Method for improving oxygen reduction activity of catalyst in catalytic layer of fuel cell

Through the interaction of protonation of nitrogen-rich materials and PFSA ionomers, the -SO3-groups are blocked and the oxygen permeability is improved, and the problem of reduced oxygen reduction activity of the catalyst is solved, achieving efficient fuel cell performance output and stability. for the application of low-precious metal catalysts.

CN118943386APending Publication Date: 2024-11-12INST OF ENERGY HEFEI COMPREHENSIVE NAT SCI CENT (ANHUI ENERGY LAB)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411049062.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-12

Smart Images

  • Figure CN118943386A_ABST
    Figure CN118943386A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving oxygen reduction activity of a catalyst in a catalytic layer of a fuel cell, and belongs to the technical field of fuel cells. The preparation method comprises the following steps: in the preparation process of catalyst slurry, firstly adding a protonated nitrogen-rich material to interact with a PFSA ionomer, then adding a catalyst, fully homogenizing and dispersing, coating a proton exchange membrane with the catalyst slurry, and drying to prepare a catalyst layer with high oxygen reduction activity. The catalyst layer modified by the protonated nitrogen-rich material prepared by the preparation method can effectively reduce poisoning of sulfonic acid groups to a catalyst, increase the proportion of an ionomer amorphous region beneficial to local oxygen transmission, improve the proton conductivity of the catalyst layer, and is particularly suitable for performance improvement of a low-noble-metal-loading membrane electrode under high current density; the method has the advantages of simple and effective preparation process, low cost and the like. In addition, the protonated nitrogen-rich material stably exists in the catalyst layer, so that the durability of the membrane electrode is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of proton exchange membrane fuel cells, and in particular relates to a method for improving the oxygen reduction activity of a catalyst in a catalytic layer of a fuel cell. Background Art

[0002] Proton exchange membrane fuel cells (PEMFCs) can directly convert the chemical energy of hydrogen into electrical energy. They have the advantages of cleanliness, high efficiency, and rapid start-up. They are an electrochemical energy conversion device with great application potential. At present, the key challenge restricting their large-scale commercial application is how to achieve good performance output and stability with low usage of precious metals (Pt, Pb). In the traditional catalyst slurry preparation process, the perfluorosulfonic acid (PFSA) ionomer that plays a proton transfer role is fully stretched after homogenization and dispersion, and directly contacts the catalyst surface. In the catalytic layer formed after drying, the PFSA ionomer will be deposited on the catalyst surface to form a nano-thick film layer, which hinders the local transmission of oxygen to the catalyst surface; in addition, the sulfonic acid group (-SO3-) on its side chain will specifically adsorb on the surface of the catalyst active site, poisoning the catalyst and causing a significant decrease in the catalyst mass activity. Therefore, blocking the -SO3- group and improving the oxygen permeability of the PFSA ionomer is of great significance to improve the expression of the oxygen reduction activity of the catalyst in the catalytic layer, thereby reducing the usage of precious metal catalysts and improving the performance of PEMFC.

[0003] Rolfi et al. increased the oxygen permeability of the ionomer by 20% by introducing 2,2,4-trifluoro-5-trifluoromethoxy-1,3-dioxolane (MDO) structure into the PFSA matrix, significantly improving the peak power density of the membrane electrode (AndreaRolfi, et al, J. Power Sources, 2018, 396, 95.). Katzenberg et al. conducted liquid phase free radical polymerization of perfluoro[2-methylene-4-methyl-1,3-dioxolane] monomer (PFMMD) and perfluoro[4-methyl-3,6-dioxy-octane-7-ene]sulfonyl fluoride (PFSVE), followed by hydrolysis reaction, directly removing tetrafluoroethylene (TFE) monomer from the matrix structure (Adlai Katzenberg et al, J. Am. Chem. Soc., 2020, 142, 3742.). This new PFMMD skeleton destroys the crystallinity of the matrix and increases the free volume fraction of the ionomer. Compared with commercial PFSA ionomers, the oxygen permeability of this ionomer has increased by about 140%. However, the introduction of a rigid molecular structure into the PFSA ionomer matrix will lead to a decrease in its proton conductivity. Li et al. treated the catalyst carbon support with amination to make it positively charged, so that the PFSA ionomer can be evenly distributed on the catalyst surface and form a thinner nanofilm layer, reducing the local oxygen transport resistance by 11.5% (Chenzhao Li et al, Energy Environ. Sci., 2023, 16, 2977). However, this method still cannot avoid the problem of specific adsorption of -SO3- groups on the catalyst surface and poisoning the catalyst. Professor Wang Bo's team at Beijing Institute of Technology first proposed and constructed a porous covalent organic framework (COF) ionomer suitable for the catalyst layer of fuel cells, which significantly improved the mass transfer efficiency of the catalyst layer, and increased the mass activity of the platinum carbon (Pt / C) catalyst and the peak power density of the fuel cell by 1.6 times (Qingnuan Zhang et al, Science, 2022, 378, 181). However, how to reduce the size of these materials from micrometer to nanometer to make them more suitable for ultra-thin structures with low platinum catalyst layers remains an important challenge. Summary of the invention

[0004] The purpose of the present invention is to provide a simple and feasible method for blocking -SO3- groups and improving the oxygen permeability of PFSA ionomers, aiming at the problem of high local oxygen transmission resistance and -SO3- group poisoning at the PFSA ionomer-catalyst interface in the catalytic layer, which causes the catalyst oxygen reduction activity to decrease. The present invention uses the rich amino sites of the protonated nitrogen-rich material to interact with the -SO3- groups, induces the microstructure change of the PFSA ionomer, reduces its crystallinity, and improves the oxygen permeability of the ionomer; this strong interaction blocks the PFSA ionomer -SO3- groups, which is equivalent to building a "barrier layer" at the PFSA ionomer-SO3-group-catalyst interface, preventing the -SO3- groups from being specifically adsorbed on the surface of the catalyst active site; in addition, the protonation of the nitrogen-rich material can provide an additional proton source at the PFSA ionomer-catalyst interface, accelerate proton transfer, and then break the balance between the interface reaction and the material transfer at the interface, and improve the oxygen reduction performance of the catalyst in the catalytic layer.

[0005] The objective of the present invention is achieved through the following technical solutions: A method for improving the oxygen reduction activity of a catalyst in a fuel cell catalyst layer comprises the following steps: Step 1: Preparation of protonated nitrogen-rich material The nitrogen-rich material and concentrated acid are weighed according to a mass ratio of the nitrogen-rich material to the concentrated acid of 1:20-150, and then the two are mixed and ultrasonic etching is continued for 1-20 hours; deionized water is weighed according to a volume ratio of the concentrated acid to deionized water of 1:0.5-3, and the deionized water is added to the mixed solution of the nitrogen-rich material and the concentrated acid, and the mixture is allowed to stand for 0.1-20 hours to obtain a powder suspension; the powder is extracted by suction filtration, and repeatedly washed with deionized water for 1-5 times, and the protonated nitrogen-rich material powder is obtained after vacuum drying at 60°C for 1-20 hours.

[0006] Step 2: Preparation of protonated nitrogen-rich material modified catalyst slurry According to the mass ratio of PFSA ionomer to the protonated nitrogen-rich material prepared in step 1 of 1:0.01~0.1, the PFSA ionomer solution and the protonated nitrogen-rich material are weighed, and then the two are mixed and added to the high volatility solution, the mass concentration of the PFSA ionomer is controlled to be 0.1~10 wt%, and ultrasonic dispersion is performed for 10~40 mins at room temperature to obtain a PFSA ionomer mixed solution that interacts with the protonated nitrogen-rich material; then the catalyst is weighed according to the mass ratio of the catalyst to the PFSA ionomer of 1:0.1~1.2, and after wetting with a small amount of ultrapure water, it is added to the PFSA ionomer mixed solution that interacts with the protonated nitrogen-rich material, homogenized for 10~30 mins, dispersed for 5~40 mins, and degassed for 1~20 mins to obtain a protonated nitrogen-rich material modified catalyst slurry.

[0007] Step 3: Preparation of Catalytic Layer Coated Proton Exchange Membrane The proton exchange membrane is laid flat on a heating table at a temperature of 40-90°C, and then the protonated nitrogen-rich material modified catalyst slurry prepared in step 2 is coated on both sides of the proton exchange membrane. After drying, a catalyst layer coated proton exchange membrane assembly can be obtained.

[0008] In the above technical solution, the concentrated acid in step 1 is one of concentrated nitric acid, concentrated sulfuric acid, trifluoroacetic acid, trifluoroformic acid or a mixture of concentrated nitric acid and concentrated sulfuric acid.

[0009] In the above technical solution, the nitrogen-rich material in step 1 is one of a nitrogen-containing carbon material, a nitrogen-containing covalent organic framework material or a nitrogen-containing silica material.

[0010] In the above technical solution, the high volatility solution described in step 2 is one of water, isopropanol, ethanol, propanol, ethylene glycol or glycerol, or a mixed solution of two or more thereof.

[0011] In the above technical solution, the catalyst described in step 2 is one of a platinum-based catalyst, a palladium-based catalyst, a carbon-based catalyst or a single-atom catalyst.

[0012] In the above technical solution, the dispersion method described in step 2 is one of ultrasound, ball milling or mechanical high-speed shearing.

[0013] In the above technical solution, the coating method described in step 3 is one of slit coating, ultrasonic spraying, electrostatic spraying, screen printing, transfer or scraping.

[0014] Compared with other technologies, the present invention has the following advantages after adopting the above technical solution: (1) The present invention utilizes the abundant amino sites of the protonated nitrogen-rich material to interact with the -SO3- groups of the PFSA ionomer, thereby inducing changes in the microstructure of the PFSA ionomer, reducing its crystallinity, and achieving an improvement in the oxygen permeability of the PFSA ionomer.

[0015] (2) The present invention utilizes protonated nitrogen-rich materials to block the -SO3- groups of PFSA ionomers, which is equivalent to constructing a "barrier layer" at the interface of the -SO3- groups of PFSA ionomers and catalysts, thereby preventing the -SO3- groups from being specifically adsorbed on the surface of the catalyst active sites, thereby releasing more catalyst active sites.

[0016] (3) The present invention can provide an additional proton source at the PFSA ionomer-catalyst interface by protonating the nitrogen-rich material, thereby accelerating proton transfer, thereby breaking the balance between the interfacial reaction and the material transfer at the interface, and improving the oxygen reduction performance of the catalyst in the catalytic layer.

[0017] (4) The fuel cell catalyst layer prepared by the present invention has higher catalyst oxygen reduction reaction activity than the traditional catalyst layer.

[0018] (5) The method of the present invention provides a simple and effective method for improving the oxygen reduction performance of the catalyst in the catalytic layer. The PEMFC assembled with the membrane electrode prepared in large quantities by this method has good performance output and stability, and is particularly suitable for membrane electrodes with low precious metal loading. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The present invention will be further described below in conjunction with the accompanying drawings.

[0020] Figure 1 Curve 1 and Curve 2 in the middle are high-resolution X-ray photoelectron spectroscopy (XPS) of Pt 4f of the catalytic layer of Example 1 and Comparative Example 1, respectively.

[0021] Figure 2 Curve 1, curve 2 and curve 3 are polarization curves of membrane electrodes prepared in Example 1, Comparative Example 1 and Comparative Example 2, respectively. Curve 4, curve 5 and curve 6 are power density curves corresponding to membrane electrodes prepared in Example 1, Comparative Example 1 and Comparative Example 2, respectively. Operating conditions: battery operating temperature 80 °C, 0.3 L min-1 of anode and cathode respectively. -1 The pure hydrogen gas and pure oxygen gas are of pure hydrogen gas and the absolute pressure of the anode and cathode outlet gas is 50 kPa.

[0022] Figure 3 Curve 1 and curve 2 are polarization curves of membrane electrodes prepared in Example 2 and Comparative Example 1, respectively. Curve 3 and curve 4 are power density curves corresponding to membrane electrodes prepared in Example 2 and Comparative Example 1, respectively. Operating conditions: battery operating temperature 80 °C, 0.3 L min -1 The pure hydrogen gas and pure oxygen gas are of pure hydrogen gas and the absolute pressure of the anode and cathode outlet gas is 50 kPa.

[0023] Figure 4 Curves 1 and 2 are polarization curves of membrane electrodes prepared in Example 3 and Comparative Example 1, respectively. Curves 3 and 4 are power density curves of membrane electrodes prepared in Example 3 and Comparative Example 1, respectively. Operating conditions: battery operating temperature 80 °C, 0.3 L min -1 The pure hydrogen gas and pure oxygen gas are of pure hydrogen gas and the absolute pressure of the anode and cathode outlet gas is 50 kPa. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below in conjunction with specific examples and drawings, but this does not represent the only embodiment of the present invention. The following examples are helpful for those skilled in the art to further understand the present invention, but do not limit the present invention in any form. It should be pointed out that, for those of ordinary skill in the art, it is obvious that several improvements or optimizations can be easily made without departing from the ideas and principles of the present invention, which all belong to the protection scope of the present invention.

[0025] Example 1 (1) Preparation of protonated carbon nitride (pCN) C3N4 and concentrated nitric acid and concentrated sulfuric acid (volume ratio of 3:1) were weighed in a mass ratio of 1:50, and then the two were mixed and ultrasonic etching was continued for 4 hours; deionized water was weighed in a volume ratio of 1:2 between the mixed solution of concentrated nitric acid and concentrated sulfuric acid and deionized water, and the deionized water was added to the mixed solution of C3N4 and concentrated nitric acid and concentrated sulfuric acid, and the mixture was allowed to stand for 8 hours to obtain a white colloidal suspension; the white colloid was extracted by suction filtration, and was repeatedly washed with deionized water for 3 times, and protonated carbon nitride powder was obtained after vacuum drying at 60°C for 8 hours.

[0026] (2) Preparation of pCN modified catalyst slurry PFSA ionomer solution and pCN were weighed according to a mass ratio of PFSA ionomer to pCN of 1:0.05, and then the two were mixed and added to an ethanol solution, the mass concentration of PFSA ionomer was controlled to be 0.5 wt%, and ultrasonic dispersion was performed at room temperature for 40 mins to obtain a PFSA ionomer mixed solution interacting with pCN; then a platinum-based catalyst was weighed according to a mass ratio of platinum-based catalyst to PFSA ionomer of 1:0.8, and after wetting with a small amount of ultrapure water, it was added to the PFSA ionomer mixed solution interacting with pCN, homogenized for 20 mins, dispersed for 10 mins, and degassed for 10 mins to obtain a pCN modified catalyst slurry.

[0027] (3) Preparation of catalytic layer coated proton exchange membrane The proton exchange membrane is laid flat on a heating table at a temperature of 60°C, and then the pCN modified catalyst slurry obtained in step (1) is sprayed on both sides of the proton exchange membrane. After drying, a catalyst layer coated proton exchange membrane assembly is obtained.

[0028] (4) Performance evaluation of PEMFC based on pCN modified catalyst layer assembly Gas diffusion electrodes were assembled on both sides of the proton exchange membrane assembly coated with a pCN modified catalyst layer, and a fuel cell membrane electrode assembly was obtained after hot pressing. The obtained membrane electrode assembly was assembled into a fuel cell fixture for testing. The cell temperature was 80 °C, and 0.3 L min was passed into the anode and cathode respectively.-1 The absolute pressure of the gas at the anode and cathode outlets is 50 kPa. The polarization curve obtained by testing the membrane electrode assembly of Example 1 corresponds to Figure 2 Middle curve 1, power density curve corresponding to Figure 2 The high-resolution XPS spectrum of Pt 4f of the catalytic layer prepared in Example 1 corresponds to Figure 1 Middle curve 1.

[0029] Example 2 (1) Preparation of protonated graphene Graphene and concentrated nitric acid and concentrated sulfuric acid (volume ratio of 3:1) were weighed in a mass ratio of 1:50, and then the two were mixed and ultrasonic etching was continued for 4 hours; deionized water was weighed in a volume ratio of 1:2 between the mixed solution of concentrated nitric acid and concentrated sulfuric acid and deionized water, and the deionized water was added to the mixed solution of graphene and concentrated nitric acid and concentrated sulfuric acid, and the mixture was allowed to stand for 8 hours; the product was extracted by filtration, and was repeatedly washed with deionized water for 3 times, and protonated graphene powder was obtained after vacuum drying at 60 °C for 8 hours.

[0030] (2) Preparation of protonated graphene modified catalyst slurry PFSA ionomer solution and protonated graphene were weighed according to a mass ratio of PFSA ionomer to protonated graphene of 1:0.01, and then the two were mixed and added to a propylene glycol solution, the mass concentration of the PFSA ionomer was controlled to be 5 wt%, and ultrasonic dispersion was performed at room temperature for 40 mins to obtain a PFSA ionomer mixed solution interacting with protonated graphene; then a platinum-based catalyst was weighed according to a mass ratio of the platinum-based catalyst to the PFSA ionomer of 1:0.6, and after wetting with a small amount of ultrapure water, it was added to the PFSA ionomer mixed solution interacting with protonated graphene, homogenized for 10 mins, dispersed for 20 mins, and degassed for 5 mins to obtain a protonated graphene modified catalyst slurry.

[0031] Steps (3)-(4) are the same as those in Example 1 (3)-(4). The polarization curve obtained by testing the membrane electrode assembly of Example 2 corresponds to Figure 3 Middle curve 1, power density curve corresponding to Figure 3 Middle curve 2.

[0032] Example 3 (1) Preparation of protonated two-dimensional covalent organic framework materials C3N4 and trifluoroacetic acid were weighed according to a mass ratio of 1:20 between the two-dimensional covalent organic framework material and trifluoroacetic acid, and then the two were mixed and ultrasonically dispersed for 4 hours; deionized water was weighed according to a volume ratio of trifluoroacetic acid and deionized water of 1:4, and the deionized water was added to the mixed solution of the two-dimensional covalent organic framework material and trifluoroacetic acid, and allowed to stand for 8 hours; the suspended powder was extracted by filtration, and washed repeatedly with deionized water for 3 times, and the protonated two-dimensional covalent organic framework powder was obtained after vacuum drying at 60 °C for 8 hours.

[0033] (2) Preparation of protonated two-dimensional covalent organic framework material modified catalyst slurry The PFSA ionomer solution and the protonated nitrogen-rich material were weighed according to a mass ratio of PFSA ionomer to protonated two-dimensional covalent organic framework material of 1:0.1, and then the two were mixed and added to an isopropanol solution, the mass concentration of the PFSA ionomer was controlled to be 1 wt%, and ultrasonic dispersion was performed at room temperature for 40 mins to obtain a PFSA ionomer mixed solution that interacted with the protonated two-dimensional covalent organic framework material; then a platinum-based catalyst was weighed according to a mass ratio of the platinum-based catalyst to the PFSA ionomer of 1:0.8, and after wetting with a small amount of ultrapure water, it was added to the PFSA ionomer mixed solution that interacted with the protonated two-dimensional covalent organic framework material, homogenized for 10 mins, dispersed for 20 mins, and degassed for 5 mins to obtain a protonated two-dimensional covalent organic framework material modified catalyst slurry.

[0034] Steps (3)-(4) are the same as those in Example 1 (3)-(4). The polarization curve obtained by testing the membrane electrode assembly of Example 3 corresponds to Figure 4 Middle curve 1, power density curve corresponding to Figure 4 Middle curve 2.

[0035] Comparative test Comparative Example 1 (1) Preparation of traditional catalyst slurry A certain amount of PFSA ionomer was weighed and dissolved in ethanol, and the mass concentration of PFSA ionomer was controlled to be 0.3 wt%. The mixture was ultrasonically dispersed at room temperature for 10 mins. Then, a platinum-based catalyst was weighed according to a mass ratio of platinum-based catalyst to PFSA ionomer of 1:0.6. After being moistened with a small amount of ultrapure water, the catalyst was added to the PFSA ionomer solution, homogenized for 10 mins, dispersed for 20 mins, and degassed for 5 mins to obtain a traditional catalyst slurry.

[0036] (2) Preparation of catalytic layer coated proton exchange membrane The proton exchange membrane is laid flat on a heating table at a temperature of 60° C., and then the conventional catalyst slurry obtained in step (1) is sprayed on both sides of the proton exchange membrane. After drying, a catalyst layer coated proton exchange membrane assembly is obtained.

[0037] (3) PEMFC performance evaluation based on traditional catalyst layer assembly Gas diffusion electrodes were assembled on both sides of the conventional catalyst layer coated proton exchange membrane assembly, and the fuel cell membrane electrode assembly was obtained after hot pressing. The obtained membrane electrode assembly was assembled into a fuel cell fixture for testing. The cell temperature was 80 °C, and 0.3 L min was passed into the anode and cathode respectively. -1 The absolute pressure of the gas at the anode and cathode outlets is 50 kPa. The polarization curve obtained by testing the membrane electrode assembly of Example 1 corresponds to Figure 2 Middle curve 2, power density curve corresponding to Figure 2 Middle curve 5.

[0038] The high-resolution XPS spectrum of Pt 4f of the catalytic layer prepared in Comparative Example 1 corresponds to Figure 1 Middle curve 2.

[0039] Comparative Example 2 (1) Preparation of carbon nitride (C3N4) modified catalyst slurry PFSA ionomer solution and C3N4 were weighed according to a mass ratio of PFSA ionomer to C3N4 of 1:0.05, and then the two were mixed and added to an ethanol solution, the mass concentration of the PFSA ionomer was controlled to be 0.5 wt%, and ultrasonic dispersion was performed at room temperature for 40 mins to obtain a PFSA ionomer mixed solution that interacted with C3N4; then a platinum-based catalyst was weighed according to a mass ratio of the platinum-based catalyst to the PFSA ionomer of 1:0.8, and after wetting with a small amount of ultrapure water, it was added to the PFSA ionomer mixed solution that interacted with C3N4, homogenized for 20 mins, dispersed for 10 mins, and degassed for 10 mins to obtain a C3N4 modified catalyst slurry.

[0040] Steps (2)-(3) are the same as those in Comparative Example 1 (2)-(3). The polarization curve obtained by testing the membrane electrode assembly of Comparative Example 2 corresponds to Figure 2 Middle curve 3, power density curve corresponding to Figure 2 Middle curve 6.

[0041] Test results of the present invention: Figure 1Curves 1 and 2 in the middle are high-resolution X-ray photoelectron spectra (XPS) of Pt 4f in the catalytic layer of Example 1 and Comparative Example 1, respectively. XPS result analysis shows that, compared with pure carbon-supported platinum catalyst (TKK-Pt / C), the binding energy of Pt 4f (71.96 eV) of Comparative Example 1 with the addition of PFSA ionomer is significantly higher than that of TKK-Pt / C (71.67 eV), mainly due to the specific adsorption of -SO3- groups in PFSA on the Pt surface. The binding energy of Pt4f (71.75 eV) of Example 1 modified with pCN is lower than that of Comparative Example 1, which is mainly due to the strong interaction between pCN and -SO3- groups, which builds a barrier layer at the interface between -SO3- groups and Pt, avoiding direct contact between -SO3- groups and the Pt surface.

[0042] Figure 2 Curve 1, curve 2 and curve 3 are polarization curves of membrane electrodes prepared in Example 1, Comparative Example 1 and Comparative Example 2, respectively. Curve 4, curve 5 and curve 6 are power density curves corresponding to membrane electrodes prepared in Example 1, Comparative Example 1 and Comparative Example 2, respectively. Compared with Comparative Example 1 in which a PEMFC is assembled from a conventional catalyst layer, the peak power density of Comparative Example 2 in which nitrogen-rich material C3N4 is added and that of Example 1 in which protonated nitrogen-rich material pCN is added are higher than that of Comparative Example 1. Due to the provision of an additional proton source, the peak power density of Example 1 is also significantly higher than that of Comparative Example 2. Especially in the mass transfer region with high current density, Example 1 has a peak power density of 6A cm -2 The voltage at the electric density is 0.37 V, which is much higher than 0.25 V of Comparative Example 1 and 0.30 V of Comparative Example 2.

[0043] Figure 3 Curve 1 and curve 2 are polarization curves of membrane electrodes prepared in Example 2 and Comparative Example 1, respectively. Curve 3 and curve 4 are power density curves corresponding to membrane electrodes prepared in Example 2 and Comparative Example 1, respectively. It can be seen from the figure that the fuel cell performance of Example 2 is better than that of Figure 2 The fuel cell performance of Comparative Example 1 is shown.

[0044] Figure 4 Curve 1 and curve 2 are polarization curves of membrane electrodes prepared in Example 3 and Comparative Example 1, respectively. Curve 3 and curve 4 are power density curves of membrane electrodes prepared in Example 3 and Comparative Example 1, respectively. It can be seen from the figure that the fuel cell performance of Example 3 is better than that of Figure 2 The fuel cell performance of Comparative Example 1 is shown.

[0045] Finally, it should be noted that: Obviously, the above embodiments are only examples for clearly explaining the present invention, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the scope of protection of the present invention.

Claims

1. A method for improving the oxygen reduction activity of a catalyst in a fuel cell catalyst layer, characterized in that: The steps include: Step 1: Preparation of protonated nitrogen-rich material Weigh the nitrogen-rich material and concentrated acid in a mass ratio of 1:20-150, then mix the two, and continue ultrasonic etching for 1-20 h; weigh deionized water in a volume ratio of concentrated acid to deionized water of 1:0.5-3, add the deionized water to the mixed solution of the nitrogen-rich material and the concentrated acid, let it stand for 0.1-20 h, and obtain a powder suspension; extract the powder by suction filtration, and repeatedly wash it with deionized water for 1-5 times, and then vacuum dry it at 60 ° C for 1-20 h to obtain a protonated nitrogen-rich material powder; Step 2: Preparation of protonated nitrogen-rich material modified catalyst slurry According to the mass ratio of PFSA ionomer to the protonated nitrogen-rich material prepared in step 1 of 1:0.01~0.1, the PFSA ionomer solution and the protonated nitrogen-rich material are weighed, and then the two are mixed and added to the high volatility solution, the mass concentration of the PFSA ionomer is controlled to be 0.1~10 wt%, and ultrasonic dispersion is performed for 10~40 mins at room temperature to obtain a PFSA ionomer mixed solution that interacts with the protonated nitrogen-rich material; then the catalyst is weighed according to the mass ratio of the catalyst to the PFSA ionomer of 1:0.1~1.2, and after wetting with a small amount of ultrapure water, it is added to the PFSA ionomer mixed solution that interacts with the protonated nitrogen-rich material, homogenized for 10~30 mins, dispersed for 5~40 mins, and degassed for 1~20 mins to obtain a protonated nitrogen-rich material modified catalyst slurry; Step 3: Preparation of Catalytic Layer Coated Proton Exchange Membrane The proton exchange membrane is laid flat on a heating table at a temperature of 40-90°C, and then the protonated nitrogen-rich material modified catalyst slurry prepared in step 2 is coated on both sides of the proton exchange membrane. After drying, a catalyst layer coated proton exchange membrane assembly can be obtained.

2. The method for improving the oxygen reduction activity of a platinum-based catalyst in a fuel cell catalyst layer according to claim 1, characterized in that: The concentrated acid in step 1 is one of concentrated nitric acid, concentrated sulfuric acid, trifluoroacetic acid, trifluoroformic acid or a mixture of concentrated nitric acid and concentrated sulfuric acid.

3. The method for improving the oxygen reduction activity of a platinum-based catalyst in a fuel cell catalyst layer according to claim 1, characterized in that: The nitrogen-rich material in step 1 is one of a nitrogen-containing carbon material, a nitrogen-containing covalent organic framework material or a nitrogen-containing silica material.

4. The method for improving the oxygen reduction activity of a platinum-based catalyst in a fuel cell catalyst layer according to claim 1, characterized in that: The high volatility solution described in step 2 is one of water, isopropanol, ethanol, propanol, ethylene glycol or glycerol, or a mixed solution of two or more thereof.

5. The method for improving the oxygen reduction activity of a platinum-based catalyst in a fuel cell catalyst layer according to claim 1, characterized in that: The catalyst described in step 2 is one of a platinum-based catalyst, a palladium-based catalyst, a carbon-based catalyst or a single-atom catalyst.

6. The method for improving the oxygen reduction activity of a platinum-based catalyst in a fuel cell catalyst layer according to claim 1, characterized in that: The dispersion method in step 2 is one of ultrasound, ball milling or mechanical high-speed shearing.

7. The method for improving the oxygen reduction activity of a platinum-based catalyst in a fuel cell catalyst layer according to claim 1, characterized in that: The coating method described in step 3 is one of slit coating, ultrasonic spraying, electrostatic spraying, screen printing, transfer printing or scraping.