Silicon-carbon composite material with folded graphene adaptive to volume expansion as well as preparation method and application of silicon-carbon composite material

By using alternate composite structures of pleated graphene and silicon nanosheets in lithium-ion batteries, the expansion effect of silicon nanosheets is buffered, and the problem of conducting network failure caused by silicon volume expansion is solved, and a high capacity and high stability silicon-carbon composite is achieved Materials, simple process and low cost, suitable for large-scale production.

CN118943349APending Publication Date: 2024-11-12MONTA VISTA ENERGY TECH CORP (ANHUI)
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310542223.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The volume expansion of silicon as the negative electrode material of lithium-ion batteries leads to damage to the conductive network, causing the battery to fail after multiple cycles. It is difficult for the prior art to find a balance between cost and stability, especially the cost of electrospinning and chemical vapor deposition technology. High and difficult to produce on a large scale.

Method used

The alternating composite structure is formed by wrinkled graphene and silicon nanosheets. The expansion effect of the silicon nanosheets is buffered by the carbon cladding layer, and combined with ball milling and low-temperature sintering processes, a high-stability and low-cost silicon-carbon composite material is formed.

Benefits of technology

It realizes high capacity and high stability in the negative electrode of lithium-ion battery, long-term stability of the conductive network, and simple process, low cost and easy to produce on a large scale.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943349A_ABST
    Figure CN118943349A_ABST
Patent Text Reader

Abstract

The invention discloses a silicon-carbon composite material with folded graphene adaptive to volume expansion as well as a preparation method and application of the silicon-carbon composite material. The silicon-carbon composite material is provided with a carbon coating layer and a silicon nanosheet / wrinkled graphene alternating composite structure, and the carbon coating layer wraps the silicon nanosheet / wrinkled graphene alternating composite structure. The silicon nanosheet / wrinkled graphene alternating composite structure forms an irregular space to buffer the expansion effect of the silicon nanosheet, and the wrinkled graphene generates elastic deformation to adapt to the volume expansion of the silicon nanosheet when the silicon nanosheet is subjected to charge and discharge volume expansion; the preparation method comprises the following steps: mixing and ball-milling the wrinkled graphene oxide and the silicon nanosheet to obtain an intermediate of the wrinkled graphene oxide composite nano silicon wafer, adding an organic carbon source for sintering, and carrying out heat treatment and carbonization to obtain the product. The high elasticity of the wrinkled graphene is utilized, the method adapts to volume expansion of the silicon nanosheet, a good conductive network can be kept, and the preparation method is simple, low in cost and easy to popularize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium batteries, and in particular relates to a silicon-carbon composite material with wrinkled graphene adapted to volume expansion, and a preparation method and application thereof. Background Art

[0002] Silicon negative electrode material is the key negative electrode material for lithium-ion batteries developed in the past decade. Compared with the theoretical capacity of graphite of 375mAh / g, silicon has an ultra-high theoretical capacity of 4200mAh / g. However, as a negative electrode, the volume expansion caused by the embedding of a large number of lithium ions in silicon is greater than 300%, resulting in stress extrusion inside the negative electrode active layer during the cyclic charge and discharge process, resulting in cracking of the negative electrode active layer and destruction of the conductive network after multiple cycles, causing the battery device to fail quickly and unable to work stably for a long time, which brings great challenges to the design of negative electrode materials.

[0003] At present, in order to overcome this problem, the following three technical routes are mainly focused on: (1) Silicon nano-processing technology, by reducing the size of silicon particles so that the maximum stress generated by their volume expansion does not exceed the elastic stress limit that the particles can tolerate, so that the particles do not break and can maintain the electron transmission inside a single particle. However, the synthesis conditions of silicon nanowires are extremely harsh and the cost is high. (2) Silicon composite technology, by compounding various carbon nanomaterials with silicon, more conductive channels are provided, the conductivity of the negative electrode active layer is enhanced, and the electronic transmission channel breakage caused by volume expansion is slowed down. For example, Chinese invention patent CN113644250A obtains nitrogen-phosphorus co-doped ternary composite powder by co-sintering silicon nanoparticles with carbon nanotubes and organic matter. There are a large number of pores between the composite powder particles to provide space for the volume expansion of silicon. However, the implementation case shows that the performance of the composite material obtained by this method also decays very quickly. Similarly, Chinese invention patent CN115101741A wraps silicon micron particles with graphene, but it also cannot solve the problem of conductive network destruction caused by volume expansion; Chinese invention patent CN114976024A grows silicon nanoparticles in situ on the graphene surface, and its dense structure cannot meet the high stability requirements of long-term charging and discharging. Chinese invention patent CN112599731A uses polyaniline and silicon nanoparticles to composite, and wraps a carbon layer on the surface of silicon nanoparticles. The resulting composite material has good stability and high capacity, but polyaniline is expensive and cannot meet the needs of industrial production. In the field of carbon composites, the most successful technical solution for obtaining highly stable negative electrode materials is to embed silicon nanoparticles into carbon fibers by electrospinning, and the carbon fibers form a porous conductive active layer with each other. For example, Chinese invention patent CN114639807A adopts this method, and the negative electrode material obtained still has an objective discharge capacity after 500 cycles. Similarly, there is the Chinese invention patent CN114566634A, in which the silicon-carbon composite material prepared by electrospinning also exhibits excellent cycle stability and high capacity characteristics. However, electrospinning technology is expensive and difficult to mass produce. (3) Structural regulation strategy. This technical solution is to design a microscopic internal structure so that the silicon particles are distributed in the pore structure of the conductive network, thereby offsetting the volume expansion of the silicon particles and obtaining a stable conductive network. For example, the Chinese invention patent CN1 15020689A uses porous carbon chemistry as a carrier to deposit silicon nanoparticles so that they are distributed inside the porous carbon, forming a silicon-restricted volume expansion with pore space. This technical solution is in line with the idea of ​​high-capacity and high-stability silicon-carbon composite material structural design.However, chemical vapor deposition is often used to composite layered materials on the surface of a flat substrate. It is difficult to control the uniformity of depositing nanoparticles or nanocoatings on the surface of a powder. Although in recent years, there have been methods of enhancing the contact between the powder and the decomposition airflow by stirring in a rotary kiln or enhancing the contact between the airflow and the material by a fluidized bed technology, the effect of large-scale preparation is not ideal, and the uniformity still needs to be improved. Therefore, it is even more impossible to achieve effective deposition of nanoparticles in the inner pores of nanomaterials. Other methods, such as realizing the expected composite material structure through multi-step composite technology, also have a large number of patents disclosed, such as Chinese invention patent CN114824238A, in order to solve the problem of falling off caused by volume expansion between silicon nanoparticles and the conductive network, functionalized silicon nanoparticles by polyethyleneimine and polydopamine copolymers, and then composited with graphene oxide, and finally annealed at high temperature to obtain carbon-coated enhanced graphene / silicon nanoparticle composite materials. This material has a rich pore structure, sufficient encapsulation of special polymers, good combination with graphene oxide and subsequent carbonization, so that a tightly combined porous structure is finally formed, which is conducive to maintaining the stability of the conductive network and improving the overall performance. However, the price of polyethyleneimine and polydopamine copolymers is extremely high, making it difficult to prepare composite materials at low cost and unable to meet the needs of industrial production. However, this type of technical solution proves that the appropriate spatial structure design can achieve high capacity and high stability of silicon-based negative electrode materials. The key is that the process cost is acceptable to the market.

[0004] Therefore, it is an urgent problem to provide a rationally designed silicon-based composite material to achieve high capacity and high stability of silicon-based negative electrode materials while taking into account simple process flow and low cost. Summary of the invention

[0005] The present invention provides a silicon-carbon composite material with wrinkled graphene adapted to volume expansion and a preparation method thereof, the purpose of which is to solve the problem of decreased conductivity after multiple cycles due to volume expansion of silicon materials. This silicon-carbon composite material with wrinkled graphene adapted to volume expansion utilizes the high elasticity of wrinkled graphene, and can maintain the stability of the internal conductive network during the repeated charge and discharge volume expansion of silicon particles to achieve high capacity and high stability of the negative electrode material. At the same time, the preparation method provided by the present invention has a simple process flow, low cost, and is easy to promote.

[0006] In order to achieve the above technical effects, the present invention adopts the following technical solutions:

[0007] The present invention provides a silicon-carbon composite material with wrinkled graphene adapted to volume expansion, the silicon-carbon composite material comprising a carbon coating layer, a silicon nanosheet and wrinkled graphene; the wrinkled graphene and the silicon nanosheet form an alternating composite structure with wrinkles / sheet layers;

[0008] The carbon coating layer is wrapped on the surface of the alternating composite structure;

[0009] The alternating composite structure forms irregular spaces, which can buffer the expansion effect of the silicon nanosheets.

[0010] Furthermore, the silicon nanosheet / wrinkled graphene alternating composite structure is formed by embedding or embedding the silicon nanosheet in the wrinkled graphene oxide.

[0011] The present invention also provides a method for preparing the above-mentioned wrinkled graphene-adaptive silicon-carbon composite material with volume expansion: wrinkled graphene oxide and silicon nanosheets are mixed and ball-milled to obtain an intermediate of wrinkled graphene oxide composite nano-silicon sheets, an organic carbon source is added for sintering, and then heat-treated and carbonized to obtain a silicon-carbon composite material having the silicon nanosheet / wrinkled graphene alternating composite structure and wrapped by a carbon coating layer.

[0012] Furthermore, the above preparation method comprises the following steps:

[0013] S1. Grinding silicon powder into silicon nanosheets;

[0014] S2. ball-milling the graphene oxide to obtain wrinkled graphene oxide, mixing it with the silicon nanosheets in S1 and continuing to ball-mill, and spray-drying to obtain a silicon nanosheet composite wrinkled graphene oxide intermediate;

[0015] S3. The intermediate is mixed with an organic carbon source and carbonized in an inert atmosphere to obtain a carbon-encapsulated intermediate:

[0016] S4. Vacuum sintering the carbon-coated intermediate in S3 to obtain the silicon-carbon composite material with wrinkled graphene adapted to volume expansion.

[0017] Furthermore, the mass ratio of the graphene oxide to the silicon nanosheets is 3 to 7:5.

[0018] Furthermore, the silicon powder nano-sand in S1 is milled for 4 to 12 hours, the graphene oxide in S2 is ball-milled for 3 to 9 hours, and the wrinkled graphene oxide and the silicon nanosheets in S2 are mixed and ball-milled for 10 to 240 minutes.

[0019] Furthermore, the silicon nanosheets in S1 have a thickness of 5 to 200 nm, are ground with 0.2 mm zirconium beads, and have a ball-to-mass ratio of 20 to 5:1 during grinding in S1.

[0020] Furthermore, the carbonization temperature in S3 is 250° C. to 350° C., the carbonization time is 60 to 120 minutes, and the organic carbon source is one or a combination of two or more of glucose, urea, sucrose, maltose, polyvinyl alcohol, chitosan, and chitin.

[0021] Furthermore, the vacuum sintering temperature in S4 is 600°C to 1400°C, the vacuum sintering time is 3 to 4 hours, and the vacuum degree of the vacuum sintering is 5*10 ~2 Entrust.

[0022] The wrinkled graphene-adapted silicon-carbon composite material with volume expansion mentioned above or the wrinkled graphene-adapted silicon-carbon composite material with volume expansion prepared by the preparation method of the present invention is used in the negative electrode of lithium-ion batteries.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1) The present invention provides a silicon-carbon composite material with wrinkled graphene adapted to volume expansion. The microscopic reversible large strain characteristics brought about by the high elasticity of wrinkled graphene can enable the conductive network to adapt to the stress generated by the volume expansion of silicon nanosheets without the conductive contact points falling off. Its simple composite structure can extremely effectively stabilize the electron transmission from the internal conductive network of the electrode to the electrochemically active silicon nanosheets, ensuring that the negative electrode can store and output high capacity in a long-term and stable manner.

[0025] 2) The present invention uses graphene and silicon powder as raw materials, synthesizes a highly stable composite material through a technical route suitable for existing process equipment, obtains wrinkled graphene oxide by ball milling graphene oxide, and obtains an intermediate of wrinkled graphene oxide composite nano-silicon sheet by co-ball milling with silicon nanosheets, adds an organic carbon source and sintered at low temperature with the intermediate to achieve uniform mixing, and then carbonizes the organic carbon source by high-temperature sintering and completely transforms the wrinkled graphene oxide into wrinkled graphene, thereby strengthening the structural stability of the conductive contact point. The raw materials required for this method are completely available in the market, and the preparation of the target material is achieved through a simple process, with low cost and easy large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 This is a schematic diagram of the process for preparing a silicon-carbon composite material according to Example 1 of the present invention.

[0028] Figure 2 This is a scanning electron microscope (SEM) image of the silicon-carbon composite material prepared in Example 1 of the present invention.

[0029] Figure 3 This is a scanning electron microscope (SEM) image of the silicon-carbon composite material prepared in Example 2 of the present invention.

[0030] Figure 4 This is a scanning electron microscope (SEM) image of the silicon-carbon composite material prepared in Example 3 of the present invention.

[0031] Figure 5 This is a charge and discharge curve diagram of the first cycle of the silicon-carbon composite material prepared in Example 1 of the present invention.

[0032] Figure 6 This is a cycle curve diagram of the first 150 cycles of the silicon-carbon composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0033] The present invention will be more fully understood through the following detailed description, which should be read in conjunction with the accompanying drawings. Detailed embodiments of the present invention are disclosed herein; however, it should be understood that the disclosed embodiments are only exemplary of the present invention, which can be embodied in various forms. Therefore, the specific functional details disclosed herein should not be interpreted as limiting, but only as the basis of the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in virtually any appropriate detailed embodiment.

[0034] The present invention uses graphene and silicon powder as raw materials, synthesizes a highly stable composite material through a technical route suitable for existing process equipment, obtains wrinkled graphene oxide by ball milling graphene oxide, and obtains an intermediate of wrinkled graphene oxide composite nano-silicon sheets by co-ball milling with silicon nanosheets, adds an organic carbon source and sinters with the intermediate at low temperature to achieve uniform mixing, and then carbonizes the organic carbon source through high-temperature sintering and completely transforms the wrinkled graphene oxide into wrinkled graphene, thereby enhancing the structural stability of the conductive contact point.

[0035] Example 1

[0036] This embodiment provides a silicon-carbon composite material with wrinkled graphene adapted to volume expansion, see Figure 1 , is a schematic diagram of the preparation process of this embodiment, wherein nano silicon powder is sand-milled to obtain silicon nanosheets, graphene oxide is ball-milled to obtain wrinkled graphene oxide, silicon nanosheets and wrinkled graphene oxide are mixed and ball-milled and spray-dried to obtain an intermediate, and the intermediate is pyrolyzed by an organic carbon source to obtain a silicon-carbon composite material with wrinkled graphene adapted to volume expansion. Specifically, the preparation steps are as follows:

[0037] 1. Preparation of Silicon Nanosheets

[0038] 100 g of 200 nm silicon powder was ultrasonically dispersed in 900 g of anhydrous ethanol to prepare a silicon-ethanol dispersion with a solid content of 10%. The dispersion was poured into the grinding chamber of a nano sand mill and 1 kg of 0.2 mm zirconium beads were added. The dispersion was sand milled for 4 h while maintaining the grinding chamber temperature at 20°C and the rotation speed at 2100 r / min. After the grinding liquid was removed, it was dried in a vacuum oven at 60°C to obtain silicon nanosheets.

[0039] 2. Preparation of Silicon Nanosheet Composite Wrinkled Graphene Oxide Intermediates

[0040] a. 5 g of graphene oxide was ultrasonically dispersed in 200 mL of deionized water and added into a ball mill with a mass ratio of balls to graphene oxide of 20:1. After ball milling for 3 h, a wrinkled graphene dispersion was obtained.

[0041] b. Weigh 5 g of silicon nanosheets from step 1 and add them to the wrinkled graphene dispersion, continue ball milling for 1 hour, and then spray dry to obtain a solid powder of silicon nanosheet composite wrinkled graphene oxide intermediate. The spray drying conditions are: inlet temperature of 220°C, outlet temperature of 120°C, and feed rate of 10 mL / min.

[0042] 3. Preparation of carbon-coated composite intermediates

[0043] Weigh 5 g of the solid powder obtained in step 2 and 2 g of glucose, grind and mix them evenly in a mortar, and then transfer them to a quartz tube furnace. Carbonize them at a heating rate of 2 °C / min to 300 °C in an argon atmosphere, and keep the temperature constant for 1 h to obtain a carbon-coated composite intermediate.

[0044] 4. Preparation of silicon-carbon composite materials

[0045] The carbon-coated composite intermediate obtained in step 3 is placed in a vacuum sintering furnace and the vacuum degree is maintained at less than 5*10 ~2 The temperature was raised to 1000°C at 1°C / min for vacuum sintering, and the temperature was kept constant for 4 hours. The block material was obtained, and the block material was crushed through a 500-mesh sieve to obtain a silicon-carbon composite material.

[0046] Example 2

[0047] The difference between Example 2 and Example 1 is that in step 1, zirconium beads are added to the silicon-ethanol dispersion and ground for 8 hours, and the other conditions remain the same as in Example 1.

[0048] Example 3

[0049] The difference between Example 3 and Example 1 is that in step 1, the silicon-ethanol dispersion is added with zirconium beads and ground for 12 hours, and the other conditions are consistent with those of Example 1.

[0050] Example 4

[0051] The difference between Example 4 and Example 1 is that in step 2, 3 g of graphene oxide is weighed and dispersed in deionized water, the mass ratio of graphene oxide to silicon nanosheets is 3:5, and the graphene oxide ball milling time is 6 hours. The other conditions are the same as those in Example 1.

[0052] Example 5

[0053] The difference between Example 5 and Example 1 is that in step 2, 7 g of graphene oxide is weighed and dispersed in deionized water, the mass ratio of graphene oxide to silicon nanosheets is 7:5, and the graphene oxide ball milling time is 9 hours. The other conditions are the same as those in Example 1.

[0054] Example 6

[0055] The difference between Example 6 and Example 1 is that in step 1, 0.5 kg of 0.2 mm zirconium beads are added, the mass ratio of zirconium beads to silicon powder is 5:1, and the other conditions are consistent with Example 1.

[0056] Example 7

[0057] The difference between Example 7 and Example 1 is that in step 1, 2 kg of 0.2 mm zirconium beads are added, the mass ratio of zirconium beads to silicon powder is 20:1, and the other conditions are consistent with Example 1.

[0058] Example 8

[0059] The difference between Example 8 and Example 1 is that the organic carbon source in step 3 is chitosan, and the other conditions are consistent with Example 1.

[0060] Example 9

[0061] The only difference between Example 9 and Example 1 is that the mixing ball milling time in step 2.b of Example 9 is 10 minutes, and the other conditions remain the same as in Example 1.

[0062] Example 10

[0063] The only difference between Example 10 and Example 1 is that the mixing ball milling time in step 2.b of Example 10 is 240 min, and the other conditions remain the same as in Example 1.

[0064] Embodiment 11

[0065] The only difference between Example 11 and Example 1 is that the thickness of the silicon nanosheet in step 2.b of Example 11 is 100 nm, and the other conditions remain the same as in Example 1.

[0066] Example 12

[0067] The only difference between Example 12 and Example 1 is that the thickness of the silicon nanosheet in step 2.b of Example 12 is 5 nm, and the other conditions remain the same as in Example 1.

[0068] Example 13

[0069] The only difference between Example 13 and Example 1 is that the carbonization temperature in step 3 of Example 13 is 250°C, and the other conditions remain the same as in Example 1.

[0070] Embodiment 14

[0071] The only difference between Example 14 and Example 1 is that the carbonization temperature in step 3 of Example 14 is 350°C, and the other conditions remain the same as in Example 1.

[0072] Embodiment 15

[0073] The only difference between Example 15 and Example 1 is that the vacuum sintering time in step 4 is 3 hours, and the other conditions remain the same as in Example 1.

[0074] Example 16

[0075] The only difference between Example 16 and Example 1 is that the vacuum degree in step 4 of Example 16 is 10*10 ~2 The other conditions are the same as those in Example 1.

[0076] Embodiment 17

[0077] The only difference between Example 17 and Example 1 is that the organic carbon source in step 3 of Example 17 is chitosan, and the other conditions remain the same as in Example 1.

[0078] Embodiment 18

[0079] The only difference between Example 18 and Example 1 is that in step 3 of Example 18, chitin and chitosan are used as carbon sources in a mass ratio of 1:1, and the other conditions remain the same as in Example 1.

[0080] Embodiment 19

[0081] The only difference between Example 19 and Example 1 is that the vacuum sintering temperature in step 4 of Example 19 is 600° C., and the other conditions remain the same as those of Example 1.

[0082] Embodiment 20

[0083] The only difference between Example 20 and Example 1 is that the vacuum pyrolysis temperature in step 4 of Example 20 is 1400°C, and the other conditions remain the same as those of Example 1.

[0084] Comparative Example 1

[0085] The only difference between Comparative Example 1 and Example 1 is that in step 4 of Comparative Example 1, the high-temperature furnace is heated to 1000° C. at a heating rate of 1° C. / min in an argon atmosphere and maintained at this temperature for 4 hours, and the other conditions remain consistent with Example 1.

[0086] Comparative Example 2

[0087] The only difference between Comparative Example 2 and Example 1 is that in step 4 of Comparative Example 2, the high-temperature furnace is heated to 1000°C at a heating rate of 5°C / min in an argon atmosphere and maintained at this temperature for 4 hours. The other conditions remain consistent with Example 1.

[0088] Comparative Example 3

[0089] The only difference between Comparative Example 3 and Example 1 is that in step 1 of Comparative Example 3, zirconium beads are added to the silicon-ethanol dispersion and ground for 24 hours, and the other conditions remain the same as those of Example 1.

[0090] Comparative Example 4

[0091] The only difference between Comparative Example 4 and Example 1 is that 2 g of graphene oxide is added in step 2a of Comparative Example 4, and the other conditions remain the same as those of Example 1.

[0092] Comparative Example 5

[0093] The only difference between Comparative Example 5 and Example 1 is that 8 g of graphene oxide is added in step 2a of Comparative Example 5, and the other conditions remain the same as those of Example 1.

[0094] Morphological characterization and performance testing

[0095] The morphology of the silicon-carbon composite materials prepared in Examples 1 to 3 was observed using a scanning electron microscope (SEM). Figure 2 , Figure 3 , Figure 4 The scanning electron microscope (SEM) images of the silicon-carbon composite materials prepared in Examples 1, 2 and 3 of the present invention are shown respectively. Figure 2 , Figure 3 , Figure 4 It is intuitively explained that the silicon-carbon composite material prepared by the preparation method of the present invention has a wrinkled-lamellar structure, which is an alternating composite structure formed by silicon nanosheets / wrinkled graphene. The wrinkled structure of graphene formed at different ball milling times in Examples 1 to 3, the longer the ball milling time, the more serious the wrinkle deformation. The silicon nanosheets are embedded or embedded in the wrinkled graphene during the grinding process, and the gap formed between the two alleviates the expansion effect of the silicon-based material. The carbon coating layer is wrapped around the surface of the alternating composite structure formed by silicon nanosheets / wrinkled graphene.

[0096] The first cycle charge and discharge performance of the silicon-based composite material prepared in Example 1 was tested (under 0.2C lithium removal / 0.2C lithium insertion conditions).

[0097] Figure 5 This is a charge and discharge curve diagram of the first cycle of the silicon-carbon composite material prepared in Example 1 of the present invention. Figure 5 This indicates that when the silicon-carbon composite material prepared in Example 1 is embedded with lithium, there is a weak peak at 1.2 V corresponding to the beginning of SEI formation. Figure 6 This is a cycle curve diagram of the first 150 cycles of the silicon-carbon composite material prepared in Example 1 of the present invention. Figure 6 It shows that the first-cycle charge and discharge capacities of the composite material are 1065.6 mAh / g and 843.7 mAh / g, respectively, corresponding to a first-cycle coulombic efficiency of 79.1%. After 150 cycles, the composite material still has a reversible capacity of 618.2 mAh / g and an irreversible capacity of 628.2 mAh / g.

[0098] The electrochemical properties of the silicon-carbon composite materials prepared in Examples 1-20 and Comparative Examples 1-5 were tested. All the prepared silicon-carbon composite materials were assembled into CR2025 type button half-cells.

[0099] The specific assembly process is as follows: lithium metal sheet is used as the counter electrode; 1M Li PF6 / EC∶DEC∶DMC (1∶1∶1) is used as the electrolyte; polypropylene microporous membrane is used as the separator; active material, CE~300j, sodium carboxymethyl cellulose (CMC), and styrene butadiene latex (SBR) are prepared into slurry according to the mass ratio of 8∶1∶0.5∶0.5, evenly coated on carbon-coated copper foil and placed in a vacuum drying oven at 80℃ for 4h to make electrode sheets. The battery is assembled in a glove box filled with Ar gas. The model of the battery test system is LANDCT3002A, and the voltage range is 0.001~2V.

[0100] The mass fraction of Si and the lithium storage performance of the silicon-carbon composite materials prepared in Examples 1 to 20 and Comparative Examples 1 to 5 are shown in Table 1:

[0101] Table 1: Comparison of Si mass fraction and lithium storage capacity in silicon-carbon composite materials

[0102]

[0103]

[0104] The test data of comparative examples 1 to 5 indicate that the sanding time of silicon nanosheets and the ball milling time of graphene have a significant effect on the comprehensive electrochemical performance of the final negative electrode material. Examples 1 to 3 are silicon-carbon composite materials prepared by sanding silicon nanosheets at different times. The longer the sanding time, the smaller and thinner the silicon nanosheets obtained, and the more uniform the size, which is conducive to the diffusion of lithium ions along the surface and edges of the silicon nanosheets. At the same time, the large specific surface area is conducive to the composite with graphene, making the silicon nanosheets embedded or embedded in the reduced graphene more conductive, reducing the electron / ion transmission resistance, and having outstanding comprehensive electrochemical performance. Prolonging the sanding time is conducive to obtaining silicon nanosheets with better performance, but the longer the sanding time is not necessarily better. In comparative example 3, the excessively long sanding time causes side reactions between the surface of the silicon nanosheets and the grinding medium, which ultimately causes the electrochemical performance of the silicon-carbon composite material to decline. See Figure 2 , Figure 3 , Figure 4 , are scanning electron microscope (SEM) images of the silicon-carbon composite materials prepared in Examples 1, 2 and 3 of the present invention, respectively. It can be seen intuitively from the figure that the degree of graphene wrinkling is positively correlated with the ball milling time. The wrinkled graphene is more likely to wrap the silicon nanosheets inside, forming irregular spaces to buffer the expansion effect of the silicon-based material during lithiation / delithiation. In addition, the high elasticity of the wrinkled graphene itself can maintain the stability of the internal conductive network during the repeated charge and discharge volume expansion of the silicon nanosheets to achieve high capacity and high stability of the negative electrode material.

[0105] Comparing Example 1 with Examples 4 to 5, when graphene oxide and silicon nanosheets are mixed and ground, increasing the proportion of graphene oxide can increase the mass fraction of Si in the silicon-carbon composite material, and its electrochemical performance will also be improved accordingly. Example 1 and Comparative Examples 4 and 5 show that the first efficiency and capacity retention rate of the silicon-carbon nanomaterial obtained when the mass ratio of graphene oxide to silicon nanosheets exceeds 3 to 7:5 are not good. Too little graphene oxide cannot provide an effective buffer expansion network, and too much graphene oxide itself forms a large number of irreversible lithium insertion sites, which reduces the first coulomb efficiency.

[0106] Examples 1, 9 and 10 illustrate that the amount of wrinkled graphene in the composite material obtained when the mixing and milling time is short is not enough to alleviate the expansion of silicon; if the mixing and milling time is too long, the wrinkle degree will increase and the silicon nanosheets will lose good contact. Therefore, the appropriate milling time is conducive to the preparation of silicon-carbon nanocomposites. The silicon nanosheets used in Examples 11 and 12 are 100nm and 5nm in size, respectively. The smaller the size, the more side reactions on its surface, the lower the first coulomb efficiency, but the capacity retention rate will increase slightly. Examples 13 and 14 show that the reduction temperature of wrinkled graphene affects the performance of silicon-carbon composite materials. The lower reaction temperature of 250°C results in less removal of functional groups such as hydroxyl groups in graphene, and the first coulomb efficiency of the obtained material is lower. On the contrary, the first efficiency and cycle retention rate are improved.

[0107] Table 1 also shows that the size of the sand-milling spheroidal mass ratio affects the quality of the synthesized silicon nanosheets. Examples 1, 6, and 7 synthesized three types of silicon nanosheets at different spheroidal mass ratios. Under the same sand-milling time, a spheroidal mass ratio that is too low will lead to insufficient sand-milling, and the obtained silicon material will be more irregular and thicker in layers, which is not conducive to the next step of compounding, and the expansion effect will be more obvious; the performance of the silicon-based material obtained with a spheroidal mass ratio that is too high has no significant improvement. Selecting a suitable spheroidal mass ratio is not only conducive to obtaining a silicon-carbon composite material with good comprehensive electrochemical properties, but also helps to reduce costs and energy losses.

[0108] Table 1 also shows that vacuum conditions and the selection of a suitable organic carbon source are necessary conditions for synthesizing silicon-carbon materials. Example 8 uses chitosan as an organic carbon source, and the first coulombic efficiency of the silicon-carbon material obtained is higher; Example 1 and Comparative Examples 1-2 explore the effect of setting the gas conditions during sintering on the electrochemical properties of silicon-carbon composite materials. The volatile components in the material components are quickly discharged in a vacuum, which makes the sintering of the material more compact to a certain extent, forming a more uniform structure and reducing the charge conduction resistance.

[0109] In summary, the present invention provides a silicon-carbon composite material with wrinkled graphene adapted to volume expansion, and the microscopic reversible large strain characteristics brought by the high elasticity of wrinkled graphene can make the conductive network adapt to the stress generated by the volume expansion of silicon nanosheets without the conductive contact points falling off, and the silicon nanosheet / wrinkled graphene alternating composite structure forms an irregular space to buffer the expansion effect of silicon nanosheets. Its simple composite structure can effectively stabilize the electron transmission from the internal conductive network of the electrode to the electrochemically active silicon nanosheets, ensuring that the negative electrode can store and output high capacity in a long-term and stable manner. The preparation method provided by the present invention is simple, the raw materials are easily available, and it can be promoted.

[0110] It should be understood that the above examples are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A silicon-carbon composite material with wrinkled graphene adapted to volume expansion, characterized in that: The silicon-carbon composite material comprises a carbon coating layer, a silicon nanosheet and wrinkled graphene; the wrinkled graphene and the silicon nanosheet form an alternating composite structure with wrinkles / sheet layers; The carbon coating layer is wrapped on the surface of the alternating composite structure; The alternating composite structure forms irregular spaces, which can buffer the expansion effect of the silicon nanosheets.

2. The wrinkled graphene-adapted silicon-carbon composite material according to claim 1, characterized in that: The alternating composite structure is formed by the silicon nanosheets being embedded or embedded in the wrinkled graphene oxide; The silicon nanosheet expands in volume during the charge and discharge process, and the wrinkled graphene produces elastic deformation to adapt to the volume expansion of the silicon nanosheet.

3. A method for preparing a silicon-carbon composite material with wrinkled graphene adapted to volume expansion as claimed in any one of claims 1 to 2, characterized in that: The wrinkled graphene oxide and silicon nanosheets are mixed and ball-milled to obtain an intermediate of wrinkled graphene oxide composite nano-silicon sheets, an organic carbon source is added for sintering, and then carbonized to obtain a silicon-carbon composite material having the silicon nanosheet / wrinkled graphene alternating composite structure and wrapped by a carbon coating layer.

4. The method for preparing a wrinkled graphene-adapted silicon-carbon composite material according to claim 3, characterized in that: The following steps are involved: S1. Grinding silicon powder to obtain silicon nanosheets; S2. ball-milling the graphene oxide to obtain wrinkled graphene oxide, mixing it with the silicon nanosheets in S1 and continuing to ball-mill, and spray-drying to obtain a silicon nanosheet composite wrinkled graphene oxide intermediate; S3. The intermediate is mixed with an organic carbon source and carbonized in an inert atmosphere to obtain a carbon-encapsulated intermediate: S4. Vacuum sintering the carbon-coated intermediate in S3 to obtain the silicon-carbon composite material with wrinkled graphene adapted to volume expansion.

5. A method for preparing a silicon-carbon composite material with wrinkled graphene adapted to volume expansion according to claim 4, characterized in that The mass ratio of the graphene oxide to the silicon nanosheets is 3 to 7:

5.

6. A method for preparing a wrinkled graphene-adapted silicon-carbon composite material according to claim 4, characterized in that: The silicon powder in S1 is sand-milled for 4 to 12 hours; and / or, the graphene oxide in S2 is ball-milled for 3 to 9 hours; And / or, the wrinkled graphene oxide and the silicon nanosheets in S2 are mixed and then ball-milled for 10 to 240 minutes.

7. A method for preparing a wrinkled graphene-adapted silicon-carbon composite material according to claim 4, characterized in that: The thickness of the silicon nanosheet in S1 is 5 to 200 nm; and / or, grinding with 0.2 mm zirconium beads in S1; And / or, the ball-to-mass ratio during grinding in S1 is 20 to 5:

1.

8. A method for preparing a wrinkled graphene-adapted silicon-carbon composite material according to claim 4, characterized in that: The carbonization temperature in S3 is 250°C to 350°C; And / or, the carbonization time is 60 to 120 minutes; And / or, the organic carbon source is one or a combination of two or more of glucose, urea, sucrose, maltose, polyvinyl alcohol, chitosan and chitin.

9. A method for preparing a wrinkled graphene-adapted silicon-carbon composite material according to claim 4, characterized in that: The vacuum sintering temperature in S4 is 600° C. to 1400° C.; And / or, the heating rate during vacuum sintering is 1-5°C / min; And / or, the vacuum sintering time is 3 to 4 hours; And / or, the vacuum degree of vacuum sintering is 10*10 -2 ~5*10 -2 Entrust.

10. Use of the wrinkled graphene-adapted silicon-carbon composite material for volume expansion as described in any one of claims 1 to 2 or the wrinkled graphene-adapted silicon-carbon composite material for volume expansion prepared by the preparation method of any one of claims 3 to 9 in the negative electrode of a lithium-ion battery.

Citation Information

Cited By

  • Carbon microsphere material, preparation method of carbon microsphere material, silicon-carbon composite material and application of silicon-carbon composite material