Wide-temperature-range high-safety lithium ion soft package battery and preparation method thereof

By using ternary positive electrodes coated with lithium manganese iron phosphate, silicon-carbon-medium-phase carbon microsphere composite negative electrodes and polyimide nanofiber separators in lithium-ion soft-pack batteries, the existing batteries have been solved in high capacity and wide range. The shortcomings in the temperature domain and high safety have achieved the improvement of high energy density, long cycle life and safety performance.

CN118943464APending Publication Date: 2024-11-12WUHAN UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411005887.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing lithium-ion soft-pack batteries have shortcomings in high capacity, wide temperature range and high safety, which are difficult to meet application needs.

Method used

A ternary material coated with lithium manganese iron phosphate is used as the positive electrode, and a silicon-carbon-medium-phase carbon microsphere composite material is used as the negative electrode, and a polyimide nanofiber separator is combined to improve the energy density, cycle stability and safety performance of the battery.

Benefits of technology

It significantly improves the capacity, circulation performance and safety of lithium-ion batteries, can maintain excellent electrochemical performance under high and low temperature conditions, and avoid explosion and fire during needle puncture, extending service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943464A_ABST
    Figure CN118943464A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium ion batteries, and relates to a wide-temperature-range high-safety lithium ion soft package battery and a preparation method, a soft package battery cell comprises a positive electrode, a negative electrode and a diaphragm between the positive electrode and the negative electrode, and the material of the positive electrode comprises a lithium manganese iron phosphate coated ternary material; the material of the negative electrode comprises a silicon carbon-mesophase carbon microsphere composite material; and the diaphragm is a polyimide nanofiber diaphragm. According to the wide-temperature-range high-safety lithium ion soft package battery, a silicon carbon-mesophase carbon microsphere composite material is adopted as a negative electrode, a lithium manganese iron phosphate coated ternary positive electrode is adopted as a positive electrode material, and polyimide nanofibers are adopted as a diaphragm. According to the present invention, the battery cell has characteristics of good safety and high stability, does not easily produce combustion or explosion and other dangerous conditions, can give consideration to the electrical performance, and improves the capacity, the charge-discharge rate, the long cycle performance and the wide temperature range performance of the lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium-ion batteries, and in particular relates to a wide-temperature range high-safety lithium-ion soft-pack battery and a preparation method thereof. Background Art

[0002] Lithium-ion batteries are important energy storage devices that are currently widely used in portable electronic devices, electric vehicles, energy storage systems and other fields. Among them, the negative electrode material plays a vital role in battery performance and cycle life. In order to improve the energy density, cycle stability and charge and discharge rate of lithium-ion batteries, researchers have been committed to developing high-capacity and high-rate negative electrode slurries. The material system of existing soft-pack batteries: lithium cobalt oxide + graphite; nickel cobalt lithium manganese oxide + graphite; lithium manganese oxide + graphite, etc., is difficult to meet the application requirements of high capacity, wide temperature range and high safety. Therefore, it is necessary to develop a wide temperature range and high safety lithium-ion soft-pack battery. Summary of the invention

[0003] In view of the deficiencies of the above-mentioned prior art, the present invention provides a wide temperature range high-safety lithium-ion soft-pack battery and a preparation method thereof. The specific technical scheme is as follows:

[0004] The first object of the present invention is to provide a lithium-ion soft-pack battery with a wide temperature range and high safety, wherein the battery cell comprises a positive electrode, a negative electrode and a separator between the positive electrode and the negative electrode.

[0005] The material of the positive electrode includes a ternary material coated with lithium manganese iron phosphate;

[0006] The material of the negative electrode includes a silicon-carbon-mesophase carbon microsphere composite material;

[0007] The membrane is a polyimide nanofiber membrane.

[0008] The present invention uses a silicon-carbon-mesophase carbon microsphere composite material as the negative electrode to improve the capacity and long cycle performance of the lithium-ion battery. The present invention uses a ternary positive electrode coated with lithium iron manganese phosphate as the positive electrode material. Due to the addition of lithium iron manganese phosphate, it has higher stability at extremely low temperatures. The use of a ternary positive electrode coated with lithium iron manganese phosphate as a positive electrode material not only has a high energy density but also improves safety performance. The present invention uses a polyimide (PI) nanofiber diaphragm to increase the charge and discharge rate of the battery; the PI diaphragm can withstand high temperatures above 250 degrees Celsius. When the diaphragm is pierced, the local overheating caused by the micro-short circuit or small-area short circuit of the battery will not melt the PI diaphragm and cause the perforation area to continue to expand, that is, it will not cause the short circuit area to continue to expand, causing thermal runaway and causing the battery to explode and catch fire. The battery of the present invention using the above-mentioned battery core material has significantly improved safety during acupuncture, while taking into account the electrochemical energy storage performance.

[0009] Furthermore, the silicon-carbon-mesophase carbon microsphere composite material is porous silicon filled with mesophase carbon microspheres coated with hard carbon.

[0010] The present invention adopts porous silicon filled with hard carbon-coated mesophase carbon microspheres as the negative electrode of the lithium-ion battery. During the cycle, the mesophase carbon microspheres can alleviate the volume expansion of the silicon negative electrode, and the hard carbon outer coating layer can reduce the side reaction between the silicon negative electrode and the electrolyte and form a stable solid electrolyte interface layer, which significantly improves the performance of the porous silicon negative electrode material, thereby improving the capacity and long cycle performance of the lithium-ion battery. Under high and low temperature conditions, silicon and hard carbon can provide excellent high and low temperature electrochemical performance, thereby improving the wide temperature range performance of the lithium-ion battery.

[0011] Furthermore, the method for preparing the negative electrode sheet comprises the following steps:

[0012] Step A1: Sodium carboxymethyl cellulose and deionized water are sol-formed, wherein the mass ratio of the sodium carboxymethyl cellulose to the deionized water is 3:(95-100), and the sol-formed solution is prepared by high-speed stirring for 1-3 hours, and the stirring speed is 30 RPM for revolution and 1300 RPM for rotation;

[0013] Step A2: Add the conductive agent to the prepared glue solution 1, and stir at high speed for 1 to 2 hours to prepare glue solution 2, with the stirring speed being 35 RPM for revolution and 3500 RPM for rotation;

[0014] Step A3: adding a silicon-carbon-mesophase carbon microsphere composite material and graphite in a mass ratio of (20-30):75 to the above-mentioned glue solution 2, and stirring under vacuum for 2-3 hours, with a vacuum degree of -85 KPa, and a stirring speed of 42 RPM for revolution and 4500 RPM for rotation, to obtain a first mixture;

[0015] Step A4: adding the water-based adhesive to the first mixture, and slowly stirring for 0.5 to 1 hour to obtain a second mixture, wherein the stirring speed is 30 RPM for revolution and 1300 RPM for rotation;

[0016] Step A5: testing and adjusting the viscosity of the second mixture by a viscometer, the viscosity range is 1500-5000 MPa.S, and then filtering through a 200-mesh sieve to obtain a negative electrode slurry;

[0017] Step A6: After the electrode slurry is evenly coated on the surface of the 6 μm copper foil by a coating device, the coating thickness is 130-150 μm, and then dried to form an electrode sheet;

[0018] Step A7: rolling and slitting the electrode sheet to a thickness of 90 to 110 μm and a width of 72 to 73 mm to obtain a negative electrode sheet;

[0019] Furthermore, the conductive agent includes SuperP-Li, Ketjen black, CNT, conductive carbon black and the like.

[0020] Furthermore, the water-based adhesive is a mixed solution of styrene butadiene (SBR) emulsion and water-based polyacrylate (PAA) emulsion, and the mass ratio of the water-based adhesive to the styrene butadiene (SBR) emulsion and the water-based polyacrylate (PAA) emulsion is 1:1.

[0021] Furthermore, the method for preparing the positive electrode sheet comprises the following steps:

[0022] Step B1: mixing a ternary positive electrode material coated with lithium manganese iron phosphate and an oily binder polyvinylidene fluoride (PVDF) in a mass ratio of (93-99):2 to obtain a positive electrode slurry;

[0023] Step B2: coating the positive electrode slurry on the surface of the aluminum foil, rolling and slicing to obtain a positive electrode sheet with a coating thickness of 120 to 150 μm, a rolling thickness of 90 to 120 μm, and a slicing width of 69 to 70 mm.

[0024] The second object of the present invention is to provide a method for preparing the above-mentioned wide temperature range high-safety lithium-ion soft-pack battery, the preparation steps of which are:

[0025] Step C1: Winding the positive electrode sheet, the negative electrode sheet and the polyimide nanofiber separator into a battery core, and covering the core with a finishing glue;

[0026] Step C2: welding the positive electrode sheet and the negative electrode sheet to the tabs, the length of the welding end of the tab welding is 12 to 20 mm, and the thickness of the toe glue of the tab welding is 16 to 30 μm;

[0027] Step C3: Assemble with the aluminum-plastic film with pre-punched holes, and perform top sealing and side sealing to form a non-liquid-injected soft-pack battery cell;

[0028] Step C4: injecting electrolyte into the unliquid-injected soft-pack battery cell to form a liquid-injected soft-pack battery cell;

[0029] Step C5: placing the liquid-injected soft-pack battery cell at rest until the electrolyte is fully infiltrated, forming the battery cell, and then exhausting and sealing the formed battery cell to form a soft-pack battery cell;

[0030] Step C6: Perform the formation process.

[0031] The formation process adopts a constant power charging method to make the whole battery in a high current state when the charging acceptance capacity is high, and in a relatively low current state when the charging acceptance capacity is low, thereby improving the current utilization rate and the initial charging and discharging efficiency of the battery.

[0032] Furthermore, the formation process includes an activation constant current stage, a low voltage constant current charging stage and a constant voltage charging stage;

[0033] The activation constant current stage is used to detect whether the battery status is normal and preliminarily activate the battery to charge 0.02C to 3.0V;

[0034] The low-voltage constant-current charging stage is used to open and enrich the lithium ion channels in the electrodes and diaphragms, so as to facilitate the subsequent rapid formation of 0.05C charging to a battery terminal voltage of 3.45 to 3.65V;

[0035] The constant voltage charging stage is used to promote the conversion of active substances in the deep layer of the electrode. The battery formation is completed when the constant voltage of 4.0V reaches 0.1C.

[0036] The beneficial effects of the present invention are:

[0037] The present invention adopts a silicon-carbon-mesophase carbon microsphere composite material as the negative electrode, a lithium manganese iron phosphate-coated ternary positive electrode as the positive electrode material, and polyimide nanofibers as a separator. The battery exhibits excellent safety, wide temperature range characteristics and long cycle life. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a charge and discharge curve diagram of the soft-pack battery prepared in Example 1 of the present invention at a super-large current density at -50 degrees Celsius;

[0039] Figure 2 This is a long cycle performance diagram of the soft-pack battery prepared in Example 1 of the present invention at a super-large current density at -50 degrees Celsius. DETAILED DESCRIPTION

[0040] The principles and features of the present invention are described below in conjunction with examples. The examples are only used to explain the present invention and are not used to limit the scope of the present invention.

[0041] Embodiment 1:

[0042] A method for preparing a wide temperature range high-safety lithium-ion soft-pack battery comprises the following steps:

[0043] 1. Preparation of negative electrode:

[0044] Step A1: Sodium carboxymethyl cellulose and deionized water in a mass ratio of 3:97 are solned and stirred at high speed for 2 hours to prepare a colloid solution 1, with a stirring speed of revolution 30 RPM and rotation 1300 RPM;

[0045] Step A2: Add the conductive agent conductive carbon black to the above-prepared glue solution 1, and stir at high speed for 2 hours to prepare glue solution 2, with the stirring speed: revolution 35RPM, rotation 3500RPM;

[0046] Step A3: adding silicon-carbon-mesophase carbon microsphere composite material and graphite in a mass ratio of 25:75 to the above-mentioned glue solution 2, and stirring under vacuum (vacuum degree -85Kpa), stirring speed for 3 hours: revolution 42RPM, rotation 4500RPM, to obtain a first mixture;

[0047] Step A4: adding an aqueous binder (accounting for 2% of the total solid matter) to the above-mentioned first mixture, and slowly stirring for 1 hour to obtain a second mixture, the stirring speed: revolution 30RPM, rotation 1300RPM; the aqueous binder is a mixed solution of styrene butadiene (SBR) emulsion and aqueous polyacrylate (PAA) emulsion, and the mass ratio of the aqueous binder to the aqueous polyacrylate (PAA) emulsion is 1:1.

[0048] Step A5: testing and adjusting the viscosity of the second mixture by a viscometer, the viscosity range is 1500-5000 MPaS, and then filtering through a 200-mesh sieve to obtain a negative electrode slurry;

[0049] Step A6: After the electrode slurry is evenly coated on the surface of the 6μmPET composite copper foil through a coating device, the coating thickness is 130-150μm, and then dried to form an electrode sheet;

[0050] Step A7: Roll and slice the electrode sheet to obtain a negative electrode sheet with a rolling thickness of 90 to 110 μm and a electrode sheet width of 72 to 73 mm.

[0051] 2. Preparation of positive electrode:

[0052] Step B1: mixing the lithium manganese iron phosphate coated ternary positive electrode material and the oily binder (polyvinylidene fluoride PVDF) to obtain a positive electrode slurry;

[0053] Step B2: Coat the positive electrode slurry on the surface of 10μm PET composite aluminum foil, roll and slice to obtain positive electrode sheets with a coating thickness of 120-150μm, a rolling thickness of 90-120μm, and a slice width of 69-70mm.

[0054] 3. Preparation of soft pack batteries:

[0055] Step C1: Winding the positive electrode sheet, the negative electrode sheet and the polyimide nanofiber separator into a battery core, and covering the core with a finishing glue;

[0056] Step C2: performing tab welding on the positive electrode sheet and the negative electrode sheet, wherein the length of the welding end of the tab welding is 15 mm, and the thickness of the toe glue of the tab welding is 20 μm;

[0057] Step C3: Assemble with the aluminum-plastic film with pre-punched holes, and perform top sealing and side sealing to form a non-liquid-injected soft-pack battery cell;

[0058] Battery tray: The thickness of the aluminum-plastic film is 150μm. The battery tray is punched on one side. There is no side at the bottom of the battery, and it is pressed to form a pit with one side open. The battery tray is divided into a tray body area and an air bag area. The tray body area is used to place the battery cell, and the air bag area is used to contain the gas generated during the battery formation process.

[0059] Battery cover: It adopts aluminum-plastic film with the same specifications and materials as the battery slot. The battery cover is a flat structure, and the size of the battery cover is the same as the flat projection size of the battery slot.

[0060] Step C4: injecting a set amount (2.5 g / Ah) of electrolyte (main components are 1.15 M LiPF6, PS, FEC, EC, PC, DMC, DEC) into the uninjected soft-pack battery cell to form an injected soft-pack battery cell;

[0061] Step C5: placing the liquid-injected soft-pack battery cell at rest until the electrolyte is fully infiltrated, forming the battery cell, and then exhausting and sealing the formed battery cell to form a soft-pack battery cell;

[0062] Step C6: performing a formation process, wherein the formation process includes an activation constant current stage, a low voltage constant current charging stage, and a constant voltage charging stage;

[0063] The activation constant current stage is used to detect whether the battery status is normal and preliminarily activate the battery to charge 0.02C to 3.0V;

[0064] The low-voltage constant-current charging stage is used to open and enrich the lithium ion channels in the electrodes and diaphragms, so as to facilitate the subsequent rapid formation of 0.05C charging to a battery terminal voltage of 3.45 to 3.65V;

[0065] The constant voltage charging stage is used to promote the conversion of active substances in the deep layer of the electrode. The battery formation is completed when the constant voltage of 4.0V reaches 0.1C.

[0066] Testing Procedure:

[0067] Capacity division process: charge at 0.25C to 4.2V, let stand for 5 minutes, then discharge at 0.25C to 2.75V. After capacity division, the battery can achieve a capacity retention rate greater than or equal to 80% after 2000 cycles at 1C current.

[0068] Low temperature discharge process: charge at room temperature 1C to 4.2V (at -50 to 50 degrees Celsius), leave for 16 hours and then discharge (1 to 3C) to 2.5V.

[0069] Low-temperature charge and discharge cycle process: After being placed at a low temperature of -50 degrees Celsius for 16 hours, charge to 4.2V at 0.1C, place for 5 minutes, and then discharge to 2.5V at 0.5C. After 1000 cycles, the capacity retention rate is greater than or equal to 80%.

[0070] Figure 1 The charge and discharge curve of the soft-pack battery prepared in this embodiment at a super-large current density at -50 degrees Celsius; Figure 1 As shown, the soft-pack battery prepared in this embodiment can charge and discharge normally at a super-large current density at -50 degrees Celsius, and works normally at low temperature.

[0071] Figure 2 This is a long cycle performance diagram of the soft pack battery prepared in this embodiment at a super-large current density at -50 degrees Celsius; Figure 2 As shown, after the soft-pack battery prepared in this embodiment is cycled 1000 times at -50 degrees Celsius, the capacity retention rate is still greater than 80%, and the low-temperature long-cycle working performance is excellent.

[0072] The puncture test of the soft-pack battery prepared in Example 1 of the present invention shows that the temperature rises extremely low, there is no smoke, and there is no explosion after puncture. The maximum temperature of the battery cell surface is 53 degrees Celsius, and the voltage can still be maintained for 8 to 10 hours before dropping below 2.0V.

[0073] This embodiment prepares a wide temperature range high-safety lithium-ion soft-pack battery, using porous silicon filled with mesophase carbon microspheres coated with hard carbon as the negative electrode material, and combined with other ingredients such as aqueous adhesives, it can improve the compatibility of the electrolyte and the negative electrode material, further improve the performance of the battery, and effectively improve the discharge capacity of the battery; during the cycle, the mesophase carbon microspheres can alleviate the volume expansion of the silicon negative electrode, and the hard carbon outer coating can reduce the side reactions between the silicon negative electrode and the electrolyte and form a stable solid electrolyte interface layer. The performance of the porous silicon negative electrode material is significantly improved, thereby improving the capacity and long cycle performance of the lithium-ion battery. Under high and low temperature conditions, silicon and hard carbon can provide excellent high and low temperature electrochemical properties, thereby improving the wide temperature range performance of lithium-ion batteries.

[0074] Ternary positive electrode and lithium iron manganese phosphate are used as positive electrode materials. Due to the addition of lithium iron manganese phosphate, the capacity retention rate of lithium iron manganese phosphate can reach about 75% at extremely low temperatures. The lithium iron manganese phosphate battery is the same as the traditional lithium iron phosphate battery in structure, and the composition of the positive electrode material is also similar. Therefore, it also has higher stability and is not prone to dangerous situations such as combustion or explosion, thereby improving safety performance. That is, the ternary positive electrode coated with lithium iron manganese phosphate as the positive electrode material not only has high energy density but also improves safety performance.

[0075] The use of polyimide nanofiber diaphragm can increase the charge and discharge rate of the battery; it has a long service life and improves the cycle life; it has low heat generation and good safety. The PI diaphragm can withstand high temperatures above 250 degrees Celsius. When the diaphragm is pierced, the local overheating caused by the micro-short circuit or small area short circuit of the battery will not melt the PI diaphragm and cause the perforation area to continue to expand, that is, it will not cause the short circuit area to continue to expand and the temperature will not be out of control, causing the battery to explode and catch fire.

[0076] The test results show that the combination of the three ensures that the battery has high and low temperature electrochemical and safety performance, and the safety is significantly improved during needle puncture, while taking into account the electrical performance and meeting the application requirements of soft-pack batteries.

[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A wide temperature range high safety lithium ion soft pack battery, characterized in that: The invention comprises a battery cell, wherein the battery cell comprises a positive electrode, a negative electrode and a separator between the positive electrode and the negative electrode. The material of the positive electrode includes a ternary material coated with lithium manganese iron phosphate; The material of the negative electrode includes a silicon-carbon-mesophase carbon microsphere composite material; The membrane is a polyimide nanofiber membrane.

2. The wide temperature range high safety lithium ion soft pack battery according to claim 1, characterized in that: The silicon-carbon-mesophase carbon microsphere composite material is porous silicon filled with mesophase carbon microspheres coated with hard carbon.

3. The wide temperature range high safety lithium ion soft pack battery according to claim 1, characterized in that: The method for preparing the negative electrode sheet comprises the following steps: Step A1: Sodium carboxymethyl cellulose and deionized water are sol-formed, wherein the mass ratio of the sodium carboxymethyl cellulose to the deionized water is 3:(95-100), and the sol-formed solution is prepared by high-speed stirring for 1-3 hours, and the stirring speed is 30 RPM for revolution and 1300 RPM for rotation; Step A2: Add the conductive agent to the prepared glue solution 1, and stir at high speed for 1 to 2 hours to prepare glue solution 2, with the stirring speed being 35 RPM for revolution and 3500 RPM for rotation; Step A3: adding a silicon-carbon-mesophase carbon microsphere composite material and graphite in a mass ratio of (20-30):75 to the above-mentioned glue solution 2, and stirring under vacuum for 2-3 hours, with a vacuum degree of -85 KPa, and a stirring speed of 42 RPM for revolution and 4500 RPM for rotation, to obtain a first mixture; Step A4: adding the water-based adhesive to the first mixture, and slowly stirring for 0.5 to 1 hour to obtain a second mixture, wherein the stirring speed is 30 RPM for revolution and 1300 RPM for rotation; Step A5: testing and adjusting the viscosity of the second mixture by a viscometer, the viscosity range is 1500-5000 MPa.S, and then filtering through a 200-mesh sieve to obtain a negative electrode slurry; Step A6: After the electrode slurry is evenly coated on the surface of the 6 μm composite copper foil by a coating device, the coating thickness is 130-150 μm, and then dried to form an electrode sheet; Step A7: Roll and slit the electrode sheet to a thickness of 90 to 110 μm and a width of 72 to 73 mm to obtain a negative electrode sheet.

4. The wide temperature range high safety lithium ion soft pack battery according to claim 1, characterized in that: The conductive agent includes SuperP-Li, Ketjen black, CNT, and conductive carbon black.

5. The wide temperature range high safety lithium ion soft pack battery according to claim 1, characterized in that: The aqueous adhesive is a mixed solution of styrene-butadiene SBR emulsion and aqueous polyacrylate PAA emulsion. The preferred aqueous adhesive is a mixed solution of styrene-butadiene SBR emulsion and aqueous polyacrylate PAA emulsion in a mass ratio of 1:

1.

6. The wide temperature range high safety lithium ion soft pack battery according to claim 1, characterized in that: The method for preparing the positive electrode sheet comprises the following steps: Step B1: mixing the lithium manganese iron phosphate coated ternary positive electrode material and the oily binder polyvinylidene fluoride PVDF in a mass ratio of (93-99):2 to obtain a positive electrode slurry; Step B2: coating the positive electrode slurry on the surface of the aluminum foil, rolling and slicing to obtain a positive electrode sheet with a coating thickness of 120 to 150 μm, a rolling thickness of 90 to 120 μm, and a slicing width of 69 to 70 mm.

7. A method for preparing a wide temperature range high safety lithium ion soft pack battery according to any one of claims 1 to 6, characterized in that: The preparation steps are: Step C1: Winding the positive electrode sheet, the negative electrode sheet and the polyimide nanofiber separator into a battery core, and covering the core with a finishing glue; Step C2: welding the positive electrode sheet and the negative electrode sheet to the tabs, wherein the length of the welding end of the tabs is 12 to 20 mm, and the thickness of the toe glue of the tabs is 16 to 30 μm; Step C3: Assemble with the aluminum-plastic film with pre-punched holes, and perform top sealing and side sealing to form a non-liquid-injected soft-pack battery cell; Step C4: injecting electrolyte into the unliquid-injected soft-pack battery cell to form a liquid-injected soft-pack battery cell; Step C5: placing the liquid-injected soft-pack battery cell at rest until the electrolyte is fully infiltrated, forming the battery cell, and then exhausting and sealing the formed battery cell to form a soft-pack battery cell; Step C6: Perform the formation process.

8. The wide temperature range high safety lithium ion soft pack battery according to claim 7, characterized in that: The formation process includes an activation constant current stage, a low voltage constant current charging stage and a constant voltage charging stage; The activation constant current stage is used to detect whether the battery status is normal and preliminarily activate the battery to charge 0.02C to 3.0V; The low-voltage constant-current charging stage is used to open and enrich the lithium ion channels in the electrodes and diaphragms, so as to facilitate the subsequent rapid formation of 0.05C charging to a battery terminal voltage of 3.45 to 3.65V; The constant voltage charging stage is used to promote the conversion of active substances in the deep layer of the electrode. The battery formation is completed when the constant voltage of 4.0V reaches 0.1C.

9. The wide temperature range high safety lithium ion soft pack battery according to claim 1, characterized in that: The battery can work at -55-70 degrees.

Citation Information

Patent Citations

  • Lithium ion battery, its formation method and preparation method

    CN102324570A

  • Formation method of aqueous iron-lithium battery

    CN104638311A

  • Lithium ion battery positive electrode composite material and preparation method and application thereof

    CN114512655A

  • Preparation method of lithium ion battery

    CN116544393A

  • Silicon-carbon composite material as well as preparation method and application thereof

    CN117497716A