Secondary battery and electric device

By providing a fibrous solid electrolyte layer on the surface of the positive and negative electrode sheets of the secondary battery, the problem of thermal runaway and insufficient circulation performance of the battery under improper use is solved, and its safety and circulation performance are improved.

CN118943479APending Publication Date: 2024-11-12SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411191327.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing secondary batteries are prone to thermal runaway under improper use, leading to safety problems, and the instability of high nickel and silicon-carbon materials affects their cycling performance.

Method used

A solid electrolyte layer containing a fibrous solid electrolyte is provided on the surface of the active material layer of the positive electrode and the negative electrode sheet to provide mechanical buffering and active ion conduction capabilities, and improve the safety and circulation performance of the battery.

Benefits of technology

Through the use of the fibrous solid electrolyte layer, the safety of the battery during extrusion and needle puncture is enhanced, and the thermal safety and cycling performance are improved, reducing the impedance impact of the battery's electrical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015621370000151
    Figure BDA0005015621370000151
  • Figure BDA0005015621370000162
    Figure BDA0005015621370000162
  • Figure BDA0005015621370000171
    Figure BDA0005015621370000171
Patent Text Reader

Abstract

The invention discloses a secondary battery and an electric device, and belongs to the technical field of batteries. According to the invention, the solid electrolyte layer containing the fibrous solid electrolyte is arranged on at least one surface of the positive electrode active material layer or the negative electrode active material layer, so that mechanical buffer with a strong robust structure is effectively provided for the positive electrode piece or the negative electrode piece, and the safety of the secondary battery in extrusion and needling processes is improved; meanwhile, the solid electrolyte layer containing the fibrous solid electrolyte can effectively conduct active ions, the critical threshold value of battery liquid injection design can be increased, and the thermal safety of the secondary battery is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a secondary battery and an electrical device. Background Art

[0002] With the rapid development of science and technology, secondary batteries are being used more and more widely in electric vehicles, hybrid vehicles, renewable energy storage and other fields.

[0003] At present, secondary batteries need to use high nickel and silicon-carbon materials in pursuit of high energy density. The instability of these materials themselves causes secondary batteries to be very prone to thermal runaway under improper use conditions, thus causing a series of safety problems.

[0004] In view of this, this application is filed. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a secondary battery and an electrical device, thereby effectively improving the safety and cycle performance of the secondary battery.

[0006] To achieve the above-mentioned object, the first aspect of the present application provides a secondary battery, comprising a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer sequentially arranged on at least one surface of the positive electrode current collector;

[0007] The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer arranged in sequence on at least one surface of the negative electrode current collector;

[0008] A solid electrolyte layer containing a fibrous solid electrolyte is disposed on a surface of the positive electrode active material layer or the negative electrode active material layer away from the current collector.

[0009] As an embodiment of the present application, the length of the fibrous solid electrolyte is 0.5 to 8 μm.

[0010] As an embodiment of the present application, the diameter of the fibrous solid electrolyte is 50 to 200 nm.

[0011] As an embodiment of the present application, the mass percentage of the fibrous solid electrolyte in the solid electrolyte layer is 10 to 50%.

[0012] As an embodiment of the present application, the thickness of the solid electrolyte layer is 4 to 20 μm.

[0013] As an embodiment of the present application, the fibrous solid electrolyte includes a fibrous oxide solid electrolyte.

[0014] As an embodiment of the present application, the fibrous oxide solid electrolyte includes fibrous Li 1+x Al x Ti 2-x (PO4)3, fibrous Li 7-y Ln3Z 2-y O 12 , fibrous Li 3z La 2 / 3-z TiO3, where 0≤x≤0.5, 0≤y≤0.2, 0≤z≤0.16.

[0015] As an embodiment of the present application, the solid electrolyte layer further includes a lithium salt, and the mass percentage of the lithium salt in the solid electrolyte layer is 10 to 50%.

[0016] As an embodiment of the present application, the solid electrolyte layer further includes a matrix polymer, and the mass percentage of the matrix polymer in the solid electrolyte layer is 2.5-5%.

[0017] As an embodiment of the present application, the lithium salt includes LiTFSl, LiPF6, LiALO2, LiNbO3, LiAsF6, LiBF4, LiCl, LiAlCl4, LiSbF6, LiSCN, LiCl, LiNO3, LiCF3SO3, LiCF3CO2, LiN(CF3SO2)2(LiTFSI), LiN(FSO2)2(LiFSI), LiN(C4F9SO2)2, Li2B 12 F 12 , LiAsF6, LiB(C2O4)2(LiBOB).

[0018] As an embodiment of the present application, the matrix polymer includes at least one of cellulose acetate, polyethylene, epoxy resin, polyvinylidene fluoride, ethylene-ethyl acrylate copolymer, ethylene-vinyl acetate copolymer, polybutene, polyamide, polyvinylidene fluoride, polytetrafluoroethylene, polyethylene oxide, polyacetonitrile, and polymethyl acrylate.

[0019] As an embodiment of the present application, a first solid electrolyte layer containing a first fibrous solid electrolyte is disposed on a surface of the positive electrode active material layer away from the positive electrode current collector, and a second solid electrolyte layer containing a second fibrous solid electrolyte is disposed on a surface of the negative electrode active material layer away from the negative electrode current collector;

[0020] The first fibrous solid electrolyte comprises fibrous Li 1+x Al x Ti 2-x (PO4)3, the second fibrous solid electrolyte comprises fibrous Li7-y Ln3Z 2-y O 12 , where 0≤x≤0.5, 0≤y≤0.2, 0≤z≤0.16.

[0021] A second aspect of the present application provides an electrical device, comprising the secondary battery described above.

[0022] The beneficial effects of the present invention are as follows: the present application sets a solid electrolyte layer containing a fibrous solid electrolyte on at least one surface of the positive electrode active material layer or the negative electrode active material layer, effectively providing a strong and robust structural mechanical buffer for the positive electrode plate or the negative electrode plate, improving the safety of the secondary battery during extrusion and acupuncture. At the same time, the solid electrolyte layer containing the fibrous solid electrolyte can effectively conduct active ions, can increase the critical threshold of the battery injection design, and effectively improve the thermal safety of the secondary battery. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0024] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0025] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0026] The reagents or instruments used in this application without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.

[0027] The embodiment of the present application provides a secondary battery, including a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer sequentially arranged on at least one surface of the positive electrode current collector;

[0028] The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer arranged in sequence on at least one surface of the negative electrode current collector;

[0029] A solid electrolyte layer containing a fibrous solid electrolyte is disposed on a surface of the positive electrode active material layer or the negative electrode active material layer away from the current collector.

[0030] The present application creatively arranges a solid electrolyte layer containing a fibrous solid electrolyte on the surface of the positive electrode active material layer or the negative electrode active material layer away from the current collector, effectively providing a strong and robust structural mechanical buffer for the positive electrode plate or the negative electrode plate, thereby improving the safety of the secondary battery during extrusion and acupuncture. At the same time, the solid electrolyte layer containing the fibrous solid electrolyte can effectively conduct active ions, thereby increasing the critical threshold of the battery injection design and effectively improving the thermal safety of the secondary battery.

[0031] Among them, the introduction of fibrous solid electrolyte into the solid electrolyte layer can effectively improve the solid content and stability of the slurry during the slurry preparation process due to the increased spatial hindrance. At the same time, the contact between the fibrous solid electrolyte and the surface can improve the ability of the solid electrolyte layer to conduct active ions, thereby reducing the impedance of the solid electrolyte layer and reducing the impact on the electrical performance of the secondary battery. At the same time, during the processing and rolling of the positive electrode sheet and / or the negative electrode sheet, the use of fibrous solid electrolyte can effectively improve the toughness of the electrode sheet.

[0032] In one embodiment, the length of the fibrous solid electrolyte is 0.5 to 8 μm, for example, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 8 μm or a range consisting of any two of these values. The length of the fibrous solid electrolyte within the above range can improve the safety performance and cycle performance of the secondary battery.

[0033] In one embodiment, the length of the fiber-shaped solid electrolyte is 1 to 5 μm. The length of the fiber-shaped solid electrolyte within the above range can further improve the safety performance and cycle performance of the secondary battery.

[0034] In one embodiment, the diameter of the fibrous solid electrolyte is 50 to 200 nm, for example, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, or a range consisting of any two of these values. When the diameter of the fibrous solid electrolyte is within the above range, the cycle performance of the secondary battery can be improved while ensuring the safety performance of the secondary battery.

[0035] In one embodiment, the mass percentage of the fibrous solid electrolyte in the solid electrolyte layer is 10-50%, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range consisting of any two values ​​thereof. The content of the fibrous solid electrolyte within the above range can improve the safety performance and cycle performance of the secondary battery.

[0036] In one embodiment, the thickness of the solid electrolyte layer is 4 to 20 μm, for example, 4 μm, 5 μm, 6 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm or a range consisting of any two of these values. The thickness of the solid electrolyte layer within the above range can improve the safety performance of the secondary battery and reduce the impact of impedance on the secondary battery.

[0037] In one embodiment, the fibrous solid electrolyte includes a fibrous oxide solid electrolyte.

[0038] In one embodiment, the fibrous oxide solid electrolyte comprises fibrous Li 1+x Al x Ti 2-x (PO4)3, fibrous Li 7-y Ln3Z 2-y O 12 , fibrous Li 3z La 2 / 3-z TiO3, where 0≤x≤0.5, 0≤y≤0.2, 0≤z≤0.16.

[0039] In one embodiment, the solid electrolyte layer also includes a lithium salt, and the mass percentage of the lithium salt in the solid electrolyte layer is 10-50%, for example, it can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range consisting of any two of these values.

[0040] In one embodiment, the lithium salt includes LiTFSl, LiPF6, LiALO2, LiNbO3, LiAsF6, LiBF4, LiCl, LiAlCl4, LiSbF6, LiSCN, LiCl, LiNO3, LiCF3SO3, LiCF3CO2, LiN(CF3SO2)2(LiTFSI), LiN(FSO2)2(LiFSI), LiN(C4F9SO2)2, Li2B 12 F 12 , LiAsF6, LiB(C2O4)2(LiBOB).

[0041] In one embodiment, the solid electrolyte layer also includes a matrix polymer, and the mass percentage of the matrix polymer in the solid electrolyte layer is 2.5-5%, for example, it can be 2.5%, 2.6%, 2.8%, 3%, 3.2%, 3.5%, 4%, 4.2%, 4.5%, 4.8%, or 5%.

[0042] In one embodiment, the matrix polymer includes at least one of cellulose acetate, polyethylene, epoxy resin, polyvinylidene fluoride, ethylene-ethyl acrylate copolymer, ethylene-vinyl acetate copolymer, polybutene, polyamide, polyvinylidene fluoride, polytetrafluoroethylene, polyethylene oxide, polyacetonitrile, and polymethyl acrylate.

[0043] In one embodiment, a first solid electrolyte layer containing a first fibrous solid electrolyte is disposed on a surface of the positive electrode active material layer away from the positive electrode current collector, and a second solid electrolyte layer containing a second fibrous solid electrolyte is disposed on a surface of the negative electrode active material layer away from the negative electrode current collector.

[0044] By arranging a solid electrolyte layer containing a fibrous solid electrolyte on the surface of the positive electrode active material layer and the negative electrode active material layer away from the current collector, a strong and robust structural mechanical buffer is effectively provided for the positive electrode plate and the negative electrode plate, thereby improving the safety of the secondary battery during extrusion and acupuncture. At the same time, the solid electrolyte layer containing the fibrous solid electrolyte can effectively conduct active ions, thereby improving the critical threshold of the battery injection design and effectively improving the thermal safety of the secondary battery.

[0045] In one embodiment, the length of the first fibrous solid electrolyte is 0.5 to 8 μm, for example, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 8 μm or a range consisting of any two of these values. The length of the first fibrous solid electrolyte is within the above range, which can improve the safety performance and cycle performance of the secondary battery.

[0046] In one embodiment, the length of the first fibrous solid electrolyte is 1 to 5 μm. The length of the first fibrous solid electrolyte within the above range can further improve the safety performance and cycle performance of the secondary battery.

[0047] In one embodiment, the length of the first fibrous solid electrolyte is 2 to 3 μm.

[0048] In one embodiment, the diameter of the first fibrous solid electrolyte is 50-200 nm, for example, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, or a range consisting of any two of these values. The diameter of the first fibrous solid electrolyte is within the above range, which can improve the cycle performance of the secondary battery while ensuring the safety performance of the secondary battery.

[0049] In one embodiment, the diameter of the first fibrous solid electrolyte is 60-100 nm. The diameter of the first fibrous solid electrolyte is within the above range, which can further improve the cycle performance of the secondary battery while ensuring the safety performance of the secondary battery.

[0050] In one embodiment, the length of the second fibrous solid electrolyte is 0.5 to 8 μm, for example, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 8 μm or a range consisting of any two of these values. The length of the second fibrous solid electrolyte within the above range can improve the safety performance and cycle performance of the secondary battery.

[0051] In one embodiment, the length of the second fibrous solid electrolyte is 1 to 5 μm. The length of the second fibrous solid electrolyte within the above range can further improve the safety performance and cycle performance of the secondary battery.

[0052] In one embodiment, the length of the second fibrous solid electrolyte is 2 to 3 μm.

[0053] In one embodiment, the diameter of the second fibrous solid electrolyte is 50-200 nm, for example, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, or a range consisting of any two of these values. The diameter of the second fibrous solid electrolyte is within the above range, which can further improve the cycle performance of the secondary battery while ensuring the safety performance of the secondary battery.

[0054] In one embodiment, the diameter of the second fibrous solid electrolyte is 60-100 nm. The diameter of the second fibrous solid electrolyte is within the above range, which can further improve the cycle performance of the secondary battery while ensuring the safety performance of the secondary battery.

[0055] The present application controls the diameter and length of the first fibrous solid electrolyte and the second fibrous solid electrolyte so as to better provide a strong and robust structural mechanical buffer for the positive electrode plate and the negative electrode plate, thereby improving the safety of the secondary battery during extrusion and acupuncture. At the same time, it can better improve the spatial hindrance effect, better improve the stability, and improve the ability of the solid electrolyte layer to conduct active ions, thereby effectively improving the safety and cycle performance of the secondary battery.

[0056] In one embodiment, the mass percentage of the first fibrous solid electrolyte in the first solid electrolyte layer is 10-50%, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range consisting of any two values ​​thereof. The content of the first fibrous solid electrolyte within the above range can improve the safety performance and cycle performance of the secondary battery.

[0057] In one embodiment, the mass percentage of the first fibrous solid electrolyte in the first solid electrolyte layer is 25-35%. The content of the first fibrous solid electrolyte within the above range can further improve the safety performance and cycle performance of the secondary battery.

[0058] In one embodiment, the mass percentage of the second fibrous solid electrolyte in the second solid electrolyte layer is 10-50%, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range consisting of any two values ​​thereof. The content of the second fibrous solid electrolyte within the above range can improve the safety performance and cycle performance of the secondary battery.

[0059] In one embodiment, the mass percentage of the second fibrous solid electrolyte in the second solid electrolyte layer is 25-35%. The content of the second fibrous solid electrolyte within the above range can further improve the safety performance and cycle performance of the secondary battery.

[0060] The present application controls the mass percentage of the first fibrous solid electrolyte and the second fibrous solid electrolyte in the first solid electrolyte layer and the second solid electrolyte layer respectively within this range, thereby effectively reducing the substantial increase in impedance caused by the solid electrolyte layer, reducing the impact on the electrical performance of the secondary battery, and further improving the slurry stability and the toughness of the positive electrode sheet and the negative electrode sheet.

[0061] In one embodiment, the thickness of the first solid electrolyte layer is 4 to 20 μm, for example, 4 μm, 5 μm, 6 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm or a range consisting of any two of these values.

[0062] In one embodiment, the thickness of the first solid electrolyte layer is 4-15 μm.

[0063] In one embodiment, the thickness of the second solid electrolyte layer is 4 to 20 μm, for example, 3 μm, 4 μm, 5 μm, 6 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm or a range consisting of any two of these values.

[0064] In one embodiment, the thickness of the second solid electrolyte layer is 4-15 μm.

[0065] In one embodiment, the thickness of the first solid electrolyte layer is D1 μm, the thickness of the second solid electrolyte layer is D2 μm, and D1+D2≤16.

[0066] In one embodiment, the first fibrous solid electrolyte and the second fibrous solid electrolyte each independently comprise a fibrous oxide solid electrolyte.

[0067] In one embodiment, the first fibrous solid electrolyte comprises fibrous Li 1+x Al x Ti 2-x (PO4)3, the second fibrous solid electrolyte comprises fibrous Li 7-y Ln3Z 2-y O 12 , where 0≤x≤0.5, 0≤y≤0.2, 0≤z≤0.16.

[0068] In one embodiment, the first solid electrolyte layer also includes a first lithium salt, and the mass percentage of the first lithium salt in the first solid electrolyte layer is 10-50%, for example, it can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range consisting of any two of these values.

[0069] In one embodiment, the first solid electrolyte layer also includes a first matrix polymer, and the mass percentage of the first matrix polymer in the first solid electrolyte layer is 2.5-5%, for example, it can be 2.5%, 2.6%, 2.8%, 3%, 3.2%, 3.5%, 4%, 4.2%, 4.5%, 4.8%, or 5%.

[0070] In one embodiment, the second solid electrolyte layer further includes a second lithium salt, and the mass percentage of the second lithium salt in the second solid electrolyte layer is 10-50%, for example, it can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range consisting of any two of these values.

[0071] In one embodiment, the second solid electrolyte layer also includes a second matrix polymer, and the mass percentage of the second matrix polymer in the second solid electrolyte layer is 2.5-5%, for example, it can be 2.5%, 2.6%, 2.8%, 3%, 3.2%, 3.5%, 4%, 4.2%, 4.5%, 4.8%, or 5%.

[0072] In one embodiment, the first lithium salt and the second lithium salt independently include LiTFSl, LiPF6, LiALO2, LiNbO3, LiAsF6, LiBF4, LiCl, LiAlCl4, LiSbF6, LiSCN, LiCl, LiNO3, LiCF3SO3, LiCF3CO2, LiN(CF3SO2)2(LiTFSI), LiN(FSO2)2(LiFSI), LiN(C4F9SO2)2, Li2B 12 F 12 , LiAsF6, LiB(C2O4)2(LiBOB).

[0073] In one embodiment, the first matrix polymer and the second matrix polymer independently include at least one of cellulose acetate, polyethylene, epoxy resin, polyvinylidene fluoride, ethylene-ethyl acrylate copolymer, ethylene-vinyl acetate copolymer, polybutene, polyamide, polyvinylidene fluoride, polytetrafluoroethylene, polyethylene oxide, polyacetonitrile, and polymethyl acrylate.

[0074] In one embodiment, the first solid electrolyte layer also includes a first binder, and the mass percentage of the first binder in the first solid electrolyte layer is 20-50%, for example, it can be 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range consisting of any two of these values.

[0075] In one embodiment, the second solid electrolyte layer also includes a second binder, and the mass percentage of the second binder in the second solid electrolyte layer is 20-50%, for example, it can be 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range consisting of any two of these values.

[0076] In one embodiment, the first solid electrolyte layer also includes a first dispersant, and the mass percentage of the first dispersant in the first solid electrolyte layer is 0.01-0.1%, for example, it can be 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1% or a range consisting of any two of these values.

[0077] In one embodiment, the second solid electrolyte layer also includes a second dispersant, and the mass percentage of the second dispersant in the second solid electrolyte layer is 0.01-0.1%, for example, it can be 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1% or a range consisting of any two of these values.

[0078] In one embodiment, the preparation method of the fibrous oxide electrolyte is:

[0079] (1) uniformly mixing a salt solution of a solid electrolyte constituent element and a first solvent to obtain a first mixed solution;

[0080] (2) mixing the organic acid and the second solvent uniformly to obtain a second mixed solution;

[0081] (3) mixing the first mixed solution and the second mixed solution evenly to obtain a precursor solution,

[0082] (4) The precursor solution and the water-soluble polymer solution are mixed evenly to obtain a spinning solution, and the spinning solution is spun and calcined to obtain a fibrous oxide solid electrolyte.

[0083] In one embodiment, the air flow velocity of the spinning is 10 to 50 m / s, for example, it can be 10 m / s, 12 m / s, 15 m / s, 18 m / s, 20 m / s, 25 m / s, 30 m / s, 35 m / s, 40 m / s, 45 m / s, 50 m / s or a range consisting of any two of the values.

[0084] In one embodiment, the calcination temperature is 500-1500°C, for example, it can be 500°C, 550°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C or a range consisting of any two of the values.

[0085] In one embodiment, the calcination time is 1 to 10 hours, for example, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours or a range consisting of any two values ​​therein.

[0086] The present application controls the diameter and length of the fibrous solid electrolyte by controlling the spinning air flow velocity, calcination temperature and calcination time.

[0087] In one embodiment, the first solvent and the second solvent independently include at least one of water, acetone, ethanol, methanol, N,N-dimethylformamide, ethylene glycol dimethyl sulfoxide, cyclopentane, tetrahydrofuran, 2-methyltetrahydrofuran, ethylene nitrate, ethylene carbonate, 1,4-butyrolactone, and dimethylacetamide.

[0088] In one embodiment, the mass percentage of the water-soluble polymer in the water-soluble polymer solution is 2-20%, for example, it can be a range consisting of any two values ​​of 2%, 4%, 5%, 6%, 8%, 10%, 12%, 15%, 18%, and 20%.

[0089] In one embodiment, the water-soluble polymer includes at least one of polyvinyl alcohol, polyethylene glycol, polyacrylonitrile, and polyvinyl pyrrolidone.

[0090] In one embodiment, the organic acid includes at least one of citric acid, malic acid, and tartaric acid.

[0091] In one embodiment, the molar ratio of the organic acid to the second solvent is 1:(1-4), for example, 1:1, 1:2, 1:3, 1:4 or a range consisting of any two values ​​therein.

[0092] In one embodiment, the volume ratio of the salt solution to the first solvent is 1:(1-5), for example, it can be 1:1, 1:2, 1:3, 1:4, 1:5 or a range consisting of any two values ​​therein.

[0093] In one embodiment, the volume ratio of the first mixed liquid to the second mixed liquid is 1:(1-5), for example, it can be 1:1, 1:2, 1:3, 1:4, 1:5 or a range consisting of any two values ​​therein.

[0094] In one embodiment, the volume ratio of the precursor solution to the water-soluble polymer solution is (2-10):1, for example, it can be 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1 or a range consisting of any two values ​​therein.

[0095] More specifically, the fibrous Li 1+x Al x Ti 2-x The specific steps of (PO4)3 (1) are as follows: (1) according to Li 1+ xAl x Ti 2-x The stoichiometric ratio in (PO4)3 is respectively weighed into lithium nitrate, aluminum nitrate, phosphoric acid, titanium nitrate, and nitric acid and mixed evenly with the first solvent to obtain a first mixed solution.

[0096] More specifically, the fibrous Li 7-y Ln3Z 2-y O 12 The step (1) is specifically as follows: (1) lithium nitrate, lanthanum nitrate, zirconium oxychloride, titanium nitrate, nitric acid and a first solvent are uniformly mixed to obtain a first mixed solution.

[0097] In one embodiment, the positive electrode active material can be selected from sodium iron composite oxide, sodium cobalt composite oxide, sodium manganese composite oxide, sodium nickel composite oxide, sodium nickel titanium composite oxide, sodium nickel manganese composite oxide, sodium iron manganese composite oxide, sodium nickel cobalt manganese composite oxide, sodium iron phosphate compound, sodium manganese phosphate compound, sodium cobalt phosphate compound, lithium nickel cobalt manganese oxide, lithium phosphate, etc. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries can also be used. These positive electrode active materials can be used alone or in combination of two or more.

[0098] In the present application, the type of positive electrode current collector is not particularly limited, and it can be any material known to be suitable for use as a positive electrode current collector. In one embodiment, the positive electrode current collector includes metal materials such as aluminum, stainless steel, nickel plating, titanium, tantalum, and carbon materials such as carbon cloth and carbon paper. In one embodiment, the positive electrode current collector is a metal material. In one embodiment, the positive electrode current collector is aluminum.

[0099] There is no particular restriction on the form of the positive electrode current collector. When the positive electrode current collector is a metal material, the positive electrode current collector may be in the form of metal foil, metal cylinder, metal strip roll, metal plate, metal foil, metal plate mesh, stamped metal, foamed metal, etc. When the positive electrode current collector is a carbon material, the positive electrode current collector may include but is not limited to a carbon plate, a carbon film, a carbon cylinder, etc.

[0100] In the present application, there is no particular limitation on the negative electrode current collector, as long as the purpose of the present application can be achieved, for example, it can be copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, foam nickel, foam copper or a composite current collector.

[0101] In one embodiment, the negative electrode active material can be natural graphite, artificial graphite, mesophase microcarbon beads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, SiO, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structured lithium titanate Li4Ti5O 12, at least one of Li-Al alloy and metallic lithium.

[0102] In one embodiment, the first binder and the second binder mentioned in the present application independently include at least one of polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, nitrocellulose, styrene-butadiene rubber, nitrile rubber, fluororubber, isoprene rubber, polybutadiene rubber, ethylene-propylene rubber, polyvinylidene fluoride, polytetrafluoroethylene, and fluorinated polyvinylidene fluoride.

[0103] In the secondary battery mentioned in the present application, a separator is usually provided between the positive electrode and the negative electrode to prevent short circuit. The material and shape of the separator are not particularly limited as long as the effect of the present application is not significantly impaired.

[0104] In one embodiment, the separator includes a porous sheet or non-woven fabric having excellent liquid retention. The materials of the resin or glass fiber separator include, but are not limited to, polyolefin, aromatic polyamide, polytetrafluoroethylene, polyethersulfone, and the like.

[0105] In one embodiment, the polyolefin is polyethylene or polypropylene. In some embodiments, the polyolefin is polypropylene. The materials of the above-mentioned diaphragm can be used alone or in any combination.

[0106] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.

[0107] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0108] In some embodiments, the type of the electrolyte is not specifically limited. The electrolyte includes an electrolyte salt and an organic solvent. The specific types of the electrolyte salt and the organic solvent are not specifically limited and can be selected according to actual needs. The electrolyte may also include additives. The types of the additives are not particularly limited and may be film-forming additives for the positive electrode and / or the negative electrode, or additives that can improve certain properties of the battery, such as additives that improve the high or low temperature performance of the battery.

[0109] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape.

[0110] An embodiment of the present application provides an electric device, comprising the secondary battery described above, wherein the secondary battery serves as a power supply for the electric device.

[0111] Exemplarily, the above-mentioned electrical devices may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0112] The present application is further described below with specific embodiments:

[0113] Example 1

[0114] A method for preparing a secondary battery comprises the following steps:

[0115] (1) Fibrous LiAl 0.3 Ti 1.7 Preparation of PO4:

[0116] Add 1 part by mass of lithium nitrate, aluminum nitrate, phosphoric acid, titanium nitrate and nitric acid according to the element ratio and mix with 10 parts by mass of anhydrous ethanol at 50° C. to obtain a first mixed solution;

[0117] Mix citric acid and ethylene glycol in a molar ratio of 1:2 to obtain a second mixed solution;

[0118] The first mixed solution and the second mixed solution were mixed in a volume ratio of 1:2, and then stirred at 50° C. to obtain a precursor solution;

[0119] The precursor solution and 10% by mass PVA (polyvinyl alcohol) solution were mixed and stirred at a volume ratio of 4:1 to obtain a spinning solution, and spinning was performed at an air flow velocity of 30 m / s;

[0120] The spun material was calcined at 800°C for 3 hours.

[0121] The prepared fibrous LiAl 0.3 Ti 1.7 PO4 is 2.5 μm in length and 80 nm in diameter.

[0122] (2) Fibrous Li7La3Zr2O 12 Preparation:

[0123] Add 1 part by mass of lithium nitrate, lanthanum nitrate, zirconium oxychloride, titanium nitrate and nitric acid according to a certain element ratio and mix with 10 parts by mass of anhydrous ethanol at 50° C. to obtain a first mixed solution;

[0124] Mix citric acid and ethylene glycol in a molar ratio of 1:2 to obtain a second mixed solution;

[0125] The first mixed solution and the second mixed solution were mixed in a volume ratio of 1:2, and then stirred at 50° C. to obtain a precursor solution;

[0126] The precursor solution and 10% by mass PVA solution were mixed and stirred in a volume ratio of 3:1 to obtain a spinning solution, and spinning was performed at an air flow velocity of 30 m / s;

[0127] The spun material was calcined at a temperature of 1200°C for 5 hours.

[0128] As-prepared fibrous Li7La3Zr2O 12 The length is 2μm and the diameter is 100nm.

[0129] (3) Preparation of positive electrode sheet:

[0130] The mass ratio of NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 O2), polyvinylidene fluoride, conductive carbon black SP, carbon nanotubes CNT, and solvent N-methylpyrrolidone are mixed into a uniform positive electrode slurry, and then the slurry is evenly coated on an aluminum foil, and then rolled after drying at 110°C to obtain a positive electrode active material layer;

[0131] Polyvinylidene fluoride, fibrous LiAl 0.3 Ti 1.7 PO4, lithium bis(trifluoromethylsulfonyl)imide, dispersant BYK, cellulose acetate, and solvent N-methylpyrrolidone are mixed into a uniform first solid electrolyte slurry. A transfer coater is used with a knife edge adjusted to 20 μm to coat the first solid electrolyte slurry on the surface of the positive electrode active material layer. After drying at 110°C, the composite positive electrode sheet is rolled to form a first solid electrolyte layer with a thickness of 4 μm, which is then cut to obtain a positive electrode sheet.

[0132] (4) Preparation of negative electrode sheet:

[0133] Graphite, silicon dioxide, polyacrylic acid PAA, conductive carbon black SP, carbon nanotubes CNT, and solvent N-methylpyrrolidone in a mass ratio of 85:9:3:2:1 are mixed to form a uniform negative electrode slurry, and then the slurry is evenly coated on a copper foil, and then rolled after drying at 105° C. to obtain a negative electrode active material layer;

[0134] Polyvinylidene fluoride, fibrous Li7La3Zr2O 12, lithium bis(trifluoromethylsulfonyl)imide, dispersant BYK, cellulose acetate, and solvent N-methylpyrrolidone are mixed into a uniform second solid electrolyte slurry, and a transfer coater is used with a knife edge adjusted to 20 μm to coat the second solid electrolyte slurry on the surface of the negative electrode active material layer. After drying at 110° C., the composite negative electrode sheet is roll-pressed to form a second solid electrolyte layer with a thickness of 4 μm, and then cut to obtain a negative electrode sheet.

[0135] (5) Assembly of secondary battery: The separator is a polyethylene porous membrane; dimethyl carbonate and ethylene carbonate are mixed in a ratio of 4:6, and lithium hexafluorophosphate is added thereto as an electrolyte solution, wherein the molar concentration of lithium hexafluorophosphate is 1 mol / L. The positive electrode sheet, the negative electrode sheet, and the separator are stacked to obtain a bare cell, which is then packaged and injected with electrolyte solution to form a soft-pack battery to obtain a secondary battery.

[0136] Embodiments 2 to 11

[0137] Examples 2 to 11: Changing the fibrous LiAl 0.3 Ti 1.7 PO4, fibrous Li7La3Zr2O 12 The spinning air flow rate, calcination temperature and time in the preparation process can adjust the fibrous LiAl 0.3 Ti 1.7 PO4, fibrous Li7La3Zr2O 12 The diameter and length of the

[0138] Embodiments 12 to 15

[0139] Examples 12 to 15 change the mass percentage of the binder and the fibrous solid electrolyte in the first solid electrolyte slurry and the second solid electrolyte slurry, and then adjust the content of the fibrous solid electrolyte in the first solid electrolyte layer and the second solid electrolyte layer, as shown in Table 1 for details.

[0140] Embodiments 16 to 18

[0141] In Examples 16 to 18, the coating amount was changed to adjust the thickness of the first solid electrolyte layer and the second solid electrolyte layer, as shown in Table 1.

[0142] Embodiment 19

[0143] The difference between Example 19 and Example 1 is that the fibrous Li7La3Zr2O 12 Added to the first solid electrolyte layer, the fibrous LiAl 0.3 Ti 1.7 PO4 is added to the second solid electrolyte layer (i.e., fibrous Li7La3Zr2O 12、LiAl 0.3 Ti 1.7 PO4 interchange), see Table 1 for details.

[0144] Embodiment 20

[0145] The difference between Example 20 and Example 1 is that Example 20 does not contain a second solid electrolyte layer.

[0146] Embodiment 21

[0147] The difference between Example 21 and Example 1 is that Example 21 does not contain a first solid electrolyte layer.

[0148] Embodiment 22

[0149] The difference between Example 22 and Example 1 is that the coating amount is changed to adjust the first solid electrolyte layer, and the second solid electrolyte layer is not included, as shown in Table 1 for details.

[0150] Comparative Example 1

[0151] The difference between Comparative Example 1 and Example 20 is that Comparative Example 1 uses an equal amount of granular LiAl 0.3 Ti 1.7 PO4 replaces fibrous LiAl 0.3 Ti 1.7 PO4.

[0152] Comparative Example 2

[0153] The difference between Comparative Example 2 and Example 21 is that Comparative Example 2 uses an equal amount of granular Li7La3Zr2O 12 Replacement of fibrous Li7La3Zr2O 12 .

[0154] Table 1

[0155]

[0156]

[0157] The secondary batteries obtained in Examples 1 to 22 and Comparative Examples 1 to 2 were subjected to performance tests, and the specific test items and methods are as follows:

[0158] Battery thermal stability safety performance test method:

[0159] After the battery is clamped, fully charge it to 100% SOC; at 25±5℃, heat it to 150℃ at a rate of 5℃ / min and keep it warm for 30min; then heat it to 170℃ at 5℃ / min and keep it warm for 60min; observe the battery condition.

[0160] Battery 25℃ cycle test method:

[0161] Step 1: Place the battery in a 25℃ constant temperature box and let it stand for 60 minutes until the battery temperature stabilizes at 25±3℃ before performing subsequent operations; Step 2: Discharge at a constant current of 1C to 2.5V; Step 3: Charge at a constant current of 1C to 4.25, then charge at a constant voltage until the current value reaches 0.05C rate value to complete the charging process; Step 4: Let the battery stand for 10 minutes; Step 5: Discharge at a constant current of 1C to 2.5V, and obtain the capacity value at this time, which is defined as C0; Step 6: Charge at a constant current of 1C0 to 4.25V, then charge at a constant voltage until the current value reaches 0.05C0 rate value to complete the charging process; Step 7: Let the battery stand for 10 minutes; Step 8: Discharge at a constant current of 1C0 to 2.5V; Step 9: Let the battery stand for 10 minutes; Step 10: Repeat steps 6 and 9 for 1000 cycles.

[0162] Table 2

[0163]

[0164]

[0165] It should be noted that the hot box safety test is to raise the temperature to a certain temperature, then keep it warm, and observe the time it takes for the battery to fail. For example, the test result of Example 1 "170°C 35min" means that the battery prepared in Example 1 did not fail after being kept warm at 170°C for 35min.

[0166] As can be seen from Table 2, the present application provides a solid electrolyte layer containing a fibrous solid electrolyte on at least one surface of the positive electrode active material layer or the negative electrode active material layer, which effectively improves the safety performance and cycle performance of the secondary battery.

[0167] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A secondary battery, comprising a positive electrode sheet and a negative electrode sheet, characterized in that: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer sequentially arranged on at least one surface of the positive electrode current collector; The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer arranged in sequence on at least one surface of the negative electrode current collector; A solid electrolyte layer containing a fibrous solid electrolyte is disposed on a surface of the positive electrode active material layer or the negative electrode active material layer away from the current collector.

2. The secondary battery according to claim 1, characterized in that: The length of the fibrous solid electrolyte is 0.5 to 8 μm; And / or, the diameter of the fibrous solid electrolyte is 50 to 200 nm.

3. The secondary battery according to claim 1, characterized in that: The mass percentage of the fibrous solid electrolyte in the solid electrolyte layer is 10-50%.

4. The secondary battery according to claim 1, characterized in that: The thickness of the solid electrolyte layer is 4-20 μm.

5. The secondary battery according to claim 1, characterized in that: The fibrous solid electrolyte includes a fibrous oxide solid electrolyte.

6. The secondary battery according to claim 5, characterized in that: The fibrous oxide solid electrolyte includes fibrous Li 1+x Al x Ti 2-x (PO4)3, fibrous Li 7-y LqCy 2-y O 12 , fibrous Li 3z La 2 / 3-z TiO3, where 0≤x≤0.5, 0≤y≤0.2, 0≤z≤0.

16.

7. The secondary battery according to claim 1, characterized in that: The solid electrolyte layer further comprises a lithium salt, wherein the mass percentage of the lithium salt in the solid electrolyte layer is 10 to 50%; And / or, the solid electrolyte layer further comprises a matrix polymer, and the mass percentage of the matrix polymer in the solid electrolyte layer is 2.5-5%.

8. The secondary battery according to claim 7, characterized in that: The matrix polymer includes at least one of cellulose acetate, polyethylene, epoxy resin, polyvinylidene fluoride, ethylene-ethyl acrylate copolymer, ethylene-vinyl acetate copolymer, polybutene, polyamide, polyvinylidene fluoride, polytetrafluoroethylene, polyethylene oxide, polyacetonitrile, and polymethyl acrylate.

9. The secondary battery according to claim 1, characterized in that: The surface of the positive electrode active material layer away from the positive electrode current collector is provided with a first solid electrolyte layer containing a first fibrous solid electrolyte, and the surface of the negative electrode active material layer away from the negative electrode current collector is provided with a second solid electrolyte layer containing a second fibrous solid electrolyte; The first fibrous solid electrolyte comprises fibrous Li 1+x Al x Ti 2-x (PO4)3, the second fibrous solid electrolyte comprises fibrous Li 7-y LqCy 2-y O 12 , where 0≤x≤0.5, 0≤y≤0.2, 0≤z≤0.

16.

10. The secondary battery according to claim 9, characterized in that: Satisfy at least one of the following (a) to (d): (a) the length of the first fibrous solid electrolyte is 0.5 to 8 μm; (b) the diameter of the first fibrous solid electrolyte is 50 to 200 nm; (c) the length of the second fibrous solid electrolyte is 0.5 to 8 μm; (d) The diameter of the second fibrous solid electrolyte is 50 to 200 nm.

11. The secondary battery according to claim 9, characterized in that: The mass percentage of the first fibrous solid electrolyte in the first solid electrolyte layer is 10-50%; And / or, the mass percentage of the second fibrous solid electrolyte in the second solid electrolyte layer is 10-50%.

12. The secondary battery according to claim 9, characterized in that: The thickness of the first solid electrolyte layer is 4 to 20 μm; And / or, the thickness of the second solid electrolyte layer is 4-20 μm.

13. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Flexible all-solid-state polymer lithium battery and production method thereof

    CN107634184A

  • Solid-state battery and method for manufacturing same

    CN111509292A

  • Composite solid electrolyte membrane, preparation method thereof and lithium ion battery

    CN111816910A

  • Composite solid electrolyte membrane, preparation method thereof and lithium ion battery

    CN111816916A

  • Composite solid electrolyte / electrode, preparation method thereof and solid lithium oxygen battery

    CN115332688A