Electrode material and preparation method thereof
By using aluminum powder of different particle sizes to layer in electrode material preparation, the specific surface area and bending resistance of the electrode material are improved, the problems of large volume of aluminum electrolytic capacitors and easy cracking of foils are solved, and high electrostatic capacity and The effect of small volume.
Patent Information
- Application Number
- CN202411092748.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing aluminum electrolytic capacitors are large in size and have high requirements for the bending resistance of the anode foil during winding. Microcracks are prone to appear on the edges of the foil, and it is difficult to achieve thin, light and small development of the electronic machine.
An electrode material preparation method is adopted. Through the glueing, plastic film and sintering process, aluminum powder with different particle sizes is stacked in layers to increase the specific surface area and bending resistance of the electrode material, and achieve high electrostatic capacity and small volume.
It effectively solves the problem of high bending performance requirements for the anode foil and easy cracking of the edges of the foil in capacitor preparation, and realizes small volume and high capacity under specific voltage resistance conditions, and does not require etching and has less contamination.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrode materials, and in particular to an electrode material and a preparation method thereof. Background Art
[0002] Sintered foil electrolytic capacitor is a new type of high-performance electrolytic capacitor newly developed in the 21st century. Its advantage is that it improves the specific capacitance and production efficiency of electrolytic capacitors. However, most of the existing aluminum electrolytic capacitors are wound. Wound aluminum electrolytic capacitors are formed by winding electrolytic paper, positive foil and negative foil together. This method causes the volume of wound aluminum electrolytic capacitors to be larger, and the bending resistance of the anode foil is required to be higher during the winding process, and micro cracks are prone to appear on the edges of the foil. In addition, the electronic whole machine is developing rapidly towards thin, light and small. As aluminum electrolytic capacitors, which have irreplaceable functions in circuits, the large volume of aluminum electrolytic capacitors has become a limiting factor. Summary of the invention
[0003] In view of the problems existing in the prior art, the present invention provides a method for preparing an electrode material. The electrode material obtained by the preparation method provided by the present invention has a large specific surface area, and the electrostatic capacitance of the capacitor made therefrom is high, thereby achieving small volume and high capacity under specific withstand voltage conditions.
[0004] In one aspect, the present invention provides a method for preparing an electrode material, the preparation method comprising:
[0005] S1 Gluing: Mixing the solvent and the cross-linking agent, performing glue treatment, and obtaining glue solution;
[0006] S2 Plastic film: Disperse aluminum powder in glue solution and pressurize to obtain the material to be processed; wherein the plastic film is performed twice or more, and the particle size D of aluminum powder used in two adjacent plastic films is 50 different;
[0007] S3 sintering: sintering the material to be processed to obtain the electrode material.
[0008] The electrode material obtained by the preparation method provided by the present invention has a large specific surface area and high bending resistance. The capacitor manufactured by the electrode material has a high electrostatic capacitance, and a small volume and high capacity under specific withstand voltage conditions are achieved. Therefore, the method of the present invention can effectively solve the problem that when preparing capacitors, the bending resistance of electrode foils such as anode foils is high during the winding process, and micro cracks are prone to appear on the edges of the foils.
[0009] The present invention may further include at least one of the following technical features:
[0010] According to the embodiment of the present invention, the type of solvent is not particularly limited, and the solvent can be selected from at least one of ethanol, water, toluene, acetone, and ethylene glycol ethyl ether, but is not limited to the above options.
[0011] According to an embodiment of the present invention, the type of crosslinking agent is not particularly limited, and the crosslinking agent can be selected from at least one of epoxy resin, vinyl alcohol resin, fluoroethylene resin, epoxy resin, paraffin, and ethyl cellulose, but is not limited to the above options.
[0012] According to an embodiment of the present invention, the mass ratio of the solvent to the cross-linking agent may be (5-100):1.
[0013] According to an embodiment of the present invention, the mass ratio of the solvent to the cross-linking agent is preferably (5-50):1.
[0014] According to an embodiment of the present invention, the mass ratio of the solvent to the cross-linking agent is preferably (5-20):1.
[0015] According to an embodiment of the present invention, the mass ratio of the solvent to the cross-linking agent is preferably (5-10):1.
[0016] According to an embodiment of the present invention, the mass ratio of the solvent to the cross-linking agent is preferably (5-7.5):1.
[0017] According to an embodiment of the present invention, the mass ratio of the solvent to the cross-linking agent is preferably (7.5-10):1.
[0018] Optionally, the mass ratio of the solvent to the cross-linking agent is any value in the range of (5-100): 1. Specifically, the mass ratio of the solvent to the cross-linking agent is 5:1, 7.5:1, 10:1, 12.5:1, 15:1, 17.5:1, 20:1, 22.5:1, 25:1, 27.5:1, 30:1, 32.5:1, 35:1, 37.5:1, 40:1, 42.5:1, 45:1, 47.5:1, 50:1, 52.5:1, 55:1 1, 57.5:1, 60:1, 62.5:1, 65:1, 67.5:1, 70:1, 72.5:1, 75:1, 77.5:1, 80:1, 82.5:1, 85:1, 87.5:1, 90:1, 92.5:1, 95:1, 97.5:1, 100:1, or a range consisting of any two endpoints thereof, or any value within the range.
[0019] According to an embodiment of the present invention, the aluminum powder used in the S2 plastic film is independently selected from any one of small-particle aluminum powder and large-particle aluminum powder.
[0020] Unless otherwise specified, the "small-particle aluminum powder" and "large-particle aluminum powder" described in the present invention refer to two aluminum powders with different particle sizes (such as average particle size), and the particle size of the small-particle aluminum powder is smaller than that of the large-particle aluminum powder.
[0021] According to an embodiment of the present invention, the particle size D of the aluminum powder used in two adjacent plastic films is 50 different.
[0022] According to an embodiment of the present invention, the small particle aluminum powder D 50 0.1-3.5μm.
[0023] According to an embodiment of the present invention, the small particle aluminum powder D 50 Preferably it is 0.5-3.0 μm.
[0024] According to an embodiment of the present invention, the small particle aluminum powder D 50 Preferably it is 1.0-3.0 μm.
[0025] According to an embodiment of the present invention, the small particle aluminum powder D 50 Preferably it is 1.5-3.0 μm.
[0026] According to an embodiment of the present invention, the small particle aluminum powder D 50 Preferably it is 1.5-2.5 μm.
[0027] Optionally, small particle aluminum powder D 50 It can be any value in the range of 0.1-3.5 μm. Specifically, the small particle aluminum powder D 50 It is 0.1 μm, 0.5 μm, 1.0 μm, 1.5 μm, 2.0 μm, 2.5 μm, 3.0 μm, 3.5 μm, or a range consisting of any two endpoints thereof, or any value within the range.
[0028] According to an embodiment of the present invention, the large-particle aluminum powder D 50 3.5-20μm.
[0029] According to an embodiment of the present invention, the large-particle aluminum powder D 50 Preferably it is 3.5-15 μm.
[0030] According to an embodiment of the present invention, the large-particle aluminum powder D 50 Preferably it is 3.5-10 μm.
[0031] According to an embodiment of the present invention, the large-particle aluminum powder D 50 Preferably it is 3.5-5.5 μm.
[0032] According to an embodiment of the present invention, the large-particle aluminum powder D 50 Preferably it is 3.5-4.5 μm.
[0033] Optionally, large particle aluminum powder D 50 It can be any value within the range of 3.5-20μm. Large particle aluminum powder D 50 It is 3.5μm, 4.0μm, 4.5μm, 5.0μm, 5.5μm, 6.0μm, 7.0μm, 8.0μm, 9.0μm, 10.0μm, 11.0μm, 12.0μm, 13.0μm, 14.0μm, 15.0μm, 16.0μm, 17.0μm, 8.0μm, 19.0μm, 20.0μm, or a range consisting of any two endpoints of the above or any value within the range.
[0034] When the aluminum powder particle size is less than 0.1 μm, the void size after sintering is too small, making it difficult for the electrolyte to penetrate; and when the aluminum powder particle size is greater than 20 μm, the specific surface area after sintering is too low, resulting in reduced capacity.
[0035] Low particle size shows high specific surface area and small void size. When the aluminum powder particle size is small, the voids in the powder layer are small. After formation, the voids are further reduced and spheroidized, and a dense and brittle aluminum oxide film is generated on the surface of the voids. When the formation voltage is large, a large area of powder adhesion will occur, blocking the voids and making it difficult for the electrolyte to penetrate; high particle size shows low specific surface area and large void size. When the aluminum powder particle size is large, the voids in the powder layer are large, and the electrolyte is easier to penetrate. After formation, the voids are reduced and spheroidized, and a certain size can still be maintained to allow the electrolyte to penetrate. After sintering, large-particle aluminum powder has a larger sintering neck (the overlapping part between aluminum powders), and the aluminum powders in the powder layer are more firmly bonded. Therefore, the present invention adopts the layered stacking method of aluminum powders with different particle sizes to produce a sintered body, ensuring that when the formation voltage is large, there will be no large-area powder adhesion, which will block the gaps and make it difficult for the electrolyte to penetrate, and the electrolyte will be easier to penetrate; the electrostatic capacitance of the capacitor made from the sintered body made by the method of the present invention is higher than that of the capacitor made from the sintered body obtained by stacking aluminum powder with a single particle size.
[0036] According to an embodiment of the present invention, in S2 film molding, the lead is placed in a mold and film molding is performed.
[0037] According to an embodiment of the present invention, the lead wire is preferably aluminum foil.
[0038] According to an embodiment of the present invention, the mold can be selected from any shape, preferably cylindrical, cube or cuboid.
[0039] According to an embodiment of the present invention, S2 plastic film includes S2.1 primary plastic film, S2.2 secondary plastic film; optionally, S2.3 tertiary plastic film is also included.
[0040] According to an embodiment of the present invention, the mold volume used for the secondary molding of S2.2 is larger than the mold volume used for the primary molding of S2.1, and the mold volume used for the tertiary molding of S2.3 is larger than the mold volume used for the secondary molding of S2.2.
[0041] According to an embodiment of the present invention, in S3, a pre-sintering treatment is performed before sintering. Optionally, the pre-sintering treatment temperature is 300-450°C; Optionally, the pre-sintering treatment time is 0.1-100h, preferably 0.1-20h, preferably 0.1-10h.
[0042] Specifically, the temperature of the pre-sintering treatment is any value in the range of 300-450° C. The temperature of the pre-sintering treatment is 300° C., 350° C., 400° C., 450° C., or a range consisting of any two endpoints thereof or any value within the range.
[0043] Specifically, the time of the pre-sintering treatment is any value in the range of 0.1-100h. The time of the pre-sintering treatment is 0.1h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 30h, 40h, 50h, 60h, 70h, 80h, 90h, 100h or a range consisting of any two endpoints thereof or any value within the range.
[0044] According to an embodiment of the present invention, optionally, in S3, the sintering temperature is 500-650°C.
[0045] According to an embodiment of the present invention, optionally, in S3, the sintering time is 0.1-100 h, preferably 1-50 h, preferably 1-20 h, preferably 1-10 h.
[0046] Specifically, the sintering temperature is any value in the range of 500-650° C. The sintering temperature is 500° C., 550° C., 600° C., 640° C., or a range consisting of any two endpoints thereof, or any value within the range.
[0047] Specifically, the sintering time is any value in the range of 0.1-100h. The sintering time is 0.1h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 30h, 40h, 50h, 60h, 70h, 80h, 90h, 100h or a range consisting of any two endpoints thereof or any value within the range.
[0048] According to an embodiment of the present invention, in the S2 plastic film, the mass ratio of aluminum powder to adhesive liquid is independently (0.1-10):1.
[0049] According to an embodiment of the present invention, in the S2 plastic film, the mass ratio of aluminum powder to adhesive liquid is independently (0.1-8):1.
[0050] According to an embodiment of the present invention, in the S2 plastic film, the mass ratio of aluminum powder to adhesive liquid is independently (0.1-5):1.
[0051] According to an embodiment of the present invention, in the S2 plastic film, the mass ratio of aluminum powder to adhesive liquid is independently (0.1-1):1.
[0052] Optionally, in the S2 plastic film, the mass ratio of aluminum powder to the adhesive is any value in the range of (0.1-10): 1. Specifically, in the S2 plastic film, the mass ratio of aluminum powder to the adhesive is independently 0.1: 1, 0.2: 1, 0.3: 1, 0.4: 1, 0.5: 1, 0.6: 1, 0.7: 1, 0.8: 1, 0.9: 1, 1: 1, 2: 1, 3: 1, 4: 1, 5: 1, 6: 1, 7: 1, 8: 1, 9: 1, 10: 1, or a range consisting of any two of the above endpoints or any value within the range.
[0053] According to an embodiment of the present invention, the sintering in S3 is carried out under vacuum, inert or reducing atmosphere; the inert atmosphere is selected from but not limited to at least one of helium, neon, argon and nitrogen; the reducing atmosphere is selected from but not limited to at least one of hydrogen, alkanes and alkenes.
[0054] According to an embodiment of the present invention, the pressure of the pressurizing molding is independently 2-10 MPa.
[0055] According to an embodiment of the present invention, the pressure of the pressurizing molding is independently 2-5 MPa.
[0056] Optionally, the pressure of the press molding is independently any value in the range of 2-10 MPa. The pressure of the press molding is independently 2 MPa, 2.5 MPa, 3.0 MPa, 3.5 MPa, 4.0 MPa, 4.5 MPa, 5.0 MPa, 5.5 MPa, 6.0 MPa, 6.5 MPa, 7.0 MPa, 7.5 MPa, 8.0 MPa, 8.5 MPa, 9.0 MPa, 9.5 MPa, 10 MPa, or a range consisting of any two endpoints thereof or any value within the range.
[0057] In a second aspect, the present invention provides an electrode material prepared by the method described in the first aspect.
[0058] In a third aspect, the present invention provides a capacitor, wherein the electrode material used in the capacitor is prepared by the preparation method described in the first aspect;
[0059] Or it is the electrode material described in the second aspect.
[0060] Compared with the prior art, the present invention has the following technical effects:
[0061] 1. The preparation method of the present invention can effectively solve the problem that the bending resistance of the anode foil is high during the winding process when preparing the capacitor, and micro cracks are prone to appear on the edge of the foil;
[0062] 2. The electrode material obtained by the preparation method provided by the present invention has a large specific surface area, and the capacitor produced by the electrode material has a high electrostatic capacity, achieving a small volume and high capacity under specific withstand voltage conditions; and
[0063] 3. The preparation method of the present invention does not require etching treatment and has relatively little pollution. DETAILED DESCRIPTION
[0064] The embodiments of the present invention are described in detail below. Unless otherwise specified, all scientific and technological terms used in the present invention have the same meaning as those generally understood by those skilled in the art to which the present invention belongs. All patents and publications to which the present invention relates are incorporated herein by reference in their entirety. The term "comprising" or "including" is an open expression, i.e., including the contents specified in the present invention, but does not exclude the contents of other aspects.
[0065] According to the embodiment provided by the present invention, the present invention particularly provides
[0066] A method for preparing an electrode material, the method comprising:
[0067] S1 Gluing: Mixing the solvent and the cross-linking agent, performing glue treatment, and obtaining glue solution;
[0068] Wherein, the solvent is selected from at least one of ethanol, water, toluene, acetone and ethylene glycol ethyl ether.
[0069] The cross-linking agent is selected from at least one of epoxy resin, vinyl alcohol resin, fluoroethylene resin, epoxy resin, paraffin and ethyl cellulose.
[0070] Optionally, the mass ratio of the solvent to the cross-linking agent is (5-100):1; preferably (5-50):1; preferably (5-20):1; preferably (5-10):1; preferably (5-7.5):1; preferably (7.5-10):1; preferably 5:1, 7.5:1, 10:1.
[0071] S2 Plastic film: Disperse aluminum powder in glue solution and pressurize to obtain the material to be processed; wherein the plastic film is performed twice or more, and the particle size D of aluminum powder used in two adjacent plastic films is 50 different.
[0072] The mass ratio of aluminum powder to glue liquid is independently (0.1-10):1; preferably (0.1-8):1; preferably (0.1-5):1; preferably (0.1-1):1.
[0073] The aluminum powder used in the S2 plastic film is independently selected from any one of small-particle aluminum powder or large-particle aluminum powder.
[0074] The particle size of small aluminum powder is D 50 It is 0.1-3.5μm; preferably 0.5-3.0μm; preferably 1.0-3.0μm; preferably 1.5-3.0μm; preferably 1.5-2.5μm; preferably 1.5μm, 2μm, 2.5μm.
[0075] Particle size D of large aluminum powder 50 It is 3.5-20μm, preferably 3.5-15μm, preferably 3.5-10μm, preferably 3.5-5.5μm, preferably 3.5-4.5μm, preferably 3.5μm, 4.0μm, 4.5μm.
[0076] The pressure of the pressurization molding is independently 2-10 MPa; preferably 2-5 MPa; preferably 2MPa, 2.5MPa, 3MPa, 3.5MPa, 4.0MPa, 4.5MPa, 5MPa.
[0077] S3 sintering: in a vacuum, inert or reducing atmosphere, pre-sinter the material to be treated at 300-450° C. for 0.1-20 h, and then sinter at 500-650° C. for 0.1-20 h to obtain the electrode material.
[0078] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. In the examples, if no specific conditions are specified, the conditions described in the specification or the conventional conditions or the conditions recommended by the manufacturer are followed. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0079] Example 1
[0080] S1 Gluing: Mix ethylene glycol ethyl ether and ethyl cellulose (the mass ratio of ethylene glycol ethyl ether to ethyl cellulose is 7.5:1), and perform glue treatment to obtain glue solution ①;
[0081] S2 plastic film
[0082] S2.1 First film forming: 30g D 50Aluminum powder with a particle size of 4.0 μm is added to 170 g of glue solution ① to be dispersed in the glue solution to obtain a first solid coating liquid ①; a lead is placed at the center of a mold 1, the first solid coating liquid ① is injected into the mold 1, and a first pressurization treatment (pressure is 2.5 MPa) is performed, and the mold is demolded after molding to obtain a primary plastic film material ①;
[0083] S2.2 Secondary mold: 30g D 50 Aluminum powder with a particle size of 2.0 μm is added to another 170 g of glue solution ① to be dispersed in the glue solution to obtain a second solid coating solution ①; a primary plastic film material ① is placed in the center of a mold 2, and the second solid coating solution ① is injected, and a second pressurization treatment (pressure is 2.5 MPa) is performed, and the mold is demolded after molding to obtain a material to be treated ①;
[0084] S3 sintering: Place the material to be processed ① in a nitrogen atmosphere, pre-sinter at 350°C for 1 hour, then heat to 600°C and sinter for 5 hours to obtain electrode material ①.
[0085] Example 2
[0086] S1 Gluing: Mix ethylene glycol ethyl ether and ethyl cellulose (the mass ratio of ethylene glycol ethyl ether to ethyl cellulose is 7.5:1), and perform glue treatment to obtain glue solution ②;
[0087] S2 plastic film
[0088] S2.1 First film forming: 30g D 50 Aluminum powder with a particle size of 2.0 μm is added to 170 g of glue solution ② to be dispersed in the glue solution to obtain a first solid coating liquid ②; a lead is placed at the center of a mold 1, the first solid coating liquid ② is injected into the mold 1, and a first pressurization treatment (pressure is 2.5 MPa) is performed, and the mold is demolded after molding to obtain a primary plastic film material ②;
[0089] S2.2 Secondary mold: 30g D 50 Aluminum powder with a particle size of 4.0 μm is added to another 170 g of glue solution ② to be dispersed in the glue solution to obtain a second solid coating solution ②; a primary plastic film material ② is placed in the center of the mold 2, and the second solid coating solution ② is injected, and a second pressurization treatment (pressure is 2.5 MPa) is performed, and the mold is demolded after molding to obtain a material to be treated ②;
[0090] S3 sintering: Place the material to be processed ② in a nitrogen atmosphere, pre-sinter at 350°C for 1 hour, then heat to 600°C and sinter for 5 hours to obtain electrode material ②.
[0091] Example 3
[0092] S1 Gluing: Mix ethylene glycol ethyl ether and ethyl cellulose (the mass ratio of ethylene glycol ethyl ether to ethyl cellulose is 7.5:1), and perform glue treatment to obtain glue solution ③;
[0093] S2 plastic film
[0094] S2.1 First film forming: 30g D 50 Aluminum powder with a diameter of 2.0 μm is added to 170 g of glue solution ③ to be dispersed in the glue solution to obtain a first solid coating liquid ③; a lead is placed at the center of the mold 1, the first solid coating liquid ③ is injected into the mold 1, and a first pressurization treatment (pressure is 2.5 MPa) is performed, and the mold is demolded after molding to obtain a primary plastic film material ③;
[0095] S2.2 Secondary mold: 30g D 50 Aluminum powder with a particle size of 4.0 μm is added to another 170 g of glue solution ③ to be dispersed in the glue solution to obtain a second solid coating solution ③; the primary plastic film material ③ is placed in the center of the mold 2, the second solid coating solution ③ is injected, and a second pressurization treatment (pressure is 2.5 MPa) is performed, and the mold is demolded after molding to obtain a secondary plastic film material ③;
[0096] S2.3 Three times plastic film: 30g D 50 Aluminum powder with a diameter of 2.0 μm is added to another 170 g of glue solution ③ to disperse it in the glue solution to obtain a third solid coating liquid ③; the secondary plastic film material ③ is placed in the center of the mold 3, the third solid coating liquid ③ is injected, and a third pressurization treatment (pressure is 2.5 MPa) is performed, and the mold is demolded after molding to obtain the material to be treated ③;
[0097] S3 sintering: Place the material to be processed ③ in a nitrogen atmosphere, pre-sinter at 350°C for 1 hour, then heat to 600°C and sinter for 5 hours to obtain electrode material ③.
[0098] Comparative Example 1
[0099] S1 Gluing: Mix ethylene glycol ethyl ether and ethyl cellulose (the mass ratio of ethylene glycol ethyl ether to ethyl cellulose is 7.5:1), and perform glue treatment to obtain glue solution ④.
[0100] S2 plastic film
[0101] S2.1 First film forming: 30g D 50 Aluminum powder with a diameter of 2.0 μm is added to 170 g of glue solution ④ to be dispersed in the glue solution to obtain a first solid coating liquid ④; a lead is placed at the center of the mold 1, the first solid coating liquid ④ is injected into the mold 1, and a first pressurization treatment (pressure is 2.5 MPa) is performed, and the mold is demolded after molding to obtain a primary plastic film material ④;
[0102] S2.2 Secondary film: 30g D50 Aluminum powder with a particle size of 2.0 μm is added to another 170 g of glue solution ④ to be dispersed in the glue solution to obtain a second solid coating solution ④; a primary plastic film material ④ is placed in the center of the mold 2, and the second solid coating solution ④ is injected, and a second pressurization treatment (pressure is 2.5 MPa) is performed, and the mold is demolded after molding to obtain a material to be treated ④;
[0103] S3 sintering: Place the material to be processed ④ in a nitrogen atmosphere, pre-sinter at 350° C. for 1 hour, then heat to 600° C. and sinter for 5 hours to obtain electrode material ④.
[0104] Comparative Example 2
[0105] S1 Gluing: Mix ethylene glycol ethyl ether and ethyl cellulose (the mass ratio of ethylene glycol ethyl ether to ethyl cellulose is 7.5:1), and perform glue treatment to obtain glue solution ⑤.
[0106] S2 plastic film
[0107] S2.1 First film forming: 30g D 50 Aluminum powder with a diameter of 4.0 μm is added to 170 g of glue solution ⑤ to be dispersed in the glue solution to obtain a first solid coating liquid ⑤; a lead is placed at the center of the mold 1, the solid coating liquid ⑤ is injected into the mold 1, and a first pressurization treatment (pressure is 2.5 MPa) is performed, and the mold is demolded after molding to obtain a primary plastic film material ⑤;
[0108] S2.2 Secondary film: 30g D 50 Aluminum powder with a particle size of 4.0 μm is added to another 170 g of glue solution ④ to be dispersed in the glue solution to obtain a second solid coating solution ⑤; a primary plastic film material ⑤ is placed in the center of the mold 2, and the second solid coating solution ⑤ is injected, and a second pressurization treatment (pressure is 2.5 MPa) is performed, and the mold is demolded after molding to obtain a material to be treated ⑤;
[0109] S3 sintering: Place the material to be processed ⑤ in a nitrogen atmosphere, pre-sinter at 350° C. for 1 hour, then heat to 600° C. and sinter for 5 hours to obtain electrode material ⑤.
[0110] Comparative Example 3
[0111] On one side of the aluminum foil, 50 μm of the first solid coating liquid ④ prepared in Comparative Example 1 was first coated, and then 50 μm of the first solid coating liquid ⑤ prepared in Comparative Example 2 was coated, and after drying and forming; on the reverse side, 50 μm of the first solid coating liquid ④ prepared in Comparative Example 1 was first coated, and then 50 μm of the first solid coating liquid ⑤ prepared in Comparative Example 2 was coated, and after drying and forming, a material to be treated ⑥ was obtained; the material to be treated ⑥ was placed in a nitrogen atmosphere, pre-sintered at 350° C. for 1 hour, and then heated to 600° C. and sintered for 5 hours to obtain an electrode material ⑥.
[0112] Because the foil is thick and easy to break, it is difficult to achieve subsequent formation and winding, and the electrostatic capacitance of the foil cannot be measured.
[0113] Performance Test:
[0114] The electrostatic capacity of the prepared electrode materials ①-⑤ was measured respectively
[0115] Test method: After subjecting electrode materials ①-⑤ to a 510V chemical treatment in a boric acid aqueous solution (50 g / L), the results were measured using an ammonium borate aqueous solution (3 g / L).
[0116] Table 1
[0117] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 <![CDATA[Effective volume (cm 3 )]]> 6.28 6.25 6.26 6.28 6.25 <![CDATA[Capacitance (μF / cm 3 )]]> 87.25 86.89 89.41 85.33 85.36
[0118] It can be seen from Table 1 that the electrode material prepared by the method of the present invention has a higher electrostatic capacitance than that of Comparative Example 1 and Comparative Example 2.
[0119] It can be seen from Comparative Example 3 that the preparation method of the present invention can effectively solve the problem that when preparing capacitors, the bending resistance of the anode foil is required to be high during the winding process, and micro cracks are prone to appear on the edges of the foil.
[0120] In the description of this specification, the description with reference to the terms "some embodiments", "other embodiments", "embodiment", "example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0121] Although the embodiments and examples of the present invention have been shown and described above, it is to be understood that the above embodiments and examples are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments and examples within the scope of the present invention.
Claims
1. A method for preparing an electrode material, characterized in that: The preparation method comprises: S1 Gluing: Mixing the solvent and the cross-linking agent, performing glue treatment, and obtaining glue solution; S2 Plastic film: Aluminum powder is dispersed in the glue solution and pressed to obtain the material to be processed; wherein the plastic film is performed twice or more, and the particle size D of the aluminum powder used in the two adjacent plastic films is 50 different; S3 sintering: sintering the material to be processed to obtain the electrode material.
2. The method for preparing an electrode material according to claim 1, characterized in that: The solvent is selected from at least one of ethanol, water, toluene, acetone and ethylene glycol ether; The crosslinking agent is selected from at least one of epoxy resin, vinyl alcohol resin, fluoroethylene resin, epoxy resin, paraffin and ethyl cellulose; Optionally, the mass ratio of the solvent to the cross-linking agent is (5-100):1; preferably (5-50):1; preferably (5-20):1; Preferably it is (5-10):1; preferably it is (5-7.5):1; preferably it is (7.5-10):1; preferably it is 5:1, 7.5:1, 10:
1.
3. The method for preparing an electrode material according to claim 1, characterized in that: The aluminum powder used in the S2 plastic film is independently selected from any one of small-particle aluminum powder or large-particle aluminum powder.
4. The method for preparing the electrode material according to claim 3, characterized in that: The particle size of small aluminum powder is D 50 0.1-3.5 μm; preferably 0.5-3.0 μm; preferably 1.0-3.0 μm; preferably 1.5-3.0 μm; preferably 1.5-2.5 μm; preferably 1.5 μm, 2 μm, 2.5 μm; Particle size D of large aluminum powder 50 It is 3.5-20μm, preferably 3.5-15μm, preferably 3.5-10μm, preferably 3.5-5.5μm, preferably 3.5-4.5μm, preferably 3.5μm, 4.0μm, 4.5μm.
5. The method for preparing an electrode material according to claim 1, characterized in that: In S3, the sintering temperature is 500-650°C; optionally, the sintering time is 1-20h; preferably 1-10h; Optionally, before sintering, a pre-sintering treatment is performed, wherein the temperature of the pre-sintering treatment is 300-450° C.; Optionally, the pre-sintering treatment time is 0.1-20 hours, preferably 0.1-10 hours.
6. The method for preparing an electrode material according to claim 1, characterized in that: In the S2 plastic film, the mass ratio of aluminum powder to adhesive liquid is independently (0.1-10):1; preferably (0.1-8):1; preferably (0.1-5):1; preferably (0.1-1):
1.
7. The method for preparing an electrode material according to claim 1, characterized in that: In the S2 plastic film, the pressure of the pressurized molding is independently 2-10MPa; preferably 2-5MPa; preferably 2MPa, 2.5MPa, 3MPa, 3.5MPa, 4.0MPa, 4.5MPa, 5MPa.
8. The method for preparing an electrode material according to claim 1, characterized in that: S3 sintering is carried out in vacuum, inert or reducing atmosphere; Optionally, the inert atmosphere is selected from at least one of helium, neon, argon and nitrogen; Optionally, the reducing atmosphere is selected from at least one of hydrogen, alkanes and alkenes.
9. An electrode material, characterized in that: The method is prepared by any one of claims 1 to 8.
10. A capacitor, characterized in that: The electrode material used in the capacitor is prepared by the preparation method according to any one of claims 1 to 8; Or it is the electrode material as described in claim 9.
Citation Information
Patent Citations
Improved production method of solid electrolytic condenser
CN103456502A
Aluminum electrolytic capacitor and preparation method thereof
CN109994318A
Aluminum alloy foil for electrolytic capacitor, aluminum alloy laminated foil for electrolytic capacitor, and manufacturing method therefor
JP2005294281A
Electrode material for aluminum electrolytic capacitor and method of manufacturing the same