Modified ternary material as well as preparation method and application thereof

By using a polydopamine coating layer modified by dodecanthiol on the ternary material, the problem of poor wetting of polydopamine coating material in the electrolyte is solved, and the diffusion efficiency of lithium ions and the circulation performance of the battery are improved. Achieve higher capacity and better cycle performance.

CN118943324APending Publication Date: 2024-11-12GEM WUXI ENERGY MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410990751.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the polydopamine-coated ternary material has poor wetting properties in the electrolyte, which affects the solvation of lithium ions after deintercalation, resulting in low battery capacity and cycling performance.

Method used

The polydopamine coating modified by n-dodecanthiol is used to increase the lipophilic ability of the ternary material surface through the hydrophobic and maltodonthiol long chain reaction of polydopamine and n-dodecanthiol, forming a modified ternary material and improving The wetting property of the electrolyte and the diffusion efficiency of lithium ions.

Benefits of technology

Effectively reduce the degree of corrosion of residual alkali and electrolyte on the surface of the material, improve the capacity and circulation performance of the material, and enhance the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943324A_ABST
    Figure CN118943324A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of battery material preparation, and particularly relates to a modified ternary material and a preparation method and application thereof. The modified ternary material provided by the invention comprises a ternary material and a coating layer, and the coating layer comprises n-dodecanethiol modified polydopamine. The modified ternary material contains a modified polydopamine coating layer, and the oleophylic ability of the modified coating layer is enhanced, so that the capacity and cycle performance of the material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery material preparation, and specifically relates to a modified ternary material and a preparation method and application thereof. Background Art

[0002] Because traditional lead-acid batteries and nickel-cadmium batteries have low energy efficiency and serious pollution, while lithium-ion batteries have the advantages of high safety, low cost, and environmental friendliness, they are favored by researchers. Lithium-ion batteries are specifically divided into lithium power batteries, lithium consumer batteries, and lithium energy storage batteries according to the usage scenarios and energy size. As the main application end of lithium batteries, lithium power batteries have begun to use high energy density on a large scale due to the need for endurance, and the cycle and safety performance are slightly poor, but the comprehensive indicators are balanced. When the cycle life of the power battery is less than 80% of the initial capacity, it needs to be retired. How to improve the cycle performance of the positive electrode material is currently a problem that the retired lithium battery industry is committed to solving.

[0003] As the main positive electrode material on the market, ternary materials have the advantages of high energy density and good cycle performance. Therefore, they play an increasingly important role in the field of semi-solid and all-solid-state batteries and are typical representatives of lithium battery positive electrode materials currently used on a large scale. However, they also have their own disadvantages in terms of material properties: (1) The high residual alkali on the surface of ternary materials will cause the battery cell to swell, thus affecting the material's cycle performance; (2) Ni on the surface of ternary materials 4+ It is easily corroded by the electrolyte, causing material capacity and cycle attenuation.

[0004] At present, the residual alkali on the surface is generally removed by washing with water, and the electrolyte is physically isolated by metal oxide coating to prevent the surface Ni 4+ Corroded. These two solutions are relatively cumbersome. The existing technology uses polydopamine to coat ternary materials. Although it can solve the problem of high residual alkali and easy corrosion of materials by electrolytes, if the polydopamine-coated ternary materials are used directly, it will cause poor electrolyte wettability and affect the solvation of lithium ions after deintercalation. Therefore, it is necessary to develop a modified ternary material containing a modified polydopamine coating layer, which has enhanced lipophilicity and thus improves the material capacity and cycle performance. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the prior art polydopamine-coated ternary material in the electrolyte, which affects the solvation of lithium ions after deintercalation and leads to low battery capacity and cycle performance, thereby providing a modified ternary material and its preparation method and application.

[0006] To this end, the present invention provides the following technical solutions.

[0007] The invention provides a modified ternary material, comprising a ternary material and a coating layer, wherein the coating layer comprises polydopamine modified with n-dodecyl mercaptan.

[0008] In an optional embodiment, the molar content of the polydopamine in the ternary material is 0.01-1%.

[0009] The present invention provides a method for preparing a modified ternary material, comprising the following steps:

[0010] (1) dopamine and the ternary material are mixed, and a polydopamine-coated ternary material is prepared after polymerization reaction;

[0011] (2) The polydopamine-coated ternary material is mixed with n-dodecyl mercaptan to obtain a modified ternary material.

[0012] In an optional embodiment, the molar ratio of the dopamine, the n-dodecyl mercaptan and the ternary material is (1-10):(1-50):100;

[0013] Preferably, the molar ratio of the dopamine to the n-dodecyl mercaptan is 1:5.

[0014] In an optional embodiment, the preparation step of the ternary material includes: mixing a lithium source and nickel-cobalt-manganese hydroxide, and sintering to obtain the ternary material;

[0015] Preferably, the lithium source is at least one of lithium hydroxide, lithium carbonate and lithium oxide;

[0016] Preferably, the sintering is carried out in an oxygen atmosphere;

[0017] Preferably, the sintering temperature is 750-1050° C., and the sintering time is 10-12 hours.

[0018] In an optional embodiment, the step (1) specifically includes: first stirring and mixing dopamine and the ternary material, and first drying to obtain the polydopamine-coated ternary material.

[0019] In an optional embodiment, the dopamine is at least one of a dopamine monomer and a dopamine hydrochloride monomer;

[0020] Preferably, the first stirring and mixing speed is 500-1000 rpm, and the first stirring and mixing time is 60-120 min;

[0021] Preferably, the first drying is performed under vacuum;

[0022] Preferably, the temperature of the first drying is 105-165°C.

[0023] In an optional embodiment, the ternary material is Li a Ni x Co y Mn z O2;

[0024] Wherein, a, x, y, and z represent the molar ratio of corresponding elements, 0<a<1.10, 0<x<1, 0<y<1, 0<z<1, and x+y+z=1.

[0025] In an optional embodiment, in step (2), the mixing is performed by a second stirring mixing method;

[0026] In an optional embodiment, the step of second drying is further included after the polydopamine-coated ternary material is mixed with n-dodecyl mercaptan.

[0027] In an optional embodiment, the second stirring and mixing speed is 500-1000 rpm, and the second stirring and mixing time is 30-120 min;

[0028] Preferably, the second drying is performed under vacuum;

[0029] Preferably, the temperature of the second drying is 285-300° C. The n-dodecyl mercaptan-modified polydopamine is achieved in the second stirring process, and the purpose of the second drying is to remove unreacted n-dodecyl mercaptan, because a small amount of n-dodecyl mercaptan will remain in the actual reaction process.

[0030] In the present invention, the preparation method of the modified ternary material specifically includes: performing a first stirring and mixing of dopamine and the ternary material, performing a first drying after solid-liquid separation, and obtaining a polydopamine-coated ternary material; performing a second stirring and mixing of the polydopamine-coated ternary material and n-dodecyl mercaptan, performing a second drying after solid-liquid separation, and obtaining a modified ternary material; wherein, preferably, the first stirring and mixing speed is 500-1000rpm, and the time is 60-120min; the second stirring speed is 500-1000rpm, and the time is 30-120min; the first drying and the second drying are carried out under vacuum, the first drying temperature is 105-165°C, and the second drying temperature is 285-300°C.

[0031] In an optional embodiment, the first drying time is 1-10 hours; the second drying time is 1-2 hours;

[0032] In an optional embodiment, the solid-liquid separation speed is 2000-6000rpm;

[0033] The present invention provides an application of a modified ternary material prepared by the above preparation method in a lithium ion battery.

[0034] The technical solution of the present invention has the following advantages:

[0035] 1. The modified ternary material provided by the present invention comprises a ternary material and a coating layer, wherein the coating layer comprises polydopamine modified with n-dodecyl mercaptan. The modified ternary material can effectively reduce the residual alkali on the surface of the material and the degree of electrolyte erosion, increase the lipophilicity of the material, and thus improve the capacity and cycle performance of the battery made of the material. Specifically, the present invention adopts polydopamine coating, which can be evenly coated on the surface of the ternary material to form a physical isolation layer to prevent the electrolyte from corroding the surface of the ternary material; at the same time, the polydopamine with good adhesion coats the positive electrode particles, so that the surface of the ternary material has the functional groups of polydopamine, that is, the ternary material has the characteristics of polydopamine. Polydopamine is a hydrophilic and oleophobic material with poor electrolyte wettability. The present invention adopts n-dodecyl mercaptan to modify polydopamine. The hydrophobic and lipophilic long chains of n-dodecyl mercaptan react with the functional groups of polydopamine, and the strong oil absorption capacity of the long-chain alkane is utilized to increase the adsorption capacity of the surface of the ternary material to the electrolyte, which is more conducive to Li + Solvation can improve the diffusion efficiency of lithium ions entering the electrolyte, which can solve the problem of poor electrolyte wettability in ternary materials coated with polydopamine alone, increase the material's lipophilicity, and improve the material's capacity and cycle performance.

[0036] 2. The present invention provides a method for preparing an in-situ coated positive electrode material, the method comprising: (1) mixing dopamine and a ternary material, and preparing a polydopamine-coated ternary material after polymerization; (2) mixing the polydopamine-coated ternary material with n-dodecyl mercaptan to prepare a modified ternary material. The modified ternary material prepared by the preparation method can effectively reduce the residual alkali on the surface of the material and the degree of electrolyte corrosion, increase the lipophilicity of the material, and thus improve the capacity and cycle performance of the battery made of the material. Specifically, the present invention utilizes the characteristics that residual alkali on the surface of the ternary material is soluble in water and dopamine is oxidized to form polydopamine in an alkaline environment to prepare the polydopamine-coated ternary material, and the preparation method is simple; the preparation method mixes the polydopamine-coated ternary material with n-dodecyl mercaptan, utilizes the hydrophobic and lipophilic long chain of n-dodecyl mercaptan to perform lipophilic modification on the polydopamine to increase its lipophilic ability, overcomes the defects of the prior art polydopamine-coated positive electrode material in poor wettability in the electrolyte, which affects the solvation after lithium ion deintercalation, and the modified ternary material finally prepared has a relatively complete surface polymer layer, good wettability to the electrolyte, and good capacity and cycle performance.

[0037] 3. The preparation method of the in-situ coated positive electrode material provided by the present invention adopts dopamine monomer to carry out polymerization reaction. The dopamine monomer can carry out polymerization reaction in an alkaline environment with a pH value > 7.5 without an initiator, and the residual alkali on the surface of the ternary material of the present invention is dissolved in water, so that the system presents an alkaline environment (pH value > 7.5), and dopamine can spontaneously carry out polymerization reaction. On the other hand, the molecular weight of the dopamine monomer used for the polymerization reaction is controllable.

[0038] 4. The preparation method of the in-situ coated positive electrode material provided by the present invention, the modified polydopamine has good lipophilic properties, on the one hand, it can increase the wettability of the organic solvent in the electrolyte to the surface of the ternary material, and expand the contact area with the electrolyte; on the other hand, it can indirectly adsorb the solvent molecules in the electrolyte through the coordination of metal ions, so that the Li diffused to the surface of the material + It is easier to solvate, which improves the diffusion efficiency of lithium ions in the electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0040] Figure 1 It is a capacity retention rate diagram of the positive electrode materials prepared in Examples 1-5 of the present invention and Comparative Examples 1-3, wherein the horizontal axis is the number of cycles and the vertical axis is the capacity retention rate. DETAILED DESCRIPTION

[0041] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0042] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0043] Example 1

[0044] This embodiment provides a method for preparing a modified ternary material, comprising the following steps:

[0045] (1) 10.5 mol LiOH, 10 mol Ni0.83 Co 0.12 Mn 0.05 (OH)2 was mixed evenly by a high-speed mixer and sintered at 750℃ for 10h in an oxygen atmosphere to obtain the ternary material Li 1.0 Ni 0.83 Co 0.12 Mn 0.05 O2; dissolving 10 mol of the ternary material in 500 g of water, adding 1 mol of dopamine monomer, and stirring at 500 rpm for 60 min to obtain a first solution; after solid-liquid separation of the first solution at 2000 rpm centrifuge, drying at 105° C. for 5 h, obtaining 10 mol of polydopamine-coated ternary material, wherein the molar content of polydopamine in the ternary material is 1%;

[0046] (2) 10 mol of the polydopamine-coated ternary material was mixed with 5 mol of n-dodecyl mercaptan, and stirred at 500 rpm for 30 min to obtain a second solution; the second solution was separated into solid and liquid at 2000 rpm in a centrifuge, and then dried at 285° C. for 1 h to obtain a modified ternary material.

[0047] Example 2

[0048] This embodiment provides a method for preparing a modified ternary material, comprising the following steps:

[0049] (1) 10.5 mol LiOH, 10 mol Ni 0.83 Co 0.12 Mn 0.05 (OH)2 was mixed evenly by a high-speed mixer and sintered at 750℃ for 10h in an oxygen atmosphere to obtain the ternary material Li 1.0 Ni 0.83 Co 0.12 Mn 0.05 O2; dissolving 10 mol of the ternary material in 500 g of water, adding 0.1 mol of dopamine monomer, and stirring at 1000 rpm for 120 min to obtain a first solution; after solid-liquid separation of the first solution at 4000 rpm centrifuge, drying at 165° C. for 10 h, obtaining 10 mol of polydopamine-coated ternary material, the molar content of polydopamine in the ternary material being 0.01%;

[0050] (2) 10 mol of the above-mentioned polydopamine-coated ternary material was mixed with 0.5 mol of n-dodecyl mercaptan, and stirred at 500 rpm for 120 min to obtain a second solution; after the second solution was solid-liquid separated at 4000 rpm in a centrifuge, it was dried at 300° C. for 2 h to obtain a modified ternary material.

[0051] Example 3

[0052] This embodiment provides a method for preparing a modified ternary material, comprising the following steps:

[0053] (1) 10.5 mol LiOH, 10 mol Ni 0.83 Co 0.12 Mn 0.05 (OH)2 was mixed evenly by a high-speed mixer and sintered at 750℃ for 10h in an oxygen atmosphere to obtain the ternary material Li 1.0 Ni 0.83 Co 0.12 Mn 0.05 O2; dissolving 10 mol of the ternary material in 500 g of water, adding 0.5 mol of dopamine monomer, and stirring at 500 rpm for 60 min to obtain a first solution; after solid-liquid separation of the first solution at 2000 rpm centrifuge, drying at 105° C. for 1 h, obtaining 10 mol of polydopamine-coated ternary material, wherein the molar content of polydopamine in the ternary material is 0.5%;

[0054] (2) 10 mol of the polydopamine-coated ternary material was mixed with 2.5 mol of n-dodecyl mercaptan, and stirred at 500 rpm for 30 min to obtain a second solution; the second solution was separated into solid and liquid at 2000 rpm in a centrifuge, and then dried at 285° C. for 1 h to obtain a modified ternary material.

[0055] Example 4

[0056] This embodiment provides a method for preparing a modified ternary material, comprising the following steps:

[0057] (1) 10.5 mol LiOH, 10 mol Ni 0.83 Co 0.12 Mn 0.05 (OH)2 was mixed evenly by a high-speed mixer and sintered at 750℃ for 10h in an oxygen atmosphere to obtain the ternary material Li 1.0 Ni 0.83 Co 0.12 Mn 0.05 O2; dissolving 10 mol of the ternary material in 500 g of water, adding 1 mol of dopamine monomer, and stirring at 500 rpm for 60 min to obtain a first solution; after solid-liquid separation of the first solution at 2000 rpm centrifuge, drying at 105° C. for 5 h, obtaining 10 mol of polydopamine-coated ternary material, wherein the molar content of polydopamine in the ternary material is 1%;

[0058] (2) 10 mol of the polydopamine-coated ternary material was mixed with 2 mol of n-dodecyl mercaptan, and stirred at 500 rpm for 30 min to obtain a second solution; the second solution was separated into solid and liquid at 2000 rpm in a centrifuge, and then dried at 285° C. for 1 h to obtain a modified ternary material.

[0059] Example 5

[0060] This embodiment provides a method for preparing a modified ternary material, comprising the following steps:

[0061] (1) 10.5 mol LiOH, 10 mol Ni 0.83 Co 0.12 Mn 0.05 (OH)2 was mixed evenly by a high-speed mixer and sintered at 900℃ for 12h in an oxygen atmosphere to obtain the ternary material Li 1.0 Ni 0.83 Co 0.12 Mn 0.05 O2; dissolving 10 mol of the ternary material in 500 g of water, adding 0.3 mol of dopamine hydrochloride monomer, and stirring at 500 rpm for 60 min to obtain a first solution; after solid-liquid separation of the first solution at 6000 rpm centrifuge, drying at 135° C. for 7 h, obtaining 10 mol of polydopamine-coated ternary material, wherein the molar content of polydopamine in the ternary material is 0.3%;

[0062] (2) 10 mol of the above-mentioned polydopamine-coated ternary material was mixed with 1.5 mol of n-dodecyl mercaptan, and stirred at 800 rpm for 100 min to obtain a second solution; after the second solution was solid-liquid separated at 6000 rpm in a centrifuge, it was dried at 295° C. for 1 h to obtain a modified ternary material.

[0063] Comparative Example 1

[0064] This comparative example provides a method for preparing a ternary material, comprising the following steps:

[0065] (1) 10.5 mol LiOH, 10 mol Ni 0.83 Co 0.12 Mn 0.05 (OH)2 was mixed evenly by a high-speed mixer and sintered at 750℃ for 10h in an oxygen atmosphere to obtain the ternary material Li 1.0 Ni 0.83 Co 0.12 Mn 0.05O2; dissolve 10 mol of the ternary material in 500 g of water, add 1 mol of dopamine monomer, and stir at 500 rpm for 60 min to obtain a first solution; after solid-liquid separation of the first solution at 2000 rpm in a centrifuge, dry it at 105°C for 5 h to obtain a ternary material, in which the molar content of polydopamine in the ternary material is 1%.

[0066] Comparative Example 2

[0067] This comparative example provides a method for preparing a ternary material, comprising the following steps:

[0068] (1) 10.5 mol LiOH, 10 mol Ni 0.83 Co 0.12 Mn 0.05 (OH)2 was mixed evenly by a high-speed mixer and sintered at 750℃ for 10h in an oxygen atmosphere to obtain the ternary material Li 1.0 Ni 0.83 Co 0.12 Mn 0.05 O2; 10 mol of the ternary material was dissolved in 500 g of water, and stirred at 500 rpm for 60 min to obtain a first solution; after the first solution was separated from the solid and liquid in a centrifuge at 2000 rpm, it was dried at 105°C for 5 h to obtain the ternary material.

[0069] Comparative Example 3

[0070] This comparative example provides a method for preparing a ternary material, comprising the following steps:

[0071] (1) 10.5 mol LiOH, 10 mol Ni 0.83 Co 0.12 Mn 0.05 (OH)2 was mixed evenly by a high-speed mixer and sintered at 750℃ for 10h in an oxygen atmosphere to obtain the ternary material Li 1.0 Ni 0.83 Co 0.12 Mn 0.05 O2; dissolving 10 mol of the ternary material in 500 g of water, adding 1 mol of dopamine monomer, and stirring at 500 rpm for 60 min to obtain a first solution; after solid-liquid separation of the first solution at 2000 rpm centrifuge, drying at 105° C. for 5 h to obtain a polydopamine-coated ternary material, wherein the molar content of polydopamine in the ternary material is 1%;

[0072] (2) 10 mol of the polydopamine-coated ternary material was mixed with 5 mol of ethanol and stirred at 500 rpm for 30 min to obtain a second solution; the second solution was solid-liquid separated at 2000 rpm in a centrifuge and dried at 85° C. for 1 h to obtain a ternary material.

[0073] Test Example 1

[0074] This test example provides the performance tests of the modified ternary materials of each embodiment and comparative example, as follows:

[0075] (1) Electrochemical properties of modified ternary materials:

[0076] Assemble the battery: weigh the modified ternary material, conductive carbon black and PVDF according to the mass ratio of 90:5:5, mix them, add the solvent NMP to prepare the positive electrode slurry, evenly coat the slurry on the aluminum foil, bake at 105℃ for 1h, cut the baked electrode pieces and put them into the tablet press for compaction at 25Mpa, cut out small discs, assemble them under nitrogen atmosphere, put the small discs into the positive electrode side of the button battery housing, with the fluorine-coated side facing the positive electrode, drop 50μL of 1mol / L electrolyte (EC, EMC and DMC in a volume ratio of 1:1:1), put in the diaphragm and then drop 50μL of electrolyte, put in the pure lithium sheet, gasket, shrapnel, button the negative electrode housing, and encapsulate it into a CR2032 button battery.

[0077] Test method:

[0078] (1) 0.1C first discharge measurement: The battery was charged at 0.1C and discharged at 0.1C once. The results are shown in Table 1.

[0079] (2) 0.5C first discharge measurement: The battery was charged at 0.5C and discharged at 0.5C once. The results are shown in Table 1.

[0080] (3) 1C first discharge measurement: The battery was charged at 1C and discharged at 1C once. The results are shown in Table 1.

[0081] (4) Cycle test method: The battery was charged at 0.1C and discharged at 0.1C for 200 cycles, and the capacity retention rate at different cycles was calculated. The results are shown in Tables 1 and Figure 1 .

[0082] Table 1 Performance of batteries made of modified ternary materials in various embodiments and comparative examples

[0083]

[0084]

[0085] As can be seen from Table 1, after the modified ternary material of the present invention is made into a battery, the 0.1C first discharge is greater than 203.0mAh / g, the 0.5C first discharge is greater than 197.2mAh / g, and the 1C first discharge is greater than 192.6mAh / g. The capacity retention rate after 200 cycles is maintained at about 94.0% of the initial discharge capacity. The modified ternary material prepared by the present invention has excellent performance. It can be seen from Examples 1 and 4 that when the molar ratio of dopamine and n-dodecyl mercaptan is 1:5, the capacity retention rate and the first effect of the battery can be further optimized, indicating that when the molar ratio of dopamine and n-dodecyl mercaptan is preferably 1:5, the wettability of the ternary material in the electrolyte can be improved, further promoting the entry of lithium ions into the solvent, thereby improving the electrical performance. In Example 4, the amount of n-dodecyl mercaptan added is less than that in Example 1. The lipophilic alkyl long chain in n-dodecyl mercaptan does not completely replace the aromatic group of polydopamine, so that polydopamine still has certain oleophobic properties. There are still certain oleophobic aromatic groups on the surface of the ternary material, and the electrolyte wettability is improved, but it is still insufficient. The poor electrolyte wettability will hinder the diffusion of lithium ions into the electrolyte, and thus the capacity and cycle performance are reduced compared with Example 1.

[0086] Compared with the embodiment, in Comparative Example 1, n-dodecyl mercaptan was not added to modify polydopamine for lipophilicity, and the 0.1C first discharge, 0.5C first discharge, and 1C first discharge of the prepared battery decreased, and the capacity retention rate after 200 cycles decreased significantly, indicating that only using unmodified polydopamine, due to the strong oleophobicity of polydopamine, will inhibit the solvation of lithium ions into the electrolyte, affecting the capacity and cycle performance. Conversely, it is proved that adding n-dodecyl mercaptan to modify polydopamine for lipophilicity can significantly improve the capacity and cycle performance of the prepared modified ternary material; Comparative Example 2 was not coated with polydopamine, and dopamine and n-dodecyl mercaptan were not added. Its 0.1C first discharge, 0.5C first discharge, 1C first discharge, and capacity retention rate after 200 cycles are significantly reduced compared with Examples 1-5, but are improved compared with Comparative Example 1, which reversely indicates that the use of unmodified polydopamine-coated ternary materials reduces the specific capacity and capacity retention rate of the prepared battery; Comparative Example 3 uses ethanol to treat polydopamine, and the 0.1C first discharge, 0.5C first discharge, 1C first discharge reduction, and capacity retention rate after 200 cycles of the battery made of the prepared ternary material are also greatly reduced, indicating that other common modifiers cannot replace n-dodecyl mercaptan to achieve the effect of lipophilic modification. It can be seen from Comparative Examples 1-3 that the polydopamine-coated ternary material modified with n-dodecyl mercaptan will greatly affect the 0.1C first discharge, 0.5C first discharge, 1C first discharge reduction, and capacity retention rate after 200 cycles of the generated modified ternary material.

[0087] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A modified ternary material, characterized in that: The invention comprises a ternary material and a coating layer, wherein the coating layer comprises polydopamine modified with n-dodecyl mercaptan.

2. The modified ternary material according to claim 1, characterized in that: The molar content of the polydopamine in the ternary material is 0.01-1%.

3. A method for preparing a modified ternary material, characterized in that: The following steps are involved: (1) dopamine and the ternary material are mixed, and a polydopamine-coated ternary material is prepared after polymerization reaction; (2) The polydopamine-coated ternary material is mixed with n-dodecyl mercaptan to obtain a modified ternary material.

4. The preparation method according to claim 3, characterized in that: The molar ratio of the dopamine, the n-dodecyl mercaptan and the ternary material is (1-10):(1-50):100; Preferably, the molar ratio of the dopamine to the n-dodecyl mercaptan is 1:

5.

5. The preparation method according to claim 3 or 4, characterized in that: The step (1) specifically comprises: first stirring and mixing dopamine and the ternary material, and first drying to obtain the polydopamine-coated ternary material.

6. The preparation method according to claim 5, characterized in that: The dopamine is at least one of a dopamine monomer and a dopamine hydrochloride monomer; Preferably, the first stirring and mixing speed is 500-1000 rpm, and the first stirring and mixing time is 60-120 min; Preferably, the first drying is performed under vacuum; Preferably, the temperature of the first drying is 105-165°C.

7. The preparation method according to any one of claims 3 to 5, characterized in that: The ternary material is Li a Ni x Co y Mn z O2; Wherein, a, x, y, and z represent the molar ratio of corresponding elements, 0<a<1.10, 0<x<1, 0<y<1, 0<z<1, and x+y+z=1.

8. The preparation method according to claim 3, characterized in that: In step (2), the mixing is performed by a second stirring mixing method; and / or, After the polydopamine-coated ternary material is mixed with n-dodecyl mercaptan, a second drying step is also included.

9. The preparation method according to claim 8, characterized in that: The second stirring and mixing speed is 500-1000 rpm, and the second stirring and mixing time is 30-120 min; Preferably, the second drying is performed under vacuum; Preferably, the second drying temperature is 285-300°C.

10. Use of the modified ternary material according to any one of claims 1 to 2 or the modified ternary material prepared by the preparation method according to any one of claims 3 to 9 in lithium-ion batteries.

Citation Information

Cited By

  • Positive electrode material, composite positive electrode material, positive electrode plate, preparation methods of positive electrode material and positive electrode plate, and lithium ion power battery

    CN119786576A