Electrolyte and battery
By adding additives of perfluorosulfonic acid groups and C-F groups to the metal battery electrolyte solution, the solid electrolyte phase is formed, which solves the short circuit and thermal runaway caused by dendrite generation, and improves the cycle stability and ion transport performance of the battery .
Patent Information
- Application Number
- CN202411072859.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-12
AI Technical Summary
Metal batteries are prone to dendrites during the charge and discharge cycle, resulting in short circuits and thermal runaway, threatening the safety and reliability of the battery.
Provided an electrolyte solution containing a perfluorosulfonic acid group and at least one C-F group, which can form a solid electrolyte phase on the surface of a metal-based electrode, reduce the risk of dendrite generation, alleviate short circuit and thermal runaway problems, and improve ion transport performance.
Effectively inhibit the growth of dendrites, extend the cycle life of the battery, improve the safety and performance stability of the battery, and reduce the occurrence of side reactions.
Smart Images

Figure CN118943482A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrolytes, and in particular to an electrolyte and a battery. Background Art
[0002] In metal battery technology, especially in the research and development and application of high-performance batteries such as lithium metal batteries, a long-standing technical challenge is the formation of dendrites. During the long-term charge and discharge cycle of metal batteries, due to the uneven deposition and stripping of metal ions (such as lithium ions) on the electrode surface, branch-like metal dendrites are easily formed. Once these dendrites grow to a size sufficient to pierce the battery separator, they will cause a short circuit between the positive and negative electrodes of the battery. Short circuits not only lead to a sharp drop in battery performance, but are also likely to generate a large amount of heat due to excessive current, leading to thermal runaway, which seriously threatens the safety and reliability of the battery. Therefore, how to effectively inhibit the growth of dendrites and improve the cycle stability and safety of metal batteries has become a hot spot and difficulty in current battery technology research. Summary of the invention
[0003] The main purpose of the present invention is to provide a metal to solve the technical problem that metal batteries are prone to generate dendrites during the charge and discharge cycle.
[0004] To achieve the above object, the present invention provides an electrolyte, wherein the electrolyte comprises an additive, wherein the additive contains a perfluorosulfonic acid group and at least one CF group.
[0005] In some embodiments of the present invention, the additive comprises at least one of the following structural formulas:
[0006]
[0007] R in the structural formula (III) comprises an organic hydrocarbon chain containing a CF group, and the number of the CF groups is greater than or equal to 2;
[0008] R in the structural formula (IV) comprises an organic hydrocarbon chain containing CF groups, and the number of the CF groups is greater than or equal to 2.
[0009] In some embodiments of the present invention, the number of CF groups in R in the structural formula (III) is greater than or equal to 9;
[0010] and / or, the number of CF groups in R in the structural formula (IV) is greater than or equal to 9;
[0011] and / or, R in the structural formula (III) comprises an organic hydrocarbon chain containing only CF groups;
[0012] and / or, R in the structural formula (IV) comprises an organic hydrocarbon chain containing only CF groups;
[0013] And / or, the structural formula of the additive is as follows:
[0014]
[0015] In some embodiments of the present invention, based on 100% of the total mass of the electrolyte, the content of the additive is 0.1% to 10%.
[0016] In some embodiments of the present invention, the electrolyte further includes a solvent and a metal salt.
[0017] In some embodiments of the present invention, the solvent includes an organic solvent and / or an aqueous solvent.
[0018] In some embodiments of the present invention, the solvent is an organic solvent, and the organic solvent includes fluoroethylene carbonate, linear ethylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, methyl propionate (MP), methyl butyrate, ethyl acetate (EA), ethyl propionate, ethyl butyrate, fluoroethylene carbonate, 1,4-butyrolactone and γ-butyrolactone, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (E MC), methyl formate (MF), methyl acetate (MA), fluoroethylene carbonate (FEC), ethyl propionate (EP), γ-butyrolactone (GBL), tetrahydrofuran (THF), 2-methyltetrahydrofuran (2MeTHF), 1,3-dioxolane (DOL), 4-methyl-1,3-dioxolane (4MeDOL), triethylene glycol dimethyl ether (DG), dimethyl sulfone (MSM), dimethyl ether (DME), vinyl sulfite (ES), propylene sulfite (PS), dimethyl sulfite (DMS), and diethyl sulfite (DES).
[0019] In some embodiments of the present invention, the metal salt includes at least one of lithium salt, sodium salt, potassium salt, aluminum salt, and magnesium salt.
[0020] In some embodiments of the present invention, the lithium salt includes lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethylsulfonyl imide) (LiTFSI), lithium bis(fluoromethylsulfonyl imide) (LiFSI), lithium trifluoromethylsulfonate (LiCF3SO3), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), LiAsF6, LiClO4, lithium bis(trifluoromethyl)borate (LiBOB), lithium difluorooxalatoborate (LiDFOB), lithium trifluoromethylsulfonate (LiCF3SO3), di(trifluoromethyl) ... One or more of lithium sulfonate (liquid) imide [LiN(CF3SO2)2, LiTFSI] and its derivatives, perfluoroalkyl lithium phosphate [LiPF3(C2F5)3, LiFAP], lithium tetrafluorooxalate phosphate [LiPF4(C2O4)], lithium bis(oxalatoborate) (LiBOB), lithium tris(catechol) phosphate (LTBP) and sulfonated polysulfonamide lithium salt, LiPF6, LiClO4, LiCoO2, LiBF4, LiAsF6, LiNO3, LiCO3, LiCl.
[0021] The present invention also provides a battery, comprising the electrolyte as described above.
[0022] In some embodiments of the present invention, the battery comprises a lithium ion battery, a sodium ion battery, a potassium ion battery, an aluminum ion battery or a magnesium ion battery.
[0023] The beneficial effects that can be achieved by the present invention are:
[0024] The electrolyte provided by the present invention contains an additive, and the additive contains a perfluorosulfonic acid group (-SO3H) and at least one CF group. The perfluorosulfonic acid group (-SO3H) has the electron-accepting property of a Lewis acid, and the CF group has a stable adsorption property, which can help the additive adhere to the surface of the metal-based electrode of the battery to form a solid electrolyte phase (SEI). The formed solid electrolyte phase can not only effectively reduce the risk of dendrite generation during the charge and discharge cycle of the battery, alleviate the problem of short circuit caused by dendrite generation, and then thermal runaway, but also can achieve efficient ion transmission performance, and can also inhibit the corrosion of the metal electrode by the electrolyte, thereby reducing the occurrence of side reactions in the battery during the cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0026] Figure 1FIG. 1 is a schematic diagram of an electrolyte acting on a battery electrode according to an embodiment of the present invention.
[0027] Figure 2 This is a SEM image of a solid electrolyte phase formed on the surface of a metal-based electrode according to an embodiment of the present invention.
[0028] Figure 3 It is a comparison chart of battery performance test of Example 1 of the present invention and Comparative Example 1.
[0029] Figure 4 It is a comparison chart of battery performance test of Example 1 of the present invention and Comparative Example 1.
[0030] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0031] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] In the present invention, descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0034] Metal batteries are prone to produce dendrites during long-term charge and discharge cycles, which in turn cause short circuits and lead to thermal runaway of the battery.
[0035] In view of this, the present invention provides an electrolyte that can be applied to metal batteries.
[0036] The electrolyte of the present invention contains an additive, and the additive contains a perfluorosulfonic acid group and at least one CF group. The perfluorosulfonic acid group (-SO3H) in the additive has the electron-accepting property of Lewis acid, and combined with the CF group with stable adsorption, can be attached to the surface of the metal-based electrode of the battery to form a solid electrolyte phase. The formed solid electrolyte can not only effectively reduce the risk of dendrite generation in the battery during the charge and discharge cycle, alleviate the problem of short circuit caused by dendrite generation, and then thermal runaway, but also can achieve efficient ion transmission performance, and can also inhibit the corrosion of the metal electrode by the electrolyte, thereby reducing the occurrence of side reactions in the battery during the cycle.
[0037] In the present invention, the additive can form a solid electrolyte phase on various metal-based surfaces, including but not limited to lithium, sodium, potassium, aluminum, and magnesium. Therefore, in some embodiments, the metal-based electrode of the battery includes a lithium metal-based electrode, a sodium metal-based electrode, a potassium metal-based electrode, an aluminum metal-based electrode, or a magnesium metal-based electrode, which has a wide range of applications.
[0038] In some embodiments, the metal-based electrode includes a metal-based cathode.
[0039] In some embodiments, the additive comprises at least one of the following structural formulas:
[0040]
[0041] Wherein, R in the structural formula (III) includes an organic hydrocarbon chain containing CF, and the number of CF groups is greater than or equal to 2; R in the structural formula (IV) includes an organic hydrocarbon chain containing CF, and the number of CF groups is greater than or equal to 2.
[0042] The perfluorosulfonic acid group in the additive having the structural formula (I) is connected with a CF group, has electron-accepting properties and adsorption properties, and can be attached to the surface of the metal-based electrode to form a solid electrolyte phase.
[0043] The perfluorosulfonic acid group in the additive having the structural formula (II) is connected with a CF group, has electron-accepting properties and adsorption properties, and can be attached to the surface of the metal-based electrode to form a solid electrolyte phase.
[0044] The perfluorosulfonic acid group in the additive having the structural formula (III) is connected to an organic hydrocarbon chain containing CF, and the number of CF groups is greater than or equal to 2. For example, the number of CF groups can be 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, etc. The CF long chain has stable adsorption, and combined with the Lewis acid electron-accepting characteristics of the perfluorosulfonic acid group, it can be firmly attached to the surface of the metal-based electrode of the battery to form a compact solid electrolyte phase, which can greatly reduce the risk of dendrite generation during high-current charging and discharging, alleviate the problem of short circuit caused by dendrite generation in the battery, and then thermal runaway, etc., and the compact solid electrolyte phase can also effectively improve the ion transmission performance, and further inhibit the corrosion of the metal electrode by the electrolyte, and reduce the generation of side reactions during the battery cycle.
[0045] The perfluorosulfonic acid group in the additive of structural formula (IV) is connected to an organic hydrocarbon chain containing CF, and the number of CF groups is greater than or equal to 2. For example, the number of CF groups can be 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, etc. The CF long chain has a relatively stable adsorption property. Combined with the Lewis acid electron-accepting property of the perfluorosulfonic acid group, it can be firmly attached to the surface of the metal-based electrode of the battery to form a compact solid electrolyte phase, which can greatly reduce the risk of dendrite generation during high current charging and discharging, alleviate the problem of short circuit caused by dendrite generation in the battery, and then thermal runaway, etc., and the compact solid electrolyte phase can also effectively improve the ion transmission performance, and further inhibit the corrosion of the metal electrode by the electrolyte, and reduce the generation of side reactions in the battery during the cycle.
[0046] In some embodiments, R in structural formula (III) includes an organic hydrocarbon chain containing only CF groups, and the hydrogen atoms on the organic hydrocarbon chain of the additive are completely replaced by fluorine atoms to obtain a long CF chain with relatively stable adsorption. Combined with the Lewis acid electron-withdrawing properties of perfluorosulfonic acid, it can firmly adhere to the surface of the metal-based electrode to form a tight and firm solid electrolyte phase.
[0047] In some embodiments, R in structural formula (IV) includes an organic hydrocarbon chain containing only CF groups, and the hydrogen atoms on the organic hydrocarbon chain of the additive are completely replaced by fluorine atoms to obtain a long CF chain with relatively stable adsorption. Combined with the Lewis acid electron-withdrawing properties of perfluorosulfonic acid, it firmly adheres to the surface of the metal-based electrode to form a tight and firm solid electrolyte phase.
[0048] In some embodiments, the additive is perfluorosulfonic acid with the chemical formula C4F9SO4H, which contains a perfluorosulfonic acid group and a long chain of CF organic hydrocarbons containing 9 CF groups, and has stable adsorption. Combined with the Lewis acid electron-withdrawing properties of the perfluorosulfonic acid group, it can firmly adhere to the surface of the metal-based electrode of the battery to form a compact solid electrolyte phase, which can greatly reduce the risk of dendrite formation during high-current charging and discharging, alleviate the problem of short circuit caused by dendrite formation in the battery, and then thermal runaway. In addition, the compact solid electrolyte phase can effectively improve the ion transmission performance, and further inhibit the corrosion of the metal electrode by the electrolyte, and reduce the generation of side reactions during the battery cycle.
[0049] In some embodiments, the structural formula of perfluorosulfonic acid having the chemical formula C4F9SO4H is as follows:
[0050]
[0051] In this embodiment, perfluorosulfonic acid with the chemical formula C4F9SO4H has a long CF chain and contains abundant CF groups. When added to the electrolyte, the additive can firmly adhere to the surface of the metal-based electrode of the battery with the help of abundant CF groups to form a compact solid electrolyte phase, greatly reducing the risk of dendrite formation during high current charging and discharging.
[0052] Perfluorosulfonic acid additives containing perfluorosulfonic acid groups can be widely used in the production of proton exchange membranes for fuel cells, but the amount used is large, resulting in high costs. In the present invention, the additive having a perfluorosulfonic acid group of the present invention is applied to the electrolyte of the battery, and a small amount can exert a good effect, which can effectively control costs.
[0053] Exemplarily, based on 100% of the total mass of the electrolyte, the content of the additive is 0.1% to 10%, which can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.1%, 9.2%, 9.3%, 9.4%, 9.5%, 9.6%, 9.7%, 9.8%, 9.9%, 10%, etc. Any value in the range of 0.1% to 10%, a small amount of addition can have a better effect. In this embodiment, the additive is added in an amount of 0.1% to exert a good effect of inhibiting dendrite formation, ion transport and alleviating electrolyte corrosion of metal electrodes, but it is not advisable to add too much to prevent the electrolyte from being too acidic and corroding the positive electrode material.
[0054] In some embodiments, the electrolyte further includes a solvent and a metal salt, wherein the solvent is used to dissolve and disperse the solutes in the electrolyte, and the metal salt plays a role in transporting ions.
[0055] As mentioned above, perfluorosulfonic acid additives containing perfluorosulfonic acid groups can be widely used in the production of proton exchange membranes for fuel cells. However, after the membrane is formed, it is extremely dependent on water because water promotes the dissociation of sulfonic acid groups and proton conduction. In order to ensure the high performance and stability of the fuel cell, it is necessary to keep the water content in the proton exchange membrane stable and sufficient, which makes the proton exchange membrane formed by perfluorosulfonic acid compounds difficult to use under high temperature and low humidity conditions. In the present invention, the additive having a perfluorosulfonic acid group of the present invention is applied to an electrolyte containing a non-aqueous solvent and applied to a metal battery. The solid electrolyte phase can be formed on the surface of the metal-based electrode without relying on water. It does not rely on water in reducing the risk of dendrites in the battery, improving ion transmission, and reducing the risk of electrolyte corrosion of the electrode, and has low dependence on application conditions.
[0056] Exemplarily, in the present invention, the solvent in the electrolyte includes an organic solvent, and the organic solvent includes fluoroethylene carbonate, linear ethylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, ethyl butyrate, fluoroethylene carbonate, 1,4-butyrolactone and γ-butyrolactone, propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, formic acid, At least one of methyl ester, methyl acetate, fluoroethylene carbonate, ethyl acetate, γ-butyrolactone, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, triethylene glycol dimethyl ether, dimethyl sulfone, dimethyl ether, vinyl sulfite, propylene sulfite, dimethyl sulfite, and diethyl sulfite. The above organic solvents have a good dissolving and dispersing effect on solutes in the electrolyte, such as additives, and are conducive to forming a uniform and compact solid electrolyte phase on the surface of the metal-based electrode in contact with the electrolyte.
[0057] It is understandable that the solvent in the electrolyte of the present invention may include an aqueous solvent in addition to an organic solvent, but in the application of the present invention, the additive does not rely on water to exert its effect.
[0058] In the present invention, the additive can be attached to the surface of various metal matrices to form a solid electrolyte phase, such as a lithium metal matrix, a sodium metal matrix, a potassium metal matrix, an aluminum metal matrix, a magnesium metal matrix, etc. Therefore, the electrolyte of the present invention is suitable for various metal batteries, such as lithium ion batteries, sodium ion batteries, potassium ion batteries, aluminum ion batteries, magnesium ion batteries, etc., and has a wide range of applications.
[0059] Based on this, different metal salts can be selected according to different types of metal batteries. In some embodiments, the metal salt includes at least one of lithium salt, sodium salt, potassium salt, aluminum salt, and magnesium salt. When applied to lithium-ion batteries, the metal salt in the electrolyte may include lithium salt, when applied to sodium-ion batteries, the metal salt in the electrolyte may include sodium salt, when applied to potassium-ion batteries, the metal salt in the electrolyte may include potassium salt, when applied to aluminum-ion batteries, the metal salt in the electrolyte may include aluminum salt, and when applied to magnesium-ion batteries, the metal salt in the electrolyte may include magnesium salt.
[0060] In some embodiments, the metal salt in the electrolyte includes a lithium salt, and the lithium salt includes lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium bis(fluoromethylsulfonyl)imide (LiFSI), lithium trifluoromethylsulfonate (LiCF3SO3), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), LiAsF6, LiClO4, lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiDFOB ...borate (Li Lithium (trifluoromethylsulfonate)imide [LiN(CF3SO2)2, LiTFSI] and its derivatives, lithium perfluoroalkyl phosphate [LiPF3(C2F5)3, LiFAP], lithium tetrafluorooxalate phosphate [LiPF4(C2O4)], lithium bis(oxalatoborate) (LiBOB), lithium tris(catechol) phosphate (LTBP) and sulfonated polysulfonamide lithium salt, one or more of LiPF6, LiClO4, LiCoO2, LiBF4, LiAsF6, LiNO3, LiCO3, LiCl.
[0061] In the present invention, the preparation method of the electrolyte comprises the following steps: dissolving the metal salt and the additive in the solvent, and mixing to obtain the electrolyte. In some embodiments, stirring can be used to promote the rapid dissolution and dispersion of the solute to obtain a uniform electrolyte, illustratively, using a vacuum stirrer for stirring.
[0062] The present invention also provides a battery, which includes the electrolyte as described above and has at least all the beneficial effects of the electrolyte as described above.
[0063] The additives in the above-mentioned electrolyte of the present invention can be attached to the surface of various metal matrices to form a solid electrolyte phase. Therefore, the battery of the present invention includes a lithium ion battery, a sodium ion battery, a potassium ion battery, an aluminum ion battery or a magnesium ion battery. The additive forms a solid electrolyte phase on the surface of the metal-based electrode of the above types of batteries, which can not only effectively reduce the risk of dendrites generated in the metal-based electrodes of the battery, and alleviate the problems of thermal runaway caused by short circuits caused by dendrites during the charge and discharge cycle of the battery, but also can achieve efficient ion transmission performance, and also play a role in inhibiting the corrosion of the metal electrode by the electrolyte, thereby reducing the side reactions of the battery during the cycle.
[0064] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following specific embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0065] Example 1
[0066] 1. Preparation of positive electrode sheet
[0067] The positive electrode active material LFP, electrolyte material, conductive agent Super-P, and binder SBR are mixed in a mass ratio of 8:1:1, and the solvent NMP is added. The mixture is stirred under the action of a vacuum mixer until the system becomes uniform to obtain a positive electrode slurry; the positive electrode slurry is evenly coated on the two surfaces of the positive electrode current collector aluminum foil, dried at room temperature, and then transferred to an oven for further drying, and then cold pressed and cut to obtain positive electrode sheets.
[0068] 2. Preparation of negative electrode sheet
[0069] The lithium foil is attached to the two surfaces of the negative electrode current collector copper foil by rolling, and then cut into negative electrode sheets of the required size.
[0070] 3. Preparation of electrolyte
[0071] According to the relevant parameters shown in Table 1, lithium salt and additive (hereinafter referred to as PFSA) are dissolved in fluorocarbonate and linear carbonate, and a uniform electrolyte is obtained under stirring of a vacuum stirrer. The additive in this embodiment is perfluorosulfonic acid, the chemical formula is C4F9SO4H, and the structural formula is as follows:
[0072]
[0073] 4. Prepare the diaphragm
[0074] PE separator is selected as the separator for lithium metal batteries.
[0075] 5. Preparation of lithium metal batteries
[0076] The positive electrode sheet, electrolyte, separator and lithium negative electrode sheet prepared above are stacked in sequence to prepare a lithium metal battery under a pressure of 0.5 MPa.
[0077] Example 2 and Example 3
[0078] Example 2 The positive electrode sheet, negative electrode sheet and separator of Example 1 are selected, and a lithium metal battery is prepared with reference to the preparation method of the lithium metal battery of Example 1. However, the formula of the electrolyte of Example 2 is different from that of the electrolyte of Example 1, and the content of the perfluorosulfonic acid compound is different, as shown in Table 1 for details.
[0079] Example 4 and Example 5
[0080] In Example 4 and Example 5, the positive electrode sheet, negative electrode sheet and separator of Example 1 are selected, and lithium metal batteries are prepared with reference to the preparation method of the lithium metal battery of Example 1. However, the electrolyte of Example 2 has a different formula from the electrolyte of Example 1, and different lithium salts are selected, as shown in Table 1 for details.
[0081] Comparative Example 1
[0082] Comparative Example 1 The positive electrode sheet, negative electrode sheet and separator of Example 1 were selected, and a lithium metal battery was prepared with reference to the preparation method of the lithium metal battery of Example 1. However, the electrolyte of Example 2 had a different formula from the electrolyte of Example 1, and no perfluorosulfonic acid compound was added, as shown in Table 1 for details.
[0083] Performance Testing
[0084] 1. The surface of the metal-based electrode of Example 1 was characterized by scanning electron microscopy. Figure 2 , a solid electrolyte phase is formed on the surface of the metal-based electrode.
[0085] 2. Taking Example 1 as an example, the electrolyte contains 1% of the additive perfluorosulfonic acid, and the schematic diagram of the perfluorosulfonic acid acting on the negative electrode is as follows: Figure 1 As shown, the CF organic hydrocarbon chain with stable adsorption and the perfluorosulfonic acid group with Lewis acid electron-donating characteristics can be firmly adsorbed on the surface of the lithium metal electrode to form a solid electrolyte phase.
[0086] 3. Test the performance of the lithium metal batteries prepared in Examples 1 to 5 and Comparative Example 1.
[0087] Cyclic performance test 1: The components of the embodiment and the comparative example were assembled into lithium metal symmetrical batteries, and the battery was heated at 25°C and a current density of 10 mA cm -1 The specific capacity reaches 10 mAh cm -1 The test results are shown in Table 1. The results of Example 1 and Comparative Example 1 can also be seen in Table 1. Figure 3 The result of Example 1 is expressed as an experimental sample, and the result of Comparative Example 1 is expressed as a comparative sample.
[0088] Cycle performance test 2: The components of the embodiment and the comparative example were assembled into a lithium metal full battery, charged to 4.2V at 1C constant current at 25°C, and then discharged to 2.5V at 1C constant current, which was a charge and discharge cycle. The first discharge capacity was 100%, and the number of cycles when the discharge capacity dropped to 80% was the cycle life. The capacity retention rate was measured. The test results are shown in Table 1. The results of embodiment 1 and comparative example 1 can also be seen in Table 1. Figure 4 The result of Example 1 is expressed as an experimental sample, and the result of Comparative Example 1 is expressed as a comparative sample.
[0089] Table 1
[0090]
[0091] It can be seen from Table 1 that Examples 1 to 5 add 1%, 2%, 5%, 1%, and 2% additives to ordinary LiPF6 electrolyte (BE) and assemble them into lithium metal symmetrical batteries. The additives in the electrolyte can form a solid electrolyte phase on the surface of the metal-based electrode of the battery. The formed solid electrolyte phase can not only effectively reduce the risk of dendrite generation during the charge and discharge cycle of the battery, alleviate the problem of short circuit caused by dendrite generation and subsequent thermal runaway, but also can achieve efficient ion transport performance, and can also inhibit the corrosion of the metal electrode by the electrolyte, thereby reducing the occurrence of side reactions in the battery during the cycle.
[0092] Test results such as Figure 3 and Figure 4 As shown, the symmetrical battery is at 10 mA cm -1 and 10mAh·cm -1 The battery was cycled for up to 600 hours under the condition of 1000 mAh·mg / L, and in the full battery test 2, after 600 cycles, it still had about 110 mAh·mg / L. -1 The capacity retention rate reaches more than 55%, which prolongs the cycle life of the battery. No additives are added to the electrolyte of Comparative Example 1, and the performance of the lithium metal symmetric battery assembled therefrom is reduced.
[0093] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. An electrolyte, characterized in that: The electrolyte includes an additive containing a perfluorosulfonic acid group and at least one CF group.
2. The electrolyte according to claim 1, characterized in that The additive comprises at least one of the following structural formulas: R in the structural formula (III) comprises an organic hydrocarbon chain containing a CF group, and the number of the CF groups is greater than or equal to 2; R in the structural formula (IV) comprises an organic hydrocarbon chain containing CF groups, and the number of the CF groups is greater than or equal to 2.
3. The electrolyte according to claim 2, characterized in that R in the structural formula (III) comprises an organic hydrocarbon chain containing only CF groups; and / or, R in the structural formula (IV) comprises an organic hydrocarbon chain containing only CF groups; and / or, the number of CF groups in R in the structural formula (III) is greater than or equal to 9; and / or, the number of CF groups in R in the structural formula (IV) is greater than or equal to 9; And / or, the structural formula of the additive is as follows:
4. The electrolyte according to claim 1, characterized in that Based on 100% of the total mass of the electrolyte, the content of the additive is 0.1% to 10%; And / or, the electrolyte further comprises a solvent and a metal salt.
5. The electrolyte according to claim 4, characterized in that The electrolyte includes a solvent, and the solvent includes an organic solvent and / or an aqueous solvent.
6. The electrolyte according to claim 5, characterized in that The solvent is an organic solvent, and the organic solvent includes at least one of fluoroethylene carbonate, linear ethylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, ethyl butyrate, fluoroethylene carbonate, 1,4-butyrolactone and γ-butyrolactone, propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, methyl formate, methyl acetate, fluoroethylene carbonate, ethyl acetate, γ-butyrolactone, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, triethylene glycol dimethyl ether, dimethyl sulfone, dimethyl ether, ethylene sulfite, propylene sulfite, dimethyl sulfite, and diethyl sulfite.
7. The electrolyte according to claim 4, characterized in that The electrolyte includes a metal salt, and the metal salt includes at least one of a lithium salt, a sodium salt, a potassium salt, an aluminum salt, and a magnesium salt.
8. The electrolyte according to claim 7, characterized in that The metal salt is a lithium salt, and the lithium salt includes one or more of lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl imide), lithium bis(fluoromethylsulfonyl imide), lithium trifluoromethylsulfonate, lithium tetrafluoroborate, lithium difluorophosphate, LiAsF6, LiClO4, lithium bis(oxalatoborate) and lithium di(fluorooxalatoborate), lithium trifluoromethylsulfonate, lithium bis(trifluoromethylsulfonate)imide and its derivatives, perfluoroalkyl lithium phosphate, lithium tetrafluorooxalate phosphate, lithium bis(oxalatoborate), lithium tris(catechol) phosphate and sulfonated polysulfonamide lithium salt, LiPF6, LiClO4, LiCoO2, LiBF4, LiAsF6, LiNO3, LiCO3, and LiCl.
9. A battery, characterized in that: The battery comprises the electrolyte according to any one of claims 1 to 8.
10. The battery according to claim 9, characterized in that The battery includes a lithium ion battery, a sodium ion battery, a potassium ion battery, an aluminum ion battery or a magnesium ion battery.