Manufacturing method of axial ultrathin chip product

By adopting axial ultra-thin chip manufacturing methods in the wafer thinning process, including grinding, diffusion and metallization, optimize chip thickness and thermal resistance, the problems of increasing chip area and high material consumption are solved, and the stability and Stress resistance improves surge level and switching time.

CN118943015AInactive Publication Date: 2024-11-12GALAXY SEMICON HLDG LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411042547.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing wafer thinning process leads to an increase in chip area, high material consumption, and high power loss under high-frequency electronic circuits, making it easy to fail.

Method used

Using axial ultra-thin chip manufacturing method, including selecting a single wafer with a resistivity of 15-23Ω*cm, performing front grinding, pre-diffusion, back grinding, boron diffusion, double-side grinding, surface metallization and packaging treatment, and optimizing chip thickness and thermal resistance, reduce mechanical stress damage, and improve stability through low-temperature welding and reflow treatment.

Benefits of technology

The compactness and stability of the chip structure are achieved, material consumption and power consumption are reduced, stress resistance and welding heat resistance are improved, surge level and switching time are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943015A_ABST
    Figure CN118943015A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductor separation device production, and particularly discloses a manufacturing method of an axial ultrathin chip product. The invention discloses a method for manufacturing an axial ultrathin chip product. The method comprises the following steps: S1, wafer selection: selecting a single crystal wafer with the resistivity of 15-23 omega * cm and the thickness of 220-240 microns as a wafer to be processed; s2, wafer treatment: performing front grinding, pre-diffusion, back grinding, boron diffusion, double-sided grinding, surface metallization and scribing treatment on the wafer to be treated to obtain an intermediate wafer; and S3, packaging: carrying out welding, acid pickling, gluing, curing, mold pressing, aging, reflow soldering and secondary aging treatment on the intermediate wafer to obtain a semi-finished diode. The diode prepared by the invention has the advantages of small pores, small size, low risk, excellent stress resistance, excellent welding heat resistance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of semiconductor separation device production, and more specifically, it relates to a method for manufacturing an axial ultra-thin chip product. Background Art

[0002] Integrated circuit chips are constantly developing in the direction of high density and thinness. In order to meet the requirements, wafers need to be thinned and cut. Wafer thinning technology is a key technology for stacked chip packaging, and the thinning process is an important process in chip production, which has a great impact on the production quality of chips. In the current wafer thinning process, the wafer is generally thinned to a predetermined thickness range first, and then the wafer is cut into individual chips. However, as the frequency in electronic circuits becomes higher and higher, the products become smaller and thinner, and the power becomes larger and larger. The corresponding fast rectifier and ultra-fast rectifier devices have a larger and larger power loss. In order to avoid failure, the chip area used becomes larger and larger, consuming a lot of materials. Summary of the invention

[0003] In order to improve the problem of increasing chip area and high material consumption, the present application provides a technical solution using the following:

[0004] The present application provides a method for manufacturing an axially ultra-thin chip product, comprising the following steps:

[0005] S1. Wafer selection: Select a single crystal wafer with a resistivity of 15-23Ω*cm and a thickness of 220-240μm as the wafer to be processed;

[0006] S2, wafer processing: front grinding, pre-diffusion, back grinding, boron diffusion, double-sided grinding, surface metallization, and dicing are performed on the wafer to be processed to obtain an intermediate wafer;

[0007] S3, packaging: the intermediate wafer is subjected to welding, pickling, gluing, curing, molding, aging, reflow soldering, and secondary aging treatment to obtain a semi-finished diode.

[0008] By adopting the above technical solution, the thickness of the chip is optimized in this application, and the base width is compressed while reducing the thermal resistance of the chip. The thickness of the chip can be further reduced by grinding and thinning processes such as front grinding, back grinding, and double-sided grinding, so that the structure of the final chip product is more compact. The front grinding process can reduce or reduce the mechanical stress damage caused by cutting and maintain the integrity of the wafer.

[0009] The present application performs a reflow soldering impact test on the packaged aged product, which can effectively reduce the stress failure caused by subsequent wave soldering or reflow soldering stress damage, and improve the stability of the diode product.

[0010] Optionally, in step S2, the front side grinding has a grinding thickness of 5-10 μm.

[0011] By adopting the above technical solution, the thickness of the front grinding is optimized. The appropriate grinding thickness can reduce the chip thickness and reduce the mechanical stress damage caused by cutting.

[0012] Optionally, in step S2, the sheet resistance R□ after the pre-diffusion is 0.36-0.45Ω*cm, and the paper source process is used in the pre-diffusion.

[0013] By adopting the above technical solution, the paper source process is preferably used in the pre-diffusion, which can improve the uniformity of the diffusion source distribution, enable the chip to obtain consistent diffusion parameters, reduce the block resistance of the N region, and then reduce the forward voltage drop of the chip, thereby reducing the total power consumption of the product.

[0014] Optionally, in step S2, the back surface is ground to a thickness of 15-20 μm.

[0015] Optionally, in step S2, the resistor block resistance R□ after boron diffusion is 0.10-0.12Ω*cm, and the junction depth is 90-110μm.

[0016] By adopting the above technical solution, the present application optimizes the resistance and junction depth during the boron diffusion process, enables boron to be evenly deposited on the wafer surface, and is not prone to forming a dead layer, thereby effectively improving the performance and service life of chip products.

[0017] Optionally, in step S2, the thickness of the wafer after double-sided grinding is 175-185 μm.

[0018] By adopting the above technical solution, the total thickness of the chip is fully reduced through double-sided thinning, and the total thickness of the wafer is appropriate, which can make the structure of the chip product more compact and reduce the amount of material used.

[0019] Optionally, in step S2, the surface metallization includes the following steps: placing the double-sided ground diffusion sheet in a corrosive solution for corrosion, cleaning, cleaning with a phosphoric acid solution, chemically nickel plating, cleaning and drying, deep burning, pickling, secondary nickel plating, cleaning and drying, deep burning, pickling, gold plating, and drying; wherein the thickness of a single nickel plating is ≤0.3μm, and the thickness of the gold plating is ≤0.02μm.

[0020] By adopting the above technical solution, double-layer nickel plating and surface metallization treatment are performed on the surface of the wafer, the thickness of the nickel plating layer is thinned, the surface stress caused by the metallization treatment on the surface of the wafer is effectively reduced, and a thinner gold is electroplated on the surface. The overall structure of the wafer changes little. Due to the inertness of gold itself, the storage time of the wafer at room temperature and humidity can be effectively increased, the solderability of the wafer is improved, and the stability of the chip product is improved.

[0021] Optionally, in step S3, in the welding operation, a welding sheet with a thickness of 0.1 mm-0.25 mm and a silver content of ≥3% is selected.

[0022] By adopting the above technical solution and selecting thick solder sheets for packaging, the possibility of chip deformation after thinning can be effectively reduced, the chip's ability to resist stress impact can be effectively improved, and the use effect of the chip product can be maintained.

[0023] Optionally, in step S3, during the welding process, the temperature of the welding furnace is 313-335° C., and the time for which the temperature of the welding furnace is greater than 300° C. is controlled within 7.5-12 minutes.

[0024] By adopting the above technical solution, the welding temperature is optimized in the present application. By performing welding processing at a lower temperature, the welding pores of the wafer can be made smaller, which is beneficial to improving the forward voltage drop and voltage consistency, and effectively improving the problem of excessively large pores in tunnel furnace welding.

[0025] Optionally, in step S3, during the secondary aging, the wafer is baked for 12-16 hours.

[0026] By adopting the above technical solution, reflow soldering is more likely to cause stress damage to the wafer. By baking the wafer, the stress impact damage caused to the wafer during reflow soldering can be released.

[0027] In summary, this application has the following beneficial effects:

[0028] 1. Since the present application performs grinding and low-temperature welding on the wafer, the welding pores are smaller during packaging, and the forward voltage drop and voltage consistency are better, which can overcome the problem of excessively large welding pores in the tunnel furnace.

[0029] 2. In this application, the thickness of the nickel plating layer on the surface of the wafer is thinned, the surface stress caused by metallization is reduced, and a thinner gold plating layer is added. The overall cost remains basically unchanged, which can effectively increase the storage time of the wafer at room temperature and humidity, and improve the product stability and solderability.

[0030] 3. The manufacturing method of the present application can overcome the stress damage problem of thin large-size chips under drastic temperature changes, and improve the stress resistance and welding heat resistance of thin chip products.

[0031] 4. The manufacturing method of the present application can improve the surge level to a certain extent, from the original 140A to 170A.

[0032] 5. The manufacturing method of the present application can achieve faster switching time and smaller forward voltage drop at the same chip size. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of the grinding method in the embodiment of the present application. DETAILED DESCRIPTION

[0034] The present application is further described in detail below with reference to the embodiments.

[0035] Example

[0036] Example 1

[0037] The present application provides a method for manufacturing an axially ultra-thin chip product, comprising the following steps:

[0038] S1. Wafer selection: Select a single crystal wafer with a resistivity of 15Ω*cm and a thickness of 220μm

[111] radial direction as the wafer to be processed;

[0039] S2. Wafer processing:

[0040] S21, front side grinding: grinding the front side of the wafer to be processed, specifically, the grinding thickness is 5 μm;

[0041] S22, pre-diffusion: phosphorus pre-diffusion is performed using a paper source process. After phosphorus pre-diffusion, the sheet resistance R□ is 0.36Ω*cm;

[0042] S23, back grinding: grinding the back of the wafer after phosphorus pre-diffusion, specifically, the grinding thickness is 15 μm;

[0043] S24, boron diffusion: boron diffusion is performed on the wafer after back grinding. During the boron diffusion, the sheet resistance R□ is controlled to be 0.1Ω*cm and the junction depth is 90μm;

[0044] S25, double-sided grinding: double-sided grinding of the boron-diffused wafer to make the thickness of the wafer 180 μm;

[0045] S26, gold plating treatment: place the double-sided polished wafer in a polishing solution (hydrofluoric acid: buffer mass ratio is 1:20), corrode for 30 seconds, repeat three times, wash, and then place the wafer in a 5% by mass Hammer powder solution, soak for 30 seconds, wash with hot water, and then use acid solution (H3PO4:H2O2:H2O mass ratio is 1:1:5) to clean, wash with water, nickel plate, control the thickness of the nickel layer to 0.3μm, clean, dry, burn deep, rinse with acid to remove surface oxidation, nickel plate twice, control the thickness of the nickel layer to 0.3μm, clean, dry, burn deep, rinse with acid to remove surface oxidation, gold plate, the thickness of the gold layer is 0.02μm, wash, dry, and dry at 75℃ for 20min;

[0046] S27, scribing: scribing the gold-plated wafer to obtain an intermediate wafer;

[0047] S3, packaging:

[0048] S31, welding: welding the intermediate wafer, specifically, using solder containing 3% silver and 0.1 mm thick, controlling the welding furnace temperature at 313-335°C, and maintaining the welding furnace temperature ≥ 300°C for a total of 7.5 minutes;

[0049] S32, pickling treatment: pickling and etching the soldered chip at 21°C;

[0050] S33, intermediate processing: gluing, curing, molding, and aging the pickled chip to obtain a semi-finished diode;

[0051] S34, reflow soldering: take the semi-finished diode and perform reflow soldering. Specifically, when the chip size is greater than 88 mil, the number of reflow soldering is 2 times; when the chip size is less than 88 mil, the number of reflow soldering is two times;

[0052] S35, secondary aging: bake the semi-finished diode after reflow soldering at 150°C for 12 hours.

[0053] Example 2

[0054] The present application provides a method for manufacturing an axially ultra-thin chip product, comprising the following steps:

[0055] S1. Wafer selection: Select a single crystal wafer with a resistivity of 18Ω*cm and a thickness of 230μm

[111] radial direction as the wafer to be processed;

[0056] S2. Wafer processing:

[0057] S21, front side grinding: grinding the front side of the wafer to be processed, specifically, the grinding thickness is 8 μm;

[0058] S22, pre-diffusion: phosphorus pre-diffusion is performed using a paper source process. After phosphorus pre-diffusion, the sheet resistance R□ is 0.40Ω*cm;

[0059] S23, back grinding: grinding the back side of the wafer after phosphorus pre-diffusion, specifically, the grinding thickness is 18 μm;

[0060] S24, boron diffusion: Boron diffusion is performed on the wafer after back grinding. During the boron diffusion, the sheet resistance R□ is controlled to be 0.11Ω*cm and the junction depth is 100μm;

[0061] S25, double-sided grinding: double-sided grinding of the boron-diffused wafer to make the wafer thickness 185 μm;

[0062] S26, gold plating treatment: place the double-sided polished wafer in a polishing solution (hydrofluoric acid: buffer mass ratio is 1:20), corrode for 30 seconds, repeat three times, wash, and then place the wafer in a 5% by mass Hammer powder solution, soak for 30 seconds, wash with hot water, and then use acid solution (H3PO4:H2O2:H2O mass ratio is 1:1:5) to clean, wash with water, nickel plate, control the thickness of the nickel layer to 0.3μm, clean, dry, burn deep, rinse with acid to remove surface oxidation, nickel plate twice, control the thickness of the nickel layer to 0.3μm, clean, dry, burn deep, rinse with acid to remove surface oxidation, gold plate, the thickness of the gold layer is 0.02μm, wash, dry, and dry at 75℃ for 25min;

[0063] S27, scribing: scribing the gold-plated wafer to obtain an intermediate wafer;

[0064] S3, packaging:

[0065] S31, welding: welding the intermediate wafer, specifically, using solder containing 3% silver and 0.15 mm in thickness, controlling the welding furnace temperature at 313-335°C, and maintaining the welding furnace temperature ≥ 300°C for a total of 10 minutes;

[0066] S32, pickling treatment: pickling and etching the soldered chip at 21°C;

[0067] S33, intermediate processing: gluing, curing, molding, and aging the pickled chip to obtain a semi-finished diode;

[0068] S34, reflow soldering: take the semi-finished diode and perform reflow soldering. Specifically, when the chip size is greater than 88 mil, the number of reflow soldering is 2 times; when the chip size is less than 88 mil, the number of reflow soldering is two times;

[0069] S35, secondary aging: bake the semi-finished diode after reflow soldering at 150°C for 14 hours.

[0070] Example 3

[0071] The present application provides a method for manufacturing an axially ultra-thin chip product, comprising the following steps:

[0072] S1. Wafer selection: Select a single crystal wafer with a resistivity of 23Ω*cm and a thickness of 240μm

[111] radial direction as the wafer to be processed;

[0073] S2. Wafer processing:

[0074] S21, front side grinding: grinding the front side of the wafer to be processed, specifically, the grinding thickness is 10 μm;

[0075] S22, pre-diffusion: phosphorus pre-diffusion is performed using a paper source process. After phosphorus pre-diffusion, the sheet resistance R□ is 0.45Ω*cm;

[0076] S23, back grinding: grinding the back of the wafer after phosphorus pre-diffusion, specifically, the grinding thickness is 20 μm;

[0077] S24, boron diffusion: Boron diffusion is performed on the wafer after back grinding. During the boron diffusion, the sheet resistance R□ is controlled to be 0.12Ω*cm and the junction depth is 110μm;

[0078] S25, double-sided grinding: double-sided grinding of the boron-diffused wafer to make the wafer thickness 190 μm;

[0079] S26, gold plating treatment: place the double-sided polished wafer in a polishing solution (hydrofluoric acid: buffer mass ratio is 1:20), corrode for 30 seconds, repeat three times, wash, and then place the wafer in a 5% by mass Hammer powder solution, soak for 30 seconds, wash with hot water, and then use acid solution (H3PO4:H2O2:H2O mass ratio is 1:1:5) to clean, wash with water, nickel plate, control the thickness of the nickel layer to 0.3μm, clean, dry, burn deep, rinse with acid to remove surface oxidation, nickel plate twice, control the thickness of the nickel layer to 0.3μm, clean, dry, burn deep, rinse with acid to remove surface oxidation, gold plate, the thickness of the gold layer is 0.02μm, wash, dry, and dry at 75℃ for 30min;

[0080] S27, scribing: scribing the gold-plated wafer to obtain an intermediate wafer;

[0081] S3, packaging:

[0082] S31, welding: welding the intermediate wafer, specifically, using solder containing 3% silver and 0.1 mm thick, controlling the welding furnace temperature at 313-335°C, and maintaining the welding furnace temperature ≥ 300°C for a total of 12 minutes;

[0083] S32, pickling treatment: pickling and etching the soldered chip at 21°C;

[0084] S33, intermediate processing: gluing, curing, molding, and aging the pickled chip to obtain a semi-finished diode;

[0085] S34, reflow soldering: take the semi-finished diode and perform reflow soldering. Specifically, when the chip size is greater than 88 mil, the number of reflow soldering is 2 times; when the chip size is less than 88 mil, the number of reflow soldering is 1 time;

[0086] S35, secondary aging: bake the semi-finished diode after reflow soldering at 150°C for 16 hours.

[0087] Comparative Example

[0088] Comparative Example 1

[0089] The present application provides a method for manufacturing an axially ultra-thin chip product, comprising the following steps:

[0090] S1. Wafer selection: Select a single crystal wafer with a resistivity of 15Ω*cm and a thickness of 220μm

[111] radial direction as the wafer to be processed;

[0091] S2. Wafer processing:

[0092] S21, pre-diffusion: phosphorus pre-diffusion is performed using a paper source process. After phosphorus pre-diffusion, the sheet resistance R□ is 0.36Ω*cm;

[0093] S22, back grinding: grinding the back side of the wafer after phosphorus pre-diffusion, specifically, the grinding thickness is 15 μm;

[0094] S23, boron diffusion: boron diffusion is performed on the wafer after back grinding. During the boron diffusion, the sheet resistance R□ is controlled to be 0.1Ω*cm and the junction depth is 90μm;

[0095] S24, double-sided grinding: double-sided grinding of the boron-diffused wafer to make the wafer thickness 180 μm;

[0096] S25, gold plating treatment: the double-sided polished wafer is placed in a polishing liquid (hydrofluoric acid: buffer mass ratio is 1:20), the etching treatment is repeated for 30 seconds, and the wafer is washed. Then the wafer is placed in a 5% by mass Hammer powder solution, soaked for 30 seconds, washed with hot water, and then washed with acid (H3PO4:H2O2:H2O mass ratio is 1:1:5), washed with water, nickel plated, the thickness of the nickel layer is controlled to be 0.3 μm, washed, dried, burned deep, rinsed with acid to remove surface oxidation, nickel plated for the second time, the thickness of the nickel layer is controlled to be 0.3 μm, washed, and dried;

[0097] S26, scribing: scribing the gold-plated wafer to obtain an intermediate wafer;

[0098] S3, packaging:

[0099] S31, welding: welding the intermediate wafer, specifically, using solder containing 3% silver and 0.1 mm thick, controlling the welding furnace temperature at 313-335°C, and maintaining the welding furnace temperature ≥ 300°C for a total of 7.5 minutes;

[0100] S32, pickling treatment: pickling and etching the chip after welding;

[0101] S33, intermediate processing: gluing, curing, molding and aging the chip after pickling to obtain a semi-finished diode.

[0102] Performance testing

[0103] (1) Surge capability test: Use the PIF8000 test system to perform surge capability test on diode products.

[0104] After testing, the surge capacity of the diode products in Examples 1 to 3 is ≥ 170A / mm 2 Specifically, the surge capacity of the diode product in Example 1 is 170A / mm 2 The surge capacity of the diode product in Example 2 is 175A / mm 2 The surge capacity of the diode product in Example 3 is 172A / mm 2 The surge capacity of the diode product in Comparative Example 1 is 140A / mm 2 .

[0105] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for manufacturing an axially ultra-thin chip product, characterized in that: The following steps are involved: S1. Wafer selection: Select a single crystal wafer with a resistivity of 15-23Ω*cm and a thickness of 220-240μm as the wafer to be processed; S2, wafer processing: front grinding, pre-diffusion, back grinding, boron diffusion, double-sided grinding, surface metallization, and dicing are performed on the wafer to be processed to obtain an intermediate wafer; S3, packaging: the intermediate wafer is subjected to welding, pickling, gluing, curing, molding, aging, reflow soldering, and secondary aging treatment to obtain a semi-finished diode.

2. The method for manufacturing an axially ultra-thin chip product according to claim 1, characterized in that: In step S2, the front surface is ground to a thickness of 5-10 μm.

3. The method for manufacturing an axially ultra-thin chip product according to claim 1, characterized in that: In step S2, the sheet resistance R□ after the pre-diffusion is 0.36-0.45Ω*cm, and the paper source process is used in the pre-diffusion.

4. The method for manufacturing an axially ultra-thin chip product according to claim 1, characterized in that: In step S2, the back surface is ground to a thickness of 15-20 μm.

5. The method for manufacturing an axially ultra-thin chip product according to claim 1, characterized in that: In step S2, the resistor block resistance R□ after boron diffusion is 0.10-0.12Ω*cm, and the junction depth is 90-110μm.

6. The method for manufacturing an axially ultra-thin chip product according to claim 1, characterized in that: In step S2, the thickness of the wafer after double-sided grinding is 175-185 μm.

7. The method for manufacturing an axially ultra-thin chip product according to claim 1, characterized in that: In step S2, the surface metallization includes the following steps: placing the double-sided polished diffusion sheet in a corrosive solution for corrosion, cleaning, cleaning with a phosphoric acid solution, chemically nickel plating, cleaning and drying, deep burning, pickling, secondary nickel plating, cleaning and drying, deep burning, pickling, gold plating, and drying; wherein the thickness of a single nickel plating is ≤0.3μm, and the thickness of the gold plating is ≤0.02μm.

8. The method for manufacturing an axially ultra-thin chip product according to claim 1, characterized in that: In step S3, in the welding process, a welding sheet with a thickness of 0.1 mm-0.25 mm and a silver content of ≥3% is selected.

9. The method for manufacturing an axially ultra-thin chip product according to claim 1, characterized in that: In step S3, during the welding process, the temperature of the welding furnace is 313-335°C, and the time when the temperature of the welding furnace is greater than 300°C is controlled within 7.5-12 minutes.

10. The method for manufacturing an axially ultra-thin chip product according to claim 1, characterized in that: In step S3, during the secondary aging, the semi-finished diode is baked for 12-16 hours.

Citation Information

Patent Citations

  • Matchable fast recovery diode (FRD) of integrated gate commutate thyristor and manufacturing method of matchable fast recovery diode

    CN104701386A

  • Method for fabricating one-way transient voltage suppressor (TVS) chip by printing process

    CN109755116A

  • Transient diode and packaging process thereof

    CN111403366A