Composite carrier and preparation method thereof, catalyst and preparation method thereof, and fuel cell
By using metal oxides containing oxygen vacancies in fuel cell catalysts and recombining them with carbon support, the problem of insufficient conductivity and corrosion resistance is solved, and the activity and performance of the catalyst are significantly improved, especially in high oxygen environments.
Patent Information
- Application Number
- CN202410983501.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
The electrical conductivity and corrosion resistance of existing fuel cell catalysts are insufficient, resulting in deterioration of performance, especially in high humidity and high voltage conditions.
The metal oxide containing oxygen vacancy is combined with a carbon support, and the conductivity of the metal oxide is adjusted through oxygen vacancy is improved to form a composite support, and the active components are loaded thereon, thereby improving the activity of the catalyst and Corrosion resistance.
It significantly improves the conductivity and corrosion resistance of the catalyst, improves the activity and performance of the catalyst, especially in high oxygen environments.
Smart Images

Figure CN118943395A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fuel cells and relates to a composite carrier and a preparation method thereof, a catalyst and a preparation method thereof, and a fuel cell. Background Art
[0002] Carbon materials have always played an indispensable role in catalyst carriers, etc. The unique advantages of size, dispersion, specific surface area, degree of graphitization, pore structure and surface state make carbon have a unique advantage as a carrier, but carbon materials are easy to oxidize, which makes fuel cells prone to corrosion when running at high humidity and high voltage, resulting in performance degradation; oxides have obvious advantages in corrosion resistance, but their conductivity is poorer than that of carbon materials.
[0003] CN104685682A provides a method for producing a fuel cell catalyst, wherein the fuel cell catalyst comprises catalyst particles and a carbon support on which the catalyst particles are supported. In this document, a carbon material is used as a support for the catalyst active component, and its corrosion resistance is relatively poor.
[0004] CN115000423A provides a hydrogen fuel cell cathode catalyst, comprising a carrier and an active metal, wherein the active metal is loaded on the carrier, wherein the carrier is selected from one or both of metal oxides and transition metal-doped metal oxides; based on the total weight of the hydrogen fuel cell cathode catalyst, the loading amount of the active metal is 20-40wt%. In this document, metal oxide is used as a carrier of the active component, and its conductivity is relatively poor.
[0005] The existing methods of directly compounding carbon materials and metal oxides cannot completely and effectively solve the disadvantage of poor conductivity of metal oxides, which leads to severe polarization and poor performance during the application of fuel cells. For example, CN114892185A dissolves metal salts in acidic solutions to prepare metal salt solutions, adds porous carbon carriers, stirs and ultrasonically disperses, and then dries, and heat-treats them under air conditions to obtain composite carriers of porous carbon-confined metal oxides. However, the carbon carriers obtained by this method can only obtain composite materials of carbon carriers and metal oxides, which can effectively improve the corrosion resistance of carbon carriers, but cannot change the defect of poor conductivity of metal oxides.
[0006] Therefore, how to improve the conductivity of fuel cell catalyst carriers while also improving their corrosion resistance is a technical problem that needs to be solved urgently. Summary of the invention
[0007] In view of the shortcomings of the prior art, the present invention aims to provide a composite carrier and preparation method, a catalyst and preparation method, and a fuel cell. In the composite carrier provided by the present invention, the conductivity of the metal oxide is adjusted by oxygen vacancies, and the corrosion resistance of the carrier is also improved; after the active component is loaded, the activity of the catalyst is also significantly improved.
[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a composite carrier, comprising a carbon carrier and a metal oxide containing oxygen vacancies composited on the surface of the carbon carrier.
[0010] The composite carrier provided by the present invention has oxygen vacancies in the metal oxide that regulate the conductivity of the metal oxide and can promote the corrosion resistance of the composite carrier in a high-oxygen environment; at the same time, it can enhance the interaction between the active components in the catalyst and the composite carrier, thereby improving the corrosion resistance of the catalyst, and the activity of the catalyst is also significantly enhanced.
[0011] In the present invention, if the metal oxide does not contain oxygen vacancies, although the corrosion resistance of the carrier is improved, a carrier with good conductivity cannot be obtained, which affects the electronic conduction in the catalyst layer.
[0012] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0013] Preferably, the carbon carrier includes any one of graphite, carbon black, porous carbon, carbon nanotubes or carbon nanofibers, or a combination of at least two thereof.
[0014] Preferably, the metal element in the metal oxide includes any one or a combination of at least two of titanium, niobium, tin, cerium, tungsten, molybdenum, iridium, ruthenium, vanadium, manganese or cadmium.
[0015] The metal oxide provided by the present invention has a high specific surface area, which can improve the corrosion resistance of the carbon carrier and at the same time play a role in dispersing catalytic active components to improve the catalytic activity of the catalyst.
[0016] Preferably, the mass ratio of the carbon support to the metal oxide is (1-10):(1-10), for example 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 1:3, 1:5, 1:8 or 1:10, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0017] In a second aspect, the present invention provides a method for preparing the composite carrier according to the first aspect, the preparation method comprising the following steps:
[0018] Mixing a metal salt, an acidic solution and a carbon support, performing a first heat treatment to obtain a composite material of the carbon support to be modified and a metal oxide, and performing a first reduction heat treatment on the composite material of the carbon support to be modified and the metal oxide to obtain the composite support;
[0019] or;
[0020] The metal salt, the carbon carrier and the solvent are mixed and subjected to a solvent thermal reduction reaction to obtain a composite carrier.
[0021] Preferably, the acidic solution comprises a hydrochloric acid solution.
[0022] The preparation method provided by the present invention can first prepare a composite material of a carbon carrier and a metal oxide, and then modify the oxygen vacancies; it can also directly obtain a composite carrier with oxygen vacancies in a one-step reaction, and those skilled in the art can select the preparation method according to the adaptability of the metal element in the metal salt; and the preparation method is simple to operate, green and economical.
[0023] Preferably, the temperature of the first heat treatment is 200-600°C, for example 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C or 600°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Preferably, the atmosphere of the first reduction heat treatment comprises a reducing atmosphere.
[0025] Preferably, the reducing atmosphere comprises a hydrogen atmosphere.
[0026] In the first reduction heat treatment process provided by the present invention, in addition to the reducing gas, other mixed gases may also be included, such as protective gas (nitrogen or inert gas).
[0027] Preferably, the temperature of the first reduction heat treatment is 150-750°C, for example, 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C or 750°C, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] Preferably, the time of the first reduction heat treatment is 10 to 120 min, for example, 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min or 120 min, etc.
[0029] Preferably, the solvent in the solvothermal reaction comprises ethylene glycol.
[0030] Preferably, the temperature of the solvent thermal reduction reaction is 100-220°C, for example 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C or 220°C, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] In a third aspect, the present invention provides a catalyst, comprising the composite carrier as described in the first aspect and an active component loaded on the composite carrier; the active component comprises oxygen vacancies.
[0032] When the catalyst provided by the present invention adopts the composite carrier of the first aspect, the oxygen vacancies in the metal oxide and the oxygen vacancies in the active component can enhance the interaction between the composite carrier and the active component, thereby achieving better dispersion of the active component and improving the catalytic activity of the catalyst.
[0033] Preferably, the loading amount of the active component is 10-90%, for example 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80% or 90%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, the active metal element in the active component includes the first metal element and / or the second metal element.
[0035] Preferably, the first metal element includes Pt.
[0036] Preferably, the second metal element includes any one of Co, Ni, Cu, Ir or Ru, or a combination of at least two of them.
[0037] In the present invention, the first metal element and the second metal element may form an alloy material.
[0038] Preferably, the active component includes active metal and / or oxides formed by active metal and metal in the composite carrier, preferably active metal and oxides formed by active metal and metal in the composite carrier.
[0039] In the catalyst provided by the present invention, when the active component contains not only active metals, the active metals and the metals in the composite carrier also form an alloyed catalyst, which significantly improves the active components of the catalyst.
[0040] In a fourth aspect, the present invention provides a method for preparing the catalyst according to the third aspect, the preparation method comprising the following steps:
[0041] The active component salt, the acid solution and the composite carrier are mixed and subjected to a second reduction heat treatment to obtain the catalyst.
[0042] The preparation method of the catalyst provided by the present invention enables the active component to be loaded in the composite carrier and also realizes the modification of the oxygen vacancies of the active component.
[0043] Preferably, the temperature of the second reduction heat treatment is 200-900°C, for example 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C or 900°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0044] The atmosphere of the second reduction heat treatment provided by the present invention may be the same as or different from the atmosphere of the first reduction heat treatment, as long as it contains a reducing gas.
[0045] If the temperature of the second reduction heat treatment is too low, a stable alloy catalyst cannot be obtained, while if the reduction temperature is too high, the alloy catalyst particles will agglomerate.
[0046] Preferably, the time of the second reduction heat treatment is 2h to 48h, for example 2h, 5h, 10h, 15h, 20h, 25h, 30h, 35h, 36h, 40h, 45h or 48h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0047] It should be noted that the present invention does not impose any special restrictions on the specific salt types of metal salts and active component salts. The present invention is applicable to any type that can be directly dissolved in the corresponding solution system and can achieve the reaction, including but not limited to sulfates, hydrochlorides, phosphates or nitrates.
[0048] In a fifth aspect, the present invention further provides a fuel cell, comprising the catalyst as described in the third aspect.
[0049] Compared with the prior art, the present invention has the following beneficial effects:
[0050] (1) The composite carrier provided by the present invention has oxygen vacancies in the metal oxide that regulate the conductivity of the metal oxide and can promote the corrosion resistance of the composite carrier in a high oxygen environment. At the same time, it can enhance the interaction between the active components in the catalyst and the composite carrier, thereby improving the corrosion resistance of the catalyst and significantly improving the activity of the catalyst.
[0051] (2) When the catalyst provided by the present invention adopts the composite carrier of the first aspect, the oxygen vacancies in the metal oxide and the oxygen vacancies in the active component can enhance the interaction between the composite carrier and the active component, thereby achieving better dispersion of the active component and improving the catalytic activity of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 This is a comparison chart of the polarization curve performance of the catalysts provided in Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0053] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0054] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions.
[0055] Example 1
[0056] This embodiment provides a composite carrier, which includes a carbon carrier and niobium oxide containing oxygen vacancies composited on the surface of the carbon carrier.
[0057] The preparation method of the composite carrier is as follows:
[0058] (1) Dissolve 0.1 g of niobium chloride in 0.1 mol / L hydrochloric acid solution to form a uniform solution;
[0059] (2) Add 1 g of carbon powder (carbon carrier), stir for 30 min, and dry by air blowing at 80 °C;
[0060] (3) heat treating the sample in step (2) at 200° C. in an air atmosphere for 1 h, and naturally cooling to room temperature to obtain a composite material of the modified carbon support and the metal oxide;
[0061] (4) The sample in step (3) was heat treated at 350° C. for 20 min in a hydrogen atmosphere, and then naturally cooled to room temperature to obtain a final composite carrier.
[0062] This embodiment also provides a catalyst, which includes the composite carrier provided above and a platinum-niobium active component containing oxygen vacancies loaded in the composite carrier; the platinum active component includes platinum nanoparticles and platinum-niobium composite oxide (the loading amount of Pt in the composite carrier is 60%).
[0063] The preparation method of the catalyst is as follows:
[0064] (5) dissolving a Pt-containing metal salt precursor (chloroplatinic acid) in a hydrochloric acid solution to obtain a uniform solution, and mixing the composite support of step (4) with the uniform solution;
[0065] (6) The mixed solution in (5) was dried by air blowing at 60° C., and then reacted at 700° C. for 1 hour in a hydrogen atmosphere to obtain the composite catalyst.
[0066] Example 2
[0067] This embodiment provides a composite carrier, which includes a carbon carrier and cerium oxide containing oxygen vacancies composited on the surface of the carbon carrier.
[0068] The preparation method of the composite carrier is as follows:
[0069] (1) 0.3 g CeCl 3 Dissolve in 50 mL of ethylene glycol to form a uniform solution;
[0070] (2) Add 1 g of carbon powder and stir for 30 min;
[0071] (3) placing the sample in step (2) in a hydrothermal reactor and reacting in a forced air drying oven at 180° C. for 3 hours;
[0072] (4) Centrifuge, wash, and dry the sample obtained in step (3) to obtain the final composite carrier.
[0073] This embodiment also provides a catalyst, which includes the composite carrier provided above and a platinum-cobalt-tungsten active component containing oxygen vacancies loaded in the composite carrier; the platinum active component includes platinum nanoparticles and platinum-cerium composite oxide (the loading amount of Pt in the composite carrier is 50%).
[0074] The preparation method of the catalyst is as follows:
[0075] (5) dissolving a Pt-containing metal salt precursor (chloroplatinic acid) in a hydrochloric acid solution to obtain a uniform solution, and mixing the composite support of step (4) with the uniform solution;
[0076] (6) The mixed solution in (5) was dried by air blowing at 60° C., and then reacted at 900° C. for 1 hour in a hydrogen atmosphere to obtain the composite catalyst.
[0077] Example 3
[0078] This embodiment provides a composite carrier, which includes a carbon carrier and niobium oxide containing oxygen vacancies composited on the surface of the carbon carrier.
[0079] The preparation method of the composite carrier is as follows:
[0080] (1) Dissolve 0.1 g of niobium chloride in 0.1 mol / L hydrochloric acid solution to form a uniform solution;
[0081] (2) Add 1 g of carbon powder (carbon carrier), stir for 30 min, and dry by air blowing at 80 °C;
[0082] (3) heat treating the sample in step (2) in an air atmosphere at 400°C for 1 h, and cooling naturally to room temperature to obtain a composite material of the modified carbon support and the metal oxide;
[0083] (4) The sample in step (3) was heat treated at 500° C. for 10 min in a hydrogen atmosphere, and then naturally cooled to room temperature to obtain a final composite carrier.
[0084] This embodiment also provides a catalyst, which includes the composite carrier provided above and a platinum active component containing oxygen vacancies loaded in the composite carrier; the platinum active component includes platinum atoms and platinum-niobium composite oxide (the loading amount of Pt in the composite carrier is 70%).
[0085] The preparation method of the catalyst is as follows:
[0086] (5) dissolving chloroplatinic acid in a hydrochloric acid solution to obtain a uniform solution, and mixing the composite carrier of step (4) with the uniform solution;
[0087] (6) The mixed solution in (5) was dried by air blowing at 60° C., and then reacted at 200° C. for 1 hour in a hydrogen atmosphere to obtain the composite catalyst.
[0088] Example 4
[0089] The difference between this embodiment and embodiment 1 is that the temperature of the second reduction heat treatment in step (6) of this embodiment is 500°C.
[0090] The rest of the preparation methods and parameters were the same as those in Example 1.
[0091] Example 5
[0092] The difference between this embodiment and embodiment 1 is that the temperature of the second reduction heat treatment in step (6) of this embodiment is 150°C.
[0093] The rest of the preparation methods and parameters were the same as those in Example 1.
[0094] Example 6
[0095] The difference between this embodiment and embodiment 1 is that the temperature of the second reduction heat treatment in step (6) of this embodiment is 1000°C.
[0096] The rest of the preparation methods and parameters were the same as those in Example 1.
[0097] Comparative Example 1
[0098] The difference between this comparative example and Example 1 is that in the composite carrier provided in this comparative example, niobium oxide does not contain oxygen vacancies.
[0099] In the preparation method, step (4) is not performed.
[0100] The rest of the preparation methods and parameters were the same as those in Example 1.
[0101] Figure 1 The polarization curve performance comparison diagram of the catalyst provided in Example 1 and Comparative Example 1 is shown. Figure 1 It can be concluded that the performance of Example 1 is higher than that of Comparative Example 1 in the entire current density range. On the one hand, the interaction between Pt and Nb changes the electronic structure of the catalyst and improves the catalytic activity; on the other hand, the oxygen vacancies improve the conductivity of the composite carrier, and the oxygen vacancies may also play a certain catalytic effect in the oxygen reduction process.
[0102] The composite carriers provided in Examples 1-6 and Comparative Example 1 were subjected to performance tests, and the test conditions included:
[0103] (1) Corrosion resistance test: The synthesized catalyst was prepared into a membrane electrode and scanned in a voltage range of 1.0-1.5 V, a scanning speed of 500 mV / s, a hydrogen atmosphere at the anode and a N2 atmosphere at the cathode. The cutoff conditions were 1.5 A / cm2 point density, voltage decay of 30 mV and ECSA decay of 40%. The corrosion resistance was compared by comparing the number of scanning cycles. The test results are shown in Table 1.
[0104] Table 1
[0105]
[0106]
[0107] Depend on Figure 1 And Table 1 can be obtained:
[0108] From the comparison between Example 1 and Example 2, it can be seen that the method can realize the modification of oxygen vacancies in metal oxides and obtain a composite material of a carbon carrier and a metal oxide. Whether the oxygen vacancies are obtained by in-situ reaction or the oxygen vacancies are subsequently modified, the corrosion resistance and conductivity of the catalyst can be improved.
[0109] From the comparison between Example 1 and Examples 4-6, it can be seen that during the second reduction heat treatment process, if the temperature is too low, a stable alloy catalyst cannot be obtained, and if the reduction temperature is too high, the alloy catalyst particles will agglomerate.
[0110] From the comparison between Example 1 and Comparative Example 1, it can be seen that if the metal oxide of the composite carrier does not contain oxygen vacancies, although the corrosion resistance of the carrier is improved, a carrier with good conductivity cannot be obtained, which affects the electronic conduction in the catalyst layer.
[0111] In summary, in the composite carrier provided by the present invention, the oxygen vacancies in the metal oxide regulate the conductivity of the metal oxide and can promote the corrosion resistance of the composite carrier to the carbon carrier in a high oxygen environment; when it is used as a catalyst, the oxygen vacancies in the metal oxide and the oxygen vacancies in the active component can enhance the interaction between the composite carrier and the active component, thereby achieving better dispersion of the active component, thereby improving the catalytic activity of the catalyst.
[0112] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A composite carrier, characterized in that The composite support comprises a carbon support and a metal oxide containing oxygen vacancies which is composited on the surface of the carbon support.
2. The composite carrier according to claim 1, characterized in that The carbon carrier comprises any one of graphite, carbon black, porous carbon, carbon nanotubes or carbon nanofibers, or a combination of at least two thereof; Preferably, the metal element in the metal oxide includes any one or a combination of at least two of titanium, niobium, tin, cerium, tungsten, molybdenum, iridium, ruthenium, vanadium, manganese or cadmium; Preferably, the mass ratio of the carbon support to the metal oxide is (1-10):(1-10).
3. A method for preparing a composite carrier according to claim 1 or 2, characterized in that: The preparation method comprises the following steps: Mixing a metal salt, an acidic solution and a carbon support, performing a first heat treatment to obtain a composite material of the carbon support to be modified and the metal oxide, and performing a first reduction heat treatment on the composite material of the carbon support to be modified and the metal oxide to obtain the composite support; or; The metal salt, the carbon carrier and the solvent are mixed and subjected to a solvent thermal reduction reaction to obtain a composite carrier.
4. The method for preparing the composite carrier according to claim 3, characterized in that: The acidic solution includes a hydrochloric acid solution; Preferably, the temperature of the first heat treatment is 200-600°C; Preferably, the atmosphere of the first reduction heat treatment comprises a reducing atmosphere; Preferably, the reducing atmosphere comprises a hydrogen atmosphere; Preferably, the temperature of the first reduction heat treatment is 150-750°C; Preferably, the first reduction heat treatment is performed for 10 to 120 minutes.
5. The method for preparing the composite carrier according to claim 3 or 4, characterized in that: The solvent in the solvothermal reaction includes ethylene glycol; Preferably, the temperature of the solvent thermal reduction reaction is 100-220°C.
6. A catalyst, characterized in that The catalyst comprises the composite carrier as claimed in claim 1 or 2 and an active component loaded on the composite carrier; the active component comprises oxygen vacancies.
7. The catalyst according to claim 6, characterized in that The loading amount of the active component is 10 to 90%; Preferably, the active metal element in the active component includes a first metal element and / or a second metal element; Preferably, the first metal element comprises Pt; Preferably, the second metal element includes any one or a combination of at least two of Co, Ni, Cu, Ir or Ru; Preferably, the active component includes active metal and / or oxides formed by active metal and metal in the composite carrier, preferably active metal and oxides formed by active metal and metal in the composite carrier.
8. A method for preparing the catalyst according to claim 6 or 7, characterized in that: The preparation method comprises the following steps: The active component salt, the acid solution and the composite carrier are mixed and subjected to a second reduction heat treatment to obtain the catalyst.
9. The method for preparing a catalyst according to claim 8, characterized in that: The temperature of the second reduction heat treatment is 200-900°C; Preferably, the second reduction heat treatment is performed for 2 to 48 hours.
10. A fuel cell, characterized in that: The fuel cell comprises the catalyst according to claim 6 or 7.
Citation Information
Patent Citations
Preparation method and application of carbon-supported nanoscale cerium oxide electrocatalyst with controllable oxygen vacancy content
CN116536695A
Fuel cell catalyst composite carrier and preparation method and application thereof
CN116722158A
Composite carbon carrier PtCoRu catalyst as well as preparation method and application thereof
CN117543030A
Fuel cell catalyst support based on doped titanium suboxides
US20200112032A1
Electrode material, method for producing same, and electrode using same, membrane electrode assembly, and solid-state polymer fuel cell