Preparation method of pre-sodium-modified sodium ferrous sulfate positive electrode plate and pre-sodium-modified sodium ion battery

By using organic sodium salt NaAc as pre-sodium additive in sodium ion batteries, a gas pore channel is formed, which solves the problem of low efficiency of sodium ferrous sulfate positive electrode material, and achieves efficient sodium ion transmission and battery performance improvement, which is suitable for large-scale Scale application.

CN118943368APending Publication Date: 2024-11-12KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410968860.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The Coulombic efficiency of sodium ferrous sulfate positive electrode material in existing sodium ion batteries is low, resulting in limited energy density, and the stability problems of existing pre-sodium additives, limiting their large-scale application.

Method used

Using organic sodium salt NaAc as pre-sodium additive, the cathode material is improved by adding NaAc in the slurry preparation stage and grinding it to form a gas pore channel, promoting sodium ion transport, and generating gas during the charging process to ensure circulation stability, thereby improving the positive electrode material. Coulomb efficiency and rate performance.

Benefits of technology

The Coulomb efficiency and rate performance of sodium ferrous sulfate cathode material is significantly improved, and the pre-sodiumization method is achieved that is simple to operate, low-cost and environmentally friendly, ensuring the cycling stability of the battery and the sodium ion transport efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943368A_ABST
    Figure CN118943368A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a pre-sodium-modified sodium ferrous sulfate positive electrode plate and a pre-sodium-modified sodium ion battery, and the preparation method comprises the following steps: step 1, weighing a certain amount of a pre-sodium-modified sodium ion battery positive electrode material, a conductive agent and a binder, uniformly grinding and mixing, adding a dispersing agent, and continuously grinding to obtain slurry; the pre-sodium-modified sodium ion battery positive electrode material comprises a positive electrode active material and a pre-sodium-modified additive, 2, uniformly coating a positive current collector with the slurry through a coating machine, wherein the positive current collector is an aluminum foil; and drying the aluminum foil carrying the slurry in a vacuum drying oven to obtain the pre-sodium-modified sodium ferrous sulfate positive electrode plate. According to the invention, the organic sodium salt is utilized to provide additional sodium, so that a sodium-rich or over-sodium-rich positive electrode is obtained, and consumed sodium ions are made up, so that the irreversible sodium loss of the positive electrode of the sodium ion battery is reduced, and the coulombic efficiency is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion batteries, and in particular relates to a method for preparing a pre-sodiumized sodium ferrous sulfate positive electrode sheet and a pre-sodiumized sodium ion battery. Background Art

[0002] Sodium-ion batteries are considered to be one of the important and potential large-scale energy storage systems due to their abundant resources, wide distribution, wide temperature range adaptability, good safety performance, and good power characteristics. The positive electrode material in sodium-ion batteries, as the source of active sodium ions in sodium-ion batteries, is crucial to the electrochemical performance of the battery. Among them, sodium ferrous sulfate positive electrode material has attracted widespread attention due to its advantages such as high operating voltage, low cost, and excellent thermal stability.

[0003] In sodium-ion batteries, Na from the positive electrode + During the migration process, an irreversible reaction occurs with the electrolyte, forming a (CEI) film on the positive electrode surface, which significantly reduces the available active sodium ions, resulting in a low coulombic efficiency, which in turn leads to a low coulombic efficiency in the first week of the full battery. According to relevant reports, some of the sodium ferrous sulfate positive electrode materials currently prepared by researchers have low coulombic efficiency, which greatly limits the energy density of sodium-ion batteries and is one of the important issues facing their commercialization process.

[0004] The pre-sodiumization additives reported so far are mainly divided into inorganic sodium salts and organic sodium salts. Inorganic sodium salts such as Na2NiO2 and NaCrO2 exhibit low sodium replenishment capacity, and they tend to stay on the positive electrode and form residues after decomposition, which has a great impact on the performance of the assembled full battery. NaN3, Na2O, Na3P and Na2S are unstable in air and require the preparation of electrodes in a glove box, which is a cumbersome process and limits their large-scale application. However, many of the organic sodium salts are electrochemically unstable under high voltage and can release sodium ions after irreversible decomposition. Organic sodium salts have the advantages of being easily available, cost-effective and environmentally friendly, and can be widely used as pre-sodiumization additives for the positive electrode of sodium-ion batteries.

[0005] Therefore, selecting suitable organic pre-sodiumization reagents is crucial to significantly improving the coulombic efficiency of positive electrode materials and the practical application of sodium-ion batteries. Summary of the invention

[0006] The purpose of the present invention is to provide an organic sodium salt NaAc additive which is simple to operate, green and economical and can effectively improve the coulombic efficiency of the sodium ferrous sulfate positive electrode, and a pre-sodiumization method and application thereof, in order to solve the problems of low coulombic efficiency and low rate performance caused by the loss of active sodium ions in the existing prepared sodium ferrous sulfate positive electrode materials. The NaAc electrode has a capacity of 326mAh g -1Theoretical capacity, another aspect worth noting is that NaAc will generate gas, when the gas is discharged from the electrode, a pore channel will be formed in the electrode, thereby promoting ion diffusion and transport, and minimizing concentration polarization. As a pre-sodium reagent, NaAc does not leave any residual mass on the electrode plate, and the elimination of its gas ensures that the cycle stability is not affected. The channel formed by gas generation effectively promotes the transmission of sodium ions, thereby significantly improving the rate performance of the electrode after pre-sodium.

[0007] The first aspect of the present invention provides a method for preparing a pre-sodiumized sodium ferrous sulfate positive electrode sheet, the steps of which are as follows:

[0008] Step 1: weigh a certain amount of pre-sodiumized sodium ion battery positive electrode material, place it in a mortar and grind and mix it, add a dispersant and continue grinding after mixing evenly to obtain a slurry; wherein the pre-sodiumized sodium ion battery positive electrode material comprises 60% to 90% of positive electrode active material, 5% to 20% of conductive agent and 5% to 20% of binder; wherein the positive electrode active material comprises a pre-sodiumized additive, and the pre-sodiumized additive accounts for 5% to 25% of the mass of the positive electrode active material.

[0009] Step 2: The slurry is evenly coated on the positive electrode current collector by a coating machine, wherein the positive electrode current collector is aluminum foil, and the coating thickness of the slurry is 50 to 200 μm; the aluminum foil carrying the slurry is placed in a vacuum drying oven and dried at 50 to 120° C. for 6 to 24 hours to obtain a pre-sodiumized sodium ferrous sulfate positive electrode sheet.

[0010] Among them, the pre-sodiumization additive has an operating potential lower than that of the full battery assembled by the sodium ion battery, and the redox reaction of the pre-sodiumization reagent is an irreversible process, thereby ensuring that the sodium ions can work normally between the positive and negative electrodes of the battery after being released, and will not be reduced to the positive electrode pre-sodiumization additive.

[0011] In one embodiment, the dispersant is one of N-methylpyrrolidone, N-dimethylamide, and dimethyl sulfoxide, and the ratio of the dispersant to the binder is about (18-22):1.

[0012] In one embodiment, the conductive agent is at least one of Ketjen black, acetylene black, and conductive carbon black.

[0013] In one embodiment, the binder is at least one of polyvinylidene fluoride, sodium carboxymethyl cellulose, and polyacrylic acid.

[0014] In a second aspect, the present invention further provides a pre-sodiumized sodium ferrous sulfate positive electrode sheet, which is prepared by the preparation method of the pre-sodiumized sodium ferrous sulfate positive electrode sheet as described above.

[0015] In a third aspect, the present invention also provides a pre-sodiumized sodium ion battery, comprising a positive electrode, a negative electrode, a diaphragm and an electrolyte, wherein the positive electrode and the negative electrode are located on both sides of the diaphragm, and the electrolyte is located between the positive electrode and the negative electrode. The positive electrode is a pre-sodiumized sodium ferrous sulfate positive electrode sheet prepared by the manufacturing method of the pre-sodiumized sodium ferrous sulfate positive electrode sheet described above, and the pre-sodiumized sodium ferrous sulfate positive electrode sheet is a round sheet with a diameter of 14 mm; the negative electrode is a sodium metal sheet, wherein the diameter of the sodium metal sheet is 16 mm and the thickness is 0.2 to 0.4 mm; the electrolyte is 0.1 mL of a sodium perchlorate / ethylene carbonate / propylene carbonate / fluoroethylene carbonate solution with a concentration of 1 mol / L; and the diaphragm is a glass fiber diaphragm with a diameter of 19 mm.

[0016] In a fourth aspect, the present invention proposes a method for improving the cycle stability of a sodium ion battery assembled with a pre-sodiumized sodium ferrous sulfate positive electrode sheet, setting the test charging voltage of the pre-sodiumized additive sodium acetate (NaAc) to 3.6-4.2V, disassembling the sodium ion battery after one cycle of charge and discharge for exhaust treatment, reassembling, and then continuing the performance test of the assembled sodium ion battery. Specifically, the sodium ion battery assembled with the pre-sodiumized sodium ferrous sulfate positive electrode sheet will produce gas during charging, and the test charging voltage set can be 3.6V, 3.7V, 3.8V, 3.9V, 4.0V, 4.1V, 4.2V.

[0017] Beneficial effects of the present invention:

[0018] (1) The present invention directly adds a pre-sodium additive during the slurry preparation stage and grinds it evenly manually. The mass of the pre-sodium additive NaAc is 5-25% of the mass of the sodium ferrous sulfate Na2Fe(SO4)2 positive electrode active material, providing a method that is simple to operate, low in cost and easy to scale up.

[0019] (2) When the gas generated by the decomposition of the NaAc pre-sodiumization additive used in the present invention is discharged from the electrode, a pore channel is formed in the electrode, thereby promoting the transmission of sodium ions. As a pre-sodiumization agent, NaAc does not leave any residual mass on the electrode plate, and the elimination of its gas ensures that the cycle stability is not affected, thereby significantly improving the rate performance of the electrode after pre-sodiumization.

[0020] (3) The present invention proposes to use organic salt NaAc as a pre-sodium additive, which is green, environmentally friendly and low-cost, and the preparation process is simple and the experimental conditions are mild.

[0021] (4) The sodium ion battery assembled with the pre-sodiumized sodium ferrous sulfate positive electrode sheet proposed in the present invention will produce gas when the charging voltage reaches 3.6 to 4.2 V during the test. The battery can be disassembled after one cycle to exhaust gas before continuing the subsequent test.

[0022] (5) The coulombic efficiency and rate performance of the sodium ion battery assembled with the pre-sodiumized sodium ferrous sulfate Na2Fe(SO4)2 positive electrode sheet provided by the technical solution of the present invention are significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 It is a schematic flow chart of a method for preparing a pre-sodiumized sodium ferrous sulfate positive electrode sheet provided in an embodiment of the present invention.

[0025] Figure 2 This is a charge and discharge curve of the sodium ion battery prepared in Example 1 without pre-sodiumization at a C / 5 rate.

[0026] Figure 3 This is a scanning electron microscope (SEM) image of the sodium ferrous sulfate-sodium ion battery material prepared in Comparative Example 1 without pre-sodiumization.

[0027] Figure 4 This is a cycle performance diagram of the pre-sodiumized sodium ion battery prepared in Example 1 at a C / 5 rate.

[0028] Figure 5 This is a scanning electron microscope (SEM) image of the electrode sheet prepared by the pre-sodiumized sodium ion battery prepared in Example 1 after one cycle at a C / 5 rate.

[0029] Figure 6 This is a cycling performance diagram of the pre-sodiumized sodium ion battery prepared in Example 2 at a C / 5 rate.

[0030] Figure 7 This is a scanning electron microscope (SEM) image of the electrode sheet prepared by the pre-sodiumized sodium ion battery prepared in Example 2 after one cycle at a C / 5 rate.

[0031] Figure 8 This is a cycle performance diagram of the pre-sodiumized sodium ion battery prepared in Example 3 at a 1C rate.

[0032] Fig. 9 This is a scanning electron microscope (SEM) image of the electrode sheet prepared by the pre-sodiumized sodium ion battery prepared in Example 3 after one cycle at a 1C rate.

[0033] Fig.10This is a cycle performance diagram of the pre-sodiumized sodium ion battery prepared in Example 4 at a C / 5 rate.

[0034] Fig.11 This is a scanning electron microscope (SEM) image of the electrode sheet prepared by the pre-sodiumized sodium ion battery prepared in Example 4 after one cycle at a C / 5 rate.

[0035] Fig.12 This is a cycling performance diagram of the pre-sodiumized sodium ion battery prepared in Example 5 at a C / 5 rate.

[0036] Fig.13 This is a scanning electron microscope (SEM) image of the electrode sheet prepared by the pre-sodiumized sodium ion battery prepared in Example 5 after one cycle at a C / 5 rate. DETAILED DESCRIPTION

[0037] Hereinafter, a method for preparing a pre-sodiumized sodium ferrous sulfate positive electrode sheet and a pre-sodiumized sodium ion battery of the present invention will be described in detail in combination with exemplary embodiments.

[0038] See also Figure 1 , Figure 1 The present invention provides a schematic flow chart of a method for preparing a pre-sodiumized sodium ferrous sulfate positive electrode sheet.

[0039] The pre-sodiumization method of the pre-sodiumized sodium ferrous sulfate positive electrode sheet comprises the following steps:

[0040] S1: In the slurry preparation stage, the pre-sodiumized sodium ion battery positive electrode is weighed according to the mass percentage, and after being weighed, it is placed in an agate mortar and ground and mixed for 10 to 60 minutes. After mixing evenly, a dispersant is added and the grinding is continued for 5 to 10 minutes to obtain a slurry; wherein, the pre-sodiumized sodium ion battery positive electrode comprises 60% to 90% of a positive electrode active material, 5% to 20% of a conductive agent and 5% to 20% of a binder, wherein the positive electrode active material comprises a pre-sodiumized additive, and the pre-sodiumized additive accounts for 5% to 25% of the mass of the positive electrode active material. Specifically, the proportion of the positive electrode active material can be 60%, 65%, 70%, 75%, 80%, 85%, 90%, the proportion of the conductive agent can be 5%, 10%, 15%, 20%, the proportion of the binder can be 5%, 10%, 15%, 20%, or other values ​​within the above range, as long as it is within the above range; the proportion of the pre-sodium additive can be 5%, 7.5%, 10%, 12.5%, 15%, 17.5%, 20%, 22.5%, 25%, or other values ​​within the above range, as long as it is within the above range.

[0041] S2: The slurry is uniformly coated on the positive electrode current collector by a coating machine, wherein the positive electrode current collector is an aluminum foil, and the coating thickness of the slurry is 50 to 200 μm; the aluminum foil carrying the slurry is placed in a vacuum oven and dried at 50 to 120° C. for 6 to 24 hours to obtain a pre-sodiumized sodium ferrous sulfate positive electrode sheet.

[0042] Specifically, in step S1, the mass of the pre-sodium additive is 5 to 25% of the mass of the positive electrode active material (Na2Fe(SO4)2), that is, it can be 5%, 7.5%, 10%, 12.5%, 15%, 17.5%, 20%, 22.5%, 25%, or other proportions within the above range.

[0043] Among them, the pre-sodiumization additive has an operating potential lower than that of the full battery assembled by the sodium ion battery, and the redox reaction of the pre-sodiumization reagent is an irreversible process, thereby ensuring that the sodium ions can work normally between the positive and negative electrodes of the battery after being released, and will not be reduced to the positive electrode pre-sodiumization additive.

[0044] In step S1, the pre-sodium additive and the positive electrode material are ground and mixed for 10 to 60 minutes. The grinding time can be 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, 60 minutes, or other time values ​​within the above range.

[0045] The binder in step S1 is one or more of polyvinylidene fluoride, sodium carboxymethyl cellulose, and polyacrylic acid.

[0046] The dispersant is one of N-methylpyrrolidone, N-dimethylamide, and dimethyl sulfoxide, and the ratio of the dispersant to the binder is (18-22): 1. Specifically, the ratio of the dispersant to the binder can be 18:1, 19:1, 20:1, 21:1, 22:1, or other ratios within the above range.

[0047] The conductive agent in step S1 is one or more of Ketjen black, acetylene black, and SuperP.

[0048] The weighing by mass percentage in step S1, including 60% to 90% positive electrode active material, 5% to 20% conductive agent and 5% to 20% binder, can be 60% positive electrode active material, 20% conductive agent and 20% binder, 70% positive electrode active material, 20% conductive agent and 10% binder, 80% positive electrode active material, 10% conductive agent and 10% binder, 90% positive electrode active material, 5% conductive agent and 5% binder.

[0049] The dispersant added in step S1 is then ground for 5 to 10 minutes, that is, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, or 10 minutes.

[0050] The aluminum foil carrying the slurry in step S2 is vacuum dried for 6-24 hours. It can be understood that the drying time can be 4 hours, 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours, 24 hours, or other time values ​​within the above range.

[0051] The coating thickness of the slurry in step S2 is 50-200 μm, that is, it can be 50 μm, 100 μm, 150 μm, 200 μm, or other values ​​within the above range.

[0052] The vacuum drying oven in step S2 is set to 50-120°C, that is, it can be 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, or other values ​​within the above range.

[0053] In this embodiment, the above-mentioned method for preparing a pre-sodiumized sodium ferrous sulfate positive electrode sheet is used. The pre-sodiumized additive is directly added in the slurry preparation stage and ground evenly, which has the advantages of simple operation, environmental protection, non-toxicity and easy large-scale production. The organic salt sodium acetate (NaAc) is used as the pre-sodiumized additive. NaAc has a capacity of 326 mAh g -1 The theoretical capacity of NaAc electrode is 99%, and the sodium utilization rate is irreversible, which means that NaAc provides almost all the sodium source during the charging process and there is no additional sodium ion storage during the discharge process. Another noteworthy aspect of NaAc is that NaAc will produce gas when charged to a certain voltage. When the gas is discharged from the electrode, pore channels will be formed in the electrode, thereby promoting ion diffusion and transport and minimizing concentration polarization. As a pre-sodiumization additive, NaAc does not leave any residual mass on the electrode plate, and the elimination of its gas ensures that the cycle stability is not affected. Therefore, the rate performance and coulombic efficiency of the prepared pre-sodiumized sodium ferrous sulfate positive electrode material are significantly improved.

[0054] On the basis of the foregoing, this embodiment also provides a pre-sodiumized sodium ion battery, comprising a positive electrode, a negative electrode, a diaphragm and an electrolyte, wherein the positive electrode and the negative electrode are located on both sides of the diaphragm, and the electrolyte is located between the positive electrode and the negative electrode. The positive electrode is a pre-sodiumized sodium ferrous sulfate positive electrode sheet prepared by the preparation method of the pre-sodiumized sodium ferrous sulfate positive electrode sheet described above, and the pre-sodiumized sodium ferrous sulfate positive electrode sheet is a round sheet with a diameter of 14 mm; the negative electrode is a sodium metal sheet, wherein the diameter of the sodium metal sheet is 16 mm and the thickness is 0.2 to 0.4 mm; the electrolyte is 0.1 mL of a sodium perchlorate / ethylene carbonate / propylene carbonate / fluoroethylene carbonate solution with a concentration of 1 mol / L; the diaphragm is a glass fiber diaphragm with a diameter of 19 mm.

[0055] The pre-sodiumized sodium ferrous sulfate positive electrode sheet prepared according to the preparation method of this embodiment is applied to a sodium ion battery, so that the pre-sodiumized sodium ion battery prepared by the above preparation method also has the advantages of the pre-sodiumized sodium ferrous sulfate positive electrode sheet.

[0056] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with specific examples, but the content of the present invention is not limited to the following examples.

[0057] Comparative Example 1

[0058] The method for preparing the non-pre-sodiumized sodium ferrous sulfate Na2Fe(SO4)2 positive electrode material used in the present invention comprises the following steps:

[0059] Step 1: weigh anhydrous Na2SO4 and anhydrous FeSO4 in a molar ratio of 1:1 and add them into a ball mill, use wet ball milling, use anhydrous ethanol as a grinding aid, and argon-filled ball mill for 4 hours at a speed of 350 rpm to obtain a highly uniformly dispersed slurry;

[0060] Step 2: Dry the slurry after ball milling in step 1 in a vacuum drying oven for 4 hours. After passing through a 200-mesh sieve, place the raw material in a tube furnace and first heat it to 250°C at a heating rate of 3°C / min, then heat it to 350°C at a heating rate of 2°C / min, calcine for 8 hours, and cool it to room temperature in the tube furnace. The obtained powder is the target product.

[0061] The positive electrode material prepared in this comparative example is sodium ferrous sulfate Na2Fe(SO4)2 which is not pre-sodiumized and is used to prepare the positive electrode sheet. The positive electrode sheet is made of slurry coated on aluminum foil and dried at 120°C in vacuum and then cut into pieces. The slurry is made by mixing the positive electrode material with conductive carbon black and polyvinylidene fluoride in a mass ratio of 7:2:1, and then adding N-methylpyrrolidone dispersant. 1M sodium perchlorate (NaClO4) dissolved in ethylene carbonate (EC) / propylene carbonate (PC) / fluoroethylene carbonate (FEC) is used as the electrolyte, the outer shell is made of stainless steel shell, the negative electrode is made of metal sodium sheet, and the positive electrode is separated from the negative electrode by a glass fiber diaphragm, and assembled into a traditional button battery. The material morphology test and electrochemical performance diagram are shown in the figure:

[0062] Figure 2 This is a charge and discharge curve of a sodium ion battery prepared with Na2Fe(SO4)2 as the positive electrode material without adding pre-sodium additives in the voltage range of 2.0-4.5V at a C / 5 rate. The first discharge capacity is about 57mAh / g, accounting for 62.6% of the theoretical capacity, and has an operating voltage of 3.6V. It can be clearly seen from the figure that the charging capacity is higher than the discharge capacity, and has a coulombic efficiency of about 90%.

[0063] Figure 3 This is a scanning electron microscope (SEM) image of Na2Fe(SO4)2 as a positive electrode material without the addition of pre-sodium additives. It can be seen that the particles of sodium ferrous sulfate are very small and easy to aggregate.

[0064] Example 1

[0065] The method for preparing the pre-sodiumized sodium ferrous sulfate positive electrode sheet provided in the embodiment of the present invention comprises the following steps:

[0066] Step 1:

[0067] In the slurry preparation stage, the pre-sodiumized sodium ion battery positive electrode is weighed by mass percentage, including 70% positive electrode active material Na2Fe(SO4)2, 20% conductive carbon black and 10% polyvinylidene fluoride, wherein the added pre-sodiumized additive NaAc accounts for 5% of the mass of the positive electrode active material. After weighing, it is placed in a mortar and ground and mixed for 15 minutes. After mixing evenly, N-methylpyrrolidone dispersant is added and ground for 5 minutes to obtain a slurry.

[0068] Step 2: The slurry is evenly coated on the positive electrode current collector by a coating machine, wherein the positive electrode current collector is aluminum foil, and the coating thickness of the slurry is 100 μm; the aluminum foil carrying the slurry is placed in a vacuum drying oven and dried at 120° C. for 12 hours to obtain a pre-sodiumized sodium ferrous sulfate positive electrode sheet.

[0069] The pre-sodiumized sodium ferrous sulfate positive electrode material prepared in this embodiment is used to prepare the positive electrode plate, and 1M sodium perchlorate (NaClO4) is dissolved in ethylene carbonate (EC) / propylene carbonate (PC) / fluoroethylene carbonate (FEC) as the electrolyte. The outer shell adopts a stainless steel shell, the negative electrode adopts a metal sodium sheet, and the positive electrode is separated from the negative electrode by a glass fiber separator to assemble into a button battery.

[0070] like Figure 4 and Figure 5 As shown, the button cell assembled with the positive electrode material added with 5% pre-sodium additive NaAc has a first discharge capacity of about 63.7mAh / g under C / 5 rate conditions in the voltage range of 2.0-4.5V. Compared with Comparative Example 1, the coulombic efficiency of the material reaches 94.2%, which is significantly increased by about 4%, and the first discharge capacity is increased by about 7mAh / g. The improvement of the coulombic efficiency and capacity of the material is due to the addition of the pre-sodium additive, which effectively replenishes the sodium ions consumed by the material during the charge and discharge process. And from the scanning electron microscope (SEM) image of the button cell assembled with the Na2Fe(SO4)2 electrode plate added with 5% NaAc after one cycle at C / 5 rate, it can be seen that due to the small amount of NaAc added, less gas is generated, and the pore channels formed when discharged from the electrode are uneven, which leads to the electrochemical performance of the sodium ion battery assembled by the material not being very obvious.

[0071] Example 2

[0072] The method for preparing the pre-sodiumized sodium ferrous sulfate positive electrode sheet provided in the embodiment of the present invention comprises the following steps:

[0073] Step 1:

[0074] In the slurry preparation stage, the pre-sodiumized sodium ion battery positive electrode is weighed by mass percentage, including 70% positive electrode active material Na2Fe(SO4)2, 20% conductive carbon black and 10% polyvinylidene fluoride, wherein the added pre-sodiumized additive NaAc accounts for 7.5% of the mass of the positive electrode active material. After weighing, it is placed in a mortar and ground and mixed for 15 minutes. After mixing evenly, N-methylpyrrolidone dispersant is added and ground for 5 minutes to obtain a slurry.

[0075] Step 2: The slurry is evenly coated on the positive electrode current collector by a coating machine, wherein the positive electrode current collector is aluminum foil, and the coating thickness of the slurry is 100 μm; the aluminum foil carrying the slurry is placed in a vacuum drying oven and dried at 120° C. for 12 hours to obtain a pre-sodiumized sodium ferrous sulfate positive electrode sheet.

[0076] The pre-sodiumized Na2Fe(SO4)2 sodium ion battery positive electrode material prepared in this embodiment is used to prepare a positive electrode sheet, using 1M sodium perchlorate (NaClO4) dissolved in ethylene carbonate (EC) / propylene carbonate (PC) / fluoroethylene carbonate (FEC) as an electrolyte, a stainless steel shell, a metallic sodium sheet for the negative electrode, and a glass fiber separator to separate the positive electrode from the negative electrode to assemble into a button battery.

[0077] like Figure 6 and Figure 7 As shown, the button cell assembled with the positive electrode material added with 7.5% pre-sodium additive has a cycle curve in the voltage range of 2.0 to 4.5V, and the first discharge capacity is about 66.5mAh / g under the C / 5 rate condition. Compared with Comparative Example 1, the coulombic efficiency of the material is significantly improved by about 5% compared with the non-pre-sodium, and the first discharge capacity is increased by about 9mAh / g. The improvement of the coulombic efficiency and capacity of the material is due to the addition of the pre-sodium additive, which effectively supplements the sodium ions consumed by the material during the charge and discharge process. The pore channels formed when the gas generated by NaAc is discharged from the electrode effectively promote the diffusion and transmission of sodium ions, so that the rate performance of the material is improved. It can be seen from the scanning electron microscope (SEM) image of the button cell assembled with the Na2Fe(SO4)2 electrode plate with 7.5% NaAc added after one cycle at C / 5 rate that the gas generated by 7.5% NaAc causes the number of holes generated in the plate to increase, and the number of holes increases compared with Example 1.

[0078] Example 3

[0079] The method for preparing the pre-sodiumized sodium ferrous sulfate positive electrode sheet provided in the embodiment of the present invention comprises the following steps:

[0080] Step 1: In the slurry preparation stage, the pre-sodiumized sodium ion battery positive electrode is weighed by mass percentage, including 70% positive electrode active material Na2Fe(SO4)2, 20% conductive carbon black and 10% polyvinylidene fluoride, wherein the added pre-sodiumized additive NaAc accounts for 10% of the mass of the positive electrode active material. After weighing, it is placed in a mortar and ground and mixed for 15 minutes. After mixing evenly, N-methylpyrrolidone dispersant is added and grinding is continued for 5 minutes to obtain a slurry.

[0081] Step 2: The slurry is evenly coated on the positive electrode current collector by a coating machine, wherein the positive electrode current collector is aluminum foil, and the coating thickness of the slurry is 100 μm; the aluminum foil carrying the slurry is placed in a vacuum drying oven and dried at 120° C. for 12 hours to obtain a pre-sodiumized sodium ferrous sulfate positive electrode sheet.

[0082] The pre-sodiumized Na2Fe(SO4)2 sodium ion battery positive electrode material prepared in this embodiment is used to prepare a positive electrode sheet, using 1M sodium perchlorate (NaClO4) dissolved in ethylene carbonate (EC) / propylene carbonate (PC) / fluoroethylene carbonate (FEC) as an electrolyte, a stainless steel shell, a metallic sodium sheet for the negative electrode, and a glass fiber separator to separate the positive electrode from the negative electrode to assemble into a button battery.

[0083] like Figure 8 and Fig. 9 As shown in the figure, the charge and discharge curve of the button cell assembled with the positive electrode material added with 10% pre-sodium additive in the voltage range of 2.0-4.5V, the first discharge capacity under the condition of 1C rate is about 65.3mAh / g, and the coulombic efficiency is increased to 99.1%. The improvement of the coulombic efficiency and capacity of the material is due to the addition of the pre-sodium additive, which effectively replenishes the sodium ions consumed by the material during the charge and discharge process. The pore channels formed when the gas generated by NaAc is discharged from the electrode effectively promote the diffusion and transmission of ions, so that the rate performance of the material is improved. In addition, from the scanning electron microscope (SEM) image of the button cell assembled with the Na2Fe(SO4)2 electrode plate added with 10% NaAc after cycling at 1C rate, it can be seen that the addition of 10% NaAc leads to the generation of a large number of holes, and the holes at 1C rate are larger than those at C / 5 rate.

[0084] Example 4

[0085] The method for preparing the pre-sodiumized sodium ferrous sulfate positive electrode sheet provided in the embodiment of the present invention comprises the following steps:

[0086] In the slurry preparation stage, the pre-sodiumized sodium ion battery positive electrode is weighed by mass percentage, including 70% positive electrode active material Na2Fe(SO4)2, 20% conductive carbon black and 10% polyvinylidene fluoride, wherein the added pre-sodiumized additive NaAc accounts for 12.5% ​​of the mass of the positive electrode active material. After weighing, it is placed in a mortar and ground and mixed for 15 minutes. After mixing evenly, N-methylpyrrolidone dispersant is added and ground for 5 minutes to obtain a slurry.

[0087] Step 2: The slurry is evenly coated on the positive electrode current collector by a coating machine, wherein the positive electrode current collector is aluminum foil, and the coating thickness of the slurry is 100 μm; the aluminum foil carrying the slurry is placed in a vacuum drying oven and dried at 120° C. for 12 hours to obtain a pre-sodiumized sodium ferrous sulfate positive electrode sheet.

[0088] The pre-sodiumized Na2Fe(SO4)2 sodium ion battery positive electrode material prepared in this embodiment is used to prepare a positive electrode sheet, using 1M sodium perchlorate (NaClO4) dissolved in ethylene carbonate (EC) / propylene carbonate (PC) / fluoroethylene carbonate (FEC) as an electrolyte, a stainless steel shell, a metallic sodium sheet for the negative electrode, and a glass fiber separator to separate the positive electrode from the negative electrode to assemble into a button battery.

[0089] like Fig.10 and Fig.11 As shown, the charge and discharge curve of the button cell assembled by adding 12.5% ​​pre-sodium additive in the voltage range of 2.0-4.5V, the first discharge capacity under C / 5 rate condition is about 71.8mAh / g, compared with comparative example 1, the coulombic efficiency of the material is significantly improved by 8.6% compared with the non-pre-sodium, and the first discharge capacity is increased by about 14mAh / g. The improvement of the coulombic efficiency and capacity of the material is due to the addition of the pre-sodium additive, which effectively supplements the sodium ions consumed by the material during the charge and discharge process. The pore channels formed when the gas generated by NaAc is discharged from the electrode effectively promote ion diffusion and transmission, so that the rate performance of the material is improved. It can be seen from the scanning electron microscope (SEM) image of the button cell assembled by the Na2Fe(SO4)2 electrode plate with 12.5% ​​NaAc after cycling at C / 5 rate that the addition of 12.5% ​​NaAc leads to the generation of a large number of holes.

[0090] Example 5

[0091] The method for preparing the pre-sodiumized sodium ferrous sulfate positive electrode sheet and the steps for assembling button batteries provided in the embodiment of the present invention include the following steps as in embodiment 4:

[0092] like Fig.12 and Fig.13 As shown, the charge and discharge curve of the button cell assembled with the positive electrode material added with 15% pre-sodium additive in the voltage range of 2.0 to 4.5V, the first discharge capacity under the C / 5 rate condition is about 68.3mAh / g, compared with comparative example 1, the coulomb efficiency of the material is significantly improved by about 8% compared with the non-pre-sodium, and the first discharge capacity is increased by about 11mAh / g. The addition of 15% NaAc leads to excessive gas generation, and the generation of excessive gas may play a role in the decomposition process of dissipating NaAc, thereby leading to poor cycle stability performance. And from the scanning electron microscope (SEM) image of the button cell assembled with the Na2Fe(SO4)2 electrode material added with 15% NaAc after one cycle of charge and discharge at C / 5 rate, it can be seen that the surface of the electrode sheet is rough and a large number of large holes are generated.

[0093] Although the present invention has been described above in conjunction with the exemplary embodiments and the accompanying drawings, it should be apparent to those skilled in the art that various modifications may be made to the above-described embodiments without departing from the spirit and scope of the claims.

Claims

1. A method for preparing a pre-sodiumized sodium ferrous sulfate positive electrode sheet, characterized in that: include Step 1, weighing a certain amount of pre-sodiumized sodium ion battery positive electrode material, conductive agent, and binder, placing them in a mortar and grinding and mixing them, adding a dispersant and continuing to grind for 5 to 10 minutes after mixing evenly, to obtain a slurry; wherein the pre-sodiumized sodium ion battery positive electrode material includes a positive electrode active material and a pre-sodiumized additive; Step 2: Evenly coat the slurry on the positive electrode current collector through a coating machine, wherein the positive electrode current collector is aluminum foil; place the aluminum foil carrying the slurry in a vacuum drying oven and dry it at 50 to 120° C. for 6 to 24 hours to obtain a pre-sodiumized sodium ferrous sulfate positive electrode sheet.

2. The preparation method according to claim 1, characterized in that: In step one, the pre-sodiumized sodium ion battery positive electrode material includes 60% to 90% of a positive electrode active material, 5% to 20% of a conductive agent and 5% to 20% of a binder, wherein the positive electrode active material includes a pre-sodiumized additive.

3. The preparation method according to claim 2, characterized in that: In step 1, the pre-sodium additive accounts for 5% to 25% of the mass of the positive electrode active material.

4. The preparation method according to claim 1, characterized in that: The dispersant is one of N-methylpyrrolidone, N-dimethylamide and dimethyl sulfoxide, and the dosage ratio of the dispersant to the binder is (18-22):

1.

5. The preparation method according to claim 1, characterized in that: The conductive agent is at least one of Ketjen black, acetylene black and conductive carbon black.

6. The preparation method according to claim 1, characterized in that: The binder is at least one of polyvinylidene fluoride, sodium carboxymethyl cellulose and polyacrylic acid.

7. The preparation method according to claim 1, characterized in that: In step 2, the coating thickness of the slurry is 50 to 200 μm.

8. A pre-sodiumized sodium ferrous sulfate positive electrode sheet, characterized in that: The pre-sodiumized sodium ferrous sulfate positive electrode sheet is prepared by the preparation method of the pre-sodiumized sodium ferrous sulfate positive electrode sheet according to any one of claims 1 to 6.

9. A pre-sodiumized sodium ion battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode and the negative electrode are located on both sides of the separator, and the electrolyte is located between the positive electrode and the negative electrode, characterized in that: The positive electrode is a pre-sodiumized sodium ferrous sulfate positive electrode sheet, which is prepared by the preparation method of the pre-sodiumized sodium ferrous sulfate positive electrode sheet according to any one of claims 1 to 7, and is a round sheet with a diameter of 14 mm; the negative electrode is a sodium metal sheet, wherein the diameter of the sodium metal sheet is 16 mm and the thickness is 0.2 to 0.4 mm; the electrolyte is 0.1 mL of a sodium perchlorate / ethylene carbonate / propylene carbonate / fluoroethylene carbonate solution with a concentration of 1 mol / L; and the diaphragm is a glass fiber diaphragm with a diameter of 19 mm.

10. A method for improving the cycle stability of a pre-sodiumized sodium ion battery, characterized in that: include: The test charging voltage of the pre-sodium additive (NaAc) was set to 3.6-4.2V, and the sodium-ion battery after one charge and discharge cycle was disassembled for exhaust treatment and then reassembled.