Functionalized nano polyphenylene sulfide fiber composite polyelectrolyte membrane and preparation method thereof

Through the composite technology of chloromethylation-quaternary ammonia functionalized nanopolyphenylene sulfide fibers and hydrophilic nanoinorganic fillers, the problem of insufficient ion conduction ability and stability of the polyelectrolyte membrane in high-temperature and strong corrosion environment is solved, and high efficiency is achieved The improvement of ion conduction, mechanical strength and chemical stability are suitable for electrochemical devices such as electrolytic water and fuel cells.

CN118943441APending Publication Date: 2024-11-12DONGHUA UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410995651.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing polyelectrolyte membranes lack ion conduction ability in high temperature and strong corrosion environments, and have poor dimensional stability, making it difficult to have high ion conduction ability, mechanical strength and chemical stability.

Method used

The nanopolyphenylene sulfide fibers are combined with hydrophilic nanoinorganic fillers to build an efficient ion transport channel through the chloromethylation-quaternary ammonia functionalization reaction, and a three-dimensional network structure is constructed through the nanofibers. Improve mechanical strength and chemical stability.

Benefits of technology

It significantly improves the ion conduction ability, mechanical strength and chemical stability of the composite polyelectrolyte membrane, and is suitable for electrochemical devices in high-temperature and strong corrosion environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943441A_ABST
    Figure CN118943441A_ABST
Patent Text Reader

Abstract

The invention relates to a functionalized nano polyphenylene sulfide fiber composite polyelectrolyte membrane and a preparation method thereof.The nano polyphenylene sulfide fiber composite polyelectrolyte membrane is adopted, and the polyelectrolyte membrane has excellent mechanical strength, thermal stability and chemical stability while the efficient ion conduction capacity is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polyelectrolyte materials, and particularly relates to a functionalized nano polyphenylene sulfide fiber composite polyelectrolyte membrane and a preparation method thereof. Background Art

[0002] Polyelectrolyte membranes are a type of functional membrane with ion conductivity, which plays an important role in energy storage electrochemical devices such as water electrolysis, fuel cells, and flow batteries. In these electrochemical devices, polyelectrolyte membranes not only play an ion conductivity function, but also isolate the crossover of the anode and cathode (positive and negative) electrodes and the reactants or products at the two electrodes. Therefore, it is crucial for these electrochemical devices to have efficient ion conductivity and good stability. However, the ion conductivity of polyelectrolyte membranes depends to a certain extent on their ability to absorb electrolytes. Polyelectrolyte membranes swell when absorbing electrolytes, which greatly reduces their dimensional stability. In addition, the operating temperature and environment of these electrochemical devices are often relatively harsh. Therefore, the preparation of high-performance polyelectrolyte membranes with high ion conductivity, mechanical strength, and good chemical stability is the key to improving the performance of such electrochemical devices. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a functionalized nano-polyphenylene sulfide fiber composite polyelectrolyte membrane and a preparation method thereof, and in particular to a functionalized nano-polyphenylene sulfide fiber composite polyelectrolyte membrane that can have high-efficiency ion conduction capability under high temperature and strong corrosion environment while ensuring stability, wherein the functionalized nano-polyphenylene sulfide fiber composite polyelectrolyte membrane has the characteristics of high ionic conductivity, high strength and high temperature resistance.

[0004] The invention provides a polyelectrolyte material, characterized in that, by weight, the polyelectrolyte material components include: 5-30 parts of a polymer binder; 5-15 parts of an additive; 20-60 parts of chloromethylated-quaternary ammonium functionalized nano polyphenylene sulfide fibers; and 20-60 parts of an inorganic filler.

[0005] Preferably, the polymer binder is one or more of polysulfone, polyethersulfone, polyetheretherketone, and polyvinylidene fluoride; the additive is one or more of polyvinyl alcohol, polyvinyl pyrrolidone, and chitosan; the inorganic filler is a hydrophilic nano-inorganic filler; the hydrophilic nano-inorganic filler includes one or more of zirconium oxide, titanium oxide, aluminum oxide, cesium oxide, and silicon oxide.

[0006] Preferably, the method for preparing the chloromethylated-quaternary ammonium functionalized nano polyphenylene sulfide fiber comprises:

[0007] Swelling the nano-polyphenylene sulfide fiber in 1,2-dichloroethane to obtain swollen nano-polyphenylene sulfide fiber;

[0008] The swollen nano-polyphenylene sulfide fibers, chloromethyl ether and a catalyst are mixed, stirred evenly, and then the solution is heated to perform a chloromethylation reaction, and then washed and dried to obtain chloromethylated nano-polyphenylene sulfide fibers;

[0009] The chloromethylated nano-polyphenylene sulfide fiber is swollen in 1,2-dichloroethane, and a trimethylamine solution is added after swelling. After stirring evenly, the temperature is raised to carry out a quaternization reaction, and the chloromethylated-quaternary ammonium functionalized nano-polyphenylene sulfide fiber is obtained after washing and drying.

[0010] Preferably, the nano polyphenylene sulfide fiber has a diameter of 200-800 nm and a length of 1-1000 μm;

[0011] More preferably, the diameter of the nano-polyphenylene sulfide fiber is 200-700 nm.

[0012] The preparation method of the nano polyphenylene sulfide fiber comprises:

[0013] According to the weight proportion of polyphenylene sulfide being 30-80wt%, polyphenylene sulfide and alkali-soluble polyester are uniformly mixed, and then extruded and granulated by a twin-screw extruder to obtain polyphenylene sulfide / alkali-soluble polyester blended masterbatch; wherein the average particle size of the alkali-soluble polyester is 1-5mm; the average particle size of the polyphenylene sulfide is 50-1000μm; the blending and granulation temperature is 245-275℃;

[0014] The polyphenylene sulfide / alkali-soluble polyester blend masterbatch is mixed with the alkali-soluble polyester according to the mass ratio of polyphenylene sulfide of 10-40wt%, and the polyphenylene sulfide / alkali-soluble polyester blend fiber is obtained after spinning, drawing and heat setting by a melt spinning machine; the polyphenylene sulfide / alkali-soluble polyester blend fiber is dissolved in alkali solution, and the alkali-soluble polyester is removed to obtain a nano polyphenylene sulfide fiber.

[0015] Preferably, the catalyst is anhydrous tin tetrachloride; the catalyst is used in excess; the chloromethyl ether is used in excess; and the trimethylamine solution is used in excess.

[0016] Preferably, the swelling time of the nano-polyphenylene sulfide fiber in 1,2-dichloroethane is 8-12 hours; the chloromethylation reaction temperature is 50-80° C., and the reaction time is 10-15 hours.

[0017] Further preferably, the chloromethylation reaction temperature is 50-60° C., and the reaction time is 13-15 h.

[0018] Preferably, the chloromethylated nano-polyphenylene sulfide fiber is swollen in 1,2-dichloroethane for 8-12 hours; the quaternization reaction temperature is 30-50° C., and the reaction time is 8-12 hours.

[0019] More preferably, the quaternization reaction temperature is 30-40° C., and the reaction time is 10-12 h.

[0020] The present invention provides a method for preparing a polyelectrolyte material, comprising:

[0021] (1) mixing a polymer binder, an additive, and an organic solvent to obtain a mixed solution;

[0022] (2) mixing chloromethylated-quaternary ammonium functionalized nano-polyphenylene sulfide fibers, inorganic fillers, and a polymer binder solution to obtain a slurry;

[0023] (3) The slurry is scraped into a film, pre-evaporated, and then placed in a coagulation bath for phase transformation into a membrane to obtain a nano-polyphenylene sulfide fiber composite polyelectrolyte membrane material.

[0024] Preferably, in the mixed solution in step (1), the mass fraction of the polymer binder is 5-30wt%, and the mass fraction of the additive is 1-15wt%; the organic solvent is one or more of N-methylpyrrolidone, dimethyl sulfoxide, and N,N-dimethylformamide.

[0025] Further preferably, the mass fraction of the polymer binder in the mixed solution is 10-25wt%.

[0026] The pre-evaporation is carried out in a forced air oven to form a wet film.

[0027] Preferably, in step (3), the pre-evaporation temperature is 60-90° C. and the time is 1-10 min.

[0028] More preferably, the pre-evaporation temperature is 70-80° C. and the time is 1-5 min.

[0029] Step (3) placing the uniformly mixed slurry on a glass plate, using a scraper to scrape it into a film, placing the scraped wet film in a blast oven for pre-evaporation, and then placing it in a coagulation bath for phase transformation into a film.

[0030] Preferably, the coagulation bath in step (3) is water, ethanol or a water / ethanol mixture.

[0031] More preferably, the coagulation bath is a 75 wt % ethanol aqueous solution.

[0032] The present invention provides an application of the polyelectrolyte material in the field of energy storage, such as water electrolysis, fuel cells, and liquid flow batteries.

[0033] The present invention constructs an efficient ion transmission channel on the surface of nano polyphenylene sulfide fiber through chloromethylation-quaternary ammonia functionalization reaction, which greatly enhances the ion conduction capacity of the composite polyelectrolyte material. At the same time, by adding hydrophilic nano inorganic fillers, the interface contact capacity between the surface and interior of the polyelectrolyte material and the electrolyte is improved, which helps the ions in the electrolyte to reach the surface of the chloromethylation-quaternary ammonia functionalized nano polyphenylene sulfide fiber faster, thereby achieving rapid ion conduction. In addition, the nanofiber constructs a three-dimensional network structure, which significantly improves the mechanical strength, thermal stability and chemical stability of the composite polyelectrolyte material. The functionalized nano polyphenylene sulfide fiber composite polyelectrolyte membrane prepared by this preparation method can be applied to electrochemical energy storage fields such as water electrolysis, fuel cells, and flow batteries.

[0034] Beneficial Effects

[0035] (1) The chloromethylated-quaternary ammonium functionalized polyphenylene sulfide fiber used in the polyelectrolyte membrane of the present invention significantly improves the ion conductivity.

[0036] (2) The present invention uses hydrophilic inorganic nanoparticles as fillers to enhance the interfacial contact ability between the polyelectrolyte membrane and the electrolyte while helping the ions in the electrolyte to quickly reach the surface of the chloromethylated-quaternary ammonium functionalized polyphenylene sulfide fiber, thereby achieving rapid ion transmission.

[0037] (2) The present invention adopts nano-polyphenylene sulfide fiber composite polyelectrolyte membrane, which not only ensures efficient ion conduction capability, but also has excellent mechanical strength, thermal stability and chemical stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 Schematic diagram of the chloromethylation-quaternary ammonia functionalization reaction of nano-polyphenylene sulfide fiber;

[0039] Figure 2 This is a physical picture of the functionalized nano-polyphenylene sulfide fiber composite polyelectrolyte membrane. DETAILED DESCRIPTION

[0040] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0041] The test methods for various properties of composite polyelectrolyte membrane are as follows:

[0042] Thickness: Refer to the film thickness test standard GB / T6672-2001 "Mechanical measurement method for the determination of thickness of plastic films and sheets", and use a microcomputer thickness tester (FFiber-Thick02) for testing, where the test pressure is 50kPa, and repeat the test for 5 groups to take the average value.

[0043] Ionic conductivity: The sample was cut into discs with a diameter of 1 cm, soaked in a 30wt% KOH solution for 12 hours, and sandwiched in the middle of an H-type electrolytic cell filled with a 30wt% KOH solution. A platinum electrode was placed on each side as anode and cathode, and the cross-linked electrochemical impedance spectrum was tested at 10kHz-0.1Hz by an electrochemical workstation. The calculation formula for ionic conductivity is as follows:

[0044] σ=L / RA

[0045] Where σ(mS cm -1 ) is the ionic conductivity, L (cm) is the membrane thickness, R (Ω) is the membrane resistance, A (cm 2 ) is the effective area of ​​the membrane.

[0046] Tensile strength: Tested using a material tensile strength tester (FFiber-tensile01). Cut the sample into 5cm long and 1cm wide strips in the same direction, with a sample holding length of 30mm and a tensile speed of 20mm / min. Test 5 groups and take the average value.

[0047] Thermal stability: The membrane was cut into circular pieces with a diameter of 1 cm and placed in a 100°C hot plate for 30 min to measure its dimensional change.

[0048] Example 1

[0049] A method for preparing a functionalized nano-polyphenylene sulfide fiber composite polyelectrolyte membrane comprises the following steps:

[0050] (1) Preparation of Nano-polyphenylene sulfide Fibers:

[0051] The polyphenylene sulfide powder with an average particle size of 300 μm and the alkali-soluble polyester particles with an average particle size of 2 mm were uniformly mixed in a ratio of 50 wt% of the polyphenylene sulfide mass, and then extruded and granulated at 250° C. using a twin-screw extruder to obtain a polyphenylene sulfide / alkali-soluble polyester blended masterbatch;

[0052] The polyphenylene sulfide / alkali-soluble polyester blend masterbatch and the alkali-soluble polyester particles with an average particle size of 2 mm were mixed in a ratio of 10 wt% of the polyphenylene sulfide mass ratio, and then spun, stretched and heat-set at 310° C. using a melt spinning machine to obtain polyphenylene sulfide / alkali-soluble polyester blended fibers;

[0053] After polyphenylene sulfide / alkali-soluble polyester blended fibers are dissolved in alkali solution, the alkali-soluble polyester is removed to obtain nano polyphenylene sulfide fibers. The prepared nano polyphenylene sulfide fibers have an average diameter of 300 nm and a length of 1-100 μm.

[0054] (2) Chloromethylation-quaternary ammonia functionalization of nano-polyphenylene sulfide fibers:

[0055] The nano-polyphenylene sulfide fiber is placed in 1,2-dichloroethane to swell for 12 hours, and then an excess of chloromethyl ether and anhydrous tin tetrachloride catalyst are added after swelling. After stirring evenly, the solution is heated to 50°C for chloromethylation reaction for 13 hours. After the reaction is completed, the chloromethylated nano-polyphenylene sulfide fiber is obtained by washing and drying.

[0056] The chloromethylated nano-polyphenylene sulfide fiber was placed in 1,2-dichloroethane to swell for 12 hours, and then an excess trimethylamine solution was added after swelling, and the mixture was stirred evenly and heated to 30°C for reaction for 10 hours. After the reaction was completed, the chloromethylated-quaternary ammonium functionalized nano-polyphenylene sulfide fiber was obtained by washing and drying.

[0057] (3) Preparation of functionalized nano-polyphenylene sulfide fiber composite polyelectrolyte membrane:

[0058] 15wt% polysulfone and 5wt% polyvinyl pyrrolidone are dissolved in N-methylpyrrolidone to prepare a polymer binder solution. In terms of mass fractions, 15 parts of polysulfone, 5 parts of polyvinyl pyrrolidone, 40 parts of chloromethylated-quaternary ammonium functionalized nano polyphenylene sulfide fibers and 40 parts of nano zirconium oxide powder are mixed evenly with the polymer binder solution according to this mass ratio. The mixed slurry is placed on a glass plate and scraped into a film using a scraper. The scraped wet film is placed in an 80℃ forced air oven for pre-evaporation for 1 minute, and then placed in a 75wt% ethanol aqueous solution for phase transformation to obtain a functionalized nano polyphenylene sulfide fiber composite polyelectrolyte membrane sample A1.

[0059] Example 2

[0060] The preparation method of this embodiment is the same as that of embodiment 1, except that: in step (1), the polyphenylene sulfide / alkali-soluble polyester blend masterbatch and the alkali-soluble polyester are melt-blended and spun at a ratio of 20wt% of polyphenylene sulfide mass ratio. The prepared nano polyphenylene sulfide fiber has an average diameter of 500nm and a length of 10-500μm. The final sample is recorded as A2.

[0061] Example 3

[0062] The preparation method of this embodiment is the same as that of embodiment 1, except that: in step (1), the polyphenylene sulfide / alkali-soluble polyester blend masterbatch and the alkali-soluble polyester are melt-blended and spun at a ratio of 30wt% of polyphenylene sulfide mass ratio. The prepared nano polyphenylene sulfide fiber has an average diameter of 700nm and a length of 50-1000μm. The final sample is recorded as A3.

[0063] Example 4

[0064] The preparation method of this embodiment is the same as that of embodiment 1, except that the reaction time of chloromethylation in step (2) is 15 h, and the reaction time of quaternization is 12 h. The final sample is recorded as B1.

[0065] Example 5

[0066] The preparation method of this embodiment is the same as that of embodiment 1, except that the chloromethylation reaction temperature in step (2) is 60° C. and the quaternization reaction temperature is 40° C. The final sample obtained is denoted as B2.

[0067] Example 6

[0068] The preparation method of this embodiment is the same as that of embodiment 1, except that the pre-evaporation time in step (3) is 3 minutes. The final sample is recorded as C1.

[0069] Example 7

[0070] The preparation method of this embodiment is the same as that of embodiment 1, except that the pre-evaporation time in step (3) is 5 minutes. The final sample obtained is recorded as C2.

[0071] Comparative Example 1

[0072] The preparation method of the composite polyelectrolyte membrane in this comparative case is the same as that in Example 1, except that the nano-polyphenylene sulfide fiber is not subjected to chloromethylation-quaternary ammonia functionalization reaction, and the composite polyelectrolyte membrane is directly prepared. The final sample is recorded as D1

[0073] Comparative Example 2

[0074] The preparation method of the composite polyelectrolyte membrane in this comparative case is the same as that in Example 1, except that no nano-polyphenylene sulfide fiber is added to the composite polyelectrolyte membrane, and the components of the composite polyelectrolyte membrane are 15 parts of polysulfone, 5 parts of polyvinyl pyrrolidone and 80 parts of nano-zirconia powder in terms of mass fractions. The final sample is recorded as D2

[0075] Comparative Example 3

[0076] The preparation method of the composite polyelectrolyte membrane in this comparative case is the same as that in Example 1, except that no nano zirconium oxide powder is added to the composite polyelectrolyte membrane, and the components of the composite polyelectrolyte membrane are 15 parts of polysulfone, 5 parts of polyvinyl pyrrolidone and 90 parts of chloromethylated-quaternary amino functionalized nano polyphenylene sulfide fibers, respectively, in terms of mass fractions. The final sample is recorded as D3

[0077] Table 1. Performance test results of composite polyelectrolyte membranes prepared by implementation examples and comparative examples

[0078]

[0079] It can be seen from Table 1 that the composite polyelectrolyte membrane made of a smaller nano polyphenylene sulfide fiber diameter has a higher ionic conductivity, which is mainly due to a larger specific surface area, but it also leads to a decrease in strength. The increase in temperature during the chloromethylation-quaternary ammonia functionalization reaction can increase the ionic conductivity of the composite polyelectrolyte membrane more than the extension of the reaction time, but the chloromethylation-quaternary ammonia functionalization reaction reduces the strength of the nano polyphenylene sulfide fiber to a certain extent. Pre-evaporation has little effect on the ionic conductivity of the composite polyelectrolyte membrane because it mainly affects the phase transition process of the polymer binder. From the comparative example, it can be seen that the ion channels on the surface of the chloromethylation-quaternary ammonia functionalized nano polyphenylene sulfide fiber can greatly improve the ionic conductivity of the polyelectrolyte membrane, and the addition of hydrophilic inorganic fillers can further enhance the ion transmission capacity of the composite polyelectrolyte membrane. The effect brought by the chloromethylation-quaternary ammonia functionalized nano polyphenylene sulfide fiber or the hydrophilic inorganic filler alone is far less than the high ionic conductivity under the interaction of the two. The differences in fiber diameter and process parameters in the embodiments and comparative examples lead to slight differences in the thickness of the polyelectrolyte membranes. However, such differences have little effect on the performance of the polyelectrolyte membranes and can be ignored.

Claims

1. A polyelectrolyte material, characterized in that: In parts by weight, the polyelectrolyte material components include: 5-30 parts of polymer binder; 5-15 parts of additives; 20-60 parts of chloromethylated-quaternary ammonium functionalized nano polyphenylene sulfide fibers; and 20-60 parts of inorganic fillers.

2. The polyelectrolyte material according to claim 1, characterized in that: The polymer binder is one or more of polysulfone, polyethersulfone, polyetheretherketone, and polyvinylidene fluoride; the additive is one or more of polyvinyl alcohol, polyvinyl pyrrolidone, and chitosan; the inorganic filler is a hydrophilic nano inorganic filler; wherein the hydrophilic nano inorganic filler includes one or more of zirconium oxide, titanium oxide, aluminum oxide, cesium oxide, and silicon oxide.

3. The polyelectrolyte material according to claim 1, characterized in that: The preparation method of the chloromethylated-quaternary ammonium functionalized nano polyphenylene sulfide fiber comprises: Swelling the nano-polyphenylene sulfide fiber in 1,2-dichloroethane to obtain swollen nano-polyphenylene sulfide fiber; The swollen nano-polyphenylene sulfide fibers, chloromethyl ether and a catalyst are mixed to carry out a chloromethylation reaction, and the chloromethylated nano-polyphenylene sulfide fibers are obtained after washing and drying; The chloromethylated nano-polyphenylene sulfide fiber is swollen in 1,2-dichloroethane, then subjected to quaternary amination reaction with a trimethylamine solution, and washed and dried to obtain the chloromethylated-quaternary ammonia functionalized nano-polyphenylene sulfide fiber.

4. The preparation method according to claim 3, characterized in that: The nano polyphenylene sulfide fiber has an average diameter of 200-800nm ​​and a length of 1-1000μm; the catalyst is anhydrous tin tetrachloride; the amount of chloromethyl ether is excessive; and the amount of trimethylamine solution is excessive.

5. The preparation method according to claim 3, characterized in that: The swelling time of the nano polyphenylene sulfide fiber in 1,2-dichloroethane is 8-12 hours; the chloromethylation reaction temperature is 50-80° C., and the reaction time is 10-15 hours.

6. The preparation method according to claim 3, characterized in that: The chloromethylated nano polyphenylene sulfide fiber is swollen in 1,2-dichloroethane for 8-12 hours; the quaternization reaction temperature is 30-50° C., and the reaction time is 8-12 hours.

7. A method for preparing a polyelectrolyte material, comprising: (1) mixing a polymer binder, an additive, and an organic solvent to obtain a mixed solution; (2) mixing chloromethylated-quaternary ammonium functionalized nano-polyphenylene sulfide fibers, inorganic fillers, and a polymer binder solution to obtain a slurry; (3) The slurry is scraped into a film, pre-evaporated, and then placed in a coagulation bath to obtain a polyelectrolyte material.

8. The preparation method according to claim 7, characterized in that: In the step (1), the mass fraction of the polymer binder in the mixed solution is 5-30wt%, and the mass fraction of the additive is 1-15wt%; the organic solvent is one or more of N-methylpyrrolidone, dimethyl sulfoxide, and N,N-dimethylformamide.

9. The preparation method according to claim 7, characterized in that: In the step (3), the pre-evaporation temperature is 60-90° C. and the time is 1-10 min; the coagulation bath is water, ethanol or a water / ethanol mixture.

10. Use of the polyelectrolyte material according to claim 1 in the field of energy storage.