Electrocatalyst for seawater electrolysis hydrogen production as well as preparation method and application of electrocatalyst
By using Ru@TiC electrocatalysts supported by ruthenium nanoparticles in seawater electrolysis hydrogen production, the existing catalysts are solved, and the high-efficiency electrolysis hydrogen production in complex seawater environments is achieved. It has good catalytic activity and stability, suitable for large-scale applications.
Patent Information
- Application Number
- CN202411101298.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-12
AI Technical Summary
Existing seawater electrolytic hydrogen production catalysts are expensive and are prone to inactivation in complex seawater environments, so they cannot be used on a large scale.
Using titanium carbide nanofibers as support, the ruthenium nanoparticles were prepared by electrospinning and the loaded ruthenium nanoparticles were quickly treated by rapid Joule heat to form Ru@TiC electrocatalyst, which solved the problem of easy agglomeration of ruthenium nanoparticles and improved the corrosion resistance of the catalyst and Catalytic activity.
It achieves efficient electrolyzed seawater hydrogen production under acidic and alkaline conditions, has good catalytic activity and stability, and is simple in preparation, economical and practical, suitable for large-scale production.
Smart Images

Figure CN118996494A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalyst technology, and in particular to an electrocatalyst for producing hydrogen by electrolysis of seawater, and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] As an important chemical raw material and one of the emerging energy sources, hydrogen is widely used in chemical production, electronics industry, aerospace and other fields. The electrolysis of water to produce hydrogen is a clean method for large-scale production of high-purity hydrogen. However, the electrolysis of water to produce hydrogen requires a large amount of high-purity water, but the earth's fresh water resources are becoming increasingly scarce. As seawater is the most abundant water resource on earth, it is of great significance to realize the direct electrolysis of seawater to produce hydrogen.
[0004] At present, one of the most promising catalysts for commercial use in seawater electrolysis hydrogen production is Pt nanoparticles supported by carbon black or activated carbon (Pt / C). By using carbon black or activated carbon as a carrier, mixing it with a chloroplatinic acid solution, and then drying, reducing, heat treating, washing and other steps, Pt nanoparticles with a particle size of about 3 to 5 nm are obtained and distributed on the surface of the carbon carrier. Although this method can achieve seawater electrolysis hydrogen production, the platinum-based precious metals in the platinum-carbon catalyst are expensive and cannot be used on a large scale. In addition, the corrosion of chloride ions and the deposition of metal cations in seawater with complex composition will cause it to deactivate, hindering the development of seawater electrolysis hydrogen production technology. Therefore, designing high-performance, low-cost, and corrosion-resistant electrocatalysts has become one of the key issues in the development of seawater electrolysis technology. Summary of the invention
[0005] In order to overcome the above problems, the present invention provides an electrocatalyst for hydrogen production by electrolysis of seawater and a preparation method and application thereof.
[0006] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0007] In a first aspect of the present invention, an electrocatalyst for producing hydrogen by electrolysis of seawater is provided, wherein the electrocatalyst is supported by titanium carbide nanofibers and loaded with ruthenium nanoparticles.
[0008] The second aspect of the present invention provides a method for preparing the electrocatalyst for producing hydrogen by electrolysis of seawater, comprising:
[0009] (1) dissolving a carbon source and a titanium source in a solvent to form a spinning solution, preparing the solution into a nanofiber membrane by an electrospinning method, and then performing a carbon thermal reduction reaction after pre-oxidation to obtain titanium carbide nanofibers;
[0010] (2) Ruthenium nanoparticles were loaded on titanium carbide nanofibers using rapid Joule thermal treatment to obtain the electrocatalyst Ru@TiC.
[0011] The third aspect of the present invention provides the use of the above-mentioned electrocatalyst for hydrogen production by seawater electrolysis in hydrogen production by seawater electrolysis.
[0012] The beneficial effects of the present invention are:
[0013] (1) The electronic structure of metallic ruthenium is similar to that of platinum, and it also has a good catalytic effect on the electrocatalytic hydrogen evolution reaction, and its price is lower. However, ruthenium nanoparticles are easy to agglomerate, which limits its application in electrocatalytic hydrogen evolution. The present invention adopts electrostatic spinning to obtain titanium carbide nanofibers. The nanofibers not only have a large specific surface area, but are also easy to load ruthenium nanoparticles. At the same time, there is a metal-carrier interaction between ruthenium and carbide, which can stabilize the loaded ruthenium nanoparticles and solve the problem of easy agglomeration of ruthenium nanoparticles. The formed electrocatalyst Ru@TiC has a larger chemical reaction active specific surface area and more abundant chemical reaction active sites, so that the catalyst has a higher catalytic reaction activity. Furthermore, titanium carbide, as a titanium-based compound, is a "transition metal interstitial compound" formed by carbon atoms being incorporated into the lattice of the parent titanium. It has good electrical conductivity and corrosion resistance, and good electrical conductivity can increase the electrocatalytic effect.
[0014] (2) The electrocatalyst Ru@TiC provided by the present invention can be used for electrolysis of seawater to produce hydrogen under acidic or alkaline conditions due to its good corrosion resistance, catalytic activity and conductivity.
[0015] (3) The electrocatalyst Ru@TiC provided by the present invention can be used for electrocatalytic hydrogen production in acidic fresh water and alkaline fresh water, as well as in acidic seawater and alkaline seawater, and has good catalytic activity and stability.
[0016] (4) The electrocatalyst Ru@TiC provided by the present invention has a simple preparation process, is economical and practical, does not require special equipment and harsh conditions, has practical value, and is easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0018] Figure 1 is a scanning electron microscope image of the titanium carbide nanofiber prepared in Example 1 of the present invention, wherein a and b are the results taken at different magnifications;
[0019] Figure 2 is an X-ray diffraction pattern of the titanium carbide nanofiber prepared in Example 1 of the present invention;
[0020] Figure 3 is a transmission electron microscope image of the Ru@TiC electrocatalyst prepared in Example 3 of the present invention, wherein a and b are the results taken at different magnifications;
[0021] Figure 4 The results of the cycle performance test of the Ru@TiC electrocatalyst obtained in Example 3 of the present invention for the hydrogen evolution reaction by electrolysis of water in an acidic environment;
[0022] Figure 5 The results of the cycle performance test of the Ru@TiC electrocatalyst obtained in Example 3 of the present invention for the electrolysis of water and hydrogen evolution reaction under acidic natural seawater conditions;
[0023] Figure 6 The results of the cycle performance test of the Ru@TiC electrocatalyst obtained in Example 3 of the present invention in the electrolysis of water and hydrogen evolution reaction in an alkaline environment;
[0024] Figure 7 The results of the cycle performance test of the Ru@TiC electrocatalyst obtained in Example 3 of the present invention in the electrolysis of water and hydrogen evolution reaction under alkaline natural seawater conditions;
[0025] Figure 8 This is the chronopotentiometric test result of the Ru@TiC electrocatalyst obtained in Example 3 of the present invention undergoing a hydrogen evolution reaction by electrolysis of water in an alkaline saturated sodium chloride environment. DETAILED DESCRIPTION
[0026] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0027] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0028] A first typical embodiment of the present invention provides an electrocatalyst for producing hydrogen by electrolysis of seawater, wherein the electrocatalyst uses titanium carbide nanofibers as a carrier and is loaded with ruthenium nanoparticles.
[0029] In one or more embodiments, the loading amount of ruthenium nanoparticles is 0.5% to 30 wt.%.
[0030] A second typical embodiment of the present invention provides a method for preparing the electrocatalyst for producing hydrogen by electrolysis of seawater, comprising:
[0031] (1) dissolving a carbon source and a titanium source in a solvent to form a spinning solution, preparing the solution into a nanofiber membrane by an electrospinning method, and then performing a carbon thermal reduction reaction after pre-oxidation to obtain titanium carbide nanofibers;
[0032] (2) Ruthenium nanoparticles were loaded on titanium carbide nanofibers using rapid Joule thermal treatment to obtain the electrocatalyst Ru@TiC.
[0033] In one or more embodiments, in step (1), the carbon source is a high molecular polymer;
[0034] Preferably, the high molecular polymer includes one or more of polyacrylonitrile (PAN), polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA) and polylactic acid (PLA).
[0035] In one or more embodiments, in step (1), the titanium source includes one of tetrabutyl titanate, tetraisopropyl titanate or titanium tetrachloride.
[0036] In one or more embodiments, in step (1), the mass ratio of the carbon source to the titanium source is 0.25 to 3:1;
[0037] In one or more embodiments, in step (1), the solvent includes one or more of N,N-dimethylformamide, acetic acid, water, ethanol or chloroform.
[0038] In one or more embodiments, in step (1), the concentration of the titanium source in the solvent is 0.5 to 3 mg / mL.
[0039] In one or more embodiments, in step (1), the process parameters of electrospinning are: the propulsion speed of the spinning solution is 0.5-2 mL / h, preferably 1 mL / h; the receiving distance is 8-30 cm, preferably 15-22 cm, and more preferably 18 cm; the voltage is 8-30 kV, preferably 14-30 kV, and more preferably 16 kV; the spinning time is 2-50 h, preferably 8-12 h, and more preferably 10 h.
[0040] In one or more embodiments, in step (1), pre-oxidation is to anneal the nanofiber membrane under air or oxygen conditions at a temperature of 100 to 280°C, preferably 200 to 280°C, and more preferably 260°C; the holding time is 0.5 to 20h, preferably 0.5 to 5h, and more preferably 2h; the heating rate is 5 to 20°C / min.
[0041] In one or more embodiments, in step (1), the carbon thermal reduction reaction is a high-temperature calcination, the calcination temperature is 1400-2200°C, preferably 1400-1600°C, and more preferably 1500°C; the calcination time is 1-12h, preferably 1-5h, and more preferably 2h; the heating rate is 5-20°C / min.
[0042] In one or more embodiments, in step (1), the width of the titanium carbide nanofibers obtained is 100 to 1000 nm.
[0043] In one or more embodiments, in step (2), the method of loading ruthenium nanoparticles on titanium carbide nanofibers by rapid Joule thermal treatment includes:
[0044] The ruthenium salt solution was drop-coated on the titanium carbide nanofibers, which were placed in a Joule heating device for heating to obtain the electrocatalyst Ru@TiC.
[0045] Preferably, the solute ruthenium salt in the ruthenium salt solution droplet includes one of ruthenium chloride or ruthenium acetylacetonate;
[0046] Preferably, the solvent in the ruthenium salt solution droplets includes one of water, methanol, ethanol or N,N-dimethylformamide.
[0047] Preferably, the Joule heat device is set to a heating temperature of 400 to 2200° C.; the Joule heat process can be repeated 1 to 10 times, with each heating time being 4 to 6 seconds.
[0048] A third typical embodiment of the present invention provides the use of the above-mentioned electrocatalyst for hydrogen production by seawater electrolysis in hydrogen production by seawater electrolysis.
[0049] In one or more embodiments, the pH value of seawater is adjusted to 0 to 3 and / or 12 to 14. Seawater can be either acidic or alkaline.
[0050] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0051] Example 1
[0052] The polymer fiber membrane is prepared by electrospinning, as follows:
[0053] Dissolve polyacrylonitrile (1.0 g) and tetrabutyl titanate (2 mL) in a mixed solution of N,N-dimethylformamide (9 mL) and acetic acid (1 mL), stir evenly to form a yellow transparent solution, which is used as a spinning solution;
[0054] The spinning solution was prepared into a fiber membrane by electrospinning. The electrospinning high voltage was 16kV, the distance between the tip of the electrospinning and the collecting device (receiving distance) was 18cm, the electrospinning time was 10h, and the propulsion speed of the spinning solution was 1mL / h. After the electrospinning was completed, a white polymer film was generated. The polymer film was placed in an oven at 60°C and dried overnight to remove the residual solvent, and finally a uniform and soft polymer fiber membrane was obtained.
[0055] The pre-oxidation process was carried out under air conditions, with a heating rate of 5°C / min, a temperature of 260°C, and a holding time of 2h; the carbonization process was carried out in an inert gas argon atmosphere, with a heating rate of 5°C / min, a temperature of 1500°C, and a holding time of 2h, to obtain a one-dimensional titanium carbide nanofiber material (TiC). Electrospinning technology is an effective method for preparing one-dimensional nanofibers. It can accurately control the diameter of the fiber, ensure the uniformity and controllability of the fiber, and the mutually entangled one-dimensional interconnected structure is conducive to the formation of a conductive network, so that its carbonization product has good conductivity, which is conducive to the electrocatalytic reaction. This method is simple to operate, has low equipment cost, and can easily adjust the composition and structure of the fiber, which is conducive to the preparation and promotion of materials.
[0056] The scanning electron microscope image of the titanium carbide material obtained in this example is as follows Figure 1 The X-ray diffraction results are shown in Figure 2 As shown in the figure, even after pre-oxidation and carbonization annealing, the fiber morphology can still be maintained, and no obvious agglomeration occurs, indicating that the carbide obtained in this treatment process is uniform and stable.
[0057] Example 2
[0058] The difference from Example 1 is that polyvinyl pyrrolidone (1 g) and tetraisopropyl titanate (2 mL) are dissolved in an ethanol solution, and the remaining preparation processes and steps are the same as those of Example 1.
[0059] Example 3
[0060] The Ru@TiC electrocatalyst with quantitative control was prepared by rapid Joule thermal treatment, as follows:
[0061] The TiC obtained in Example 1 was used as a carrier and the TiC prepared by sintering was cut into pieces of about 0.5×1 cm 2electrode; ruthenium chloride was prepared into a 10 mg / mL ruthenium chloride aqueous solution, 100 μL of the ruthenium chloride solution was transferred and drop-coated on the TiC carrier, and after drying with an infrared lamp, it was placed in a Joule-heated graphite boat, and after three inert gas washes, the Joule heat process was performed under vacuum conditions; the voltage and current of the power supply output were controlled to be 10 V and 25 A respectively, the temperature was about 1000 ° C, the heating was stopped within 4 s, and the Ru@TiC electrocatalyst was obtained after cooling to room temperature. After ICP testing, the Ru content was shown to be about 3 wt.%.
[0062] TEM images of Ru@TiC electrocatalyst Figure 3 As shown, from Figure 3 It can be found that Ru is uniformly loaded on TiC in the form of small particles.
[0063] Example 4
[0064] The Ru@TiC electrocatalyst obtained in Example 3 was used to conduct a water electrolysis hydrogen production test. The Ru@TiC electrocatalyst was cut into 0.5×0.5 cm 2 The electrode was tested in a 0.5 M sulfuric acid solution using a standard three-electrode system in an electrolytic cell, using a carbon rod as a counter electrode and a mercury / mercurous sulfate electrode as a reference electrode.
[0065] An electrochemical workstation was used as a detection and recording device, and linear sweep voltammetry was used to detect the material performance. The initial voltage was set to -0.5V, the end voltage was -1.6V, and the scan rate was 2mV / s. The initial working curve was recorded, and then cyclic voltammetry was used to detect and evaluate the stability of the material. Within the above voltage range, the scan rate was 100mV / s. After the cycle was completed, the linear sweep voltammetry was used again to test and evaluate the reacted material, and the working curve was recorded. The results are shown in Figure 4 Initially, 10mA / cm 2 The overpotential is only 25mV and the current density reaches 1A / cm 2 The overpotential is only 290 mV; and after 3000 cycles of stability testing, the performance of the Ru@TiC electrocatalyst remains almost unchanged, indicating that the catalyst has good catalytic activity and stability in the electrocatalytic hydrogen production reaction under acidic conditions.
[0066] Example 5
[0067] The difference between this embodiment and embodiment 4 is that the catalyst is tested in a 0.5 mM sulfuric acid solution. The catalyst still has good catalytic activity and stability in the electrocatalytic hydrogen production reaction under acidic conditions of pH 3.
[0068] Example 6
[0069] The difference from Example 4 is that the electrocatalyst was tested in 0.5M sulfuric acid acidic natural seawater. The rest of the preparation process and steps are the same as those in Example 4. The results are shown in FIG. Figure 5 As shown in the figure, after 3000 cycles of stability testing, the performance of the Ru@TiC electrocatalyst remained almost unchanged even in the acidic natural seawater environment, indicating that the catalyst has good catalytic activity and stability.
[0070] Example 7
[0071] The Ru@TiC electrocatalyst obtained in Example 3 was used to conduct a water electrolysis hydrogen production test. The Ru@TiC electrocatalyst was cut into 0.5×0.5 cm 2 The electrode was tested in a 1 M potassium hydroxide solution using a standard three-electrode system in an electrolytic cell, using a carbon rod as the counter electrode and a mercury / mercury oxide electrode as the reference electrode.
[0072] An electrochemical workstation was used as a detection and recording device, and linear sweep voltammetry was used to detect the material performance. The initial voltage was set to -0.6V, the end voltage was -1.6V, and the scan rate was 2mV / s. The initial working curve was recorded, and then cyclic voltammetry was used to detect and evaluate the stability of the material. Within the above voltage range, the scan rate was 100mV / s. After the cycle was completed, the linear sweep voltammetry was used again to test and evaluate the reacted material, and the working curve was recorded. The results are shown in Figure 6 Initially, 10mA / cm 2 The overpotential is only 20mV and the current density reaches 1A / cm 2 The overpotential is only 260 mV; and after 3000 cycles of stability testing, the performance of the Ru@TiC electrocatalyst remains almost unchanged, indicating that the catalyst has good catalytic activity and stability in the electrocatalytic hydrogen production reaction under alkaline conditions.
[0073] Example 8
[0074] The difference between this embodiment and embodiment 7 is that the catalyst is tested in a 0.01 M potassium hydroxide solution. The catalyst still has good catalytic activity and stability in the electrocatalytic hydrogen production reaction under alkaline conditions of pH 12.
[0075] Example 9
[0076] The difference from Example 7 is that the electrocatalyst was tested in alkaline natural seawater containing 1M potassium hydroxide. The remaining preparation processes and steps were the same as those of Example 6. The results are shown in FIG. Figure 7As shown, after 3000 cycles of stability testing, the performance of the Ru@TiC electrocatalyst remained almost unchanged even in the harsh alkaline natural seawater environment, indicating that the catalyst has good catalytic activity and stability.
[0077] Example 10
[0078] The difference from Example 7 is that the electrocatalyst was tested in a 1M potassium hydroxide solution containing saturated sodium chloride, and its stability was tested by chronopotentiometry at 500 mA / cm 2 At a current density of 100 hours, the results of the hydrogen production reaction are as follows: Figure 8 As shown, it exhibits good stability, indicating that it still has good catalytic activity, stability, and excellent corrosion resistance in extremely harsh saturated sodium chloride environment.
[0079] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An electrocatalyst for producing hydrogen by electrolysis of seawater, characterized in that: The electrocatalyst uses titanium carbide nanofibers as carriers and is loaded with ruthenium nanoparticles.
2. The electrocatalyst for producing hydrogen by electrolysis of seawater according to claim 1, characterized in that: The loading amount of ruthenium nanoparticles is 0.5% to 30wt.%.
3. The method for preparing an electrocatalyst for hydrogen production by electrolysis of seawater according to any one of claims 1 to 2, characterized in that: include: (1) dissolving a carbon source and a titanium source in a solvent to form a spinning solution, preparing the solution into a nanofiber membrane by an electrospinning method, and then performing a carbon thermal reduction reaction after pre-oxidation to obtain titanium carbide nanofibers; (2) Ruthenium nanoparticles were loaded on titanium carbide nanofibers using rapid Joule thermal treatment to obtain the electrocatalyst Ru@TiC.
4. The preparation method according to claim 3, characterized in that: In step (1), the carbon source is a high molecular polymer; preferably, the high molecular polymer includes one or more of polyacrylonitrile (PAN), polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA) and polylactic acid (PLA); Or, in step (1), the titanium source includes one of tetrabutyl titanate, tetraisopropyl titanate or titanium tetrachloride; Or, in step (1), the mass ratio of the carbon source to the titanium source is 0.25 to 3:1; Or, in step (1), the solvent includes one or more of N,N-dimethylformamide, acetic acid, water, ethanol or chloroform; Alternatively, in step (1), the concentration of the titanium source in the solvent is 0.5 to 3 mg / mL.
5. The preparation method according to claim 3, characterized in that: In step (1), the process parameters of electrospinning are: the propulsion speed of the spinning solution is 0.5-2 mL / h, preferably 1 mL / h; the receiving distance is 8-30 cm, preferably 15-22 cm, and more preferably 18 cm; the voltage is 8-30 kV, preferably 14-30 kV, and more preferably 16 kV; the spinning time is 2-50 h, preferably 8-12 h, and more preferably 10 h.
6. The preparation method according to claim 3, characterized in that: In step (1), pre-oxidation is to anneal the nanofiber membrane under air or oxygen conditions at a temperature of 100-280°C, preferably 200-280°C, and more preferably 260°C; the holding time is 0.5-20h, preferably 0.5-5h, and more preferably 2h; the heating rate is 5-20°C / min.
7. The preparation method according to claim 3, characterized in that: In step (1), the carbon thermal reduction reaction is a high temperature calcination, the calcination temperature is 1400-2200° C., preferably 1400-1600° C., and more preferably 1500° C.; the calcination time is 1-12 h, preferably 1-5 h, and more preferably 2 h; the heating rate is 5-20° C. / min; Alternatively, the width of the titanium carbide nanofibers is 100 to 1000 nm.
8. The preparation method according to claim 3, characterized in that: In step (2), the method of loading ruthenium nanoparticles on titanium carbide nanofibers by rapid Joule heat treatment includes: The ruthenium salt solution was drop-coated on the titanium carbide nanofibers, which were placed in a Joule heating device to heat and obtain the electrocatalyst Ru@TiC; Preferably, the solute ruthenium salt in the ruthenium salt solution droplet includes one of ruthenium chloride or ruthenium acetylacetonate; Preferably, the solvent in the ruthenium salt solution droplets includes one of water, methanol, ethanol or N,N-dimethylformamide; Preferably, the Joule heat device is set to a heating temperature of 400 to 2200° C.; the Joule heat process can be repeated 1 to 10 times, with each heating time being 4 to 6 seconds.
9. Use of the electrocatalyst for hydrogen production by electrolysis of seawater as claimed in any one of claims 1 to 2 and / or the electrocatalyst for hydrogen production by electrolysis of seawater prepared by the preparation method according to any one of claims 3 to 8 in hydrogen production by electrolysis of seawater.
10. The use according to claim 9, characterized in that The pH value of seawater is 0-3 and / or 12-14.
Citation Information
Patent Citations
MoS2 / TiC / C composite nanometer fiber membrane and preparation method and application thereof
CN107799314A
Ruthenium-loaded monatomic water electrolysis catalytic material and preparation method thereof
CN111001425A
MXene and transition metal sulfide composite nano-catalyst based on fiber skeleton and preparation method thereof
CN112553641A
Ruthenium-cluster-loaded defect-rich nitrogen-doped carbon nanotube catalyst as well as preparation method and application of ruthenium-cluster-loaded defect-rich nitrogen-doped carbon nanotube catalyst
CN117987866A
Nb-tio_2 catalyst support and manufacturing method thereof by using electrospinning
KR1020150028529A
Cited By
Metal oxide-polytetrafluoroethylene nano composite material, preparation method and application
CN119663339A
Preparation method of alloy film loaded noble metal electrode for alkaline hydrogen evolution
CN119956400A
A method for preparing alloy thin film supported noble metal electrode for alkaline hydrogen evolution
CN119956400B
Synthesis method of iron-doped cobalt phosphide catalyst for hydrogen production by electrolysis of untreated seawater