Fast ion conductor coated porous silicon carbon negative electrode material and preparation method thereof
By forming a high-porous porous carbon material on the silicon carbon negative electrode material and growing a fast ion conductor cladding layer in situ, the problems of low mechanical strength and poor ionic conductivity of silicon carbon composite materials are solved, and the circulation performance and energy density of lithium-ion batteries are improved .
Patent Information
- Application Number
- CN202411238982.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-12
AI Technical Summary
The existing silicon-carbon composite anode materials have low mechanical strength and poor ionic conductivity, which limits the cycle life and energy density of lithium-ion batteries.
The preparation method of fast ion conductor coated porous silicon carbon negative electrode material is formed by the steps of resin pre-carbonization, crushing and alkali mixing, activation treatment, silane deposition and chemical vapor deposition, and forming high-porous porous carbon material on its surface. Grow uniformly fast ion conductor cladding in situ to improve the mechanical strength and conductivity of the material.
It significantly improves the capacity and circulation performance of the electrode, enhances the rate performance of the negative electrode material, is simple and easy to operate, is suitable for industrial production, and reduces side reactions.
Smart Images

Figure CN118943337A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery negative electrode materials, and in particular to a fast ion conductor coated porous silicon-carbon negative electrode material and a preparation method thereof. Background Art
[0002] As an important energy source for modern portable electronic devices and electric vehicles, the energy density and cycle life of lithium-ion batteries have always been the focus of research. Silicon-based negative electrode materials have attracted much attention because of their theoretical specific capacity of up to 4200mAh / g, which is ten times that of traditional graphite negative electrodes. However, the volume of silicon changes significantly during the charging and discharging process, resulting in material pulverization and electrode failure, which seriously affects the cycle life. In order to overcome these problems, researchers have tried to improve the stability and conductivity of silicon-based negative electrodes through methods such as nano-silicon, composite material design, and surface coating. Despite the challenges, silicon-based negative electrode materials have great potential and application prospects in improving the energy density of lithium-ion batteries.
[0003] At present, the expansion of Si negative electrode is mainly alleviated by nano-sizing, and silicon is made into nano-balls, nano-wires, etc. However, the conventional grinding method can only control the Si particle size to about 100nm. At the same time, the excessive nano-sizing process will also be accompanied by the increase of the specific surface area of the material, affecting the material processing and performance. In order to solve the bottleneck of the traditional grinding method to control the size of Si particles, patent CN 116314791A uses porous carbon as a matrix and obtains a silicon-carbon composite material of nano-silicon and soft carbon by silane deposition. The amorphous carbon coating layer used in this preparation method may not provide sufficient mechanical strength and conductivity during high-rate charge and discharge, resulting in the destruction of the electrode structure; patent CN 116525805A discloses a fast ion conductor coated silicon-based composite material and its preparation method. The precursor material is obtained by uniformly mixing silicon-oxygen material, lithium-containing binder, and carbon nanotubes and spray drying, and then the precursor material is deposited on the surface of the material by a plasma method. Fast ion conductors and amorphous carbon. The electronic conductivity and ionic conductivity of the negative electrode materials prepared by this method have been improved, but its application is limited by its expensive equipment, high precursor cost, and limited sample processing capabilities. Summary of the invention
[0004] The purpose of the present invention is to provide a fast ion conductor coated porous silicon-carbon negative electrode material and a preparation method thereof, so as to solve the technical problems of low mechanical strength and poor ion conductivity of existing silicon-carbon composite negative electrode materials.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a fast ion conductor coated porous silicon-carbon negative electrode material, comprising the following steps:
[0007] (1) pre-carbonizing the resin under a nitrogen atmosphere to obtain a carbon precursor;
[0008] (2) crushing the carbon precursor and mixing it with alkali in a solid phase, and then activating and acid-washing the mixture in sequence to obtain a porous carbon material;
[0009] (3) preparing nano-silicon on the surface of the porous carbon material through a deposition reaction of a silane compound to obtain a nano-silicon deposited porous carbon substrate;
[0010] (4) introducing a carbon source gas under a protective gas atmosphere to perform chemical vapor deposition on the nano-silicon deposited porous carbon substrate to obtain a silane deposited porous carbon composite material;
[0011] (5) The silane-deposited porous carbon composite material, metal salt, phosphate solution and alkaline precipitant are mixed and then subjected to reflux reaction and calcination treatment in sequence to obtain a fast ion conductor-coated porous silicon-carbon negative electrode material.
[0012] Furthermore, in the step (1), the resin comprises one or more of phenolic resin, epoxy resin and furfural resin, the pre-carbonization temperature is 400-800° C., and the pre-carbonization time is 1-2 hours.
[0013] Furthermore, in the step (2), the alkali comprises one or more of potassium hydroxide, sodium hydroxide, strong calcium oxide, potassium carbonate and sodium carbonate, the particle size of the carbon precursor is 2 to 50 μm, and the mass ratio of the carbon precursor to the alkali is 1:1 to 5;
[0014] The temperature of the activation treatment is 500-1000°C, and the time of the activation treatment is 1-4 hours.
[0015] Furthermore, in the step (3), the silane compound comprises monosilane and / or disilane, the deposition reaction is carried out under a protective gas, the protective gas comprises one or more of nitrogen, argon and helium, the volume ratio of the silane compound to the protective gas is 1:10 to 1:1, and the flow rate of the silane compound is 0.5 to 2 L / min.
[0016] Furthermore, in the step (3), the temperature of the deposition reaction is 500-1000° C., the time of the deposition reaction is 1-2 hours, and the mass ratio of the Si skeleton in the silane compound to the C skeleton in the porous carbon material is 1:9-9:1.
[0017] Furthermore, in the step (4), the carbon source gas comprises one or more of methane, ethane, propane, acetylene and propyne, the shielding gas comprises one or more of nitrogen, argon and helium, the volume ratio of the carbon source gas to the shielding gas is 1:10 to 1:1, and the flow rate of the carbon source gas is 0.5 to 2 L / min; the temperature of the chemical vapor deposition is 500 to 1000°C, and the time is 1 to 3 hours.
[0018] Furthermore, in step (5), the metal salt comprises one or more of chloride, nitrate, sulfate and organic acid salt; the phosphate solution comprises one or more of sodium dihydrogen phosphate solution, ammonium dihydrogen phosphate solution, disodium hydrogen phosphate solution and diammonium hydrogen phosphate solution; and the alkaline precipitant comprises one or more of ammonia water, ethanolamine, sodium hydroxide and potassium hydroxide.
[0019] Furthermore, in step (5), the mixing is carried out in an organic solvent, and the organic solvent comprises one or more of methanol, ethanol, ethylene glycol, propanol, isopropanol, propylene glycol, n-butanol, acetonitrile and acetone;
[0020] In the mixed system, the concentration of the metal salt is 10 -6 ~1.0mol / L, the concentration of the silane deposited porous carbon composite material is 0.1~1000g / L, the concentration of the phosphate solution is 10 -6 ~5mol / L, the concentration of alkaline precipitant is 10 -6 ~10mol / L.
[0021] Furthermore, in step (5), the temperature of the reflux reaction is 10 to 200° C., and the time of the reflux reaction is 2 to 5 hours;
[0022] The calcination temperature is 100-600°C, and the calcination time is 1-5 hours.
[0023] The invention provides a fast ion conductor coated porous silicon-carbon negative electrode material.
[0024] Beneficial effects of the present invention:
[0025] (1) The present invention uses a chemical activation method to prepare a high-pore volume porous carbon material, and generates nano-silicon by in-situ deposition of silane in the pores. Since the high-pore volume porous carbon provides abundant deposition sites, this significantly increases the silicon content in the material, thereby effectively improving the capacity of the electrode.
[0026] (2) The present invention uses a method of co-precipitation of a phosphorus source and a metal salt to achieve secondary coating on the surface of a silicon-carbon negative electrode material. The method of the present invention is simple and easy to operate, has mild conditions, is widely applicable, is environmentally friendly, and is suitable for industrial production. The method of the present invention uses a chemical reaction to in situ grow a uniform and continuous fast ion conductor coating layer on the surface of a silicon-carbon negative electrode material. The coating layer can not only prevent direct contact between the negative electrode active material and the electrolyte solution, thereby reducing side reactions, but also significantly improve the cycle performance and rate performance of the negative electrode material by accelerating the diffusion rate of lithium ions. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The present invention is a flow chart for preparing the fast ion conductor coated porous silicon-carbon negative electrode material. DETAILED DESCRIPTION
[0028] The present invention provides a method for preparing a fast ion conductor coated porous silicon-carbon negative electrode material, comprising the following steps:
[0029] (1) pre-carbonizing the resin under a nitrogen atmosphere to obtain a carbon precursor;
[0030] (2) crushing the carbon precursor and mixing it with alkali in a solid phase, and then activating and acid-washing the mixture in sequence to obtain a porous carbon material;
[0031] (3) preparing nano-silicon on the surface of the porous carbon material through a deposition reaction of a silane compound to obtain a nano-silicon deposited porous carbon substrate;
[0032] (4) introducing a carbon source gas under a protective gas atmosphere to perform chemical vapor deposition on the nano-silicon deposited porous carbon substrate to obtain a silane deposited porous carbon composite material;
[0033] (5) The silane-deposited porous carbon composite material, metal salt, phosphate solution and alkaline precipitant are mixed and then subjected to reflux reaction and calcination treatment in sequence to obtain a fast ion conductor-coated porous silicon-carbon negative electrode material.
[0034] In the present invention, in the step (1), the resin comprises one or more of phenolic resin, epoxy resin and furfural resin, preferably phenolic resin; the pre-carbonization temperature is 400-800°C, preferably 500-700°C, and more preferably 550-650°C; the pre-carbonization time is 1-2h, preferably 1h.
[0035] In the present invention, in the step (2), the alkali comprises one or more of potassium hydroxide, sodium hydroxide, strong calcium oxide, potassium carbonate and sodium carbonate, preferably potassium hydroxide; the particle size of the crushed carbon precursor is 2 to 50 μm, preferably 10 to 40 μm, and more preferably 20 to 30 μm; the mass ratio of the carbon precursor to the alkali is 1:1 to 5, preferably 1:2 to 4, and more preferably 1:3.
[0036] In the present invention, in step (2), the temperature of the activation treatment is 500-1000° C., preferably 600-900° C., and more preferably 700-800° C.; the time of the activation treatment is 1-4 h, and preferably 2-3 h.
[0037] In the present invention, in the step (3), the silane compound comprises monosilane and / or disilane, preferably monosilane; the deposition reaction is carried out under a protective gas, the protective gas comprises one or more of nitrogen, argon and helium, preferably nitrogen; the volume ratio of the silane compound to the protective gas is 1:10 to 1:1, preferably 1:9 to 1:2, further preferably 1:8 to 1:5, more preferably 1:6; the flow rate of the silane compound is 0.5 to 2 L / min, preferably 1 L / min.
[0038] In the present invention, in the step (3), the temperature of the deposition reaction is 500-1000°C, preferably 600-900°C, and more preferably 700-800°C; the time of the deposition reaction is 1-2h, preferably 1h; the mass ratio of the Si skeleton in the silane compound to the C skeleton in the porous carbon material is 1:9-9:1, preferably 2:8-8:2, and more preferably 5:5.
[0039] In the present invention, in the step (4), the carbon source gas comprises one or more of methane, ethane, propane, acetylene and propyne, preferably acetylene and / or propyne; the shielding gas comprises one or more of nitrogen, argon and helium, preferably nitrogen; the volume ratio of the carbon source gas to the shielding gas is 1:10 to 1:1, preferably 1:9 to 1:2, and more preferably 1:6; the flow rate of the carbon source gas is 0.5 to 2 L / min, preferably 1 L / min; the temperature of the chemical vapor deposition is 500 to 1000°C, preferably 600 to 900°C, and more preferably 700 to 800°C; the time is 1 to 3 hours, preferably 2 hours.
[0040] In the present invention, in step (5), the metal salt comprises one or more of chloride, nitrate, sulfate and organic acid salt; preferably one or more of lithium nitrate, aluminum chloride and vanadium sulfate.
[0041] In the present invention, in the step (5), the phosphate solution comprises one or more of sodium dihydrogen phosphate solution, ammonium dihydrogen phosphate solution, disodium hydrogen phosphate solution and diammonium hydrogen phosphate solution, preferably disodium hydrogen phosphate solution; the alkaline precipitant comprises one or more of ammonia water, ethanolamine, sodium hydroxide and potassium hydroxide, preferably ethanolamine and / or sodium hydroxide.
[0042] In the present invention, in step (5), mixing is carried out in an organic solvent, and the organic solvent comprises one or more of methanol, ethanol, ethylene glycol, propanol, isopropanol, propylene glycol, n-butanol, acetonitrile and acetone, preferably one or more of methanol, ethanol, ethylene glycol, propanol and isopropanol.
[0043] In the present invention, in step (5), in the mixed system, the concentration of the metal salt is 10 -6 ~1.0mol / L, preferably 10 -5 ~0.1mol / L, more preferably 10 -4 ~0.01mol / L; the concentration of the silane deposited porous carbon composite material is 0.1~1000g / L, preferably 1~100g / L, and more preferably 10~80g / L; the concentration of the phosphate solution is 10 -6 ~5mol / L, preferably 10 -5 ~1mol / L, more preferably 10 -4 ~0.01mol / L; the concentration of alkaline precipitant is 10 -6 ~10mol / L, preferably 10 -5 ~1mol / L, more preferably 10 -4 ~0.1mol / L.
[0044] In the present invention, in step (5), the temperature of the reflux reaction is 10 to 200° C., preferably 50 to 150° C., and more preferably 80 to 100° C.; the time of the reflux reaction is 2 to 5 hours, and preferably 3 to 4 hours.
[0045] In the present invention, in step (5), the calcination temperature is 100-600°C, preferably 200-400°C, and more preferably 300-350°C; the calcination time is 1-5h, preferably 2-4h, and more preferably 3h.
[0046] The invention provides a fast ion conductor coated porous silicon-carbon negative electrode material.
[0047] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0048] Example 1
[0049] (1) dissolving a phenolic resin in ethanol, and drying the mixed solution containing the phenolic resin while stirring at a drying temperature of 100° C. to obtain a carbon source;
[0050] (2) Pre-carbonizing the carbon source at a pre-carbonization temperature of 550°C for a pre-carbonization time of 1 h to obtain a pre-carbonized carbon precursor, which is then crushed to a particle size of 20 μm. The crushed powder is solid-phase mixed with KOH powder at a mass ratio of 1:2, and placed in an activation furnace for activation at 800°C for 2 h. Finally, the residual alkali is removed by washing with hydrochloric acid and deionized water, and the porous carbon material is dried;
[0051] (3) The porous carbon material is placed in a vapor deposition furnace, the temperature is raised to 500° C. in a nitrogen atmosphere, and monosilane / nitrogen is introduced at a flow rate of 0.5 / 3 L / min to carry out a deposition reaction. After keeping the temperature for 60 min, the introduction of monosilane is stopped, and nitrogen is still introduced at 3 L / min;
[0052] (4) heating to 800° C., introducing acetylene / hydrogen: 0.5 / 3 L / min, carrying out chemical vapor deposition reaction, keeping the temperature for 120 min, and maintaining the introduction of hydrogen at 3 L / min during the cooling process, cooling to room temperature, and obtaining a silane-deposited porous carbon composite material;
[0053] (5) 0.2 g of silane-deposited porous carbon composite material, 0.046 g of lithium nitrate, 0.0448 g of disodium hydrogen phosphate and 0.5 g of precipitant ammonia water are mixed in 30 ml of isopropanol, and the pH is adjusted to about 2 with ammonia water; the mixture is refluxed at 90°C for 3 hours under stirring, and the obtained particles are calcined at 300°C for 2 hours after centrifugation, washing and drying to obtain a fast ion conductor coated porous silicon-carbon negative electrode material.
[0054] Example 2
[0055] (1) dissolving an epoxy resin in ethanol, and drying the mixed solution in which the phenolic resin is dissolved while stirring, at a drying temperature of 100° C., to obtain a carbon source;
[0056] (2) Pre-carbonizing the carbon source at a pre-carbonization temperature of 550°C for a pre-carbonization time of 1 h to obtain a pre-carbonized carbon precursor, which is then crushed to a particle size of 20 μm. The crushed powder is solid-phase mixed with NaOH powder at a mass ratio of 1:2, and placed in an activation furnace for activation at 700°C for 2 h. Finally, the residual alkali is removed by washing with hydrochloric acid and deionized water, and the porous carbon material is dried;
[0057] (3) The porous carbon material is placed in a vapor deposition furnace, the temperature is raised to 600° C. in an argon atmosphere, and monosilane / argon is introduced at a flow rate of 0.5 / 4 L / min to carry out a deposition reaction. After keeping the temperature for 60 min, the introduction of monosilane is stopped, and argon is still introduced at 4 L / min;
[0058] (4) heating to 900° C., introducing acetylene / hydrogen: 0.5 / 4 L / min, carrying out chemical vapor deposition reaction, keeping the temperature for 120 min, and maintaining the introduction of hydrogen at 4 L / min during the cooling process, cooling to room temperature, and obtaining a silane-deposited porous carbon composite material;
[0059] (5) 0.2 g of silane-deposited porous carbon composite material, 0.046 g of lithium nitrate, 0.0448 g of disodium hydrogen phosphate and 0.5 g of precipitant ammonia water are mixed in 30 ml of isopropanol, and the pH is adjusted to about 2 with ammonia water; the mixture is refluxed at 90°C for 3 hours under stirring, and the obtained particles are calcined at 350°C for 2 hours after centrifugation, washing and drying to obtain a fast ion conductor-coated porous silicon-carbon negative electrode material.
[0060] Example 3
[0061] Compared with Example 1, only the phenolic resin is changed to furfural resin, and the remaining steps are the same.
[0062] Example 4
[0063] Compared with Example 1, only lithium nitrate is replaced by aluminum chloride, and the remaining steps are the same.
[0064] Application Examples
[0065] A method for assembling a lithium-ion battery with a negative electrode material coated with a fast ion conductor and testing its charge and discharge performance comprises the following steps:
[0066] Add binder, conductive agent and single-walled carbon nanotube (SCNT) to the negative electrode material, stir and slurry, coat on copper foil, dry and roll to obtain negative electrode sheet; the binder used is LA132, the conductive agent is conductive carbon black (SP), and the ratio of negative electrode material, LA123, SP and SCNT is 94:4:1:1. In the electrolyte used, LiPF6 is the electrolyte with a concentration of 1.2 mol / L, and the solvent is a mixture of EC and DEC with a volume ratio of 1:1; the metal lithium sheet is the counter electrode, and the diaphragm is a polypropylene (PP) film. The button cell is assembled in a glove box filled with argon. The electrochemical performance is tested on the Wuhan Blue Electric CT2001A battery tester for charge and discharge performance, with a charge and discharge voltage range of 0.005V-2.0V and a charge and discharge rate of 0.1C, and its rate performance (0.1C-2.0C) is tested.
[0067] The performance of the lithium-ion battery obtained in the example was tested, and the test results are shown in Table 1 below.
[0068] Table 1 Performance test results
[0069]
[0070]
[0071] It can be seen from the above embodiments that the present invention provides a fast ion conductor coated porous silicon carbon negative electrode material and a preparation method thereof. The present invention adopts a chemical activation method to prepare a high pore volume porous carbon material, and generates nano silicon by in-situ deposition of silane in the pores. Since the high pore volume porous carbon provides abundant deposition sites, this significantly increases the silicon content in the material, thereby effectively improving the capacity of the electrode. The fast ion conductor coated silane deposited porous carbon negative electrode material prepared by the method of the present invention has a stable structure, high capacity and good cycle performance.
[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a fast ion conductor coated porous silicon-carbon negative electrode material, characterized in that: The following steps are involved: (1) pre-carbonizing the resin under a nitrogen atmosphere to obtain a carbon precursor; (2) crushing the carbon precursor and mixing it with alkali in a solid phase, and then activating and acid-washing the mixture in sequence to obtain a porous carbon material; (3) preparing nano-silicon on the surface of the porous carbon material through a deposition reaction of a silane compound to obtain a nano-silicon deposited porous carbon substrate; (4) introducing a carbon source gas under a protective gas atmosphere to perform chemical vapor deposition on the nano-silicon deposited porous carbon substrate to obtain a silane deposited porous carbon composite material; (5) The silane-deposited porous carbon composite material, metal salt, phosphate solution and alkaline precipitant are mixed and then subjected to reflux reaction and calcination treatment in sequence to obtain a fast ion conductor-coated porous silicon-carbon negative electrode material.
2. The preparation method according to claim 1, characterized in that: In the step (1), the resin comprises one or more of phenolic resin, epoxy resin and furfural resin, the pre-carbonization temperature is 400-800° C., and the pre-carbonization time is 1-2 hours.
3. The preparation method according to claim 1 or 2, characterized in that: In the step (2), the alkali comprises one or more of potassium hydroxide, sodium hydroxide, strong calcium oxide, potassium carbonate and sodium carbonate, the particle size of the carbon precursor is 2 to 50 μm, and the mass ratio of the carbon precursor to the alkali is 1:1 to 5; The temperature of the activation treatment is 500-1000°C, and the time of the activation treatment is 1-4 hours.
4. The preparation method according to claim 3, characterized in that: In the step (3), the silane compound comprises monosilane and / or disilane, the deposition reaction is carried out under a protective gas, the protective gas comprises one or more of nitrogen, argon and helium, the volume ratio of the silane compound to the protective gas is 1:10 to 1:1, and the flow rate of the silane compound is 0.5 to 2 L / min.
5. The preparation method according to claim 1 or 4, characterized in that: In the step (3), the temperature of the deposition reaction is 500 to 1000° C., the time of the deposition reaction is 1 to 2 hours, and the mass ratio of the Si skeleton in the silane compound to the C skeleton in the porous carbon material is 1:9 to 9:
1.
6. The preparation method according to claim 1, 2 or 4, characterized in that: In the step (4), the carbon source gas comprises one or more of methane, ethane, propane, acetylene and propyne, the protective gas comprises one or more of nitrogen, argon and helium, the volume ratio of the carbon source gas to the protective gas is 1:10 to 1:1, and the flow rate of the carbon source gas is 0.5 to 2 L / min; the temperature of the chemical vapor deposition is 500 to 1000° C., and the time is 1 to 3 hours.
7. The preparation method according to claim 6, characterized in that: In the step (5), the metal salt comprises one or more of chloride, nitrate, sulfate and organic acid salt; the phosphate solution comprises one or more of sodium dihydrogen phosphate solution, ammonium dihydrogen phosphate solution, disodium hydrogen phosphate solution and diammonium hydrogen phosphate solution; and the alkaline precipitant comprises one or more of ammonia water, ethanolamine, sodium hydroxide and potassium hydroxide.
8. The preparation method according to claim 1 or 7, characterized in that: In the step (5), the mixing is carried out in an organic solvent, wherein the organic solvent comprises one or more of methanol, ethanol, ethylene glycol, propanol, isopropanol, propylene glycol, n-butanol, acetonitrile and acetone; In the mixed system, the concentration of the metal salt is 10 -6 ~1.0mol / L, the concentration of the silane deposited porous carbon composite material is 0.1~1000g / L, the concentration of the phosphate solution is 10 -6 ~5mol / L, the concentration of alkaline precipitant is 10 -6 ~10mol / L.
9. The preparation method according to claim 8, characterized in that: In the step (5), the temperature of the reflux reaction is 10 to 200° C., and the time of the reflux reaction is 2 to 5 hours; The calcination temperature is 100-600°C, and the calcination time is 1-5 hours.
10. The fast ion conductor coated porous silicon-carbon negative electrode material prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Cited By
Method for preparing porous carbon through secondary utilization of fine powder of porous carbon airflow powder
CN120589750A
Interconnected hierarchical resin-based porous carbon material as well as preparation method and application thereof
CN120757112A
Preparation method of fast ion conductor coated porous silicon carbon material
CN121044567A
A method for preparing a porous silicon-carbon material coated with a fast ion conductor
CN121044567B
Charge-discharge low-expansion spherical silicon-carbon composite negative electrode material and preparation method thereof
CN121076116A