Lithium iron phosphate positive pole piece, preparation method thereof and lithium ion battery
By using porous conductive layers and electrode layer structures of different positive electrode active materials in lithium-ion batteries, the problem of poor conductivity of lithium iron phosphate materials is solved, the conductivity and cycling performance of the battery is improved, the battery life is extended and the safety is improved .
Patent Information
- Application Number
- CN202411212618.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
AI Technical Summary
Lithium-ion batteries cannot take into account the defects of conductivity, safety performance and circulation performance, especially the poor conductivity of lithium iron phosphate materials, resulting in poor circulation performance loss and safety performance.
The lithium iron phosphate positive electrode sheet structure is adopted, including a porous conductive layer, a first electrode layer and a second electrode layer, wherein the porous conductive layer contains a conductive substance, the positive active material in the first electrode layer is lithium iron phosphate, and the second electrode layer The positive electrode active material in the process is different from the first electrode layer, and a lithium supplement agent is provided between the electrode layers to improve the conductivity and cycling performance.
By optimizing the electrode layer structure, the battery's conductivity, cycle performance and safety performance are improved, the battery's cycle life is extended and irreversible losses are reduced.
Smart Images

Figure CN118943286A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium iron phosphate positive electrode sheet and a preparation method thereof, and a lithium ion battery. Background Art
[0002] In recent years, lithium-ion battery technology has become increasingly mature, and the situation between lithium iron phosphate and nickel-cobalt-manganese ternary positive electrode materials has changed. The weak energy density has been narrowed through the assembly structure of PACK and modules. At the same time, due to the end customers' requirements for battery safety performance, cost, and higher cycle performance, major lithium battery manufacturers have begun to develop lithium iron phosphate positive electrode materials. Although lithium iron phosphate materials have excellent cycle performance and safety performance and low cost, they have poor conductivity and are currently commonly used in the field of energy storage. Although the use of full-ear technology is increasing, the problem of poor conductivity of lithium iron phosphate batteries themselves still needs to be solved urgently.
[0003] To this end, Chinese patent document CN115133008A discloses a multi-layer composite lithium iron phosphate positive electrode sheet and its preparation method and lithium ion battery, which uses a three-layer structure and a gradient thickness arrangement to make the conductivity and ion conductivity of each area of the electrode sheet uniform, improving the battery's cycle performance, storage performance and safety performance. However, it does not take into account that after the composite, lithium iron phosphate is different from ternary materials and has a lower potential. If it is circulated at a high potential, it will cause certain damage to the structure of lithium iron phosphate, and ultimately lead to a loss of cycle performance and poor safety performance. Therefore, how to achieve a balance between conductivity, safety and cycle performance is an urgent problem to be solved in the research process of lithium ion batteries. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defect that lithium-ion batteries in the prior art cannot take into account conductivity, safety and cycle performance at the same time, thereby providing a lithium iron phosphate positive electrode plate and a preparation method thereof and a lithium-ion battery.
[0005] The present invention provides a lithium iron phosphate positive electrode plate, comprising a current collector and a porous conductive layer, a first electrode layer and a second electrode layer stacked in sequence on one side or both sides of the current collector, wherein the porous conductive layer contains a conductive substance, the positive electrode active material in the first electrode layer comprises a lithium iron phosphate material, and the positive electrode active material in the second electrode layer is different from the positive electrode active material in the first electrode layer.
[0006] Further, the positive electrode active material in the second electrode layer comprises one or more of nickel cobalt manganese oxide positive electrode material, nickel cobalt aluminum oxide positive electrode material, lithium cobalt oxide positive electrode material, lithium manganese-rich positive electrode material, lithium iron manganese phosphate positive electrode material, and lithium manganese oxide positive electrode material; and / or, the conductive material in the porous conductive layer comprises one or more of ketjen black, acetylene black, conductive carbon black, carbon nanotubes, carbon fibers, and graphene; and / or, the pore diameter in the porous conductive layer is less than 10 mm (e.g., 1-8 mm), and the porosity is 20-80%; and / or, the lithium iron phosphate material is coated with a carbon material (i.e., a carbon-coated lithium iron phosphate material). The carbon-coated lithium iron phosphate material can be made by itself according to conventional processes, or it can be made of commercially available conventional materials.
[0007] In certain preferred embodiments, in order to further extend the cycle life of the battery, the positive electrode active material in the second electrode layer is lithium nickel cobalt aluminum oxide and / or lithium manganese iron phosphate, more preferably a composition of lithium nickel cobalt aluminum oxide and lithium manganese iron phosphate in a mass ratio of 1:2-3. In certain preferred embodiments, the chemical formula of lithium manganese iron phosphate is: LiMn x Fe 1-x PO4, where 0.4≤x≤0.8, such as LiMn 0.6 Fe 0.4 PO4.
[0008] Furthermore, the porous conductive layer has holes with circular, elliptical or polygonal cross sections; preferably, the porous conductive layer has a honeycomb structure, wherein the cross sections of the holes in the honeycomb structure are hexagonal.
[0009] The polygon may be a triangle, a quadrilateral, a pentagon or a hexagon.
[0010] Further, the coating thickness of the porous conductive layer is 3-6 μm; and / or the coating thickness of the first electrode layer is 160-180 μm; and / or the coating thickness of the second electrode layer is 2.5-4 μm.
[0011] Further, in terms of weight, the first electrode layer comprises: 94-98.5 parts of lithium iron phosphate, 0.25-3 parts of a conductive agent and 1-3 parts of a binder; and / or, in terms of weight, the second electrode layer comprises 96-98 parts of a positive electrode active material and 1-2 parts of a binder; and / or, the second electrode layer also includes a lithium supplement.
[0012] Furthermore, the conductive agent is selected from at least one of conductive carbon black, Ketjen black, and carbon nanotubes; and / or the binder is selected from at least one of polyvinylidene fluoride (PVDF), polyacrylic acid, and polytetrafluoroethylene.
[0013] Furthermore, the second electrode layer also includes a lithium supplement agent. Preferably, the lithium supplement agent is selected from one or more of lithium nickel-rich lithium oxide, lithium iron-rich lithium oxide, binary lithium compounds, and lithium carbonate; preferably, the mass ratio of the positive electrode active material in the second electrode layer to the lithium supplement agent is 96-98:1-2.
[0014] In certain preferred embodiments, in order to further extend the cycle life of the battery, the lithium supplement in the second electrode layer is Li2NiO2 (LNO) and / or Li5FeO4 (LFO). More preferably, the lithium supplement in the second electrode layer is a combination of LNO and LFO in a mass ratio of 1-3:1-3.
[0015] Furthermore, in the first electrode layer, the lithium iron phosphate material is coated with a carbon material; preferably, the carbon content in the positive electrode active material in the first electrode layer is 0.5-2.5wt%; preferably, the particle size D50 of the positive electrode active material in the first electrode layer is 1-2μm.
[0016] The present invention also provides a method for preparing a lithium iron phosphate positive electrode sheet, comprising the following steps:
[0017] (1) respectively mixing the components of the porous conductive layer, the first electrode layer, and the second electrode layer with a solvent to prepare a porous conductive layer slurry, a first electrode layer slurry, and a second electrode layer slurry;
[0018] (2) Coating the porous conductive layer slurry on the current collector and drying to obtain the porous conductive layer, coating the first electrode layer slurry on the surface of the porous conductive layer and drying to obtain the first electrode layer, coating the second electrode layer slurry on the surface of the first electrode layer and drying, and rolling to obtain the lithium iron phosphate positive electrode sheet.
[0019] Furthermore, the solvent is N-methylpyrrolidone (NMP); and / or the solid content of the porous conductive layer slurry is 20-80%; and / or the solid content of the first electrode layer slurry is 40-65%; and / or the solid content of the second electrode layer slurry is 60-75%.
[0020] The porous conductive layer can be formed by direct coating by ultrasonic spraying or gravure printing, or by extrusion spraying or transfer coating followed by laser cleaning.
[0021] For the first electrode layer, after the porous conductive layer is dried, the positive electrode slurry of the first electrode layer is coated on the porous conductive layer by ultrasonic spraying, extrusion spraying, transfer coating or the like.
[0022] After the first electrode layer is dried, the second electrode layer slurry is coated on the first electrode layer by ultrasonic spraying, extrusion spraying, transfer coating or the like. The second electrode layer can be coated on the entire surface or in a mesh, honeycomb, dot or line shape.
[0023] Furthermore, a conventional drying method in the art is adopted, such as baking, and the baking temperature is 60-100°C.
[0024] The present invention also provides a lithium-ion battery, comprising any of the above-mentioned lithium iron phosphate positive electrode sheets or the lithium iron phosphate positive electrode sheets prepared by the preparation method, and also comprising a negative electrode sheet, a separator and an electrolyte.
[0025] The negative electrode sheet includes a current collector and a negative electrode active layer loaded on the current collector, wherein the negative electrode active material in the negative electrode active layer includes one or more of graphite, soft carbon, hard carbon, and mesophase carbon microspheres. The negative electrode active layer is prepared by conventional coating and cold pressing processes.
[0026] The electrolyte of the present invention can be a conventional commercially available lithium-ion battery electrolyte, or can be made by oneself using existing conventional materials, for example, an electrolyte comprising a solvent and a lithium salt can be used, wherein the solvent is selected from at least one of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate. The lithium salt is selected from sodium hexafluorophosphate. The molar concentration of the lithium salt is 0.8-1.2 mol / L. The present invention can use an existing traditional diaphragm, such as a PE diaphragm, a PP diaphragm, a PP / PE composite film, or other commercially available diaphragms.
[0027] The technical solution of the present invention has the following advantages:
[0028] 1. The lithium iron phosphate positive electrode plate provided by the present invention comprises a current collector and a porous conductive layer, a first electrode layer and a second electrode layer stacked in sequence on one side or both sides of the current collector, wherein the porous conductive layer contains a conductive substance, the positive electrode active material in the first electrode layer comprises a lithium iron phosphate material, and the positive electrode active material in the second electrode layer is different from the positive electrode active material in the first electrode layer. By comprising a current collector and a porous conductive layer comprising a conductive substance stacked in sequence on one side or both sides of the current collector, a first electrode layer comprising a lithium iron phosphate material and a second electrode layer comprising a positive electrode active material different from the positive electrode active material in the first electrode layer, the battery can simultaneously maintain high cycle performance and conductivity as well as good safety by cooperating with each other.
[0029] The present invention fully considers the problem of poor conductivity of lithium iron phosphate and irreversible loss caused by the formation of SEI film in the battery cell formation stage. A porous conductive layer including a conductive material, a first electrode layer including a lithium iron phosphate material and a second electrode layer including a positive electrode active material different from the positive electrode active material in the first electrode layer are sequentially stacked on the current collector, so that the conductivity and ion conductivity of each area of the electrode sheet are relatively uniform, the adhesion between the first electrode layer and the current collector is improved, and the rate charge and discharge performance of the battery cell is improved through the high electron transmission capacity of the porous conductive layer. At the same time, the second electrode layer has a positive electrode active material different from the positive electrode active material in the first electrode layer, so that there is a difference in potential between the two layers. The positive electrode active material of the second electrode layer is preferentially consumed during film formation, and can replace lithium iron phosphate in the formation stage to provide active lithium ions for the negative electrode to form an SEI film, reduce the irreversible loss of the battery during formation, and thus improve the cycle performance and safety performance of the battery cell.
[0030] 2. The lithium iron phosphate positive electrode plate provided by the present invention, the porous conductive layer has a honeycomb structure, which is more stable and strong than the mesh structure, and is less likely to be damaged as the degree of circulation increases, thereby further improving the cycle performance and safety performance of the battery cell.
[0031] The second electrode layer also includes a lithium supplement. Providing the lithium supplement in the second electrode layer can further increase the active lithium content of the battery cell, thereby further improving the cycle performance and safety performance of the battery cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0033] Figure 1 is a schematic cross-sectional view of the lithium iron phosphate positive electrode sheet prepared in Example 1;
[0034] Figure 2 Schematic diagram of the single-sided structure of the lithium iron phosphate positive electrode sheet prepared in Example 1;
[0035] Figure 3 It is the cycle curve of lithium-ion battery determined by performance test;
[0036] Reference numerals: 1. current collector; 2. porous conductive layer; 3. first electrode layer; 4. second electrode layer. DETAILED DESCRIPTION
[0037] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0038] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially. The carbon-coated lithium iron phosphate material was purchased from Dangsheng Technology Company, model LFP-A2, with a carbon content of 1%-1.5%.
[0039] Example 1
[0040] This embodiment provides a lithium iron phosphate positive electrode plate, such as Figure 1 and Figure 2 As shown, it includes a current collector and a porous conductive layer 2 (a honeycomb conductive layer in this embodiment) stacked on both sides of the current collector 1, a first electrode layer 3 and a second electrode layer 4, the conductive material in the porous conductive layer is Ketjen black and carbon nanotubes (mass ratio = 3:1), the positive electrode active material in the first electrode layer is a carbon-coated lithium iron phosphate material, and the positive electrode active material in the second electrode layer is lithium nickel cobalt aluminum oxide (chemical formula: LiNiCoAlO2) and lithium manganese iron phosphate (chemical formula: LiMn) with a mass ratio of 1:2. 0.6 Fe 0.4 PO4), the lithium supplement in the second electrode layer is LNO and LFO in a mass ratio of 1:1. The coating thickness of the porous conductive layer is 5 μm, the coating thickness of the first electrode layer is 170 μm, and the coating thickness of the second electrode layer is 3 μm.
[0041] The method for preparing the lithium iron phosphate positive electrode sheet comprises the following steps:
[0042] (1) Ketjen black and carbon nanotubes were weighed in a mass ratio of 3:1 and dispersed in NMP with a solid content of 60% to obtain a porous conductive layer slurry. A 5 μm honeycomb conductive network was gravure-printed on a 15 μm aluminum foil using a honeycomb coating roller, and the mixture was dried at a baking temperature of 80° C. to obtain a honeycomb conductive layer with a pore diameter of 2 mm and a porosity of 60%.
[0043] (2) Carbon-coated lithium iron phosphate material, conductive carbon black (SP), carbon nanotubes and PVDF were weighed in a mass ratio of 97.5:0.35:0.15:2.0, mixed and dispersed in NMP with a solid content of 55%, to obtain a first electrode layer slurry. The slurry was coated on an aluminum foil with a honeycomb conductive layer by a transfer coater with a coating thickness of 170 μm, and dried at a baking temperature of 95° C. to obtain a first electrode layer.
[0044] (3) Mix lithium nickel cobalt aluminum oxide and lithium manganese iron phosphate in a mass ratio of 1:2 to obtain a positive electrode active material, mix LNO and LFO in a mass ratio of 1:1 to obtain a lithium supplement, weigh the positive electrode active material, PVDF and lithium supplement in a mass ratio of 96.5:1.5:2, disperse them in NMP, and control the solid content to 70% to obtain a second electrode layer slurry. Coat the slurry on the first electrode layer with a coating thickness of 3 μm and a baking temperature of 70°C. After baking, obtain a lithium iron phosphate positive electrode sheet, and roll the sheet to 160 μm.
[0045] The present embodiment also provides a lithium ion battery and a preparation method thereof, which includes the lithium iron phosphate positive electrode sheet of the present embodiment, and also includes a negative electrode sheet, a separator and an electrode liquid. Preparation method: The lithium iron phosphate positive electrode sheet and the negative electrode sheet and the separator are wound, assembled and injected with liquid (conventional cylindrical lithium ion battery electrolyte) to form a cylindrical lithium ion battery.
[0046] The preparation method of the negative electrode sheet is as follows: weigh graphite, conductive carbon black (SP), CMC and SBR according to the mass ratio of 96.8:0.5:1.2:1.7, mix and disperse in water to obtain a negative electrode slurry with a solid content of 50%. The slurry is coated on the copper foil by a transfer coater with a coating thickness of 140μm and dried at a baking temperature of 70°C. After the baking is completed, the electrode sheet is rolled to 120μm.
[0047] Example 2
[0048] The present embodiment provides a lithium iron phosphate positive electrode sheet, including a current collector and a porous conductive layer (a honeycomb conductive layer in the present embodiment) stacked on both sides of the current collector, a first electrode layer and a second electrode layer, wherein the conductive material in the porous conductive layer is ketjen black and graphene (mass ratio = 5:1), the positive electrode active material in the first electrode layer is a carbon-coated lithium iron phosphate material, and the positive electrode active material in the second electrode layer is lithium nickel cobalt aluminum oxide (chemical formula: LiNiCoAlO2) and lithium manganese iron phosphate (chemical formula: LiMn) in a mass ratio of 1:2. 0.6 Fe 0.4 PO4), the lithium supplement is LFO.
[0049] The coating thickness of the porous conductive layer was 5 μm, the coating thickness of the first electrode layer was 170 μm, and the coating thickness of the second electrode layer was 3 μm.
[0050] The method for preparing the lithium iron phosphate positive electrode sheet comprises the following steps:
[0051] (1) Ketjen black and graphene were weighed in a mass ratio of 5:1 and dispersed in NMP with a solid content of 50% to obtain a porous conductive layer slurry. A 5 μm honeycomb conductive network was gravure printed on a 15 μm aluminum foil using a honeycomb coating roller, and the mixture was dried at a baking temperature of 80° C. to obtain a honeycomb conductive layer with a pore diameter of 4 mm and a porosity of 50%.
[0052] (2) Carbon-coated lithium iron phosphate material, conductive carbon black (SP), carbon nanotubes and PVDF were weighed in a mass ratio of 97.5:0.35:0.15:2.0, mixed and dispersed in NMP with a solid content of 55%, to obtain a first electrode layer slurry. The slurry was coated on an aluminum foil with a honeycomb conductive layer by a transfer coater with a coating thickness of 170 μm, and dried at a baking temperature of 95° C. to obtain a first electrode layer.
[0053] (3) Mix lithium nickel cobalt aluminum oxide and lithium manganese iron phosphate in a mass ratio of 1:2 to obtain a positive electrode active material, weigh the positive electrode active material, PVDF and lithium supplement in a mass ratio of 96.5:1.5:2, disperse them in NMP, and control the solid content to 70% to obtain a second electrode layer slurry. Coat the slurry on the first electrode layer with a coating thickness of 3 μm and a baking temperature of 70°C. After baking, obtain a lithium iron phosphate positive electrode sheet, and roll the sheet to 160 μm.
[0054] This embodiment also provides a lithium-ion battery and a preparation method thereof, which are basically the same as those of Embodiment 1, except that the lithium iron phosphate positive electrode sheet of Embodiment 1 is replaced by the lithium iron phosphate positive electrode sheet of Embodiment 1.
[0055] Example 3
[0056] The present embodiment provides a lithium iron phosphate positive electrode sheet, including a current collector and a porous conductive layer (a honeycomb conductive layer in the present embodiment), a first electrode layer and a second electrode layer stacked in sequence on one side of the current collector, wherein the conductive material in the porous conductive layer is ketjen black and carbon nanotubes, the positive electrode active material in the first electrode layer is a carbon-coated lithium iron phosphate material, and the positive electrode active material in the second electrode layer is lithium nickel cobalt aluminum oxide (chemical formula: LiNiCoAlO2) and lithium iron manganese phosphate (chemical formula: LiMn) in a mass ratio of 1:3. 0.6 Fe 0.4PO4), the lithium supplement is LNO and LFO in a mass ratio of 1:1. The coating thickness of the porous conductive layer is 4 μm, the coating thickness of the first electrode layer is 180 μm, and the coating thickness of the second electrode layer is 2.5 μm.
[0057] The method for preparing the lithium iron phosphate positive electrode sheet comprises the following steps:
[0058] (1) Ketjen black and carbon nanotubes were weighed in a mass ratio of 3:1 and dispersed in NMP with a solid content of 70% to obtain a porous conductive layer slurry. A 4 μm honeycomb conductive network was gravure-printed on a 15 μm aluminum foil using a honeycomb coating roller, and the mixture was dried at a baking temperature of 80° C. to obtain a honeycomb conductive layer with a pore diameter of 2 mm and a porosity of 60%.
[0059] (2) Carbon-coated lithium iron phosphate material, conductive carbon black (SP), carbon nanotubes and PVDF were weighed in a mass ratio of 97.5:0.35:0.15:2.0, mixed and dispersed in NMP with a solid content of 40%, to obtain a first electrode layer slurry. The slurry was coated on an aluminum foil with a honeycomb conductive layer by a transfer coater with a coating thickness of 180 μm, and dried at a baking temperature of 95° C. to obtain a first electrode layer.
[0060] (3) Mix lithium nickel cobalt aluminum oxide and lithium manganese iron phosphate in a mass ratio of 1:3 to obtain a positive electrode active material, mix LNO and LFO in a mass ratio of 1:1 to obtain a lithium supplement, weigh the positive electrode active material, PVDF and lithium supplement in a mass ratio of 96.5:1.5:2, disperse them in NMP, and control the solid content to 60% to obtain a second electrode layer slurry. Coat the slurry on the first electrode layer with a coating thickness of 2.5 μm and a baking temperature of 70°C. After baking, obtain a lithium iron phosphate positive electrode sheet, and roll the sheet to 160 μm.
[0061] This embodiment also provides a lithium-ion battery and a preparation method thereof, which are basically the same as those of Embodiment 1, except that the lithium iron phosphate positive electrode sheet of Embodiment 1 is replaced by the lithium iron phosphate positive electrode sheet of Embodiment 1.
[0062] Example 4
[0063] This embodiment provides a lithium iron phosphate positive electrode sheet and a preparation method thereof. The only difference from Embodiment 1 is that the positive electrode active material in the second electrode layer is different. The positive electrode active material used in this embodiment is pure lithium manganese iron phosphate (chemical formula: LiMn 0.6 Fe 0.4 PO4), and the rest are the same as in Example 1.
[0064] This embodiment also provides a lithium-ion battery and a preparation method thereof, which are basically the same as those of Embodiment 1, except that the lithium iron phosphate positive electrode sheet of Embodiment 1 is replaced by the lithium iron phosphate positive electrode sheet of Embodiment 1.
[0065] Example 5
[0066] This embodiment provides a lithium iron phosphate positive electrode plate and a preparation method thereof. The only difference from Embodiment 1 is that the positive electrode active material in the second electrode layer is different. The positive electrode active material used in this embodiment is pure lithium nickel cobalt aluminum oxide. The rest is the same as Embodiment 1.
[0067] This embodiment also provides a lithium-ion battery and a preparation method thereof, which are basically the same as those of Embodiment 1, except that the lithium iron phosphate positive electrode sheet of Embodiment 1 is replaced by the lithium iron phosphate positive electrode sheet of Embodiment 1.
[0068] Comparative Example 1
[0069] This comparative example provides a lithium iron phosphate positive electrode sheet and a preparation method thereof, which differs from Example 1 only in that the second electrode layer and the porous conductive layer are missing. That is, the first electrode layer slurry is coated on a 15μm aluminum foil by a transfer coater, the coating thickness is 170μm, and it is dried at a baking temperature of 95°C, and the electrode sheet is rolled to 160μm. The rest of the material composition and process conditions are the same as those in Example 1.
[0070] This comparative example also provides a lithium-ion battery and a preparation method thereof, which are basically the same as those of Example 1, except that the lithium iron phosphate positive electrode sheet of the comparative example is used instead of the lithium iron phosphate positive electrode sheet of Example 1.
[0071] Comparative Example 2
[0072] This comparative example provides a lithium iron phosphate positive electrode sheet and a preparation method thereof, which differs from Example 1 only in that the second electrode layer is lacking. That is, the porous conductive layer slurry is passed through a honeycomb coating roller, a 5μm honeycomb conductive network is gravure printed on a 15μm aluminum foil, and then dried at a baking temperature of 80°C, and then the first electrode layer slurry is coated on the aluminum foil with a honeycomb conductive layer by a transfer coater, the coating thickness is 170μm, and it is dried at a baking temperature of 95°C, and the electrode sheet is rolled to 160μm to obtain a lithium iron phosphate positive electrode sheet. The rest of the material composition and process conditions are the same as those in Example 1.
[0073] This comparative example also provides a lithium-ion battery and a preparation method thereof, which are basically the same as those of Example 1, except that the lithium iron phosphate positive electrode sheet of the comparative example is used instead of the lithium iron phosphate positive electrode sheet of Example 1.
[0074] Performance Testing
[0075] The electrode sheet resistance of the lithium iron phosphate positive electrode sheets of each embodiment and comparative example was tested by a commercial electrode sheet resistance meter on the market.
[0076] The above lithium-ion batteries were tested for performance according to the following methods:
[0077] Test steps:
[0078] (1) Battery cell voltage and internal resistance test: Use the battery tester BT3562 to test the battery cell voltage and internal resistance.
[0079] (2) Rate performance test: 5C rate discharge was performed at 2.0-3.65V, that is, constant current and constant voltage charging was performed at 0.5C to 3.65V, and then constant current discharge was performed at 5C to 2.0V. The 5C rate discharge retention rate and temperature rise were calculated according to the following formula: 5C rate discharge retention rate = 5C discharge capacity / 0.5C discharge capacity, temperature rise = maximum temperature of 5C discharge - starting temperature.
[0080] (3) Charge and discharge cycle test: Perform 0.5C / 1C charge and discharge cycle test at 2.0-3.65V, that is, charge to 3.65V at 0.5C with constant current and constant voltage, and cut-off current 0.05C; then discharge to 2.0V at 1C with constant current, and cycle multiple times until the battery's life ends when the capacity retention rate is ≤80%, and record the total number of battery cycles before the end of life (cycle life).
[0081] Table 1 Performance test results
[0082]
[0083]
[0084] From Table 1 and Figure 3 It can be seen that in Examples 1-5, the internal resistance of the electrode and the internal resistance of the battery cell are significantly reduced due to the use of the lithium iron phosphate positive electrode plate of the present invention, indicating that the conductive performance is significantly improved. At the same time, the cycle life is significantly improved, and the 5C rate temperature rise is significantly reduced, indicating that the cycle performance and safety performance are significantly improved.
[0085] Compared with Examples 4-5, Example 1 further prolongs the cycle life of the battery by optimizing the composition of the positive electrode active material in the second electrode layer.
[0086] Compared with Example 2, Examples 1 and 3 further extend the cycle life of the battery by optimizing the composition of the lithium supplement in the second electrode layer.
[0087] However, the cycle performance, safety performance and conductivity performance of Comparative Example 1 are very poor due to the lack of the second electrode layer and the porous conductive layer; the cycle performance of Comparative Example 2 is worse than that of Example 1 due to the lack of the second electrode layer, and its conductivity performance is better than that of Comparative Example 1.
[0088] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A lithium iron phosphate positive electrode plate, characterized in that: It includes a current collector and a porous conductive layer, a first electrode layer and a second electrode layer stacked in sequence on both sides of the current collector, the porous conductive layer contains a conductive substance, the positive electrode active material in the first electrode layer includes a lithium iron phosphate material, and the positive electrode active material in the second electrode layer is different from the positive electrode active material in the first electrode layer.
2. The lithium iron phosphate positive electrode sheet according to claim 1, characterized in that: The positive electrode active material in the second electrode layer includes one or more of nickel cobalt manganese oxide positive electrode material, nickel cobalt aluminum oxide positive electrode material, lithium cobalt oxide positive electrode material, lithium manganese-rich positive electrode material, lithium iron manganese phosphate positive electrode material, and lithium manganese oxide positive electrode material; and / or, the conductive substance in the porous conductive layer includes one or more of Ketjen black, acetylene black, conductive carbon black, carbon nanotubes, carbon fiber, and graphene; and / or, the pore diameter of the porous conductive layer is less than 10 mm, and the porosity is 20-80%; and / or, the lithium iron phosphate material is coated with a carbon material.
3. The lithium iron phosphate positive electrode sheet according to claim 1 or 2, characterized in that: The porous conductive layer has holes with circular, elliptical or polygonal cross-sections; preferably, the porous conductive layer has a honeycomb structure.
4. The lithium iron phosphate positive electrode sheet according to any one of claims 1 to 3, characterized in that: The coating thickness of the porous conductive layer is 3-6 μm; and / or the coating thickness of the first electrode layer is 160-180 μm; and / or the coating thickness of the second electrode layer is 2.5-4 μm.
5. The lithium iron phosphate positive electrode sheet according to any one of claims 1 to 4, characterized in that: In terms of weight, the first electrode layer comprises: 94-98.5 parts of lithium iron phosphate, 0.25-3 parts of a conductive agent and 1-3 parts of a binder; and / or, in terms of weight, the second electrode layer comprises 96-98 parts of a positive electrode active material and 1-2 parts of a binder.
6. The lithium iron phosphate positive electrode sheet according to claim 5, characterized in that: The conductive agent is selected from at least one of conductive carbon black, Ketjen black, and carbon nanotubes; and / or the binder is selected from at least one of polyvinylidene fluoride, polyacrylic acid, and polytetrafluoroethylene.
7. The lithium iron phosphate positive electrode sheet according to any one of claims 1 to 6, characterized in that: The second electrode layer also includes a lithium supplement agent. Preferably, the lithium supplement agent is selected from one or more of lithium nickel-rich lithium oxide, lithium iron-rich lithium oxide, binary lithium compounds, and lithium carbonate; preferably, the mass ratio of the positive electrode active material in the second electrode layer to the lithium supplement agent is 96-98:1-2.
8. A method for preparing the lithium iron phosphate positive electrode sheet according to any one of claims 1 to 7, characterized in that: The steps include: (1) respectively mixing the components of the porous conductive layer, the first electrode layer, and the second electrode layer with a solvent to prepare a porous conductive layer slurry, a first electrode layer slurry, and a second electrode layer slurry; (2) Coating the porous conductive layer slurry on the current collector and drying to obtain the porous conductive layer, coating the first electrode layer slurry on the surface of the porous conductive layer and drying to obtain the first electrode layer, coating the second electrode layer slurry on the surface of the first electrode layer and drying, and rolling to obtain the lithium iron phosphate positive electrode sheet.
9. The method for preparing a lithium iron phosphate positive electrode sheet according to claim 8, characterized in that: The solvent is N-methylpyrrolidone; and / or the solid content of the porous conductive layer slurry is 20-80%; and / or the solid content of the first electrode layer slurry is 40-65%; and / or the solid content of the second electrode layer slurry is 60-75%.
10. A lithium ion battery, characterized in that: It comprises the lithium iron phosphate positive electrode sheet as described in any one of claims 1 to 7 or the lithium iron phosphate positive electrode sheet prepared by the preparation method as described in claim 8 or 9, and also comprises a negative electrode sheet, a separator and an electrolyte.
Citation Information
Cited By
Composite pole piece, preparation method and sodium ion battery
CN120089686A
Carbon-coated lithium iron phosphate, preparation method thereof and positive plate