Sodium-ion battery electrolyte and production process thereof
The problem of insufficient performance of sodium ion batteries is solved by using the doped carbon interface formed by titanium dioxide and oleamine in sodium ion batteries, and the molecular adsorption layer of sodium dodecylbenzenesulfonate, and the problem of insufficient performance of sodium ion batteries is improved, and the conductivity and cycling stability are improved. , enhances the transmission and diffusion capabilities of sodium ions.
Patent Information
- Application Number
- CN202411274284.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-12
AI Technical Summary
In applications, sodium ion batteries have problems such as insufficient performance, mass-specific capacity and volume-specific capacity, which are mainly due to the deintercalation kinetics caused by the large sodium ion radius and the low density of carbon materials.
Titanium dioxide is used as a supporting material, long-chain molecules of oleamine are inserted into its monoclinic structure to broaden the layer spacing, and a titanium dioxide-doped carbon interface is formed through heat treatment to form an interface-coupled defective heterostructure to quickly transmit electrons. Sodium dodecylbenzenesulfonate assists the amphiphilic molecules to form a molecular adsorption layer, increasing the passivation degree of the electrode surface and forming a stable solid electrolyte phase interface film.
Enhanced the migration ability of sodium ions, improve the conductivity, shorten the diffusion distance of sodium ions, reduce the occurrence of side reactions, maintain the stability of the electrode structure, improve the transmission and diffusion ability of sodium ions, and enhance the battery Capacity retention rate and cycle stability.
Smart Images

Figure BDA0005039668330000061
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a sodium ion battery electrolyte and a production process thereof. Background Art
[0002] As a chemical power source, lithium-ion batteries (LIBs) have become an indispensable utility in today's society. Due to the in-depth research on lithium-ion battery materials and processes for more than 25 years and the discovery of new lithium resources, the cost of key components of lithium-ion batteries has dropped significantly. However, considering the increasing demand for lithium-ion batteries in the market, it is crucial to design a cheaper and more sustainable energy storage device. Sodium-ion batteries (SIBs) are an alternative. Sodium and lithium are in the same main group and have similar physical and chemical properties. Therefore, in principle, sodium-ion batteries with the same principle and similar properties can be constructed. Compared with lithium-ion batteries, the biggest advantage of sodium-ion batteries is that sodium resources are abundant and evenly distributed. The abundance of lithium in the earth's crust is only 0.0017%, while the abundance of sodium is 2.3%, which is 1353 times that of lithium. Therefore, the cost and supply guarantee of raw materials for sodium-ion batteries are far superior to those of lithium-ion batteries. And sodium ions do not react with aluminum to form an alloy, so the copper foil of the negative electrode collector of the sodium ion battery can be replaced by aluminum foil, which can not only further reduce the cost of the battery, but also reduce the weight of the battery and increase its energy density.
[0003] However, the radius of sodium ions (0.102 nm) is 34.2% larger than that of lithium ions (0.076 nm), which results in insufficient rate performance, mass specific capacity, and volume specific capacity in sodium ion battery applications due to the sodium ion deintercalation kinetics and the low density of carbon materials themselves. Summary of the invention
[0004] The object of the present invention is to provide a sodium ion battery electrolyte and a production process thereof to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a production process of sodium ion battery electrolyte, comprising the following preparation steps:
[0006] (1) Oleylamine and ethanol were mixed, stirred at 600-900 rpm for 20 min, tetrabutyl titanate was added, and stirring was continued for 20 min, deionized water was added, and stirring was continued for 100-150 min, and placed in a dark place for 12 h, and then centrifuged, the solid was collected, and dried to obtain intermediate A;
[0007] (2) Mix deionized water and ethanol, stir at 600-900 rpm for 20 min, add intermediate A, continue stirring for 20 min, react at 160° C. for 10-15 h, filter, take the solid, wash with deionized water for 3-6 times, and then dry and anneal to obtain carbon-doped titanium dioxide;
[0008] (3) Ethylene glycol dimethyl ether, sodium dodecylbenzene sulfonate and sodium acetate are mixed, stirred at 50-150 rpm for 10 min, sodium hexafluorophosphate and carbon-doped titanium dioxide are added, and stirred thoroughly to obtain a sodium ion battery electrolyte.
[0009] Furthermore, the rate of adding tetrabutyl titanate in step (1) is 10 to 30 g / min.
[0010] Furthermore, the centrifugation speed in step (1) is 8000 rpm and the time is 10 to 20 min.
[0011] Furthermore, in step (1), the mass ratio of oleylamine, ethanol, tetrabutyl titanate and deionized water is 1-4:150-300:3-6:0.5-2.
[0012] Furthermore, the annealing temperature in step (2) is 400-580° C. and the annealing time is 90-150 min.
[0013] Furthermore, in step (2), the mass ratio of deionized water, ethanol and intermediate A is 1:2:0.1-0.5.
[0014] Furthermore, the drying temperature in step (1) and step (2) is 37-50° C. and the drying time is 12 hours.
[0015] Furthermore, the step (3) is carried out under a nitrogen atmosphere.
[0016] Furthermore, in step (3), the stirring rate is 450 to 800 rpm and the time is 10 to 15 hours.
[0017] Furthermore, in step (3), the mass ratio of ethylene glycol dimethyl ether, sodium dodecylbenzene sulfonate, sodium acetate, sodium hexafluorophosphate, and carbon-doped titanium dioxide is 5-7:0.4-0.7:0.05-0.2:1.5-2:0.005.
[0018] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the present invention adopts titanium dioxide as a supporting material, and utilizes the long-chain molecules of oleylamine to be inserted into the lattice of its monoclinic structure, thereby widening the interlayer spacing of titanium dioxide, making it easier for sodium ions to enter the crystal structure and quickly charge and discharge; then, through heat treatment, a titanium dioxide-doped carbon interface is formed, wherein oxygen vacancies exist between titanium dioxide and titanium-carbon bonds, resulting in the formation of an interface-coupled defective heterostructure, which can quickly transmit electrons and is beneficial to the migration of sodium ions, thereby enhancing the electrical conductivity; then, sodium dodecylbenzene sulfonate is used to assist the amphiphilic molecule, and the hydrophilic groups in the amphiphilic molecule will be adsorbed on the surface of the positive electrode sheet with polarity, and at the same time, sodium dodecylbenzene sulfonate and the amphiphilic molecule will be adsorbed on the surface of the positive electrode sheet with polarity. The hydrophobic groups contact the electrolyte matrix to form a molecular adsorption layer. The existence of the adsorption layer prevents water molecules from directly contacting the positive electrode particles, which plays a certain degree of protection. In the cycle process, ethylene glycol dimethyl ether can increase the passivation degree of the electrode surface and form a thin, strong and stable solid electrolyte phase interface film, which effectively isolates the direct contact between the electrolyte and the electrode, shortens the diffusion distance of sodium ions, reduces the occurrence of side reactions, and maintains the stability of the electrode structure, which is more conducive to the rapid transfer of sodium ions and electrons. Titanium dioxide presents a small granular structure, which is connected together to form a coral-like porous structure under the coupling effect of ethylene glycol dimethyl ether, thereby improving the transmission and diffusion of sodium ions, the capacity retention rate of the battery and the cycle stability. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0020] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the sodium ion battery electrolyte prepared in the following examples.
[0021] Under an argon atmosphere, the battery components were assembled in the order of negative electrode shell, spring sheet, gasket, sodium metal sheet, diaphragm, sodium ion battery electrolyte (40 μL), electrode sheet and positive electrode shell to obtain a sodium ion battery.
[0022] Cycle performance: Neware charge and discharge tester was used, at 1.0C current, charging mode: constant current and constant voltage charging to 4.2V, cut-off current 0.03CmA, discharging mode: constant current discharge to 3.0V; the sample was charged and discharged 500 times, and its discharge capacity and capacity retention rate were tested.
[0023] Example 1
[0024] (1) oleylamine and ethanol were mixed, stirred at 600 rpm for 20 min, tetrabutyl titanate was added at 10 g / min, stirring was continued for 20 min, deionized water was added, stirring was continued for 100 min, and the mixture was placed in a dark place for 12 h, then centrifuged at 8000 rpm for 10 min, the solid was taken, and dried at 37° C. for 12 h to obtain intermediate A; the mass ratio of oleylamine, ethanol, tetrabutyl titanate, and deionized water was 1:150:3:0.5;
[0025] (2) Deionized water and ethanol were mixed, stirred at 600 rpm for 20 min, intermediate A was added, and stirring was continued for 20 min. The mixture was reacted at 160° C. for 10 h, filtered, and the solid was taken out and washed with deionized water for 3 times. The solid was then dried at 37° C. for 12 h, and annealed at 400° C. for 90 min to obtain carbon-doped titanium dioxide. The mass ratio of the deionized water, ethanol, and intermediate A was 1:2:0.1.
[0026] (3) Under a nitrogen atmosphere, ethylene glycol dimethyl ether, sodium dodecylbenzene sulfonate, and sodium acetate were mixed, stirred at 50 rpm for 10 min, sodium hexafluorophosphate and carbon-doped titanium dioxide were added, and stirred at 450 rpm for 10 h to obtain a sodium ion battery electrolyte; the mass ratio of ethylene glycol dimethyl ether, sodium dodecylbenzene sulfonate, sodium acetate, sodium hexafluorophosphate, and carbon-doped titanium dioxide was 5:0.4:0.05:1.5:0.005.
[0027] Example 2
[0028] (1) oleylamine and ethanol were mixed, stirred at 750 rpm for 20 min, tetrabutyl titanate was added at 20 g / min, stirring was continued for 20 min, deionized water was added, stirring was continued for 120 min, and the mixture was placed in a dark place for 12 h, and then centrifuged at 8000 rpm for 15 min. The solid was taken and dried at 40° C. for 12 h to obtain intermediate A; the mass ratio of oleylamine, ethanol, tetrabutyl titanate and deionized water was 2.5:230:4.5:1.4;
[0029] (2) Deionized water and ethanol were mixed, stirred at 750 rpm for 20 min, intermediate A was added, and stirring was continued for 20 min. The mixture was reacted at 160° C. for 12 h, filtered, and the solid was taken out and washed with deionized water for 5 times. The solid was then dried at 40° C. for 12 h, and annealed at 500° C. for 120 min to obtain carbon-doped titanium dioxide. The mass ratio of deionized water, ethanol, and intermediate A was 1:2:0.3.
[0030] (3) Under a nitrogen atmosphere, ethylene glycol dimethyl ether, sodium dodecylbenzene sulfonate, and sodium acetate were mixed, stirred at 100 rpm for 10 min, sodium hexafluorophosphate and carbon-doped titanium dioxide were added, and stirred at 600 rpm for 12 h to obtain a sodium ion battery electrolyte; the mass ratio of ethylene glycol dimethyl ether, sodium dodecylbenzene sulfonate, sodium acetate, sodium hexafluorophosphate, and carbon-doped titanium dioxide was 6:0.5:0.15:1.75:0.005.
[0031] Example 3
[0032] (1) oleylamine and ethanol were mixed, stirred at 900 rpm for 20 min, tetrabutyl titanate was added at 30 g / min, the stirring was continued for 20 min, deionized water was added, the stirring was continued for 150 min, the mixture was placed in a dark place for 12 h, and then centrifuged at 8000 rpm for 20 min. The solid was taken and dried at 50° C. for 12 h to obtain intermediate A; the mass ratio of oleylamine, ethanol, tetrabutyl titanate and deionized water was 4:300:6:2;
[0033] (2) Deionized water and ethanol were mixed, stirred at 900 rpm for 20 min, intermediate A was added, and stirring was continued for 20 min. The mixture was reacted at 160° C. for 15 h, filtered, and the solid was taken out and washed with deionized water for 6 times. The solid was then dried at 50° C. for 12 h, and annealed at 580° C. for 150 min to obtain carbon-doped titanium dioxide. The mass ratio of deionized water, ethanol, and intermediate A was 1:2:0.5.
[0034] (3) Under a nitrogen atmosphere, ethylene glycol dimethyl ether, sodium dodecylbenzene sulfonate, and sodium acetate were mixed, stirred at 150 rpm for 10 min, sodium hexafluorophosphate and carbon-doped titanium dioxide were added, and stirred at 800 rpm for 15 h to obtain a sodium ion battery electrolyte; the mass ratio of ethylene glycol dimethyl ether, sodium dodecylbenzene sulfonate, sodium acetate, sodium hexafluorophosphate, and carbon-doped titanium dioxide was 7:0.7:0.2:2:0.005.
[0035] Comparative Example 1
[0036] The difference between Comparative Example 1 and Example 2 is that step (1) is different. Step (1) is changed to: tetrabutyl titanate is added to ethanol at 20 g / min, stirring is continued for 20 min, deionized water is added, stirring is continued for 120 min, and the mixture is placed in a dark place for 12 h, followed by centrifugation at 8000 rpm for 15 min, the solid is taken, and dried at 40° C. for 12 h to obtain intermediate A; the mass ratio of tetrabutyl titanate, ethanol, and deionized water is 4.5:230:1.4; and the remaining steps are the same as those in Example 2.
[0037] Comparative Example 2
[0038] The difference between Comparative Example 2 and Example 2 is that step (2) is different. Step (2) is changed to: deionized water and ethanol are mixed, stirred at 750 rpm for 20 min, intermediate A is added, and stirring is continued for 20 min. At 160° C., the reaction is carried out for 12 h. The solid is filtered and washed with deionized water 5 times. The solid is dried at 40° C. for 12 h to obtain titanium dioxide. The mass ratio of the deionized water, ethanol and intermediate A is 1:2:0.3. The remaining steps are the same as those in Example 2.
[0039] Comparative Example 3
[0040] The difference between Comparative Example 3 and Example 2 is that there is no step (1) and step (2), and step (3) is changed to: under a nitrogen atmosphere, ethylene glycol dimethyl ether, sodium dodecylbenzene sulfonate, and sodium acetate are mixed, stirred at 100 rpm for 10 min, sodium hexafluorophosphate and are added, and stirred at 600 rpm for 12 h to obtain a sodium ion battery electrolyte; the mass ratio of ethylene glycol dimethyl ether, sodium dodecylbenzene sulfonate, sodium acetate, and sodium hexafluorophosphate is 6:0.5:0.15:1.75; the remaining steps are the same as in Example 2.
[0041] Comparative Example 4
[0042] The difference between Comparative Example 4 and Example 2 is that step (3) is different. Step (3) is changed to: under a nitrogen atmosphere, ethylene glycol dimethyl ether and sodium acetate are mixed, stirred at 100 rpm for 10 min, sodium hexafluorophosphate and carbon-doped titanium dioxide are added, and stirred at 600 rpm for 12 h to obtain a sodium ion battery electrolyte; the mass ratio of ethylene glycol dimethyl ether, sodium acetate, sodium hexafluorophosphate and carbon-doped titanium dioxide is 6:0.15:1.75:0.005; the remaining steps are the same as in Example 2.
[0043] Comparative Example 5
[0044] The difference between Comparative Example 5 and Example 2 is that step (3) is different. Step (3) is changed to: under a nitrogen atmosphere, ethylene carbonate, sodium dodecylbenzene sulfonate and sodium acetate are mixed, stirred at 100 rpm for 10 min, sodium hexafluorophosphate and carbon-doped titanium dioxide are added, and stirred at 600 rpm for 12 h to obtain a sodium ion battery electrolyte; the mass ratio of ethylene carbonate, sodium dodecylbenzene sulfonate, sodium acetate, sodium hexafluorophosphate and carbon-doped titanium dioxide is 6:0.5:0.15:1.75:0.005; the remaining steps are the same as in Example 2.
[0045] Effect example
[0046] The following Table 1 shows the performance analysis results of the sodium ion battery electrolytes of Examples 1 to 3 of the present invention and Comparative Examples 1 to 5.
[0047] Table 1
[0048]
[0049] From the comparison of the experimental data of the embodiment and the comparative example in Table 1, it can be found that the present invention uses titanium dioxide as a supporting material, and uses the long-chain molecules of oleylamine to be inserted into the lattice of its monoclinic structure, thereby widening the interlayer spacing of titanium dioxide, making it easier for sodium ions to enter the crystal structure and quickly charge and discharge. Then, through heat treatment, a titanium dioxide-doped carbon interface is formed, wherein oxygen vacancies exist between titanium dioxide and titanium-carbon bonds, resulting in the formation of an interface-coupled defective heterostructure, which can quickly transmit electrons and is beneficial to the migration of sodium ions, thereby enhancing the conductivity. Then, sodium dodecylbenzene sulfonate is used to assist the amphiphilic molecule, and the hydrophilic groups in the amphiphilic molecule will be adsorbed on the carbon-doped titanium dioxide. The surface of the positive electrode sheet has polarity, and the hydrophobic groups in the sodium dodecylbenzene sulfonate and the amphiphilic molecules are in contact with the electrolyte matrix to form a molecular adsorption layer. The existence of the adsorption layer prevents water molecules from directly contacting the positive electrode particles, which plays a certain degree of protection. In the cycle process, ethylene glycol dimethyl ether can increase the passivation degree of the electrode surface and form a thin, strong and stable solid electrolyte phase interface film, which is more conducive to the rapid transfer of sodium ions and electrons. Titanium dioxide presents a small granular structure, which is connected together under the coupling effect of ethylene glycol dimethyl ether, thereby improving the transmission and diffusion of sodium ions, the capacity retention rate of the battery and the cycle stability.
[0050] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A production process for sodium ion battery electrolyte, characterized in that: The following steps are involved: (1) Oleylamine and ethanol were mixed, stirred at 600-900 rpm for 20 min, tetrabutyl titanate was added, and stirring was continued for 20 min, deionized water was added, and stirring was continued for 100-150 min, and placed in a dark place for 12 h, and then centrifuged, the solid was collected, and dried to obtain intermediate A; (2) Mix deionized water and ethanol, stir at 600-900 rpm for 20 min, add intermediate A, continue stirring for 20 min, react at 160° C. for 10-15 h, filter, take the solid, wash with deionized water for 3-6 times, and then dry and anneal to obtain carbon-doped titanium dioxide; (3) Ethylene glycol dimethyl ether, sodium dodecylbenzene sulfonate and sodium acetate are mixed, stirred at 50-150 rpm for 10 min, sodium hexafluorophosphate and carbon-doped titanium dioxide are added, and stirred thoroughly to obtain a sodium ion battery electrolyte.
2. The production process of a sodium ion battery electrolyte according to claim 1, characterized in that: The rate of adding tetrabutyl titanate in step (1) is 10 to 30 g / min.
3. The production process of a sodium ion battery electrolyte according to claim 1, characterized in that: The centrifugation speed in step (1) is 8000 rpm and the time is 10 to 20 minutes.
4. The production process of a sodium ion battery electrolyte according to claim 1, characterized in that: The mass ratio of oleylamine, ethanol, tetrabutyl titanate and deionized water in step (1) is 1-4:150-300:3-6:0.5-2.
5. The production process of a sodium ion battery electrolyte according to claim 1, characterized in that: The annealing temperature in step (2) is 400-580° C. and the annealing time is 90-150 min.
6. The production process of a sodium ion battery electrolyte according to claim 1, characterized in that: The mass ratio of deionized water, ethanol and intermediate A in step (2) is 1:2:0.1-0.
5.
7. The production process of a sodium ion battery electrolyte according to claim 1, characterized in that: The drying temperature in step (1) and step (2) is 37-50° C. and the drying time is 12 hours.
8. The production process of a sodium ion battery electrolyte according to claim 1, characterized in that: The step (3) is carried out under a nitrogen atmosphere.
9. The production process of a sodium ion battery electrolyte according to claim 1, characterized in that: The stirring rate of step (3) is 450-800 rpm and the time is 10-15 hours.
10. The production process of a sodium ion battery electrolyte according to claim 1, characterized in that: The mass ratio of ethylene glycol dimethyl ether, sodium dodecylbenzene sulfonate, sodium acetate, sodium hexafluorophosphate and carbon-doped titanium dioxide in step (3) is 5-7:0.4-0.7:0.05-0.2:1.5-2:0.005.