Epitaxial wafer and preparation method thereof

By controlling the growth rate ratio of the nucleation layer and substrate processing of the gallium nitride epitaxial sheet, the crystal quality of the nucleation layer is optimized, the high defect density problem is solved, and the performance and uniformity of the epitaxial sheet are improved.

CN118943007AInactive Publication Date: 2024-11-12ZHONGHUAN ADVANCED SEMICONDUCTOR TECHNOLOGY CO LTD

Patent Information

Application Number
CN202410995358.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The nucleation layer of the gallium nitride (GaN) epitaxial sheet has high defect density due to lattice mismatch, which affects crystal quality and performance.

Method used

By controlling the growth rate of the first nucleation layer to be less than or equal to the growth rate of the second nucleation layer, the crystal quality and surface holes of the nucleation layer are optimized, the time for the transformation of the 3D island structure to the 2D layer growth is shortened, and the nucleation is reduced, and the nucleation is reduced. The crystal defect density of the layer. The specific method includes forming a first nucleation layer and a second nucleation layer in the reaction chamber, adjusting the flow rate and temperature of the aluminum source and nitrogen source, and ensuring that the growth rate ratio of the first nucleation layer and the second nucleation layer is 1≤ In the range of V2/V1≤10, and an aluminum layer is formed on the substrate to alleviate lattice mismatch.

Benefits of technology

The crystal quality and performance of the epitaxial sheet are improved, the defect density of the nucleation layer is reduced, the stress and warping problems are improved, the occurrence of surface microcracks is avoided, and the uniformity and conductivity of the epitaxial sheet are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943007A_ABST
    Figure CN118943007A_ABST
Patent Text Reader

Abstract

The invention discloses an epitaxial wafer and a preparation method thereof, and belongs to the technical field of semiconductor manufacturing. According to the preparation method of the epitaxial wafer, a substrate is positioned in a reaction cavity, and the preparation method comprises the following steps: forming a first nucleating layer which is positioned on the substrate; the first nucleation layer comprises a first nucleation sub-layer and a second nucleation sub-layer, the first nucleation sub-layer is located on one side of the substrate, and the second nucleation sub-layer is located on the side, away from the substrate, of the first nucleation sub-layer; wherein the rate of forming the first nucleation sublayer is a first rate V1, and the unit is mu m / h; the rate of forming the second nucleation sublayer is a second rate V2, the unit is [mu] m / h, and V1 is smaller than or equal to V2. The first rate V1 and the second rate V2 are controlled to meet the condition that V1 is smaller than or equal to V2, the crystal defect density of the first nucleating layer can be reduced, and therefore the crystal quality and performance of the epitaxial wafer are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to an epitaxial wafer and a method for preparing the same. Background Art

[0002] Gallium nitride (GaN) epitaxial wafers include nucleation layer, buffer layer, gradient buffer layer, channel layer, insertion layer, barrier layer, surface layer, etc. Among them, the nucleation layer is the basis of all subsequent epitaxial layers. Since the nucleation layer grows directly on the silicon substrate, the huge lattice mismatch between the nucleation layer and the silicon substrate makes the nucleation layer often a three-dimensional (3D) island-shaped polycrystalline structure with high defect density, which leads to a high defect density of the crystals of other subsequent epitaxial layers and affects the crystal quality and performance of the GaN epitaxial wafer. Summary of the invention

[0003] The purpose of the present application is to provide a method for preparing an epitaxial wafer, thereby reducing the crystal defect density of the first nucleation layer and improving the performance of the epitaxial wafer.

[0004] The first aspect of the present application provides a method for preparing an epitaxial wafer, wherein a substrate is placed in a reaction chamber, and the preparation method comprises:

[0005] forming a first nucleation layer, wherein the first nucleation layer is located on the substrate; the first nucleation layer comprises a first nucleation sublayer and a second nucleation sublayer, wherein the first nucleation sublayer is located on one side of the substrate, and the second nucleation sublayer is located on a side of the first nucleation sublayer away from the substrate;

[0006] The rate of forming the first nucleation sublayer is the first rate V1, in μm / h;

[0007] The rate of forming the second nucleation sublayer is a second rate V2, with a unit of μm / h, satisfying: V1≤V2.

[0008] In some embodiments, the first rate V1 and the second rate V2 satisfy: 1≤V2 / V1≤10.

[0009] In some embodiments, the first velocity V1 ranges from 0.1 to 0.3 μm / h.

[0010] In some embodiments, the second velocity V2 is in the range of 0.3-2 μm / h.

[0011] In some embodiments, the method of forming the first nucleation layer comprises:

[0012] introducing a first aluminum source and a nitrogen source into the reaction chamber;

[0013] Form a first nucleation sub-layer on the substrate; during the formation of the first nucleation sub-layer, the flow rate of the first aluminum source is a first flow rate Q1, and the flow rate of the nitrogen source is a second flow rate Q2;

[0014] Form a second nucleation sub-layer on the side of the first nucleation sub-layer facing away from the substrate; during the formation of the second nucleation sub-layer, the flow rate of the first aluminum source is a third flow rate Q3, and the flow rate of the nitrogen source is a fourth flow rate Q4;

[0015] Satisfy: Q4 / Q3 < Q2 / Q1, where the units of Q1 and Q3 are sccm, and the units of Q2 and Q4 are slm.

[0016] In some embodiments, the first flow rate Q1, the second flow rate Q2, the third flow rate Q3, and the fourth flow rate Q4 satisfy: Q1 < Q3, Q4 ≤ Q2; or, satisfy: Q1 = Q3, Q4 < Q2.

[0017] In some embodiments, the range of the first flow rate Q1 is 200 - 300 sccm.

[0018] In some embodiments, the range of the second flow rate Q2 is 1 - 5 slm.

[0019] In some embodiments, the range of the third flow rate Q3 is 300 - 6000 sccm.

[0020] In some embodiments, the range of the fourth flow rate Q4 is 0.5 - 1 slm.

[0021] In some embodiments, the first aluminum source is selected from at least one of trimethylaluminum and triethylaluminum.

[0022] In some embodiments, the nitrogen source is selected from ammonia gas.

[0023] In some embodiments, the time range for forming the first nucleation sub-layer is 1 - 5 min.

[0024] In some embodiments, the time range for forming the second nucleation sub-layer is 3 - 10 min.

[0025] In some embodiments, before forming the first nucleation layer, the preparation method further includes:

[0026] Introduce a second aluminum source into the reaction chamber to form an aluminum layer on the substrate.

[0027] In some embodiments, the second aluminum source is selected from at least one of trimethylaluminum and triethylaluminum.

[0028] In some embodiments, the flow rate of the second aluminum source is in the range of 10 to 50 sccm.

[0029] In some embodiments, the time for forming the aluminum layer is in the range of 1 to 10 minutes.

[0030] In some embodiments, the aluminum layer has a thickness ranging from 1 to 10 nm.

[0031] In some embodiments, after forming the first nucleation layer, the preparation method further comprises:

[0032] forming a second nucleation layer on a side of the first nucleation layer facing away from the substrate;

[0033] The temperature for forming the first nucleation layer is the first temperature T1, and the temperature for forming the second nucleation layer is the second temperature T2, satisfying: T1 <T2。

[0034] In some embodiments, the first temperature T1 ranges from 850 to 950°C.

[0035] In some embodiments, the second temperature T2 is in the range of 1050-1150°C.

[0036] In some embodiments, after forming the second nucleation layer on a side of the first nucleation layer facing away from the substrate, the preparation method further includes:

[0037] forming a first buffer layer on a side of the second nucleation layer away from the first nucleation layer;

[0038] A second buffer layer is formed on a side of the first buffer layer facing away from the second nucleation layer.

[0039] In some embodiments, after forming the second buffer layer, the preparation method further includes:

[0040] the channel layer on a side of the second buffer layer facing away from the first buffer layer;

[0041] forming an insertion layer on a side of the channel layer away from the second buffer layer;

[0042] forming a barrier layer on a side of the insertion layer facing away from the channel layer;

[0043] A surface layer is formed on a side of the barrier layer facing away from the insertion layer.

[0044] A second aspect of the present application provides an epitaxial wafer, comprising:

[0045] substrate;

[0046] The first nucleation layer, the first nucleation layer is located on the substrate; the first nucleation layer includes a first nucleation sub-layer and a second nucleation sub-layer, the first nucleation sub-layer is located on one side of the substrate, and the second nucleation sub-layer is located on the side of the first nucleation sub-layer away from the substrate;

[0047] Wherein, the rate of forming the first nucleation sub-layer is the first rate V1, with the unit of μm / h; the rate of forming the second nucleation sub-layer is the second rate V2, with the unit of μm / h, and it satisfies: V1 ≤ V2.

[0048] In some embodiments, the first nucleation layer has a first thickness H1, the first nucleation sub-layer has a second thickness H2, and the second nucleation sub-layer has a third thickness H3, and it satisfies: H2 + H3 ≤ H1, H2 < H3. Wherein, the units of H1, H2, and H3 are nm.

[0049] In some embodiments, the range of the first thickness H1 is 150 - 200 nm.

[0050] In some embodiments, the range of the second thickness H2 is 10 - 50 nm.

[0051] In some embodiments, the range of the third thickness H3 is 70 - 150 nm.

[0052] In some embodiments, the crystal quality of the epitaxial wafer is 400 - 750 arcsec.

[0053] The beneficial effects of the present application are as follows:

[0054] The present application provides a method for preparing an epitaxial wafer, with the substrate located in the reaction chamber. The preparation method includes: forming a first nucleation layer, the first nucleation layer is located on the substrate, the first nucleation layer includes a first nucleation sub-layer and a second nucleation sub-layer, the first nucleation sub-layer is located on one side of the substrate, and the second nucleation sub-layer is located on the side of the first nucleation sub-layer away from the substrate; wherein, the rate of forming the first nucleation sub-layer is the first rate V1, with the unit of μm / h; the rate of forming the second nucleation sub-layer is the second rate V2, with the unit of μm / h, and it satisfies: V1 ≤ V2. By controlling the first rate V1 and the second rate V2 to satisfy: V1 ≤ V2, the present application can optimize the crystal quality and surface holes of the first nucleation layer, shorten the time for the transformation from the 3D island structure to the 2D layer growth during the growth process of the first nucleation layer, and reduce the crystal defect density of the first nucleation layer, thereby improving the crystal quality and performance of the epitaxial wafer. Description of the Drawings

[0055] Figure 1 It is a schematic structural diagram of the epitaxial wafer provided by the embodiment of the present application;

[0056] Figure 2This is a test curve diagram of the crystal quality (AlN (002) FWHM) of the epitaxial wafers prepared in Example 2, Example 4 and Comparative Example 2 detected by X-ray diffractometer (XRD) in this application;

[0057] Figure 3 This is a test curve diagram of the crystal quality (GaN (002) FWHM) of the epitaxial wafers prepared in Example 1, Example 3 and Comparative Example 1 detected by X-ray diffractometer (XRD) in this application;

[0058] Figure 4 This is an atomic force microscope (AFM) image of Example 2 of the present application;

[0059] Figure 5 This is an atomic force microscope (AFM) image of Example 4 of the present application;

[0060] Figure 6 This is an atomic force microscope (AFM) image of Example 6 of the present application;

[0061] Figure 7 This is an atomic force microscope (AFM) image of Comparative Example 2 of the present application.

[0062] In the accompanying drawings, the components represented by the reference numerals are as follows:

[0063] 1. Substrate; 2. First nucleation layer; 21. First nucleation sublayer; 22. Second nucleation sublayer; 3. Aluminum layer; 4. Second nucleation layer; 5. First buffer layer; 6. Second buffer layer; 7. Channel layer; 8. Insertion layer; 9. Barrier layer; 10. Surface layer. DETAILED DESCRIPTION

[0064] The technical solution of the present application will be described clearly and completely below in conjunction with the embodiments and drawings of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application. The various embodiments of the present application may exist in the form of a range; it should be understood that the description in the form of a range is only for convenience and simplicity, and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single values ​​within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which are applicable regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any quoted numbers (fractions or integers) within the indicated range.

[0065] like Figure 1 As shown, the first aspect of the present application provides a method for preparing an epitaxial wafer, wherein a substrate 1 is located in a reaction chamber, and the preparation method comprises:

[0066] A first nucleation layer 2 is formed, and the first nucleation layer 2 is located on the substrate 1; the first nucleation layer 2 includes a first nucleation sublayer 21 and a second nucleation sublayer 22, the first nucleation sublayer 21 is located on one side of the substrate 1, and the second nucleation sublayer 22 is located on the side of the first nucleation sublayer 21 away from the substrate 1; wherein, the rate of forming the first nucleation sublayer 21 is a first rate V1, and the unit is μm / h; the rate of forming the second nucleation sublayer 22 is a second rate V2, and the unit is μm / h, satisfying: V1≤V2.

[0067] It can be understood that when the epitaxial growth method is adopted to prepare the epitaxial wafer, the rate of forming the first nucleation sublayer 21 is also the growth rate of the first nucleation sublayer 21, and the rate of forming the second nucleation sublayer 22 is also the growth rate of the second nucleation sublayer 22. The present application controls the first rate V1 and the second rate V2 to satisfy: V1≤V2, so that the growth rate of the first nucleation sublayer 21 is less than or equal to the growth rate of the second nucleation sublayer 22, thereby optimizing the crystal quality and surface holes of the first nucleation layer 2, shortening the time for the first nucleation layer 2 to transform from a three-dimensional (3D) island structure to a two-dimensional (2D) layered growth during the growth process, reducing the crystal defect density of the first nucleation layer 2, and thus improving the crystal quality and performance of the epitaxial wafer.

[0068] In some implementations, the first rate V1 and the second rate V2 satisfy: 1≤V2 / V1≤10. Specifically, the ratio of V2 / V1 may be any one of 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or a range consisting of any two values.

[0069] It can be understood that the present application controls the first rate V1 and the second rate V2 to satisfy: 1≤V2 / V1≤10, so that the growth rate of the second nucleation sublayer 22 is greater than or equal to 1 times the growth rate of the first nucleation sublayer 21, and the growth rate of the second nucleation sublayer 22 is less than or equal to 10 times the growth rate of the first nucleation sublayer 21. This can optimize the crystal quality and surface holes of the first nucleation layer 2, shorten the time for the first nucleation layer 2 to transform from a 3D island structure to a 2D layered growth during the growth process, reduce the crystal defect density of the first nucleation layer 2, and thus improve the crystal quality and performance of the epitaxial wafer.

[0070] In some embodiments, the first rate V1 ranges from 0.1 to 0.3 μm / h. Specifically, the first rate V1 (unit: μm / h) can be any one of 0.1, 0.15, 0.2, 0.22, 0.24, 0.26, 0.28, 0.3, or a range consisting of any two values.

[0071] In some embodiments, the range of the second rate V2 is 0.3 to 2 μm / h. Specifically, the second rate V2 (unit: μm / h) can be any value among 0.3, 0.5, 0.8, 1, 1.2, 1.5, 1.7, 2 or a range composed of any two of these values.

[0072] In some embodiments, the method for forming the first nucleation layer 2 includes:

[0073] Introducing a first aluminum source and a nitrogen source into the reaction chamber;

[0074] Forming a first nucleation sub-layer 21 on the substrate 1; during the formation of the first nucleation sub-layer 21, the flow rate of the first aluminum source is the first flow rate Q1, and the flow rate of the nitrogen source is the second flow rate Q2;

[0075] Forming a second nucleation sub-layer 22 on the side of the first nucleation sub-layer 21 away from the substrate 1; during the formation of the second nucleation sub-layer 22, the flow rate of the first aluminum source is the third flow rate Q3, and the flow rate of the nitrogen source is the fourth flow rate Q4;

[0076] Satisfying: Q4 / Q3 < Q2 / Q1, where the units of Q1 and Q3 are sccm, and the units of Q2 and Q4 are slm.

[0077] It can be understood that the formation rates of the first nucleation sub-layer 21 and the second nucleation sub-layer 22 are determined by the flow rate of the first aluminum source during the growth process. By controlling the V / III ratio when forming the first nucleation sub-layer 21 and the second nucleation sub-layer 22 in this application, the formation of the 3D island structure can be ensured, and the growth of higher quality during the 2D layer growth process can be ensured, improving the stress and warpage of the epitaxial wafer, and further improving the crystal quality of the subsequent epitaxial layer.

[0078] In some embodiments, the first flow rate Q1, the second flow rate Q2, the third flow rate Q3, and the fourth flow rate Q4 satisfy: Q1 < Q3, Q4 ≤ Q2.

[0079] It can be understood that by making the flow rate of the first aluminum source when forming the first nucleation sublayer 21 less than the flow rate of the first aluminum source when forming the second nucleation sublayer 22, the growth rate of the first nucleation sublayer 21 is achieved to be less than the growth rate of the second nucleation sublayer 22, thereby optimizing the crystal quality and surface holes of the first nucleation layer 2, shortening the time for the transformation of the 3D island structure to the 2D layered growth during the first nucleation layer 2, and thereby improving the overall performance of the epitaxial wafer; further, by controlling the flow rate of the nitrogen source when forming the first nucleation sublayer 21 to be greater than or equal to the flow rate of the nitrogen source when forming the second nucleation sublayer 22, the V / III ratio of the first nucleation sublayer 21 and the second nucleation sublayer 22 can be regulated, which can not only ensure the formation of the 3D island structure, but also ensure higher quality growth during the 2D layered growth process, improve the stress and warping of the epitaxial wafer, and thereby further improve the crystal quality of the subsequent epitaxial layer.

[0080] In some embodiments, the first flow rate Q1, the second flow rate Q2, the third flow rate Q3 and the fourth flow rate Q4 satisfy: Q1 = Q3, Q4 <Q2。

[0081] It can be understood that by making the flow rate of the first aluminum source when forming the first nucleation sublayer 21 equal to the flow rate of the first aluminum source when forming the second nucleation sublayer 22, the growth rates of the first nucleation sublayer 21 and the second nucleation sublayer 22 are roughly the same, and then by controlling the flow rate of the nitrogen source when forming the first nucleation sublayer 21 to be greater than the flow rate of the nitrogen source when forming the second nucleation sublayer 22, the V / III ratio of the first nucleation sublayer 21 and the second nucleation sublayer 22 can be regulated, which can not only ensure the formation of a 3D island structure, but also ensure higher quality growth in the 2D layered growth process, improve the stress and warping of the epitaxial wafer, and further improve the crystal quality of the subsequent epitaxial layer.

[0082] In some embodiments, the first flow rate Q1 ranges from 200 to 300 sccm. Specifically, the first flow rate Q1 (unit: sccm) can be any one of 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300 or a range consisting of any two values.

[0083] In some embodiments, the second flow rate Q2 ranges from 1 to 5 slm. Specifically, the second flow rate Q2 (unit: slm) can be any one of 1, 2, 3, 4, and 5, or a range consisting of any two values.

[0084] In some embodiments, the third flow rate Q3 ranges from 300 to 6000 sccm. Specifically, the third flow rate Q3 (unit: sccm) can be any one of 300, 350, 400, 450, 500, 550, and 600, or a range consisting of any two values.

[0085] In some embodiments, the range of the fourth flow rate Q4 is 0.5 to 1 slm. Specifically, the fourth flow rate Q4 (unit: slm) can be any value among 0.5, 0.6, 0.7, 0.8, 0.9, 1 or a range composed of any two of these values.

[0086] In some embodiments, the first aluminum source is selected from at least one of trimethylaluminum and triethylaluminum.

[0087] In some embodiments, the nitrogen source is selected from ammonia gas.

[0088] In some embodiments, the first nucleation layer 2 has a first thickness H1, the first nucleation sub-layer 21 has a second thickness H2, and the second nucleation sub-layer 22 has a third thickness H3, satisfying: H2 + H3 ≤ H1, H2 < H3, where the units of H1, H2, and H3 are nm.

[0089] It can be understood that forming the first nucleation layer 2 on one side of the substrate 1 can introduce compressive stress to compensate for the tensile stress of the epitaxial wafer. By controlling the first thickness H1, the second thickness H2, and the third thickness H3 to satisfy: H2 + H3 ≤ H1, H2 < H3, the stress and warping in the epitaxial growth process can be improved, the occurrence of surface microcracks can be avoided, and the quality and uniformity of the epitaxial wafer can be improved.

[0090] In some embodiments, the thickness range of the first nucleation layer 2 is 150 to 200 nm. Specifically, the thickness of the first nucleation layer 2 (unit: nm) can be any value among 150, 160, 170, 180, 190, 200 or a range composed of any two of these values.

[0091] It can be understood that by controlling the thickness range of the first nucleation layer 2 to be 150 to 200 nm, compressive stress can be introduced to compensate for the tensile stress of the epitaxial wafer, thereby improving the stress and warping in the epitaxial growth process, avoiding the occurrence of surface microcracks, reducing the defect density of the epitaxial wafer, improving the quality and uniformity of the epitaxial wafer, and thus improving the performance of the epitaxial wafer.

[0092] In some embodiments, the thickness range of the first nucleation sub-layer 21 is 10 to 50 nm. Specifically, the thickness of the first nucleation sub-layer 21 (unit: nm) can be any value among 10, 15, 20, 25, 30, 35, 40, 45, 50 or a range composed of any two of these values.

[0093] It can be understood that by controlling the thickness range of the first nucleation sub-layer 21 to be 10 to 50 nm, the lattice mismatch between the substrate 1 and the first nucleation layer 2 can be alleviated.

[0094] In some embodiments, the thickness of the second nucleation sublayer 22 ranges from 70 to 150 nm. Specifically, the thickness (unit: nm) of the second nucleation sublayer 22 can be any one of 70, 80, 90, 100, 110, 120, 130, 140, and 150, or a range consisting of any two values.

[0095] It can be understood that, in the present application, by controlling the thickness of the second nucleation sublayer 22 to be in the range of 70 to 150 nm, the crystal quality of the first nucleation layer 2 can be improved.

[0096] In some embodiments, the time range for forming the first nucleation sublayer 21 is 1 to 5 minutes. Specifically, the time (unit: min) for forming the first nucleation sublayer 21 can be any one of 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 or a range consisting of any two values.

[0097] It is understandable that by controlling the time range for forming the first nucleation sublayer 21 to be 1 to 5 minutes and the flow rates of the first aluminum source and the nitrogen source when forming the first nucleation sublayer 21 , the thickness range of the formed first nucleation sublayer 21 can be controlled.

[0098] In some embodiments, the time range for forming the second nucleation sublayer 22 is 3 to 10 minutes. Specifically, the time (unit: min) for forming the second nucleation sublayer 22 can be any one of 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10 or a range consisting of any two values.

[0099] It is understandable that by controlling the time range for forming the second nucleation sublayer 22 to be 3 to 10 minutes and the flow rates of the first aluminum source and the nitrogen source when forming the second nucleation sublayer 22 , the thickness range of the formed second nucleation sublayer 22 can be controlled.

[0100] In some embodiments, before forming the first nucleation layer 2, the preparation method further comprises:

[0101] A second aluminum source is introduced into the reaction chamber to form an aluminum layer 3 on the substrate 1 .

[0102] It can be understood that the present application can improve the lattice mismatch between the first nucleation layer 2 and the substrate 1, improve the crystal quality of the first nucleation layer 2, reduce the defect density of the epitaxial wafer, and thus improve the performance of the epitaxial wafer by forming the aluminum layer 3 on the substrate 1 before forming the first nucleation layer 2.

[0103] In some embodiments, the second aluminum source is selected from at least one of trimethylaluminum and triethylaluminum.

[0104] In some embodiments, the flow rate range of the second aluminum source is 10 to 50 sccm. Specifically, the flow rate of the second aluminum source (unit: sccm) can be any value among 10, 15, 20, 25, 30, 35, 40, 45, 50 or a range composed of any two values.

[0105] In some embodiments, the time range for forming the aluminum layer 3 is 1 to 10 min. Specifically, the time for forming the aluminum layer 3 (unit: min) can be any value among 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10 or a range composed of any two values.

[0106] In some embodiments, the thickness range of the aluminum layer 3 is 1 to 10 nm. Specifically, the thickness of the aluminum layer 3 (unit: nm) can be any value among 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or a range composed of any two values.

[0107] It can be understood that in this application, by first forming the aluminum layer 3 on the substrate 1 before forming the first nucleation layer 2 and controlling the thickness range of the aluminum layer 3 to be 1 to 10 nm, the lattice mismatch between the first nucleation layer 2 and the substrate 1 can be improved, the crystal quality of the first nucleation layer 2 can be further enhanced, the defect density of the epitaxial wafer can be reduced, and thus the performance of the epitaxial wafer can be improved.

[0108] In some embodiments, after forming the first nucleation layer 2, the preparation method further includes:

[0109] Forming a second nucleation layer 4 on the side of the first nucleation layer 2 facing away from the substrate 1;

[0110] The temperature for forming the first nucleation layer 2 is the first temperature T1, and the temperature for forming the second nucleation layer 4 is the second temperature T2, satisfying: T1 < T2, and the units of T1 and T2 are °C.

[0111] It can be understood that the temperature for forming the first nucleation layer 2 is also the growth temperature of the first nucleation layer 2, and the temperature for forming the second nucleation layer 4 is also the growth temperature of the second nucleation layer 4. In this application, by forming the second nucleation layer 4 on the side of the first nucleation layer 2 facing away from the substrate 1; and the growth temperature of the second nucleation layer 4 is greater than the growth temperature of the first nucleation layer 2, the penetrating dislocations formed during the growth of the first nucleation layer 2 can be filtered, and the crystal defect density of the first nucleation layer 2 can be reduced.

[0112] In some embodiments, the range of the first temperature T1 is 850 to 950 °C. Specifically, the first temperature T1 (unit: °C) can be any value among 850, 860, 870, 880, 890, 900, 910, 920, 930, 940, 950 or a range composed of any two values.

[0113] In some embodiments, the second temperature T2 ranges from 1050 to 1150° C. Specifically, the second temperature T2 (unit: ° C.) can be any one of 1050, 1060, 1070, 1080, 1090, 1100, 1110, 1120, 1130, 1140, and 1150, or a range consisting of any two values.

[0114] In some embodiments, after forming the second nucleation layer 4 on the side of the first nucleation layer 2 facing away from the substrate 1, the preparation method further comprises:

[0115] A first buffer layer 5 is formed on a side of the second nucleation layer 4 facing away from the first nucleation layer 2;

[0116] The second buffer layer 6 is formed on the side of the first buffer layer 5 facing away from the second nucleation layer 4 .

[0117] It can be understood that the formation of the first nucleation layer 2 on one side of the substrate 1 can introduce compressive stress to compensate for the tensile stress of the epitaxial wafer, thereby improving the stress and warping during the epitaxial growth process, avoiding the occurrence of surface microcracks, and improving the quality and uniformity of the epitaxial wafer; the formation of the second nucleation layer 4 on the side of the first nucleation layer 2 away from the substrate 1 can filter the penetrating dislocations formed by the growth of the first nucleation layer 2 and reduce the crystal defect density; the formation of the first buffer layer 5 on the side of the second nucleation layer 4 away from the first nucleation layer 2 can filter the penetrating dislocations formed by the growth of the first nucleation layer 2 and reduce the crystal defect density; the formation of the second buffer layer 6 on the side of the first buffer layer 5 away from the second nucleation layer 4, the second buffer layer 6 is a superlattice stacking structure, which can increase the impedance of the epitaxial wafer in the vertical direction, thereby improving the vertical breakdown voltage of the epitaxial wafer and the device.

[0118] In some embodiments, after forming the second buffer layer 6, the preparation method further comprises:

[0119] forming a channel layer 7 on a side of the second buffer layer 6 facing away from the first buffer layer 5;

[0120] An insertion layer 8 is formed on a side of the channel layer 7 away from the second buffer layer 6;

[0121] A barrier layer 9 is formed on a side of the insertion layer 8 facing away from the channel layer 7;

[0122] A surface layer 10 is formed on the side of the barrier layer 9 facing away from the insertion layer 8 .

[0123] It can be understood that a channel layer 7 is formed on the side of the second buffer layer 6 away from the first buffer layer 5, and the spontaneous polarization of GaN in the channel layer 7 generates a large number of conductive electrons in the channel layer 7. The electron density is higher on the side close to the insertion layer 8, making the channel layer 7 conductive; an insertion layer 8 and a barrier layer 9 are successively formed on the side of the channel layer 7 away from the second buffer layer 6. On the one hand, the piezoelectric polarization between the channel layer 7 and the barrier layer 9 will increase the electron density in the channel layer 7 and improve the conductivity of the channel layer 7. On the other hand, the insertion layer 8 will reduce the carrier scattering between the channel layer 7 and the barrier layer 9 and improve the conductivity of the channel layer 7; a surface layer 10, i.e., a cap layer, is formed on the side of the barrier layer 9 away from the insertion layer 8, which can protect the barrier layer 9 and prevent the barrier layer 9 from being oxidized, thereby improving the performance of the epitaxial wafer.

[0124] In some embodiments, the thickness of the second nucleation layer 4 is 200-300 nm. Specifically, the thickness of the second nucleation layer 4 (unit: nm) can be any one of 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300 or a range consisting of any two values.

[0125] In some embodiments, the thickness of the first buffer layer 5 is 1500-2000 nm. Specifically, the thickness (unit: nm) of the first buffer layer 5 can be any one of 1500, 1600, 1700, 1800, 1900, and 2000, or a range consisting of any two values.

[0126] In some embodiments, the thickness of the second buffer layer 6 is 1200-1800 nm. Specifically, the thickness (unit: nm) of the second buffer layer 6 can be any one of 1200, 1300, 1400, 1500, 1600, 1700, 1800 or a range consisting of any two values.

[0127] In some embodiments, the thickness of the channel layer 7 is 150-200 nm. Specifically, the thickness of the channel layer 7 (unit: nm) can be any one of 150, 160, 170, 180, 190, and 200, or a range consisting of any two values.

[0128] In some embodiments, the thickness of the insertion layer 8 is 0.5-2 nm. Specifically, the thickness of the insertion layer 8 (unit: nm) can be any one of 0.5, 1, 1.5, 2, or a range consisting of any two values.

[0129] In some embodiments, the thickness of the barrier layer 9 is 15-25 nm. Specifically, the thickness of the barrier layer 9 (unit: nm) can be any one of 15, 18, 20, 13, and 25, or a range consisting of any two values.

[0130] In some embodiments, the thickness of the surface layer 10 is 1-3 nm. Specifically, the thickness (unit: nm) of the surface layer 10 can be any one of 1, 1.5, 2, 2.5, 3, or a range consisting of any two values.

[0131] It can be understood that due to the lattice mismatch and thermal mismatch between the substrate 1 and the first nucleation layer 2, cracks are prone to form on the surface of the epitaxial layer, and the thicker the epitaxial layer, the more difficult it is to avoid surface cracks. Therefore, the first nucleation layer 2, the aluminum layer 3, the second nucleation layer 4, the first buffer layer 5, the second buffer layer 6, the channel layer 7, the insertion layer 8, the barrier layer 9 and the surface layer 10 must have a certain thickness to achieve their functions, and at the same time, an upper limit needs to be set for their thickness to avoid excessive thickness of the epitaxial layer and cause cracks on the surface of the epitaxial wafer. The present application controls the thickness of the second nucleation layer 4 to be 200-300nm, which can reduce pinholes on the surface of the second nucleation layer 4 and avoid surface cracks, while providing appropriate tensile stress to balance compressive stress and improve the crystal quality of the epitaxial wafer. By controlling the thickness of the first buffer layer 5 to be 1500-2000nm, the threading dislocations formed in the first nucleation layer 2 can be filtered. By controlling the thickness of the second buffer layer 6 to be 1200-18 00nm, the impedance of the epitaxial wafer in the vertical direction can be increased; by controlling the thickness of the channel layer 7 to 150-200nm, the channel layer 7 can have a certain thickness to improve the horizontal withstand voltage. At the same time, an overly thick channel layer 7 will lead to a decrease in the quality of its surface crystal and an increase in the defect density, which will reduce the conductivity of the channel layer 7 and deteriorate the core performance of the epitaxial wafer; by controlling the thickness of the insertion layer 8 to 0.5-2nm, it can be ensured that the insertion layer 8 completely covers the surface of the channel layer 7, inhibits the carrier scattering in the channel layer 7, and avoids the weakening of the piezoelectric polarization due to the excessive thickness of the insertion layer 8, which makes the conductivity of the channel layer 7 decrease; by controlling the thickness of the barrier layer 9 to 15-25nm, the square resistance range of the epitaxial wafer is 350-650Ω / sq to meet the needs of device preparation; by controlling the thickness of the surface layer 10 to 1-3nm, it can be ensured that the surface layer 10 covers the surface of the barrier layer 9, protects the barrier layer 9 and prevents it from oxidation.

[0132] In some embodiments, the material of the substrate 1 is selected from any one of silicon (Si), silicon carbide (SiC) or sapphire.

[0133] In some embodiments, the first buffer layer 5 includes an AlGaN layer stacked with K layers, satisfying: 2≤K≤5. Specifically, the value of K can be any one of 2, 3, 4, 5, or a range consisting of any two values.

[0134] In some embodiments, the material of the first buffer layer 5 is selected from AlGaN, and the chemical formula of AlGaN is Al x Ga 1-xN, wherein 0.05≤x≤0.95, and the molar content of Al in the first buffer layer 5 gradually decreases in the direction away from the substrate 1. Specifically, the value of x can be any one of 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, and 0.95, or a range consisting of any two values.

[0135] It can be understood that when the value of x, that is, the molar content of Al in the first buffer layer 5 satisfies the above value range, the defect density can be rapidly reduced while reducing the lattice mismatch of epitaxial growth.

[0136] In some embodiments, the second buffer layer 6 includes L stacked AlN / GaN layers, 40≤L≤60. Specifically, the value of L can be any one of 40, 42, 44, 46, 48, 50, 52, 54, 56, 58, 60 or a range consisting of any two values.

[0137] In some embodiments, in the AlN / GaN stack, the thickness of the AlN layer is 1 to 10 nm, and the thickness of the GaN layer is 10 to 50 nm. Specifically, the thickness of the AlN layer (unit: nm) can be any one of 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or a range consisting of any two values; the thickness of the GaN layer (unit: nm) can be any one of 10, 15, 20, 25, 30, 35, 40, 45, 50 or a range consisting of any two values.

[0138] In some embodiments, the material of the channel layer 7 is selected from GaN.

[0139] In some embodiments, the material of the insertion layer 8 is selected from any one of AlN, AlGaN or SiNx.

[0140] In some embodiments, the material of the barrier layer 9 is selected from AlGaN, and the chemical formula of AlGaN is Al y Ga 1-y N, wherein 0.15≤y≤0.25. Specifically, the value of y can be any one of 0.15, 0.18, 0.20, 0.23, 0.25, or a range consisting of any two values.

[0141] It can be understood that when the value of y, that is, the molar content of Al in the barrier layer 9 satisfies the above-mentioned range of values, the Al component can generate sufficient two-dimensional electron gas without increasing scattering and affecting mobility, thereby achieving an epitaxial wafer square resistance range of 350 to 650Ω / sq, which meets the requirements of device preparation.

[0142] In some embodiments, the material of the surface layer 10 is selected from any one of GaN, P-GaN, or SiNx.

[0143] The second aspect of the present application provides an epitaxial wafer, including:

[0144] A substrate 1;

[0145] A first nucleation layer 2, which is located on the substrate 1; the first nucleation layer 2 includes a first nucleation sub-layer 21 and a second nucleation sub-layer 22. The first nucleation sub-layer 21 is located on one side of the substrate 1, and the second nucleation sub-layer 22 is located on the side of the first nucleation sub-layer 21背离 the substrate 1.

[0146] Wherein, the rate of forming the first nucleation sub-layer 21 is the first rate V1, with the unit of μm / h; the rate of forming the second nucleation sub-layer 22 is the second rate V2, with the unit of μm / h, and it satisfies: V1 ≤ V2.

[0147] It can be understood that by controlling the first rate V1 and the second rate V2 of the present application to satisfy: 1 ≤ V2 / V1 ≤ 10, the growth rate of the second nucleation sub-layer 22 is greater than or equal to 1 times the growth rate of the first nucleation sub-layer 21, and the growth rate of the second nucleation sub-layer 22 is less than or equal to 10 times the growth rate of the first nucleation sub-layer 21, which can optimize the crystal quality and surface holes of the first nucleation layer 2, shorten the time for the transformation of the 3D island structure to the 2D layer growth during the growth of the first nucleation layer 2, reduce the crystal defect density of the first nucleation layer 2, and thus improve the crystal quality and performance of the epitaxial wafer.

[0148] In some embodiments, the first nucleation layer 2 has a first thickness H1, the first nucleation sub-layer 21 has a second thickness H2, and the second nucleation sub-layer 22 has a third thickness H3, which satisfies: H2 + H3 ≤ H1, H2 < H3, wherein the units of H1, H2, and H3 are nm.

[0149] It can be understood that the thickness of the first nucleation sub-layer 21 is related to the rate and time of forming the first nucleation sub-layer 21, the thickness of the second nucleation sub-layer 22 is related to the rate and time of forming the second nucleation sub-layer 22, and the thickness of the first nucleation layer 2 is positively correlated with the thickness of the first nucleation sub-layer 21 and the thickness of the second nucleation sub-layer 22. By forming the first nucleation layer 2 on one side of the substrate 1, compressive stress can be introduced to compensate for the tensile stress of the epitaxial wafer. By controlling the first thickness H1, the second thickness H2, and the third thickness H3 to satisfy: H2 + H3 ≤ H1, H2 < H3, the stress and warping during the epitaxial growth process can be improved, the occurrence of surface micro-cracks can be avoided, and the quality and uniformity of the epitaxial wafer can be improved.

[0150] In some embodiments, the thickness of the first nucleation layer 2 is in the range of 150-200 nm. Specifically, the thickness of the first nucleation layer 2 (unit: nm) can be any one of 150, 160, 170, 180, 190, 200 or a range consisting of any two values.

[0151] It can be understood that the present application can introduce compressive stress by controlling the thickness range of the first nucleation layer 2 to 150 to 200 nm to compensate for the tensile stress of the epitaxial wafer, thereby improving the stress and warping during the epitaxial growth process, avoiding the occurrence of surface microcracks, reducing the defect density of the epitaxial wafer, improving the quality and uniformity of the epitaxial wafer, and thus improving the performance of the epitaxial wafer.

[0152] In some embodiments, the thickness of the first nucleation sublayer 21 ranges from 10 to 50 nm. Specifically, the thickness (unit: nm) of the first nucleation sublayer 21 can be any one of 10, 15, 20, 25, 30, 35, 40, 45, 50 or a range consisting of any two values.

[0153] It can be understood that, in the present application, the lattice mismatch between the substrate 1 and the first nucleation layer 2 can be alleviated by controlling the thickness of the first nucleation sublayer 21 to be in the range of 10 to 50 nm.

[0154] In some embodiments, the thickness of the second nucleation sublayer 22 ranges from 70 to 150 nm. Specifically, the thickness (unit: nm) of the second nucleation sublayer 22 can be any one of 70, 80, 90, 100, 110, 120, 130, 140, and 150, or a range consisting of any two values.

[0155] It can be understood that, in the present application, by controlling the thickness of the second nucleation sublayer 22 to be in the range of 70 to 150 nm, the crystal quality of the first nucleation layer 2 can be improved.

[0156] In some embodiments, the crystal mass of the epitaxial wafer is 400-750 arcsec. Specifically, the crystal mass of the epitaxial wafer (unit: arcsec) can be any one of 400, 450, 500, 550, 600, 650, 700, 750 or a range consisting of any two values; the epitaxial wafer includes a substrate 1 and an aluminum layer 3, a first nucleation layer 2, a second nucleation layer 4, a first buffer layer 5, a second buffer layer 6, a channel layer 7, an insertion layer 8, a barrier layer 9, and a surface layer 10 stacked sequentially on one side of the substrate.

[0157] It can be understood that the epitaxial wafer provided in the present application has excellent crystal quality and device performance.

[0158] In some embodiments, after the substrate 1 is placed in the reaction chamber, the method further includes:

[0159] An etching gas is introduced into the reaction chamber to etch the substrate.

[0160] It is understandable that by introducing etching gas into the reaction chamber and etching the substrate, the strain damage layer on the surface of the substrate 1 can be removed, thereby improving the crystal quality of the subsequent epitaxial layer.

[0161] In some embodiments, the etching gas is selected from at least one of hydrogen, silane, and ethylene.

[0162] In some embodiments, the flow rate of the etching gas is 10-50 sccm. Specifically, the flow rate of the etching gas (unit: sccm) can be any one of 10, 15, 20, 25, 30, 35, 40, 45, 50 or a range consisting of any two values.

[0163] In some embodiments, the etching time is 3 to 20 minutes. Specifically, the etching time (unit: min) is any one of 3, 5, 10, 15, and 20, or a range consisting of any two values.

[0164] In some embodiments, a photoluminescence mapping (PLmapping) spectrometer is used to measure the thickness of the epitaxial wafer.

[0165] In some embodiments, the temperature of the reaction chamber and the epitaxial growth time are controlled by setting the temperature and the epitaxial growth time of the epitaxial device.

[0166] In some embodiments, the flow rate control method of the aluminum source, nitrogen source, gallium source, and etching gas is:

[0167] For gas, the gas flow rate is directly controlled by the mass flow meter; for liquid, the flow rate of the corresponding liquid is controlled by controlling the carrier gas flow rate.

[0168] The present application will be described below with reference to specific embodiments.

[0169] Example 1

[0170] S1: providing an 8-inch Si (111) substrate with a thickness of 1150 μm;

[0171] S2: In-situ hydrogen etching of the Si substrate in the epitaxial furnace, with a hydrogen flow rate of 200 slm, an etching temperature of 1060°C, and an etching time of 15 min to completely remove the strain damage layer on the surface of the Si substrate;

[0172] S3: Cool down to 730°C, adjust the hydrogen flow rate to 160 slm, and introduce trimethylaluminum with a flow rate of 20 sccm for 5 min, pre-lay a very thin aluminum layer with a thickness of 5 nm;

[0173] S4: Raise the temperature to 900°C, introduce trimethylaluminum with a flow rate of 250 sccm, and introduce ammonia with a flow rate of 3 slm for 3 minutes, and grow the first nucleation sublayer at a low speed with a thickness of 15 nm, which can better alleviate the lattice mismatch problem between the silicon substrate and the first nucleation layer;

[0174] S5: Change the flow rate of trimethylaluminum to 4000sccm and the duration to 3min, grow the second nucleation sublayer at a high speed with a thickness of 90nm, effectively shorten the time for the conversion of 3D island structure to 2D layered growth, and improve the crystal quality of the first nucleation layer;

[0175] S6: Continue to raise the temperature to 1100°C to grow a second AlN nucleation layer with a thickness of 250 nm;

[0176] S7: in-situ growing a first buffer layer on the AlN second nucleation layer, the first buffer layer comprising four AlGaN layers stacked in sequence, wherein the molar content of Al in each AlGaN layer is 80%, 50%, 30%, and 20%, respectively, and the thicknesses are 250 nm, 500 nm, 500 nm, and 500 nm, respectively;

[0177] S8: growing a second buffer layer on the first buffer layer, with a thickness of 2000 nm;

[0178] S9: growing a GaN channel layer on the second buffer layer with a thickness of 250 nm;

[0179] S10: growing an AlN insertion layer on the GaN channel layer with a thickness of 1 nm;

[0180] S11: growing an AlGaN barrier layer on the AlN insertion layer, wherein the molar content of Al in the AlGaN barrier layer is 23% and the thickness is 22 nm;

[0181] S12: growing a GaN surface layer on the AlGaN barrier layer with a thickness of 1 nm;

[0182] S13: Cooling in situ to room temperature to complete the growth of the GaN epitaxial wafer.

[0183] Example 2

[0184] The preparation method of Example 2 is the same as that of Example 1, except that steps S7 to S13 are omitted.

[0185] Example 3

[0186] The preparation method of Example 3 is the same as that of Example 1, except that: S5: the flow rate of ammonia gas is changed to 0.5 slm, the duration is 3 min, and the thickness is about 15 nm.

[0187] The preparation method of Example 4 is the same as that of Example 3, except that steps S7 to S13 are omitted.

[0188] Example 5

[0189] The preparation method of Example 5 is the same as that of Example 1, except that: S5: the flow rate of trimethylaluminum is changed to 400 sccm, the duration is 3 min, the second nucleation sublayer is grown at a high speed with a thickness of 90 nm, the flow rate of ammonia is changed to 0.5 slm, the duration is 3 min, and the thickness is about 15 nm.

[0190] The preparation method of Example 6 is the same as that of Example 5, except that steps S7 to S13 are omitted.

[0191] Comparative Example 1

[0192] The preparation method of Comparative Example 1 is the same as that of Example 1, except that: S4: the formation time of the first nucleation sublayer is 10 minutes, and step S5 is omitted.

[0193] Comparative Example 2

[0194] The preparation method of Comparative Example 2 is the same as that of Example 1, except that: S4: the formation time of the first nucleation sublayer is 10 minutes, and steps S5 and S7 to S13 are omitted.

[0195] Test method:

[0196] (1) The crystal quality (AlN (002) FWHM, peak width) of the epitaxial wafers prepared in Example 2, Example 4, Example 6, and Comparative Example 2 was measured using a high-resolution X-ray diffractometer (XRD). The test results are as follows: Figure 2 shown.

[0197] (2) The crystal quality (GaN (002) FWHM, peak width) of the epitaxial wafers prepared in Example 1, Example 3, Example 5 and Comparative Example 1 was tested by a high-resolution X-ray diffractometer (XRD). The test results are as follows: Figure 3 shown.

[0198] (3) The surface roughness Ra of the epitaxial wafers prepared in Example 2, Example 4, Example 6 and Comparative Example 2 was measured using an atomic force microscope (AFM). The test results are as follows: Figures 4 to 7 shown.

[0199] Table 1 shows the process step settings and process parameter settings of Examples 1 to 6 and Comparative Examples 1 to 2.

[0200]

[0201]

[0202] Table 2 shows the test results of Examples 1 to 6 and Comparative Examples 1 to 2.

[0203]

[0204] Result analysis:

[0205] From the test results of the AlN (002) surface crystal quality of the epitaxial wafers in Example 2, Example 4, Example 6 and Comparative Example 2, it can be seen that Example 2 has the smallest AlN (002) FWHM, that is, the aluminum nitride nucleation layer in Example 2 has the best crystal quality, indicating that the crystal quality of the AlN nucleation layer can be improved by making the growth rate of the first nucleation sublayer lower than the growth rate of the second nucleation sublayer.

[0206] From the test results of the crystal quality of the GaN (002) surface of the epitaxial wafers in Example 1, Example 2, Example 5 and Comparative Example 1, it can be seen that Example 1 has the smallest GaN (002) FWHM, that is, the gallium nitride epitaxial wafer in Example 1 has the best crystal quality, indicating that by making the growth rate of the first nucleation sublayer lower than the growth rate of the second nucleation sublayer, the crystal quality of the AlN nucleation layer can be improved, and the crystal quality of the GaN epitaxial wafer can be further improved.

[0207] From the surface morphology and surface roughness test results of the epitaxial wafers in Example 2, Example 4, Example 6 and Comparative Example 2, it can be seen that Example 4 has the smallest surface roughness Ra, and its GaN nucleation layer surface shows obvious step stripes, indicating that by making the V / III ratio of the first nucleation sublayer smaller than the V / III ratio of the second nucleation sublayer, the surface holes of the nucleation layer can be effectively improved, the crystal quality of the AlN nucleation layer can be improved, and the crystal quality of the GaN epitaxial wafer can be further improved.

[0208] The above is a detailed introduction to the present application. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for technical personnel in this field, according to the idea of ​​the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A method for preparing an epitaxial wafer, It is characterized in that The substrate (1) is placed in a reaction chamber, and the preparation method comprises: forming a first nucleation layer (2), wherein the first nucleation layer (2) is located on the substrate (1); the first nucleation layer (2) comprises a first nucleation sublayer (21) and a second nucleation sublayer (22), wherein the first nucleation sublayer (21) is located on one side of the substrate (1), and the second nucleation sublayer (22) is located on a side of the first nucleation sublayer (21) facing away from the substrate (1); The rate at which the first nucleation sublayer (21) is formed is a first rate V 1 , in μm / h; the rate of forming the second nucleation sublayer (22) is the second rate V 2 , in μm / h, satisfies: V 1 ≤V 2 .

2. The method for preparing an epitaxial wafer according to claim 1, It is characterized in that The first rate V 1 and the second rate V 2 Satisfy: 1≤V 2 / V 1 ≤10.

3. The method for preparing an epitaxial wafer according to claim 1, It is characterized in that The first rate V 1 The range is 0.1 to 0.3 μm / h; and / or The second rate V 2 The range is 0.3~2μm / h.

4. The method for preparing an epitaxial wafer according to claim 1, It is characterized in that The method for forming the first nucleation layer (2) comprises: introducing a first aluminum source and a nitrogen source into the reaction chamber; A first nucleation sublayer (21) is formed on the substrate (1); during the process of forming the first nucleation sublayer (21), the flow rate of the first aluminum source is a first flow rate Q 1 , the flow rate of the nitrogen source is the second flow rate Q 2 ; The second nucleation sublayer (22) is formed on the side of the first nucleation sublayer (21) facing away from the substrate (1); during the process of forming the second nucleation sublayer (22), the flow rate of the first aluminum source is a third flow rate Q 3 , the flow rate of the nitrogen source is the fourth flow rate Q 4 ; Satisfaction: Q 4 / Q 3 2 / Q 1 , where Q 1 and Q 3 The unit is sccm, Q 2 and Q 4 The unit is slm.​ 5. The method for preparing an epitaxial wafer according to claim 4, It is characterized in that The first flow rate Q 1 The second flow rate Q 2 , the third flow rate Q 3 and the fourth flow rate Q 4 Satisfaction: Q 1 3 , Q 4 ≤Q 2 ; or, satisfy: Q 1 =Q 3 , Q 4 2 .​​ 6. The method for preparing an epitaxial wafer according to claim 4, It is characterized in that The first flow rate Q 1 The range is 200 to 300 sccm; and / or, The second flow rate Q 2 The range is 1 to 5 slm; and / or, The third flow rate Q 3 The range is 300 to 6000 sccm; and / or, The fourth flow rate Q 4 The range is 0.5~1slm.

7. The method for preparing an epitaxial wafer according to claim 4, It is characterized in that The first aluminum source is selected from at least one of trimethylaluminum and triethylaluminum; and / or, The nitrogen source is selected from ammonia.

8. The method for preparing an epitaxial wafer according to claim 1, It is characterized in that The time range for forming the first nucleation sublayer (21) is 1 to 5 minutes; and / or, The time range for forming the second nucleation sublayer (22) is 3 to 10 minutes.

9. The method for preparing an epitaxial wafer according to claim 1, It is characterized in that Before forming the first nucleation layer (2), the preparation method further comprises: A second aluminum source is introduced into the reaction chamber to form an aluminum layer (3) on the substrate (1).

10. The method for preparing an epitaxial wafer according to claim 9, It is characterized in that The second aluminum source is selected from at least one of trimethylaluminum and triethylaluminum; and / or, The flow rate of the second aluminum source is in the range of 10 to 50 sccm; and / or, The time range for forming the aluminum layer (3) is 1 to 10 minutes; and / or, The thickness of the aluminum layer (3) is in the range of 1 to 10 nm.

11. The method for preparing an epitaxial wafer according to claim 1, It is characterized in that After forming the first nucleation layer (2), the preparation method further comprises: forming a second nucleation layer (4) on a side of the first nucleation layer (2) facing away from the substrate (1); The temperature at which the first nucleation layer (2) is formed is a first temperature T 1 The temperature at which the second nucleation layer (4) is formed is the second temperature T 2 , satisfying: T 1 <T 2 , T 1 and T 2 The unit is ℃.

12. The method for preparing an epitaxial wafer according to claim 11, It is characterized in that The first temperature T 1 The range is 850-950°C; and / or, The second temperature T 2 The range is 1050~1150℃.

13. The method for preparing an epitaxial wafer according to claim 12, It is characterized in that After forming a second nucleation layer (4) on a side of the first nucleation layer (2) facing away from the substrate (1), the preparation method further comprises: forming a first buffer layer (5) on a side of the second nucleation layer (4) facing away from the first nucleation layer (2); A second buffer layer (6) is formed on a side of the first buffer layer (5) facing away from the second nucleation layer (4).

14. The method for preparing an epitaxial wafer according to claim 13, It is characterized in that After forming the second buffer layer (6), the preparation method further comprises: forming a channel layer (7) on a side of the second buffer layer (6) facing away from the first buffer layer (5); forming an insertion layer (8) on a side of the channel layer (7) facing away from the second buffer layer (6); forming a barrier layer (9) on a side of the insertion layer (8) facing away from the channel layer (7); A surface layer (10) is formed on the side of the barrier layer (9) facing away from the insertion layer (8).

15. An epitaxial wafer, It is characterized in that include: Substrate (1); a first nucleation layer (2), the first nucleation layer (2) being located on the substrate (1); the first nucleation layer (2) comprising a first nucleation sublayer (21) and a second nucleation sublayer (22), the first nucleation sublayer (21) being located on one side of the substrate (1), and the second nucleation sublayer (22) being located on a side of the first nucleation sublayer (21) facing away from the substrate (1); The rate at which the first nucleation sublayer (21) is formed is a first rate V 1 , in μm / h; the rate of forming the second nucleation sublayer (22) is the second rate V 2 , in μm / h, satisfies: V 1 ≤V 2 .

16. The epitaxial wafer according to claim 15, It is characterized in that The first nucleation layer (2) has a first thickness H 1 The first nucleation sublayer (21) has a second thickness H 2 The second nucleation sublayer (22) has a third thickness H 3 , satisfying: H 2 +H 3 ≤H 1 , H 2 <H 3 Among them, H 1 , H 2 and H 3 The unit is nm.

17. The epitaxial wafer according to claim 16, It is characterized in that The first thickness H 1 is in the range of 150 to 200 nm; and / or, The second thickness H 2 is in the range of 10 to 50 nm; and / or, The third thickness H 3 The range is 70~150nm.

18. The epitaxial wafer according to claim 15, It is characterized in that The crystal quality of the epitaxial wafer is 400-750 arcsec.

Citation Information

Patent Citations

  • Light-emitting diode epitaxial wafer and manufacturing method therefor

    CN107946419A

  • Semiconductor heterostructure and semiconductor device

    CN111009579A

  • Silicon-based high electron mobility transistor and preparation method thereof

    CN114709261A

  • Light emitting diode epitaxial wafer and preparation method thereof

    CN114883460A

  • Ultraviolet LED epitaxial wafer, preparation method thereof and LED chip

    CN117637943A

Cited By

  • Preparation method of epitaxial wafer and epitaxial wafer

    CN120905770A