Preparation method of Sn-Bi-Ag-based welding spot EBSD sample
Through the combination of mechanical pre-polishing and ion beam treatment, the problem of uniform etching in the preparation of EBSD samples of Sn-57Bi-1Ag based solder joints was solved, which improved the sample surface quality and resolution rate, reduced the preparation cost and difficulty, and was suitable for research Service reliability of solder joints in high temperature environments.
Patent Information
- Application Number
- CN202411110126.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
AI Technical Summary
The existing Sn-57Bi-1Ag-based solder joint EBSD sample preparation method is difficult to etch evenly, resulting in uneven surface of the sample, affecting the quality of EBSD data, and is cost-effective, long periods and unstable effect.
Using a combination of mechanical pre-polishing and ion beam treatment, the surface finish and flatness of the sample are first improved by mechanical pre-polishing, and then thinned the stress layer and amorphous layer through ion beam treatment to ensure the surface quality of the sample. Specific steps include sandpaper polishing, diamond polishing and ion beam processing, controlling the energy and bombardment time of the ion beam.
The preparation of high-quality EBSD samples was achieved. The resolution rate of samples without aging reached more than 92%. After 240 hours of aging at 110°C, the resolution rate of more than 70% was maintained, which reduced the preparation difficulty and cost, significantly improved the preparation efficiency and Success rate.
Smart Images

Figure CN118937372A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of Sn-Bi-Ag based solder joint organization and orientation characterization, and in particular relates to a method for preparing a Sn-Bi-Ag based solder joint EBSD sample. Background Art
[0002] Sn-57Bi-1Ag solder has a low melting point, excellent creep resistance, wettability and conductivity, and has a very broad application prospect in the field of low-temperature electronic packaging. However, the anisotropy of the β-Sn phase and the brittleness of the Bi phase seriously affect the service reliability of Sn-57Bi-1Ag solder in high temperature environments. The method of refining the grain size of the solder matrix by doping nanoparticles is considered to be an effective solution to this problem. Therefore, it is of great significance to detect and characterize the microstructure of Sn-57Bi-1Ag-based solder joints during the aging process.
[0003] Electron backscatter diffraction (EBSD) technology is based on scanning electron microscope. It can quickly and accurately detect crystal orientation, grain size, phase interface, plastic strain and recrystallization. It is a powerful tool for studying solder microstructure and crystallographic characteristics. The service reliability of solder joints is closely related to their microstructure. Therefore, it is of great significance to study the service reliability of solder joints by detecting the changes in the micromorphology of solder joints during aging through in-situ EBSD technology.
[0004] EBSD testing requires that the surface of the sample to be tested is smooth and free of residual stress. At the same time, the size of the sample to be tested should not be too thick and the conductivity should be good. The quality of sample preparation and ensuring that the sample surface is clean and free of contamination during the aging process determine the quality of in-situ EBSD data collection.
[0005] At present, the preparation method of Sn-57Bi-1Ag-based solder joint EBSD sample is to first perform mechanical grinding and polishing, and then perform vibration polishing or electrolytic polishing. However, due to the presence of doped nanoparticles in Sn-57Bi-1Ag-based solder, the hardness of the nanoparticles is different from that of the base material, resulting in different etching speeds and difficulty in uniform etching, which causes the sample surface to be bumpy and has an adverse effect on the EBSD collection quality. Therefore, how to prepare high-quality Sn-Bi-Ag-based solder joint EBSD samples has become a technical problem that needs to be solved in this field. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing Sn-Bi-Ag based solder joint EBSD samples. The preparation method provided by the present invention can prepare high-quality EBSD samples.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing a Sn-Bi-Ag based solder joint EBSD sample, comprising the following steps:
[0009] The Sn-Bi-Ag based solder joints were subjected to mechanical pre-polishing and ion beam treatment in sequence to obtain Sn-Bi-Ag based solder joint EBSD samples;
[0010] The energy of the ion beam treatment is 2000 eV; the bombardment time of the ion beam treatment is 150 to 200 s.
[0011] Preferably, the method for preparing the Sn-Bi-Ag based solder joint comprises cutting a Sn-Bi-Ag based solder joint and then inlaying it with a denture base resin.
[0012] Preferably, the Sn-Bi-Ag based welded joint comprises one of a Cu / Sn-57Bi-1Ag / Cu joint and a Cu / Sn-57Bi-1Ag-0.5CeO2 / Cu joint.
[0013] Preferably, before the mechanical pre-polishing, the Sn-Bi-Ag based solder joints are sanded, cleaned and dried in sequence.
[0014] Preferably, the sandpaper polishing is performed using 240#, 600#, 1000#, 1500#, 2000#, 3000# and 5000# silicon carbide sandpaper in sequence.
[0015] Preferably, the mechanical pre-polishing is performed by sequentially using diamond polishing agents with particle sizes of 2.5 μm, 1.0 μm and 0.5 μm.
[0016] Preferably, the mechanical pre-polishing time using diamond polishing agents with particle sizes of 2.5 μm and 1.0 μm is independently 3 to 5 minutes.
[0017] Preferably, the mechanical pre-polishing time using a diamond polishing agent with a particle size of 0.5 μm is 3 to 6 minutes.
[0018] Preferably, the bombardment time of the ion beam treatment is 180 s.
[0019] Preferably, the vacuum degree of the ion beam treatment is less than 1×10 -8 MPa.
[0020] The present invention provides a method for preparing an EBSD sample of a Sn-Bi-Ag-based solder joint, comprising the following steps: mechanically pre-polishing and ion beam treatment are sequentially performed on the Sn-Bi-Ag-based solder joint to obtain an EBSD sample of the Sn-Bi-Ag-based solder joint; the energy of the ion beam treatment is 2000eV; and the bombardment time of the ion beam treatment is 150 to 200s. The present invention first performs mechanical pre-polishing to improve the surface quality, improve the surface finish and flatness of the sample, and then performs ion beam treatment. The sample is bombarded with an ion beam, which can make the generated stress layer and amorphous layer very thin, thereby avoiding the misleading of experimental data due to the sample preparation method; by limiting the energy and bombardment time of the ion beam treatment, the stress layer and amorphous layer can be further thinned, and the surface quality of the sample can be further improved. Experimental results show that the resolution rate of the EBSD sample without aging treatment prepared by the preparation method provided by the present invention is above 92%, and the resolution rate of the sample can still be guaranteed to be above 70% after the sample is aged at 110°C for 240 hours. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the orientation map of the Sn-Bi-Ag based solder joint EBSD sample prepared in Example 1;
[0022] Figure 2 This is the IPF image of the Sn-Bi-Ag based solder joint EBSD sample prepared in Example 1;
[0023] Figure 3 EBSD phase distribution diagram of the Sn-Bi-Ag based solder joint EBSD sample prepared in Example 2 after isothermal aging for 0h, 24h, 120h and 240h. DETAILED DESCRIPTION
[0024] The present invention provides a method for preparing a Sn-Bi-Ag based solder joint EBSD sample, comprising the following steps:
[0025] The Sn-Bi-Ag based solder joints were subjected to mechanical pre-polishing and ion beam treatment in sequence to obtain Sn-Bi-Ag based solder joint EBSD samples.
[0026] The present invention has no particular limitation on the raw materials used, and commercially available products known to those skilled in the art may be used.
[0027] In the present invention, the method for preparing the Sn-Bi-Ag based solder joint preferably comprises cutting the Sn-Bi-Ag based solder joint and then inlaying it with a denture base resin.
[0028] In the present invention, the Sn-Bi-Ag based welded joint preferably comprises one of Cu / Sn-57Bi-1Ag / Cu joint and Cu / Sn-57Bi-1Ag-0.5CeO2 / Cu. The present invention has no particular limitation on the source of the Sn-Bi-Ag based welded joint, and it can be prepared by a preparation method well known to those skilled in the art.
[0029] The present invention has no special limitation on the operation of cutting the Sn-Bi-Ag based welded joint, and conventional cutting can be performed according to the required position.
[0030] The present invention has no particular limitation on the operation of inlaying the denture base with resin, and the operation well known to those skilled in the art can be adopted.
[0031] In the present invention, the mechanical pre-polishing preferably further includes sandpaper polishing, cleaning and drying the Sn-Bi-Ag based solder joints in sequence.
[0032] In the present invention, the sandpaper polishing is preferably performed using 240#, 600#, 1000#, 1500#, 2000#, 3000# and 5000# silicon carbide sandpaper in sequence.
[0033] In the present invention, preferably, 240# and 600# silicon carbide sandpaper are used in sequence to grind the upper and lower bottom surfaces of the Sn-Bi-Ag-based solder joint. The present invention has no special limitation on the operation of grinding the upper and lower bottom surfaces of the Sn-Bi-Ag-based solder joint in sequence with 240# and 600# silicon carbide sandpaper, and the upper and lower bottom surfaces can be ground to the solder joint. The present invention grinds the upper and lower bottom surfaces of the Sn-Bi-Ag-based solder joint to improve the conductivity of the sample.
[0034] In the present invention, preferably, 1000#, 1500#, 2000#, 3000# and 5000# silicon carbide sandpaper are used in sequence to grind the test surface of the Sn-Bi-Ag based solder joint. The present invention has no special limitation on the operation of grinding the test surface of the Sn-Bi-Ag based solder joint, as long as the test surface is polished to be bright and smooth.
[0035] In the present invention, the cleaning agent used in the cleaning is preferably ethanol; the cleaning is preferably ultrasonic cleaning. The present invention has no special restrictions on the specific process parameters of the cleaning, as long as the sample is cleaned.
[0036] The present invention has no special limitation on the drying operation, as long as the surface of the sample is kept dry.
[0037] In the present invention, the mechanical pre-polishing is preferably performed by sequentially using diamond polishing agents with particle sizes of 2.5 μm, 1.0 μm and 0.5 μm. The mechanical pre-polishing of the present invention can improve the surface quality and the smoothness and flatness of the sample surface; the present invention can remove defects such as flaws, scratches and oxide layers on the sample surface by using appropriate abrasives and polishing processes, making it smoother and more uniform, so as to ensure that the sample surface can be treated more uniformly and consistently during vibration polishing to obtain accurate EBSD results.
[0038] In the present invention, the mechanical pre-polishing time using diamond polishing agents with particle sizes of 2.5 μm and 1.0 μm is independently preferably 3 to 5 minutes; the mechanical pre-polishing time using diamond polishing agents with particle size of 0.5 μm is preferably 3 to 6 minutes, more preferably 5 minutes.
[0039] In the present invention, the rotation speed of the mechanical pre-polishing is preferably 250-300 r / min.
[0040] After the mechanical pre-polishing is completed, the present invention preferably sequentially cleans and dries the sample obtained by the mechanical pre-polishing.
[0041] The present invention has no special limitation on the cleaning operation, as long as the sample is cleaned.
[0042] The present invention has no special limitation on the drying operation, as long as the surface of the sample is kept dry.
[0043] In the present invention, the energy of the ion beam treatment is 2000 eV; the bombardment time of the ion beam treatment is 150 to 200 s, preferably 180 s; the vacuum degree of the ion beam treatment is preferably <1×10 -8 The present invention performs ion beam treatment and bombards the sample with ion beam, which can make the generated stress layer and amorphous layer very thin, thereby avoiding the misleading of experimental data due to the sample preparation method; by limiting the energy and bombardment time of ion beam treatment, the stress layer and amorphous layer can be further thinned, thereby further improving the surface quality of the sample.
[0044] The present invention has no special limitation on the bombardment area of the ion beam treatment, and it can be set according to actual needs.
[0045] In the present invention, the ion beam treatment is preferably performed in an X-ray photoelectron spectrometer; the mode of the ion beam treatment is preferably Monatomic. The present invention has no special limitation on the model of the X-ray photoelectron spectrometer, and operations familiar to those skilled in the art can be used.
[0046] In the present invention, the ions used in the ion beam treatment are preferably argon ions.
[0047] The preparation method provided by the present invention effectively improves the problems of high cost, long cycle, unstable effect and the like in the preparation of EBSD samples of Sn-Bi-Ag based welded joints, and can obtain high-quality diffraction patterns on the test surface. It can characterize the changes in the microstructure, grain size and microtexture of the samples after different isothermal aging times, which is of great significance for studying the service reliability of the joints in high temperature environments.
[0048] The resolution rate of the EBSD sample without aging treatment prepared by the preparation method provided by the present invention is above 92%, and the resolution rate of the sample can still be guaranteed to be above 70% after the sample is aged at 110° C. for 240 hours; and the preparation method has low cost and simple operation, and a high-quality EBSD detection surface can be prepared in a short time, which reduces the difficulty of sample preparation and significantly improves the preparation efficiency and success rate of Sn-57Bi-1Ag-based solder EBSD samples.
[0049] The EBSD sample preparation method provided by the present invention particularly shows its unique advantages when processing materials with lower hardness, multi-phase materials and easily oxidized materials (Sn-based solder described in the present invention); in addition, ion etching of materials with added CeO2 is difficult, because different materials have different etching speeds, which will lead to inconsistent etching speeds of different materials, resulting in bumpy samples. The present invention can prepare EBSD samples with added CeO2 through parameter design.
[0050] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] Example 1
[0052] A method for preparing a Sn-Bi-Ag based solder joint EBSD sample comprises the following steps:
[0053] (1) Two Cu plates were reflow soldered with Sn-57Bi-1Ag solder to obtain Cu / Sn-57Bi-1Ag / Cu; wherein the reflow soldering parameters were: peak temperature 195°C, total soldering time 465s, and reflow time 90s;
[0054] (2) cutting a sample from the joint of the Cu / Sn-57Bi-1Ag / Cu obtained in step (1) to obtain a Cu / Sn-57Bi-1Ag / Cu joint;
[0055] (3) placing the Cu / Sn-57Bi-1Ag / Cu joint obtained in step (2) into an inlay mold, pouring a denture base resin into the mold, and ensuring that the pouring height is higher than the thickness of the solder joint; placing the inlay mold in a fume hood, and taking out the sample after the resin is completely solidified to obtain a Sn-Bi-Ag based solder joint;
[0056] (4) The upper and lower bottom surfaces of the Sn-Bi-Ag-based solder joint obtained in step (3) were polished to the solder joint with 240# and 600# silicon carbide sandpapers respectively, and then the test surface of the sample was polished to be bright and smooth with 1000#, 1500#, 2000#, 3000# and 5000# silicon carbide sandpapers respectively, and then ultrasonically cleaned with ethanol, and finally dried with cold air to obtain a treated Sn-Bi-Ag-based solder joint;
[0057] (5) mechanically pre-polishing the treated Sn-Bi-Ag-based solder joint obtained in step (4) with diamond polishing agents of particle sizes of 2.5 μm, 1 μm, and 0.5 μm, respectively, and ultrasonically cleaning with ethanol after polishing, and then drying with cold air to obtain mechanically pre-polished Sn-Bi-Ag-based solder joints; wherein the mechanical pre-polishing speed is 250 r / min, and each particle size polishing agent is polished for 4 min;
[0058] (6) The mechanically pre-polished Sn-Bi-Ag-based solder joint was placed in an X-ray photoelectron spectrometer at 1×10 -8 MPa or less vacuum conditions by Ar + The surface was treated with ion beam to obtain Sn-Bi-Ag based solder joint EBSD samples; the treatment mode was Monatomic, the energy was 2000eV, and the bombardment area was 4mm 2 , bombardment time is 180s;
[0059] The Sn-Bi-Ag based solder joint EBSD sample prepared in Example 1 was subjected to EBSD characterization. The resolution of the Sn-Bi-Ag based solder joint was 94.61%. The characterization area was recorded by taking photos. Figure 1 shown.
[0060] Figure 1 This is the orientation map of the Sn-Bi-Ag based solder joint EBSD sample prepared in Example 1; Figure 2 This is the IPF image of the Sn-Bi-Ag based solder joint EBSD sample prepared in Example 1.
[0061] according to Figure 1 and 2 The grain orientation of each grain can be analyzed, and the data is clear and reliable.
[0062] The Sn-Bi-Ag based solder joint EBSD sample prepared in Example 1 was placed in a clean culture dish, the opening of the culture dish was wrapped with plastic wrap, and the dish was placed in a 110°C forced air drying oven for isothermal aging experiment: the samples were taken out after aging for 24h, 120h and 240h for EBSD testing, and the resolution rates of the samples in each time period were 87.66%, 84.15% and 72.64%, respectively.
[0063] Example 2
[0064] A method for preparing a Sn-Bi-Ag based solder joint EBSD sample comprises the following steps:
[0065] (1) Two Cu plates were reflow soldered with Sn-57Bi-1Ag-0.5CeO2 solder to obtain Cu / Sn-57Bi-1Ag-0.5CeO2 / Cu; wherein the reflow soldering parameters were: peak temperature 195°C, total soldering time 465s, and reflow time 90s;
[0066] (2) cutting a sample from the joint of the Cu / Sn-57Bi-1Ag-0.5CeO2 / Cu obtained in step (1) to obtain a Cu / Sn-57Bi-1Ag-0.5CeO2 / Cu joint;
[0067] (3) placing the Cu / Sn-57Bi-1Ag-0.5CeO2 / Cu joint obtained in step (2) into an inlay mold, pouring a denture base resin into the mold, and ensuring that the pouring height is higher than the thickness of the solder joint; placing the inlay mold in a fume hood, and taking out the sample after the resin is completely solidified to obtain a Sn-Bi-Ag based solder joint;
[0068] (4) The upper and lower bottom surfaces of the Sn-Bi-Ag-based solder joint obtained in step (3) were polished to the solder joint with 240# and 600# silicon carbide sandpapers respectively, and then the test surface of the sample was polished to be bright and smooth with 1000#, 1500#, 2000#, 3000# and 5000# silicon carbide sandpapers respectively, and then ultrasonically cleaned with ethanol, and finally dried with cold air to obtain a treated Sn-Bi-Ag-based solder joint;
[0069] (5) mechanically pre-polishing the treated Sn-Bi-Ag-based solder joint obtained in step (4) with diamond polishing agents of particle sizes of 2.5 μm, 1 μm, and 0.5 μm, respectively, and ultrasonically cleaning with ethanol after polishing, and then drying with cold air to obtain mechanically pre-polished Sn-Bi-Ag-based solder joints; wherein the mechanical pre-polishing speed is 300 r / min, and each particle size polishing agent is polished for 3 min;
[0070] (6) The mechanically pre-polished Sn-Bi-Ag-based solder joint was placed in an X-ray photoelectron spectrometer at 1×10 -8 MPa or less vacuum conditions by Ar + The surface was treated with ion beam to obtain Sn-Bi-Ag based solder joint EBSD samples; the treatment mode was Monatomic, the energy was 2000eV, and the bombardment area was 4mm 2 , bombardment time is 180s;
[0071] The EBSD sample of the Sn-Bi-Ag based solder joint prepared in Example 2 was characterized by EBSD, and the resolution rate of the Sn-Bi-Ag based solder joint was 92.32%.
[0072] The Sn-Bi-Ag solder joint EBSD sample prepared in Example 2 was placed in a clean petri dish, the opening of the petri dish was wrapped with plastic wrap, and the dish was placed in a 110°C air drying oven for isothermal aging experiment: the sample was taken out after aging for 24h, 120h and 240h for EBSD test, and the resolution of the samples in each time period was 89.69%, 85.32% and 74.42% respectively. The photographed area was characterized each time, and the results are as follows: Figure 3 shown.
[0073] Figure 3 EBSD phase distribution diagram of the Sn-Bi-Ag based solder joint EBSD sample prepared in Example 2 after isothermal aging for 0h, 24h, 120h and 240h.
[0074] from Figure 3 It can be seen that, through the processing method of the present invention, in-situ EBSD characterization of samples during the aging process can be performed, and the test results can be guaranteed to have a high resolution rate.
[0075] Comparative Example 1
[0076] A method for preparing a Sn-Bi-Ag based solder joint EBSD sample comprises the following steps:
[0077] (1) Two Cu plates were reflow soldered with Sn-57Bi-1Ag-0.5CeO2 solder to obtain Cu / Sn-57Bi-1Ag-0.5CeO2 / Cu; wherein the reflow soldering parameters were: peak temperature 195°C, total soldering time 465s, and reflow time 90s;
[0078] (2) cutting a sample from the joint of the Cu / Sn-57Bi-1Ag-0.5CeO2 / Cu obtained in step (1) to obtain a Cu / Sn-57Bi-1Ag-0.5CeO2 / Cu joint;
[0079] (3) placing the Cu / Sn-57Bi-1Ag-0.5CeO2 / Cu joint obtained in step (2) into an inlay mold, pouring a denture base resin into the mold, and ensuring that the pouring height is higher than the thickness of the solder joint; placing the inlay mold in a fume hood, and taking out the sample after the resin is completely solidified to obtain a Sn-Bi-Ag based solder joint;
[0080] (4) The upper and lower bottom surfaces of the Sn-Bi-Ag-based solder joint obtained in step (3) were polished to the solder joint with 240# and 600# silicon carbide sandpapers respectively, and then the test surface of the sample was polished to be bright and smooth with 1000#, 1500#, 2000#, 3000# and 5000# silicon carbide sandpapers respectively, and then ultrasonically cleaned with ethanol, and finally dried with cold air to obtain a treated Sn-Bi-Ag-based solder joint;
[0081] (5) mechanically pre-polishing the treated Sn-Bi-Ag-based solder joint obtained in step (4) with diamond polishing agents of particle sizes of 2.5 μm, 1 μm, and 0.5 μm, respectively, and ultrasonically cleaning with ethanol after polishing, and then drying with cold air to obtain mechanically pre-polished Sn-Bi-Ag-based solder joints; wherein the mechanical pre-polishing speed is 250 r / min, and each particle size polishing agent is polished for 5 min;
[0082] (6) The mechanically pre-polished Sn-Bi-Ag-based solder joint was placed in an X-ray photoelectron spectrometer at 1×10 -8 MPa or less vacuum conditions by Ar + The surface was treated with ion beam to obtain Sn-Bi-Ag based solder joint EBSD samples; the treatment mode was Monatomic, the energy was 2000eV, and the bombardment area was 4mm 2 , bombardment time is 240s;
[0083] The Sn-Bi-Ag based solder joint EBSD sample prepared in Comparative Example 1 was characterized by EBSD, and the resolution rate of the Sn-Bi-Ag based solder joint was 61.38%.
[0084] By comparing Comparative Example 1 with Example 2, it can be seen that increasing the bombardment time will lead to a significant decrease in the resolution.
[0085] Comparative Example 2
[0086] A method for preparing a Sn-Bi-Ag based solder joint EBSD sample comprises the following steps:
[0087] (1) Two Cu plates were reflow soldered with Sn-57Bi-1Ag-0.5CeO2 solder to obtain Cu / Sn-57Bi-1Ag-0.5CeO2 / Cu; wherein the reflow soldering parameters were: peak temperature 195°C, total soldering time 465s, and reflow time 90s;
[0088] (2) cutting a sample from the joint of the Cu / Sn-57Bi-1Ag-0.5CeO2 / Cu obtained in step (1) to obtain a Cu / Sn-57Bi-1Ag-0.5CeO2 / Cu joint;
[0089] (3) placing the Cu / Sn-57Bi-1Ag-0.5CeO2 / Cu joint obtained in step (2) into an inlay mold, pouring a denture base resin into the mold, and ensuring that the pouring height is higher than the thickness of the solder joint; placing the inlay mold in a fume hood, and taking out the sample after the resin is completely solidified to obtain a Sn-Bi-Ag based solder joint;
[0090] (4) The upper and lower bottom surfaces of the Sn-Bi-Ag-based solder joint obtained in step (3) were polished to the solder joint with 240# and 600# silicon carbide sandpapers respectively, and then the test surface of the sample was polished to be bright and smooth with 1000#, 1500#, 2000#, 3000# and 5000# silicon carbide sandpapers respectively, and then ultrasonically cleaned with ethanol, and finally dried with cold air to obtain a treated Sn-Bi-Ag-based solder joint;
[0091] (5) mechanically pre-polishing the treated Sn-Bi-Ag-based solder joint obtained in step (4) with diamond polishing agents of particle sizes of 2.5 μm, 1 μm, and 0.5 μm, respectively, and ultrasonically cleaning with ethanol after polishing, and then drying with cold air to obtain mechanically pre-polished Sn-Bi-Ag-based solder joints; wherein the mechanical pre-polishing speed is 250 r / min, and each particle size polishing agent is polished for 5 min;
[0092] (6) The mechanically pre-polished Sn-Bi-Ag-based solder joint was placed in an X-ray photoelectron spectrometer at 1×10 -8 MPa or less vacuum conditions by Ar + The surface was treated with ion beam to obtain Sn-Bi-Ag based solder joint EBSD samples; the treatment mode was Monatomic, the energy was 3000eV, and the bombardment area was 2.25mm 2 , bombardment time is 180s;
[0093] The Sn-Bi-Ag based solder joint EBSD sample prepared in Comparative Example 2 was characterized by EBSD, and the resolution rate of the Sn-Bi-Ag based solder joint was 32.67%.
[0094] By comparing Comparative Example 2 with Example 2, it can be seen that changing the energy of ion beam processing will lead to a significant decrease in resolution.
[0095] Comparative Example 3
[0096] On the basis of Example 2, the bombardment time was changed to 130 s, and other conditions remained unchanged to obtain a Sn-Bi-Ag based solder joint EBSD sample.
[0097] The EBSD sample of the Sn-Bi-Ag based solder joint prepared in Comparative Example 3 was characterized by EBSD, and the resolution rate of the Sn-Bi-Ag based solder joint was 37.87%.
[0098] By comparing Comparative Example 3 with Example 2, it can be seen that shortening the bombardment time will also lead to a significant decrease in the resolution.
[0099] It can be seen from the above examples and comparative examples that the preparation method provided by the present invention can prepare high-quality EBSD samples.
[0100] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing Sn-Bi-Ag based solder joint EBSD samples, The following steps are involved: The Sn-Bi-Ag based solder joints were subjected to mechanical pre-polishing and ion beam treatment in sequence to obtain Sn-Bi-Ag based solder joint EBSD samples; The energy of the ion beam treatment is 2000 eV; the bombardment time of the ion beam treatment is 150 to 200 s.
2. The preparation method according to claim 1, It is characterized in that The method for preparing the Sn-Bi-Ag based solder joint comprises cutting the Sn-Bi-Ag based solder joint and then inlaying it with a denture base resin.
3. The preparation method according to claim 2, It is characterized in that The Sn-Bi-Ag based welded joints include Cu / Sn-57Bi-1Ag / Cu joints and Cu / Sn-57Bi-1Ag-0.5CeO 2 / One of Cu.
4. The preparation method according to claim 1, It is characterized in that The mechanical pre-polishing also includes sandpaper polishing, cleaning and drying the Sn-Bi-Ag based solder joints in sequence.
5. The preparation method according to claim 4, It is characterized in that The sandpaper grinding is performed by sequentially using 240#, 600#, 1000#, 1500#, 2000#, 3000# and 5000# silicon carbide sandpaper.
6. The preparation method according to claim 1, It is characterized in that The mechanical pre-polishing is performed by sequentially using diamond polishing agents with particle sizes of 2.5 μm, 1.0 μm and 0.5 μm.
7. The preparation method according to claim 6, It is characterized in that The mechanical pre-polishing time using the diamond polishing agent with a particle size of 2.5 μm and 1.0 μm is independently 3 to 5 minutes.
8. The preparation method according to claim 6, It is characterized in that The mechanical pre-polishing time using a diamond polishing agent with a particle size of 0.5 μm is 3 to 6 minutes.
9. The preparation method according to claim 1, It is characterized in that The bombardment time of the ion beam treatment is 180 s.
10. The preparation method according to claim 1, It is characterized in that The vacuum degree of the ion beam treatment is less than 1×10 - 8 MPa.