak of Er (672nm).
[0043] Figure 7 This is the PL mapping result of hBN before depositing Er quantum dots in Example 2 of the present invention. The imaging is based on the PL characteristic peak of Er (672 nm).
[0044] Figure 8 WS of Embodiment 4 of the present invention 2 PL mapping results before deposition of Tb quantum dots. The imaging is based on the PL characteristic peak of Tb (489nm). DETAILED DESCRIPTION
[0045] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, but not for limiting the scope of the present invention.
[0046] Example 1
[0047] (1) Mechanical peeling at 1 cm 2 Si / SiO 2 Graphene sample on substrate with 25 mg ErCl 3 The powders are placed together in a high temperature tube furnace;
[0048] (2) Maintain a low pressure of 1000 Pa in the tube and introduce 5 sccm H 2 and 40 sccm Ar gas, set the upstream heating temperature to 800 °C, the downstream heating temperature to 300 °C, and the deposition time to 100 min;
[0049] (3) After the deposition is completed, a 514 nm laser light source is used to perform PL mapping on the surface of the sample to be tested. The laser power is 8 mW, the single point integration time is 4 s, the moving step is 1 μm, and the imaging is based on the luminescence peak signal intensity near 672 nm.
[0050] (4) According to the position and signal intensity of the bright spots in the PL mapping image, the defect position on the surface of the sample to be tested is determined and the defect density is qualitatively determined.
[0051] (5) Finally, the Er quantum dots adsorbed on the sample surface were removed by annealing at 800°C for 3 h.
[0052] Figure 1 It is a light microscope photo of the graphene sample of Example 1 of the present invention and the corresponding PL mapping result after the graphene sample is deposited with Er quantum dots; wherein Figure 1 a is a light microscope photo of the graphene sample; Figure 1 b is the corresponding PL mapping result after Er quantum dots are deposited on the graphene sample. The imaging is based on the PL characteristic peak of Er (672nm). The defects of the graphene sample have higher adsorption energy and are more likely to adsorb Er quantum dots. Therefore, the location of the sample defects can be determined by the location of the sporadic bright spots in the PL mapping image. Figure 1b shows that the defect density of the graphene sample of Example 1 is low and the sample quality is high.
[0053] Figure 2 The PL mapping results of the graphene sample deposited with Er quantum dots after annealing in Example 1 of the present invention and the Raman spectrum curve comparison of the graphene sample before and after annealing are shown; Figure 2 a is the PL mapping result of the graphene sample deposited with Er quantum dots after annealing, and the imaging is based on the PL characteristic peak of Er (672nm); Figure 2 b is the comparison of Raman spectrum curves of graphene samples before and after annealing. Figure 2 a shows that no Er luminescence signal is detected on the surface of the graphene sample after annealing, indicating that the adsorbed Er quantum dots have been completely removed; at the same time, Figure 2 b shows that the Raman peak of the graphene sample after annealing does not have a D peak, indicating that the entire characterization process is non-destructive to graphene and the sample can be used for further characterization or device manufacturing.
[0054] Example 2
[0055] (1) Mechanical peeling at 1 cm 2 Si / SiO 2 hBN sample on substrate with 20 mg ErCl 3 The powders are placed together in a high temperature tube furnace;
[0056] (2) Maintain a low pressure of 200 Pa in the tube and introduce 5 sccm H 2 and 40 sccm Ar gas, set the upstream heating temperature to 750 °C, the downstream heating temperature to 200 °C, and the deposition time to 30 min;
[0057] (3) After the deposition is completed, a 532nm laser light source is used to perform PL mapping on the surface of the sample to be tested. The laser power is 10mW, the single point integration time is 5s, the moving step is 1μm, and the imaging is based on the luminescence peak signal intensity near 672nm;
[0058] (4) According to the position and signal intensity of the bright spots in the PL mapping image, the defect position on the surface of the sample to be tested is determined and the defect density is qualitatively determined.
[0059] (5) Finally, the Er quantum dots adsorbed on the sample surface were removed by annealing at 750°C for 5 h.
[0060] Figure 3 The optical microscope photo of the hBN sample of Example 2 of the present invention and the corresponding PL mapping result after Er quantum dots were deposited on the hBN sample; wherein Figure 3 a is a light microscope photo of the hBN sample; Figure 3b is the corresponding PL mapping result after Er quantum dots are deposited on the hBN sample. The imaging is based on the PL characteristic peak of Er (672nm). The surface defects of the few-layer hBN sample have higher adsorption energy and are more likely to adsorb Er quantum dots. Therefore, the location of the sample defects can be determined by the location of the fewer bright spots in the PL mapping image. Figure 3 b shows that the defect density is higher than that of the graphene sample, and the sample quality is slightly poor. After annealing, no Er luminescence signal was detected on the surface of the hBN sample, indicating that the adsorbed Er quantum dots have been removed completely, and the sample can be used for further characterization or device manufacturing.
[0061] Example 3
[0062] (1) Mechanical peeling at 1 cm 2 Si / SiO 2 Graphene sample on substrate with 20 mg DyCl 3 The powders are placed together in a high temperature tube furnace;
[0063] (2) Maintaining normal pressure in the tube, introduce 5 sccm H 2 and 40 sccm Ar gas, set the upstream heating temperature to 750°C, the downstream heating temperature to 300°C, and the deposition time to 300 min;
[0064] (3) After the deposition is completed, a 375 nm laser light source is used to perform PL mapping on the surface of the sample to be tested. The laser power is 8 mW, the single point integration time is 3 s, the moving step is 1 μm, and the imaging is based on the luminescence peak signal intensity near 480 nm.
[0065] (4) According to the position and signal intensity of the bright spots in the PL mapping image, the defect position on the surface of the sample to be tested is determined and the defect density is qualitatively determined.
[0066] (5) Finally, the Dy quantum dots adsorbed on the sample surface were removed by annealing at 800°C for 2 h.
[0067] Figure 4 The optical microscope photo of the graphene sample of Example 3 of the present invention and the corresponding PL mapping results after the graphene sample is deposited with Dy quantum dots and after annealing to remove the Dy quantum dots; wherein Figure 4 a is a light microscope photo of the graphene sample; Figure 4 b is the corresponding PL mapping result after the graphene sample is deposited with Dy quantum dots. The imaging is based on the PL characteristic peak of Dy (480nm); Figure 4c is the PL mapping result of the graphene sample with Dy quantum dots deposited after annealing. The imaging is based on the PL characteristic peak of Dy (480nm). The defects of the graphene sample have higher adsorption energy and are more likely to adsorb Dy quantum dots. Therefore, the location of the sample defects can be determined by the location of the sporadic bright spots in the PLmapping image. Figure 4 b shows that the defect density of the graphene sample of Example 3 is low and the sample quality is high. Figure 4 c shows that no Dy luminescence signal is detected on the surface of the graphene sample after annealing, indicating that the adsorbed Dy quantum dots have been completely removed and the sample can be used for further characterization or device manufacturing.
[0068] Example 4
[0069] (1) Mechanical peeling at 1 cm 2 Si / SiO 2 WS on substrate 2 Sample and 15 mg TbCl 3 The powders are placed together in a high temperature tube furnace;
[0070] (2) Maintain a low pressure of 20 Pa in the tube and introduce 5 sccm H 2 and 40 sccm Ar gas, set the upstream heating temperature to 600 °C, the downstream heating temperature to 50 °C, and the deposition time to 60 min;
[0071] (3) After the deposition is completed, a 375 nm laser light source is used to perform PL mapping on the surface of the sample to be tested. The laser power is 5 mW, the single point integration time is 2 s, the moving step is 1 μm, and the imaging is based on the luminescence peak signal intensity near 489 nm.
[0072] (4) According to the position and signal intensity of the bright spots in the PL mapping image, the defect position on the surface of the sample to be tested is determined and the defect density is qualitatively determined.
[0073] (5) Finally, the Tb quantum dots adsorbed on the sample surface were removed by annealing treatment at 650°C for 6 h.
[0074] Figure 5 WS of Embodiment 4 of the present invention 2 Light microscopy photos of samples and WS 2 The corresponding PL mapping results of the sample after Tb quantum dots were deposited and after annealing to remove Tb quantum dots; Figure 5 a is WS 2 Light microscopic photograph of the sample; Figure 5 b is WS 2 The corresponding PL mapping results after the sample was deposited with Tb quantum dots. The imaging was based on the PL characteristic peak of Tb (489nm). Figure 5 c is WS with Tb quantum dots deposited 2 PL mapping results of the sample after annealing, imaging is based on the PL characteristic peak of Tb (489nm). 2 The defects on the sample surface have higher adsorption energy and are more likely to adsorb Tb quantum dots. Therefore, the location of the sample defects can be determined by the location of more bright spots in the PL mapping image. Figure 5 b The defect density is high and the sample quality is poor. Figure 5 c shows WS after annealing 2 No luminescent signal of Tb was detected on the sample surface, indicating that the adsorbed Tb quantum dots had been completely removed.
[0075] Comparative Example 1
[0076] (1) A Raman mapping test was performed on the surface of the graphene sample without Er quantum dots deposited in Example 1 of the present invention using a 514 nm laser light source. The laser power was 8 mW, the single point integration time was 4 s, the moving step was 1 μm, and the imaging basis was 1345 cm -1 The signal strength of the nearby Raman peak;
[0077] (2) Using a 514 nm laser light source, a PL mapping test was performed on the surface of the graphene sample without Er quantum dots deposited in Example 1 of the present invention. The laser power was 8 mW, the single point integration time was 4 s, the moving step was 1 μm, and the imaging was based on the luminescence peak signal intensity near 672 nm.
[0078] Figure 6 The Raman mapping results and PL mapping results of the graphene sample of Example 1 of the present invention before the deposition of Er quantum dots are shown; Figure 6 a is the Raman mapping result of the graphene sample before the deposition of Er quantum dots. The imaging is based on the Raman defect peak of graphene (1345cm -1 ); Figure 6 b is the PLmapping result of the graphene sample before the deposition of Er quantum dots. The imaging is based on the PL characteristic peak of Er (672nm). Before the deposition of Er quantum dots, there are no signal points in the Ramanmapping and PL mapping of the graphene sample, and the defect position on the sample surface cannot be characterized. In contrast, it shows that the deposition of Er quantum dots can effectively characterize the defect position on the sample surface and qualitatively determine the quality of the sample.
[0079] Comparative Example 2
[0080] (1) A 532 nm laser light source was used to perform PL mapping test on the surface of the hBN sample without Er quantum dots deposited in Example 2 of the present invention. The laser power was 10 mW, the single point integration time was 5 s, the moving step was 1 μm, and the imaging was based on the luminescence peak signal intensity near 672 nm.
[0081] Figure 7 This is the PL mapping result of hBN before depositing Er quantum dots in Example 2 of the present invention. The imaging is based on the PL characteristic peak of Er (672nm). Before depositing Er quantum dots, the PL mapping of the hBN sample has no signal points, and the defect position on the sample surface cannot be characterized. In addition, the Raman spectrum of hBN has no defect peaks, and the quality of the sample cannot be judged. In contrast, it shows that the defect position on the sample surface can be effectively characterized by depositing Er quantum dots, and the quality of the sample can be qualitatively determined.
[0082] Comparative Example 3
[0083] (1) Using a 375 nm laser light source, WS without Tb quantum dots deposited in Example 4 of the present invention was 2 PL mapping test was carried out on the sample surface with a laser power of 5 mW, a single-point integration time of 2 s, a moving step of 1 μm, and imaging based on the luminescence peak signal intensity near 489 nm.
[0084] Figure 8 WS of Embodiment 4 of the present invention 2 PL mapping results before depositing Tb quantum dots. The imaging is based on the PL characteristic peak of Tb (489nm). 2 The PL mapping of the sample did not show any signal points and could not characterize the defect locations on the sample surface. 2 The Raman spectrum of the sample has no defect peaks, so it is impossible to judge the quality of the sample. In contrast, it shows that the deposition of Tb quantum dots can effectively characterize the defect position on the sample surface and qualitatively determine the quality of the sample.
[0085] It can be seen from the above examples that when rare earth quantum dots are deposited on the surface of different types of two-dimensional materials, the position and distribution density of the bright spots in the PL mapping image can be used to characterize the defect position on the sample surface and qualitatively determine the quality of the sample. After annealing, no luminescent signal of rare earth quantum dots is detected on the sample surface, indicating that the adsorbed rare earth quantum dots have been removed completely, and the sample can be used for further characterization or device manufacturing.
Claims
1. A method for detecting defects in two-dimensional materials, wherein The following steps are involved: (1) placing a two-dimensional material sample to be tested and a rare earth compound powder in a tube furnace, wherein the rare earth compound powder is located in an upstream area of the tube furnace, and the two-dimensional material sample is located in a downstream area of the tube furnace; (2) introducing a protective gas to control the pressure in the tube furnace, and controlling the temperature of the tube furnace so that the rare earth compound powder evaporates and diffuses, so as to deposit rare earth quantum dots on the two-dimensional material sample; (3) After the rare earth quantum dots are formed, a photoluminescence spectrum scanning test is performed on the surface of the two-dimensional material sample using a microfluorescence spectrometer; (4) Determine the defect position on the surface of the two-dimensional material sample based on the position and signal intensity of the bright spot in the photoluminescence spectrum scanning image, and qualitatively determine the defect density; (5) Optionally, the rare earth quantum dots adsorbed on the surface of the two-dimensional material sample are removed by annealing.
2. The method according to claim 1, in, The rare earth compound is selected from one or more of rare earth oxides and rare earth chlorides.
3. The method according to claim 1, in, The rare earth compound is selected from ErCl 3 、TbCl 3 , GdCl 3 , DyCl 3 、Eu 2 O 3 and CeO 2 One or more of the following; Preferably, the two-dimensional material sample is selected from graphene, hexagonal boron nitride or transition metal chalcogenide.
4. The method according to claim 1, in, The amount of the rare earth compound and the two-dimensional material sample in step (1) is 0.5-50 mg of the rare earth compound per square centimeter of the two-dimensional material sample.
5. The method according to claim 1, in, The protective gas is selected from H 2 , one or more of argon, nitrogen, helium and neon.
6. The method according to claim 1, in, The pressure in step (2) is 0.1-10 5 Pa.
7. The method according to claim 1, in, The temperature of the tube furnace in step (2) is controlled under the following conditions: the temperature of the upstream zone of the tube furnace is controlled to be 600-900°C, and the temperature of the downstream zone is controlled to be 20-600°C.
8. The method according to claim 1, in, The deposition time for forming rare earth quantum dots in step (2) is 10-500 minutes.
9. The method according to claim 1, in, The laser power of the microfluorescence spectrometer is 0.5-50 mW, the single-point integration time is 0.1-30 s, and the moving step length of the photoluminescence spectrum surface scan is 0.1-2 μm.
10. The method according to claim 1, in, The annealing treatment in step (5) is performed at 600-900° C. for 1-10 h.