Lithium ion battery positive electrode slurry and preparation method thereof
By using additives such as polyimide PI gel and oxylic acid in the positive electrode materials of lithium-ion batteries, the problem of gelation phenomenon of lithium-ion batteries at high pH is solved, and the fluidity and stability of the slurry are achieved Improved performance, improving the cycle life and production efficiency of the battery.
Patent Information
- Application Number
- CN202411155023.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
AI Technical Summary
During the synthesis of the positive electrode material of lithium-ion batteries, the pH value of the material is too high due to excessive lithium ions, which is prone to gel phenomenon, which affects the fluidity and processability of the slurry and reduces the cycle life of the battery.
Polyimide PI glue solution is used as the binder, and weak polar acid oxylic acid and dispersible PVP are added to adjust the viscosity through stirring, avoid dehydrogenation reaction and gel phenomenon, and improve the fluidity and stability of the slurry. sex.
It effectively avoids gel phenomenon, improves the fluidity and stability of the slurry, reduces the positive electrode impedance, and improves the cycle life and production efficiency of the battery.
Smart Images

Figure CN118943371A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to a lithium ion battery positive electrode slurry and a preparation method thereof. Background Art
[0002] Lithium iron phosphate (LiFePO4) is the most widely used positive electrode material in lithium-ion power and energy storage batteries. In order to meet the market demand for higher energy density of lithium-ion batteries, many material manufacturers are developing LiFePO4 materials with higher energy density.
[0003] The energy storage market is now pursuing large-capacity, high-energy-density batteries. Lithium iron phosphate materials are developing in the direction of high compaction, high gram capacity, and long cycle. With the increase in compaction density, especially the newly developed fourth-generation compaction density positive electrode materials by some material manufacturers, the particle size is small and the specific surface area is large. When synthesizing materials, in order to pursue the high gram capacity of the materials, there are more lithium ions in excess. As a result, the pH value of the material itself is too high and the alkalinity is high due to excessive residual lithium ions. Gel phenomenon is prone to occur during the stirring process of lithium-ion battery slurry, and the slurry loses fluidity, affecting the subsequent coating process, seriously reducing the processability and production efficiency, and causing troubles for the subsequent battery process. Summary of the invention
[0004] The purpose of the present invention is to provide a positive electrode slurry for lithium-ion batteries, which can effectively improve the gelation phenomenon of positive electrode materials, improve the fluidity and stability of the slurry, and further increase the cycle life.
[0005] The technical solution adopted by the present invention to solve the above problem is: a method for preparing positive electrode slurry of a lithium ion battery, comprising the following steps: (1) Stir the polyimide PI glue solution evenly; (2) Add the positive electrode active material, conductive agent, first additive, second additive, and solvent in sequence, knead them, and then open the stirring pot to scrape the materials; (3) After scraping, stir at high speed to adjust the viscosity to 6000-12000 mPa•s; The polyimide PI glue solution is a stirred solution of polyimide PI and solvent N-methylpyrrolidone, the first additive is oxalic acid solid; and the second additive is polyvinylpyrrolidone solid.
[0006] Preferably, the water content of the polyimide PI glue, the positive electrode active material, the conductive agent, the dispersant, the first additive, the second additive, and the solvent is less than 500 ppm.
[0007] Preferably, the positive electrode active material is one of lithium iron phosphate, lithium manganese oxide, and nickel-cobalt-manganese ternary materials.
[0008] More preferably, the positive electrode active material is lithium iron phosphate, the specific surface area of the lithium iron phosphate is less than 12.5 m2 / g, and the particle size is controlled within the range of D10>0.5 um, D50>1.3 um, and D90>4.2 um.
[0009] Preferably, the conductive agent is conductive carbon black.
[0010] Preferably, the solid content of the polyimide PI glue is 13-17%.
[0011] Preferably, the first additive is added in an amount of 0.1-0.3% by weight of the total solids, and the second additive is added in an amount of 0.1-0.3% by weight of the total solids.
[0012] Preferably, the specific parameters of stirring in step (1) are: revolution 20-25 r / min, rotation 800-1200 r / min, and stirring time 20-30 min.
[0013] Preferably, step (1) is performed under vacuum conditions.
[0014] Preferably, the specific parameters of stirring in step (2) are: revolution 25-30 r / min, rotation 1500-2500 r / min, and stirring time 90-120 min.
[0015] Preferably, the specific parameters of stirring in step (3) are: revolution 25-30 r / min, rotation 2500-3000 r / min, and stirring time 180-200 min.
[0016] Preferably, step (3) is performed under vacuum conditions.
[0017] Another object of the present invention is to provide a positive electrode slurry for a lithium ion battery, which is prepared by the above-mentioned positive electrode slurry preparation method for a lithium ion battery.
[0018] Compared with the prior art, the advantages of the present invention are: (1) In the present invention, polyimide PI glue is added to the positive electrode slurry as a binder. Under high alkalinity conditions, the binder inside the slurry is not easy to undergo dehydrogenation reaction with hydroxide, thereby avoiding gelation.
[0019] (2) The first additive and the second additive are added to the positive electrode slurry of the present invention, wherein the first additive is a weak polar acid, which can neutralize the residual alkali in the slurry and leave no residue after baking; the second additive is PVP which can be used as a dispersant. The PVP molecular structure contains a strong polar lactam hydrophilic group and a CC long-chain lipophilic group, which is well compatible with a variety of solvents and can be coated on the surface of the particles to form a good dispersion effect through steric hindrance, so that the slurry is transformed from a Newtonian fluid to a non-Newtonian fluid. The slurry viscosity is stabilized at a relatively low level, which is beneficial to reducing the positive electrode impedance and improving the battery performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Graph showing the viscosity change of the positive electrode slurry at different standing times in Example 1 and Comparative Example 1.
[0021] Figure 2 This is a graph showing the viscosity change of the positive electrode slurry at different standing times in Example 2 and Comparative Example 2. DETAILED DESCRIPTION
[0022] The present invention is further described in detail below with reference to the embodiments. Example 1
[0023] Take the 48173170-120Ah shell size as an example The raw materials of the positive electrode slurry are as follows: Anda B9 lithium iron phosphate, binder PI (model LAR235R05), conductive carbon black SP, solvent N-methylpyrrolidone, carbon nanotubes CNT, PVP K30, and oxalic acid.
[0024] Among them, lithium iron phosphate (B9): PI: SP: CNT = 95.5%: 2.5%: 1%: 1% (weight percentage), the added amount of PVPK30 is 0.2% of the total solid weight, and the added amount of oxalic acid is 0.2% of the total solid weight.
[0025] A method for preparing a positive electrode slurry for a lithium ion battery comprises the following steps: (1) First, add PI glue (15% solid content) into a 30L stirring pot, rotate at 20 r / min, 800 r / min, vacuum at -90 KPa, and stir for 20 min.
[0026] (2) First add 20 kg of lithium iron phosphate, and then add SP powder material, PVPK30, oxalic acid, and solvent N-methylpyrrolidone in sequence according to the formula system. Knead for 10 minutes and adjust the solid content to 67.5%. The specific parameters during this period are: revolution 30 r / min, rotation 2500 r / min, no vacuum, and stirring time 120 minutes.
[0027] (3) After opening the stirring pot and scraping the material, stir at high speed, with revolution speed of 30 r / min, rotation speed of 3000 r / min, vacuum of -90 KPa, and stirring time of 200 min.
[0028] (4) The viscosity of the positive electrode slurry was measured and adjusted to 8562 mPa•s by adding solvent N-methylpyrrolidone.
[0029] Comparative Example 1 The only difference from Example 1 is that the additive oxalic acid is not added, and all additives are replaced by polyvinyl pyrrolidone.
[0030] The viscosity of the positive electrode slurry in Example 1 and Comparative Example 1 was tested with the standing time, and the specific results are shown in Table 1: Table 1
[0031] The positive electrode slurries in Example 1 and Comparative Example 1 were coated on 14 μm thick aluminum foil, dried, rolled and cut to obtain positive electrode sheets with a surface density of 450 g / m 2 , electrode compaction 3.4g / cm 3 , test the adhesion and impedance of the positive electrode, the results are shown in Table 2: Table 2
[0032] Example 2
[0033] Take the 2614897-50Ah shell size as an example The raw materials of the positive electrode slurry are as follows: ternary material H3, binder PI (model LAR235R05), conductive carbon black SP, N-methylpyrrolidone, carbon nanotubes CNT, PVPK30, and oxalic acid.
[0034] Among them, lithium iron phosphate (H3): PI: SP: CNT = 96%: 2%: 1%: 1% (weight percentage), the added amount of PVPK30 is 0.2% of the total solid weight, and the added amount of acetic acid is 0.2% of the total solid weight.
[0035] A method for preparing a positive electrode slurry for a lithium ion battery comprises the following steps: (1) First, add PI glue (15% solid content) into a 30L stirring pot, rotate at 20 r / min, 800 r / min, vacuum at -90 KPa, and stir for 20 min.
[0036] (2) Add 18 kg of lithium iron phosphate, add SP powder material, PVPK30, oxalic acid, and solvent N-methylpyrrolidone according to the formula system, knead for 15 minutes, and adjust the solid content to 69%. The specific parameters during this period are: revolution at 30 r / min, rotation at 2500 r / min, no vacuum, and stirring time of 150 minutes.
[0037] (3) After opening the pot and scraping the material, stir at high speed, revolution 30r / min, rotation 3000r / min, vacuum -90KPa, stirring time 200min.
[0038] (4) The viscosity of the positive electrode slurry was measured and adjusted to 7865 mPa•s by adding solvent N-methylpyrrolidone.
[0039] Comparative Example 2 The only difference from Example 2 is that the additive oxalic acid is not added, and all additives are replaced by polyvinyl pyrrolidone.
[0040] Comparative Example 3 The only difference from Example 2 is that the additive polyvinyl pyrrolidone is not added, and all additives are replaced by oxalic acid.
[0041] The viscosity of the positive electrode slurry in Example 2 and Comparative Examples 2-3 was tested with the standing time. The specific results are shown in Table 3: Table 3
[0042] The positive electrode slurries in Example 2 and Comparative Examples 2-3 were coated on 14 μm thick aluminum foil, dried, rolled, and cut to obtain positive electrode sheets with a surface density of 450 g / m 2 , electrode compaction 3.4g / cm 3 , test the adhesion and impedance of the positive electrode, the results are shown in Table 4: Table 4
[0043] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing positive electrode slurry for lithium ion batteries, characterized in that: The following steps are involved: (1) Stir the polyimide PI glue solution evenly; (2) Add the positive electrode active material, conductive agent, first additive, second additive, and solvent in sequence, knead them, and then open the stirring pot to scrape the materials; (3) After scraping, stir at high speed to adjust the viscosity to 6000-12000 mPa•s; The polyimide PI glue solution is a stirred solution of polyimide PI and solvent N-methylpyrrolidone, the first additive is oxalic acid solid; and the second additive is polyvinylpyrrolidone solid.
2. The method for preparing positive electrode slurry for lithium ion batteries according to claim 1, characterized in that: The positive electrode active material is one of lithium iron phosphate, lithium manganese oxide, and nickel-cobalt-manganese ternary materials, and the conductive agent is conductive carbon black.
3. The method for preparing positive electrode slurry for lithium ion batteries according to claim 1, characterized in that: The first additive is added in an amount of 0.1-0.3% of the total solid weight, and the second additive is added in an amount of 0.1-0.3% of the total solid weight.
4. The method for preparing positive electrode slurry for lithium ion batteries according to claim 1, characterized in that: The solid content of the polyimide PI glue solution is 13-17%.
5. The method for preparing positive electrode slurry for lithium ion batteries according to claim 1, characterized in that: The specific parameters of stirring in step (1) are: revolution 20-25 r / min, rotation 800-1200 r / min, and stirring time 20-30 min.
6. The method for preparing a positive electrode slurry for a lithium ion battery according to claim 1, characterized in that: Step (1) is carried out under vacuum conditions.
7. The method for preparing positive electrode slurry for lithium-ion batteries according to claim 1, characterized in that: The specific parameters of stirring in step (2) are: revolution 25-30 r / min, rotation 1500-2500 r / min, and stirring time 90-120 min.
8. The method for preparing a positive electrode slurry for a lithium-ion battery according to claim 1, characterized in that: The specific parameters of stirring in step (3) are: revolution 25-30 r / min, rotation 2500-3000 r / min, and stirring time 180-200 min.
9. The method for preparing positive electrode slurry for lithium-ion batteries according to claim 1, characterized in that: Step (3) is carried out under vacuum conditions.
10. A positive electrode slurry for a lithium ion battery, characterized in that: The positive electrode slurry for a lithium-ion battery is prepared by the method for preparing the positive electrode slurry for a lithium-ion battery according to any one of claims 1 to 9.