Method for continuously measuring content of silicon and barium in geological sample and tungsten concentrate by ICP (inductively coupled plasma) emission spectrometry
Through ICP inductively coupled plasma emission spectroscopy, combined with standard solutions and specific processing steps, the problem of the inability to simultaneously determine the silicon and barium content in geological samples and tungsten concentrate in the prior art is solved, and accurate and efficient detection results are achieved.
Patent Information
- Application Number
- CN202410964141.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-12
AI Technical Summary
The existing ICP inductively coupled plasma emission spectroscopy lacks standard detection methods to simultaneously determine the content of silicon and barium in geological samples and tungsten concentrate.
ICP inductively coupled plasma emission spectroscopy is used to prepare a standard solution series, introduce inductively coupled plasma torch after atomization, draw a standard curve, and combine specific experimental instruments and parameter settings, including muffle furnace, silver crucible, and hydroxide. Treatment of sodium and hydrochloric acid to achieve accurate determination of silicon and barium.
Accurate detection of the content of silicon and barium in geological samples and tungsten concentrates is achieved, detection efficiency and accuracy are improved, and a popularizable method is provided.
Smart Images

Figure CN118937464A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of ICP inductively coupled plasma (ICP) inductively coupled plasma (ICP) inductively coupled plasma emission spectrometry (ICP) method for continuously determining the silicon and barium contents in geological samples and tungsten concentrates. Background Art
[0002] There is no standard detection method for the simultaneous determination of silicon and barium in geological samples and tungsten concentrate samples using ICP inductively coupled plasma emission spectrometry. Summary of the invention
[0003] In view of the defects of the prior art, the purpose of the present invention is to provide a method for continuously determining the silicon and barium contents in geological samples and tungsten concentrates by ICP inductively coupled plasma emission spectrometry, so as to solve the problems raised in the above-mentioned background technology.
[0004] The present invention solves the technical problem by adopting the following technical solution:
[0005] The present invention provides a method for continuously determining the silicon and barium contents in geological samples and tungsten concentrates by ICP inductively coupled plasma emission spectrometry, comprising the following steps:
[0006] Step 1: Experimental instruments and parameters:
[0007] Step 2: Preparation of reagents and standard curve:
[0008] Step 3: Sample dissolution and sample pretreatment;
[0009] Step 4: Standard curve:
[0010] The standard solution series are sequentially atomized and introduced into the inductively coupled plasma torch, and a standard curve is drawn according to the net light intensity and corresponding concentration at the analysis line of each element to be measured in the standard solution series;
[0011] Step 5: Determination
[0012] Step 6 Calculation of results:
[0013] The content of silicon and barium in geological samples and tungsten concentrates is expressed in mass fraction W, and the value is expressed in %:
[0014]
[0015] Where:
[0016] Cx----------The concentration of the element being measured in the sample solution, unit: μg / ml;
[0017] C0----------The concentration of the measured element in the blank solution, unit: μg / ml;
[0018] V-----------The value of the sample solution, unit: ml;
[0019] m-----------The mass value of the sample, unit: g.
[0020] Preferably, the instruments used are: 1. ICP 6300 inductively coupled plasma emission spectrometer (manufacturer: Thermo Fisher Scientific, USA); 2. muffle furnace temperature set to 720°C; 3. silver crucible; 4. analytical balance with an accuracy of 0.0001g; 5. single-scale pipette and single-scale volumetric flask (in accordance with the provisions of GB / T12808 and GB / T12806);
[0021] Selection of working parameters: the selected power is 1150W, the flow rate of the auxiliary gas flow is 0.5L / min, the vertical observation height is 12mm, the pump speed is 100r / min; the atomizing gas flow rate is 0.7L / min; the exposure time corresponding to the long wave is 15S, a high-salt resistant atomizer and a corresponding atomization chamber are used, and argon: high purity (99.99%).
[0022] Preferably, accurately weigh 0.1000g of the dried sample, put it into a 30ml silver crucible, add 1.5g (granular) sodium hydroxide reagent to cover the sample, place the above silver crucible in a 600℃ muffle furnace and gradually heat it to a high temperature of 720℃, keep it at 720℃ for 5-8 minutes, take out the silver crucible, cool it slightly, put it into a plastic beaker filled with 100ml boiling water for immersion, stir it evenly with a plastic rod, add 50ml of hot hydrochloric acid (1+1), wash the silver crucible with water, transfer the solution in the plastic beaker into a 250ml volumetric flask, shake it well, filter it with double-layer filter paper, and keep the filtrate for testing; silicon standard storage solution, 1000μg / ml; barium standard solution, 0.1mg / ml.
[0023] Preferably, 2.1393 g of silicon dioxide (>99.9%) which has been calcined at 1000° C. for 45 min and cooled to room temperature in a desiccator is weighed out of the silicon standard stock solution, placed in a platinum crucible with 5 g of anhydrous sodium carbonate, mixed, and melted in a high-temperature furnace at 1000° C. for 15 min; the melt is heated and dissolved in a polytetrafluoroethylene beaker with 100 ml of warm water, cooled to room temperature, transferred to a 1000 ml volumetric flask, diluted to the scale with water, mixed, and stored in a polyethylene bottle. A certified standard solution may also be used.
[0024] Preferably, weigh 0.1437 g of barium carbonate (BaCO3) in a 250 ml beaker, add a small amount of hydrochloric acid (1+1) to dissolve, boil to remove carbon dioxide, cool, quantitatively transfer to a 1000 ml volumetric flask, dilute to the scale with water, shake well, this solution contains 0.1 mg / ml of barium, and use a certified standard solution.
[0025] Preferably, the reagents and standard curve are prepared as follows: sodium hydroxide, hydrochloric acid, Ba standard solution and Si standard solution; according to the concentration in the above table, the corresponding standard solution is transferred to a 1000ml volumetric flask, 100ml hydrochloric acid solution is added, the volume is fixed, and after mixing, the mixture is transferred to a 500ml plastic reagent bottle for storage and standby use.
[0026] Preferably, the concentration of the Ba standard solution is 0.1 mg / ml; the concentration of the Si standard solution is 1 mg / ml.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The present invention can detect the percentage of silicon and barium in geological samples and tungsten concentrate samples by preparing a solution, thereby greatly improving the detection efficiency, and the result is accurate and worthy of promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the sample image being analyzed by the ICP6300 instrument;
[0030] Figure 2 This is the plasma source setting diagram for the icp6300 instrument;
[0031] Figure 3 This is the analysis parameter setting diagram for the icp6300 instrument;
[0032] Figure 4 To make up the volume, place the above into 4 1000ml volumetric flasks;
[0033] Figure 5 For storage in polyethylene bottles;
[0034] Figure 6 Figure 1. Weighing 0.1000g of sample into a 30ml silver crucible;
[0035] Figure 7 The sample is placed in a muffle furnace at 600 degrees to melt.
[0036] Figure 8 To raise the temperature to 720 degrees, maintain for 5-8 minutes;
[0037] Fig. 9 To take out the silver crucible, cool it down slightly, and put it into a plastic cup filled with 100ml hot water to soak the picture;
[0038] Fig.10 Add 50 ml of hot hydrochloric acid to each plastic cup;
[0039] Fig.11 Transfer to a 250ml volumetric flask, adjust to volume, shake well, filter with double-layer filter paper, and keep the filtrate for testing;
[0040] Fig.12 The diagram is measured when the instrument is in the best condition;
[0041] Fig.13 To check that the peak values of each element are normal graphs;
[0042] Fig.14 For Ba, the correlation coefficients at 455nm and 493nm are greater than 0.999, and for Si, the correlation coefficients at 251nm, 212nm, and 288nm are all greater than 0.999. DETAILED DESCRIPTION
[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] The method of the present embodiment for continuously determining the silicon and barium contents in geological samples and tungsten concentrates by ICP inductively coupled plasma emission spectrometry comprises the following steps:
[0045] Step 1: Experimental instruments and parameters:
[0046] Step 2: Preparation of reagents and standard curve:
[0047] Step 3: Sample dissolution and sample pretreatment;
[0048] Step 4: Standard curve:
[0049] The standard solution series are sequentially atomized and introduced into the inductively coupled plasma torch, and a standard curve is drawn according to the net light intensity and corresponding concentration at the analysis line of each element to be measured in the standard solution series;
[0050] Step 5: Determination
[0051] Each time the test is performed, a certified standard sample of the same type of ore and a blank test should be analyzed in parallel with the test sample under the same conditions. The certified standard sample should be fully dried at 105℃±5℃.
[0052] Note: The certified standard sample and the test sample should be of the same type and the properties of the two substances should be sufficiently similar to ensure that no significant changes occur during the analysis. When a certified standard sample is not available, other standard samples may be used.
[0053] When analyzing several samples at the same time, a blank test can be used if the analytical steps are the same and the reagents used come from the same reagent bottle. When analyzing several ore samples of the same type at the same time, the same certification sample can be used.
[0054] Table 2 Recommended analysis lines
[0055]
[0056] Detect the net light intensity of each element in the blank solution and the sample solution respectively, determine the concentration of each element according to the standard curve, and then calculate the content of each element in the sample. Rinse with water for about 20 seconds between two measurements. Repeat the measurement for each sample at least twice and take the average of the two numbers.
[0057] Step 6 Calculation of results:
[0058] The content of silicon and barium in geological samples and tungsten concentrates is expressed in mass fraction W, and the value is expressed in %:
[0059]
[0060] Where:
[0061] Cx----------The concentration of the element being measured in the sample solution, unit: μg / ml;
[0062] C0----------The concentration of the measured element in the blank solution, unit: μg / ml;
[0063] V-----------The value of the sample solution, unit: ml;
[0064] m-----------The mass value of the sample, unit: g.
[0065] The instruments used in this embodiment are: 1. ICP 6300 inductively coupled plasma emission spectrometer (manufacturer: Thermo Fisher Scientific, USA); 2. The temperature of the muffle furnace is set to 720°C; 3. Silver crucible; 4. Analytical balance with an accuracy of 0.0001g; 5. Single-scale pipette and single-scale volumetric flask (in accordance with the provisions of GB / T12808 and GB / T12806);
[0066] Selection of working parameters: the selected power is 1150W, the flow rate of the auxiliary gas flow is 0.5L / min, the vertical observation height is 12mm, the pump speed is 100r / min; the atomizing gas flow rate is 0.7L / min; the exposure time corresponding to the long wave is 15S, a high-salt resistant atomizer and a corresponding atomization chamber are used, and argon: high purity (99.99%).
[0067] In the present embodiment, 0.1000 g of the dried sample is accurately weighed and placed in a 30 ml silver crucible. 1.5 g (granular) sodium hydroxide reagent is added to cover the sample. The above silver crucible is placed in a 600° C. muffle furnace and gradually heated to a high temperature of 720° C. The high temperature of 720° C. is maintained for 5-8 minutes. The silver crucible is taken out, cooled slightly, and placed in a plastic beaker filled with 100 ml boiling water for leaching. The mixture is stirred evenly with a plastic rod, and 50 ml of hot hydrochloric acid (1+1) is added. The silver crucible is washed out with water, and the solution in the plastic beaker is transferred to a 250 ml volumetric flask, fully shaken, filtered with double-layer filter paper, and the filtrate is retained for testing; silicon standard storage solution, 1000 μg / ml; barium standard solution, 0.1 mg / ml.
[0068] In the silicon standard stock solution of this embodiment, 2.1393 g of silicon dioxide (>99.9%) which had been calcined at 1000° C. for 45 min and cooled to room temperature in a desiccator was weighed and placed in a platinum crucible with 5 g of anhydrous sodium carbonate, mixed, and melted in a high-temperature furnace at 1000° C. for 15 min; the melt was heated and dissolved in a polytetrafluoroethylene beaker with 100 ml of warm water, cooled to room temperature, transferred to a 1000 ml volumetric flask, diluted to the scale with water, mixed, and stored in a polyethylene bottle. A certified standard solution may also be used.
[0069] In the barium standard solution of this example, 0.1437 g of barium carbonate (BaCO3) is weighed into a 250 ml beaker, a small amount of hydrochloric acid (1+1) is added to dissolve, the carbon dioxide is boiled to remove, the solution is cooled, and the solution is quantitatively transferred into a 1000 ml volumetric flask, diluted to the scale with water, and shaken well. This solution contains 0.1 mg / ml of barium, and a certified standard solution is used.
[0070] Preparation of reagents and standard curves in this example: sodium hydroxide, hydrochloric acid, Ba standard solution and Si standard solution; according to the concentration in the following table, transfer the corresponding standard solution into a 1000ml volumetric flask, add 100ml hydrochloric acid solution, make up to volume, mix and transfer to a 500ml plastic reagent bottle for storage and stand-by.
[0071] Table 1 Silicon and barium continuous measurement standard solution series (unit: μg / ml)
[0072]
[0073] The concentration of the Ba standard solution in this embodiment is 0.1 mg / ml; the concentration of the Si standard solution is 1 mg / ml.
[0074] The method of the present embodiment for continuously determining silicon and barium in geological samples and tungsten concentrate by ICP inductively coupled plasma emission spectrometry comprises the following steps:
[0075] Step 1: Experimental instruments and parameters
[0076] Main instrument: ICP 6300 inductively coupled plasma optical emission spectrometer (manufacturer: Thermo Fisher Scientific, USA). Working parameters: The above are typical working conditions. According to the characteristics of different instruments, appropriate adjustments can be made to the given working conditions to obtain the best results.
[0077] See Figure 1 、The icp6300 instrument is analyzing the sample. Figure 2 , icp6300 instrument plasma source settings.
[0078] Figure 3 , icp6300 instrument analysis parameter settings.
[0079] Step 2: Preparation of reagents and standard curve
[0080] Main reagents:
[0081] Sodium hydroxide (superior pure granular);
[0082] Hydrochloric acid (super pure) 1+1 hydrochloric acid is prepared with hot water (prepare and use immediately);
[0083] Ba standard solution 0.1mg / ml:
[0084] Weigh 0.1437g of barium carbonate (BaCO3, the purity should be above 99.9%) into a 250ml beaker, add a small amount of hydrochloric acid (1+1) to dissolve, boil to remove carbon dioxide, cool, quantitatively transfer into a 1000mL volumetric flask, dilute to scale with water, and shake well. This solution contains 0.1mg / ml of barium. You can also use a certified standard solution.
[0085] The concentration of Si standard solution is 1 mg / ml;
[0086] Weigh 2.1393g of silicon dioxide (purity>99.9%) that has been calcined at 1000℃ for 45min and cooled to room temperature in a desiccator, place in a platinum crucible with 5g of anhydrous sodium carbonate, mix well, and melt in a high-temperature furnace at 1000℃ for 15min. Heat and dissolve the melt in a polytetrafluoroethylene beaker with 100ml of warm water, cool to room temperature, transfer to a 1000mL volumetric flask, dilute to scale with water, mix well, and store in a polyethylene bottle. Certified standard solutions can also be used.
[0087] The specific preparation method of the silicon and barium continuous measurement standard solution series is as follows:
[0088] 1. Blank Ba and Si standard solutions are both 0 μg / ml;
[0089] 2. Standard 1 Take 10 ml of Ba standard solution and 10 ml of Si standard solution;
[0090] 3. Standard 2: Take 25 ml of Ba standard solution and 40 ml of Si standard solution;
[0091] 4. Standard 3: Take 100ml of Ba standard solution and 80ml of Si standard solution;
[0092] Place the above into 4 1000ml volumetric flasks, add 100ml hydrochloric acid and dilute with water to the mark of the 1000ml volumetric flask, shake well, and store in polyethylene bottles for later use.
[0093] See Figure 4 , Place the above into 4 1000ml volumetric flasks to make up to volume; Figure 5 , and store in polyethylene bottles respectively.
[0094] The method for establishing the standard curve of this embodiment is:
[0095] After the ICP instrument has stabilized under optimal conditions for 20 minutes, the standard curve is established using the mixed standard curve solution series prepared above.
[0096] Analyze the spectrum line selection, and select Ba 455nm and 493nm, Si 212 and 251nm and 288nm at the same time. Choose different spectrum lines according to the performance of the instrument and the content of the sample.
[0097] The spectral interference and matrix interference of this method can be ignored. Since the sample solution contains a lot of salt when measuring geological samples and tungsten concentrate, the system is prone to blockage, affecting the accuracy, so attention should be paid to the sample weight and dilution multiple.
[0098] Determination of solution acidity: If the volume fraction of hydrochloric acid HCl is around 10%, the actual measured value is more accurate. However, when the volume fraction is lower than 5%, the measured value is smaller than the true value, and vice versa. It should be noted that the acidity of the standard curve solution should be kept consistent with the acidity of the sample solution as much as possible, and the actual measured value is more accurate. Each operation should be conducted under the same conditions, and a certification standard sample of the same type of ore should be analyzed in parallel with the sample and a blank test should be performed.
[0099] Step 3: The sample pretreatment method of this embodiment is:
[0100] Accurately weigh 0.1000g of the dried sample and put it into a 30ml silver crucible. Add 1.5g of granular sodium hydroxide reagent to cover the sample. Place the above silver crucible in a 600℃ muffle furnace and gradually heat it to 720℃. Keep it at 720℃ for 5-8 minutes. Take out the silver crucible, shake it gently, and cool it slightly. Put it into a plastic beaker filled with 100ml boiling water and soak it, stirring it with a plastic rod. Add 50ml of 50% hot (1+1) salt and wash out the silver crucible with water.
[0101] Transfer the solution in the plastic beaker into a 250ml volumetric flask and shake thoroughly. Filter with double-layer filter paper and keep the filtrate for testing. Prepare the standard curve solution for continuous testing of silicon and barium.
[0102] See Figure 6 , weigh 0.1000g sample into a 30ml silver crucible; Figure 7 , Place the sample in a muffle furnace at 600 degrees to melt; Figure 8 , raise the temperature to 720 degrees and maintain for 5-8 minutes; Fig. 9 1. Take out the silver crucible, cool it down slightly, and put it into a plastic cup filled with 100ml hot water for soaking;
[0103] Fig.10 , Add 50ml of hot hydrochloric acid (1+1) to each plastic cup; Fig.11 , transfer to a 250ml volumetric flask, adjust to volume, shake well. Filter with double-layer filter paper and keep the filtrate for testing; Fig.12 , measure when the instrument is in the best condition; Step 4: calibration curve and measurement.
[0104] Click on the "Method" of the ICP instrument → then open "Elements" → click "Fit", which shows that its linear correlation coefficient must be greater than 0.999.
[0105] See Fig.13 , check that the peak values of each element are normal; Fig.14 The correlation coefficients of Ba, 455nm, 493nm are greater than 0.999. The correlation coefficients of Si, 251nm, 212nm, 288nm are all greater than 0.999. The results are reliable.
[0106] When measuring, operate the instrument at the best state, measure the blank first, many instruments can automatically deduct the blank value. Then measure the value of a standard sample that comes with the sample under the same conditions, and then measure the sample. Do at least 2 parallel experiments for each sample, and repeat the measurement for each solution at least twice, and take the average of the two readings.
[0107] Step 5: Calculation of results
[0108] The content of silicon and barium in geological samples and tungsten concentrates is calculated as mass fraction W, expressed in %:
[0109]
[0110] Where:
[0111] Cx---------The concentration of the element being measured in the sample solution, in ug / ml;
[0112] Co--------The concentration of the element being measured in the blank solution, in ug / ml;
[0113] V---------the volume of the sample solution, unit: ml;
[0114] m---------The numerical value of the sample mass, unit: g.
[0115] The calculation result is expressed to two decimal places.
[0116] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and therefore, it is intended that all changes that fall within the meaning and scope of the equivalent elements of the claims be included in the invention.
[0117] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0118] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for continuously determining the silicon and barium contents in geological samples and tungsten concentrates by ICP inductively coupled plasma emission spectrometry, characterized in that: The following steps are involved: Step 1: Experimental instruments and parameters: Step 2: Preparation of reagents and standard curve: Step 3: Sample dissolution and sample pretreatment; Step 4: Standard curve: The standard solution series are sequentially atomized and introduced into the inductively coupled plasma torch, and a standard curve is drawn according to the net light intensity and corresponding concentration at the analysis line of each element to be measured in the standard solution series; Step 5: Determination Step 6: Calculate the results: The content of silicon and barium in geological samples and tungsten concentrates is expressed in mass fraction W, and the value is expressed in %: Where: Cx----------The concentration of the element being measured in the sample solution, unit: μg / ml; C0----------The concentration of the measured element in the blank solution, unit: μg / ml; V-----------The value of the sample solution, unit: ml; m-----------The mass value of the sample, unit: g.
2. The method for continuously determining the silicon and barium contents in geological samples and tungsten concentrates by ICP inductively coupled plasma emission spectrometry according to claim 1, characterized in that: Instruments used:
1. ICP 6300 inductively coupled plasma emission spectrometer (manufacturer: Thermo Fisher Scientific, USA); 2. muffle furnace temperature set to 720°C; 3. silver crucible; 4. analytical balance with an accuracy of 0.0001g; 5. single-scale pipette and single-scale volumetric flask; Selection of working parameters: the selected power is 1150W, the flow rate of the auxiliary gas flow is 0.5L / min, the vertical observation height is 12mm, the pump speed is 100r / min; the atomizing gas flow rate is 0.7L / min; the exposure time corresponding to the long wave is 15S, a high-salt resistant atomizer and a corresponding atomization chamber are used, and argon: high purity (99.99%).
3. The method for continuously determining the silicon and barium contents in geological samples and tungsten concentrates by ICP inductively coupled plasma emission spectrometry according to claim 2, characterized in that: Accurately weigh 0.1000g of the dried sample, put it into a 30ml silver crucible, add 1.5g of sodium hydroxide reagent to cover the sample, place the above silver crucible in a 600℃ muffle furnace and gradually heat it to 720℃, keep it at 720℃ for 5-8 minutes, take out the silver crucible, cool it slightly, put it into a plastic beaker filled with 100ml boiling water for immersion, stir it evenly with a plastic rod, add 50ml of hot hydrochloric acid (concentration is 1+1), wash out the silver crucible with water, transfer the solution in the plastic beaker into a 250ml volumetric flask, shake it thoroughly, filter it with double-layer filter paper, and keep the filtrate for testing; silicon standard storage solution, 1000μg / ml; barium standard solution, 0.1mg / ml.
4. The method for continuously determining the silicon and barium contents in geological samples and tungsten concentrates by ICP inductively coupled plasma emission spectrometry according to claim 3 is characterized in that: Weigh 2.1393g of silicon dioxide (>99.9%) from the silicon standard stock solution, which has been calcined at 1000℃ for 45min and cooled to room temperature in a desiccator. Place it in a platinum crucible with 5g of anhydrous sodium carbonate, mix well, and melt it in a high-temperature furnace at 1000℃ for 15min. Heat and dissolve the melt in a polytetrafluoroethylene beaker with 100ml of warm water, cool to room temperature, transfer it to a 1000ml volumetric flask, dilute to the scale with water, mix well, and store in a polyethylene bottle. Certified standard solutions can also be used.
5. The method for continuously determining the silicon and barium contents in geological samples and tungsten concentrates by ICP inductively coupled plasma emission spectrometry according to claim 4, characterized in that: Weigh 0.1437 g of barium carbonate (BaCO3) into a 250 ml beaker, add a small amount of hydrochloric acid to dissolve, boil to remove carbon dioxide, cool, transfer quantitatively into a 1000 ml volumetric flask, dilute to the scale with water, shake well, this solution contains 0.1 mg / ml barium, use a certified standard solution.
6. The method for continuously determining the silicon and barium contents in geological samples and tungsten concentrates by ICP inductively coupled plasma emission spectrometry according to claim 4, characterized in that: Preparation of reagents and standard curve: sodium hydroxide, hydrochloric acid, Ba standard solution and Si standard solution; according to the concentration in the above table, transfer the corresponding standard solution to a 1000ml volumetric flask, add 100ml hydrochloric acid solution, make up to volume, mix and transfer to a 500ml plastic reagent bottle for storage and stand-by.
7. The method for continuously determining the silicon and barium contents in geological samples and tungsten concentrates by ICP inductively coupled plasma emission spectrometry according to claim 6, characterized in that: The concentration of the Ba standard solution is 0.1 mg / ml; the concentration of the Si standard solution is 1 mg / ml.