Preparation method of naked battery cell, lithium ion battery and assembly method of lithium ion battery
By using a drying membrane with an initial temperature of 45℃-120℃ in the lithium-ion battery, directly winding it with the positive electrode sheet and the negative electrode sheet, and optimizing the drying path and conditions, the problem of high deformation rate of the lithium-ion battery is solved, and the Lower heat shrinkage and higher productivity.
Patent Information
- Application Number
- CN202410939434.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-12
AI Technical Summary
The existing lithium-ion batteries have thermal shrinkage of the diaphragm due to high temperatures during battery cell baking, which affects the battery deformation rate, resulting in a high deformation rate after charging, making it difficult to meet the actual application needs.
The drying diaphragm with an initial temperature of 45°C-120°C was directly wound with the positive and negative electrode sheets, and passed through the drying area through a folded linear route, and the drying operation conditions were optimized to reduce the heat shrinkage of the diaphragm.
It significantly reduces the deformation rate of lithium-ion batteries, improves production efficiency, and is suitable for industrial promotion.
Smart Images

Figure CN118943498A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery assembly, and in particular to a method for preparing a bare battery cell, a lithium ion battery and an assembly method thereof. Background Art
[0002] The assembly method of conventional lithium-ion batteries includes die-cutting, winding, tab welding, and cell baking. The main purpose of cell baking is to remove moisture from the diaphragm and control the subsequent gas production and side reactions of the battery. Cell baking generally includes cell assembly, oven placement, baking, cooling, moisture measurement, tray removal, and transportation, which is time-consuming. In addition, in order to meet the moisture value requirements, high baking temperatures and long baking times are required when baking the cells, which can easily aggravate the thermal shrinkage of the diaphragm.
[0003] To this end, the relevant technology bakes the positive and negative electrodes and diaphragms of the battery in the front-end process. Compared with the method of baking after packaging, it can make the heat penetrate the positive and negative electrodes and diaphragms quickly, the baking time is short, the baking process is omitted, the online time of the battery is shortened, and the moisture value requirements can be met at the same time. However, in actual applications, after the lithium-ion battery made by this technology is fully charged, it will be found that its deformation rate is high when it is disassembled.
[0004] Therefore, how to reduce the deformation rate of subsequent lithium-ion batteries when using a diaphragm baking process is a technical problem that needs to be solved urgently. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for preparing a bare cell, a lithium ion battery and an assembly method thereof.
[0006] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a method for preparing a bare battery cell, wherein the method comprises the following steps: winding a dried diaphragm, a positive electrode sheet and a negative electrode sheet to obtain a bare battery cell; wherein the initial temperature of the dried diaphragm during the winding process is 45°C-120°C.
[0007] A second aspect of the present invention provides a method for assembling a lithium ion battery, wherein the method comprises the following steps: (1) preparing a bare cell according to the method described in the first aspect of the present invention; (2) The bare cell is subjected to tab welding, film coating, packaging and liquid injection to obtain a lithium-ion battery.
[0008] The third aspect of the present invention provides a lithium ion battery prepared by the method described in the second aspect of the present invention.
[0009] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows: 1) The method for preparing the bare battery cell provided in the present invention is innovative in that the dried separator with an initial temperature of 45°C-120°C is directly wound with the positive electrode sheet and the negative electrode sheet. In other words, the separator is directly wound at a high temperature. Experimental verification shows that this unique method can reduce the deformation rate of the subsequent lithium-ion battery. 2) The method for preparing the bare cell provided in the present invention can significantly reduce the thermal shrinkage rate of the diaphragm during the drying process by optimizing the path of the diaphragm passing through the drying area; 3) The method for preparing the bare battery cell provided in the present invention can reduce the thermal shrinkage of the diaphragm as much as possible while meeting the moisture value requirements of the diaphragm by optimizing the specific operating conditions of the drying operation; 4) The lithium-ion battery assembly method provided in the present invention can significantly improve production efficiency, reduce product defect rate, and is suitable for industrial promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 It is a structural schematic diagram of a baking oven provided in the present invention; Figure 2 It is a structural schematic diagram of a baking oven provided in the present invention; Figure 3 It is a schematic diagram of a diaphragm provided by the present invention passing through a roller in an oven; Figure 4 It is a schematic diagram of a central angle α of a roller corresponding to an arc formed by a contact area between a diaphragm and a roller provided in the present invention; Figure 5 1 is a diagram showing deformation test results of the lithium-ion battery prepared in Example 1; Figure 6 1 is a diagram showing the deformation test results of the lithium-ion battery prepared in Example 2.
[0011] Description of Reference Numerals DETAILED DESCRIPTION
[0012] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0013] In the related art, when the battery cell is baked, the internal pole piece and the diaphragm are tightly stacked, and the inner layer of moisture is often difficult to escape; in addition, water vapor can only be discharged from the injection hole with a diameter of 2-3mm, so the baking effect is generally poor. In order to improve the baking effect, high vacuum, high baking temperature, and long baking time are required to achieve the required moisture value. However, high baking temperature and long baking time will aggravate the thermal shrinkage of the diaphragm. When the diaphragm shrinks severely, it can affect ionic conductivity and affect the diaphragm coating. The coating deteriorates and can cause the battery cell to short-circuit.
[0014] The first aspect of the present invention provides a method for preparing a bare battery cell, wherein the method comprises the following steps: winding a dried diaphragm, a positive electrode sheet and a negative electrode sheet to obtain a bare battery cell; wherein the initial temperature of the dried diaphragm during the winding process is 45°C-120°C.
[0015] Among them, in the present invention, the inventors have found through research that the dried diaphragm with an initial temperature of 45°C-120°C is directly wound with the positive electrode sheet and the negative electrode sheet. In other words, the diaphragm is directly wound at high temperature. It has been verified through experiments that this unique method can reduce the deformation rate of subsequent lithium-ion batteries.
[0016] In a preferred embodiment of the present invention, the initial temperature of the drying membrane during the winding process can be 45°C, 50°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 120°C, and any number between these values, preferably 80°C-100°C.
[0017] Among them, in the present invention, the inventors have found through research that when the initial temperature of the drying membrane during the winding process is greater than 120°C, the membrane is easily stretched or elongated, thereby affecting the porosity and air permeability of the membrane, and is also prone to thermal shrinkage and deformation of the membrane. When the initial temperature of the drying membrane during the winding process is less than 45°C, it is not conducive to drying out moisture. When the initial temperature of the drying membrane during the winding process is between 45°C and 120°C, the above defects are avoided to a certain extent, especially when it is between 80°C and 100°C, the effect is better.
[0018] In a preferred embodiment of the present invention, the method further includes: first drying the diaphragm to obtain a dried diaphragm with an initial temperature of 45°C-120°C, preferably 80°C-100°C, and then directly winding the dried diaphragm with the positive electrode sheet and the negative electrode sheet to obtain the bare battery cell; wherein the drying operation includes: the diaphragm is dried along a zigzag route through a drying area under the action of traction force.
[0019] Among them, in the present invention, the inventors of the present invention have also found through research that, compared with passing through the drying area along a straight line, the diaphragm passing through the drying area along a zigzag route is helpful to suppress the thermal shrinkage of the diaphragm.
[0020] In a preferred embodiment of the present invention, the diaphragm passes through a drying area along a zigzag route for drying under the action of the traction force of the winding.
[0021] Among them, in the present invention, traction is required for the diaphragm to pass through the drying area, and traction is also required for the drying diaphragm to be wound with the positive electrode sheet and the negative electrode sheet. The drying process and the winding share the same traction, so that the diaphragm can be directly wound after the drying process is completed, and there is no need to pause between the two operations, which can avoid the rebound of the diaphragm moisture caused by the time interval between the two operations, and help to further improve production efficiency.
[0022] In a preferred embodiment of the present invention, in the zigzag route, along the forward direction of the diaphragm, the distance between adjacent highest running points and lowest running points in the vertical direction is L1, the distance between two adjacent highest running points in the horizontal direction is L21, and the distance between two adjacent lowest running points in the horizontal direction is L22, wherein L1>L21 and L1>L22.
[0023] In the present invention, the zigzag route refers to the membrane passing through the drying area in a repeated "N"-shaped trend. That is, the membrane moves forward in the drying area in an "N"-shaped trend in the vertical direction. The highest and lowest running points in the zigzag route referred to in the present invention do not include the starting point and the end point of the zigzag route.
[0024] In the present invention, the "zigzag route" is carried out in a tunnel oven during the actual production process. The tunnel oven includes a box body 1 with a heating function, an upper roller layer 2, a lower roller layer 3, and a Figure 1 and Figure 2 As shown. The upper roller layer 2 and the lower roller layer 3 are arranged in the box body 1. The upper roller layer 2 is provided with a plurality of rollers in sequence along the length direction of the oven (i.e. the advancing direction of the diaphragm). Similarly, the lower roller layer 3 is provided with a plurality of rollers in sequence along the length direction of the oven (i.e. the advancing direction of the diaphragm). Furthermore, the rollers in the upper roller layer 2 and the lower roller layer 3 correspond to each other one by one. Furthermore, the rollers in the upper roller layer 2 and the rollers in the lower roller layer 3 are arranged alternately in sequence along the advancing direction of the diaphragm.
[0025] In order to adjust the distance between the rollers in the upper roller layer 2 and the rollers in the lower roller layer 3 along the advancing direction of the diaphragm, at least one of the rollers in the upper roller layer 2 and the rollers in the lower roller layer 3 can adjust the left and right positions along the advancing direction of the diaphragm. For example, in some embodiments, the rollers in the upper roller layer 2 can adjust the left and right positions along the advancing direction of the diaphragm to Figure 1 and Figure 2 The position in the oven is taken as the reference. When it is adjusted to the right, the length of the diaphragm in the oven becomes longer, and when it is adjusted to the left, the length of the diaphragm in the oven becomes shorter. Furthermore, the tunnel oven also includes an entry roller 4 and an exit roller 5. The box body 1 is a hollow structure with openings at both ends to enable the membrane to pass through the box body. An entry roller 4 and an exit roller 5 are respectively provided at the inlet and outlet ends of the box body 1, and the purpose of their provision is to allow the membrane to enter and leave the box body in a horizontal direction. The entry roller 4 and the exit roller 5 are respectively the starting point and the end point of the membrane passing through the box body 1. In practical applications, the rollers in the upper roller layer 2 and the rollers in the lower roller layer 3, plus the entry rollers and the exit rollers, the total number of rollers can be 8-24.
[0026] Among them, in the present invention, the inventor of the present invention has found through research that, compared with passing through the drying area in a straight line, the contact area between the diaphragm and the roller is larger when the diaphragm passes through the drying area along a zigzag route, forming a large-area contact, so that the roller is used to support and flatten the diaphragm that is in large-area contact with it, thereby suppressing the thermal shrinkage of the diaphragm. In addition, the large contact area will lead to large friction and traction between the two. The diaphragm can be tightened by the traction force, which can also prevent the thermal shrinkage of the diaphragm to a certain extent, and finally suppress the shrinkage in the TD direction (perpendicular to the tape running direction) and the MD direction (along the tape running direction).
[0027] In a preferred embodiment of the present invention, in the zigzag route, along the forward direction of the diaphragm, the distance L1 between the adjacent highest running points and the lowest running points in the vertical direction is 600mm-1200mm, for example, it can be 600mm, 700mm, 800mm, 900mm, 1000mm, 1100mm, 1200mm, and any number between these values, preferably 800mm-1000mm; the distance L21 between two adjacent highest running points in the horizontal direction or the distance L22 between two adjacent lowest running points in the horizontal direction are each 150mm-1000mm, for example, they can be 200mm, 300mm, 400mm, 500mm, 600mm, 700mm, 800mm, 900mm, 1000mm, and any number between these values, preferably 300mm-800mm.
[0028] In a preferred embodiment of the present invention, a distance L21 between two adjacent highest tape running points in the horizontal direction is the same as a distance L22 between two adjacent lowest tape running points in the horizontal direction.
[0029] Among them, in the present invention, the winding process needs to feed the outer diaphragm and the inner diaphragm at the same time. The outer diaphragm and the inner diaphragm can be dried in two tunnel ovens respectively, or can be dried in a double-layer tunnel oven at the same time, such as Figure 3 As shown. Among them, Figure 3 100 is a double-layer tunnel oven, 200 is a winding machine, 300 is an outer separator, 400 is an inner separator, 500 is a positive electrode sheet, and 600 is a negative electrode sheet. In this way, the outer separator and the inner separator are dried in the same environment to ensure the consistency of the drying effect, and then directly wound with the positive electrode sheet and the negative electrode sheet, which can further improve subsequent performance such as deformation rate.
[0030] In a preferred embodiment of the present invention, along the circumferential direction of the roller, the center angle α of the roller corresponding to the arc formed by the contact area between the diaphragm and the roller is greater than 60°, for example, 60-180°, preferably 120-180°.
[0031] In a preferred embodiment of the present invention, the operating conditions of the drying include: a traction force of 120gf-400gf, for example, 120gf, 150gf, 200gf, 250gf, 300gf, 350gf, 400gf, and any number between these values, preferably 200gf-300gf; a traction speed of 300mm / s-2000mm / s, for example, 300mm / s, 400mm / s, 500mm / s, 600mm / s, 700mm / s, 800mm / s, 900mm / s, 1000mm / s, 1100mm / s, 1200mm / s, 1300mm / s, 1400mm / s. m / s, 1500mm / s, 1600mm / s, 1700mm / s, 1800mm / s, 1900mm / s, 2000mm / s, and any number between these values, preferably 800mm / s-1600mm / s; the drying temperature of the drying zone is 60℃-130℃, for example, it can be 60℃, 70℃, 80℃, 90℃, 100℃, 110℃, 120℃, 130℃, and any number between these values, preferably 90℃-120℃; the drying time is 10s-60s, for example, it can be 10s, 20s, 30s, 40s, 50s, 60s, and any number between these values, preferably 30s-50s.
[0032] In the present invention, the drying time refers to the time for the membrane to pass through the drying area. The drying time in the present invention can be adjusted by adjusting the traction speed and the zigzag route. The drying operation conditions defined in the present invention can reduce the thermal shrinkage of the membrane as much as possible while meeting the membrane moisture value requirements.
[0033] In a preferred embodiment of the present invention, the drying operating conditions also include: the width of the diaphragm is 60mm-600mm, for example, it can be 60mm, 70mm, 80mm, 100mm, 200mm, 300mm, 400mm, 500mm, 600mm, and any number between these values, preferably 180mm-330mm; the thickness of the diaphragm is 7μm-20μm, for example, it can be 7μm, 8μm, 10μm, 12μm, 14μm, 16μm, 18μm, 20μm, and any number between these values, preferably 12μm-16μm.
[0034] In a preferred embodiment of the present invention, the present invention does not specifically limit the separator, positive electrode sheet and negative electrode sheet, and conventional separators, positive electrode sheets and negative electrode sheets in the art can be used in the present invention. In the present invention, the positive electrode sheet refers to a positive electrode roll with a discontinuous tab obtained after baking and die-cutting, and the negative electrode sheet refers to a negative electrode roll with a discontinuous tab obtained after baking and die-cutting.
[0035] In a preferred embodiment of the present invention, the moisture content of the positive electrode sheet is ≤200 ppm, and the moisture content of the negative electrode sheet is ≤200 ppm.
[0036] In a preferred embodiment of the present invention, the method further comprises: performing shaping treatment after winding to obtain a bare battery cell.
[0037] Among them, in the present invention, the diaphragm with an initial temperature of 45°C-120°C is directly wound with the positive electrode sheet and the negative electrode sheet and then shaped. The diaphragm within this specific temperature range is beneficial to the shaping of the bare battery cell and can reduce the deformation rate of the coated NG and subsequent lithium-ion batteries.
[0038] In a preferred embodiment of the present invention, the pressure of the shaping treatment is 1t-5t, for example, it can be 1t, 2t, 3t, 4t, 5t, and any number between these values, preferably 2t-3t; the time is 2s-10s, for example, it can be 2s, 3s, 4s, 5s, 6s, 7s, 8s, 9s, 10s, and any number between these values, preferably 4s-7s. The environment of the shaping treatment can be carried out at room temperature. The room temperature in the present invention has a known content, for example, the room temperature can be 20-25°C.
[0039] A second aspect of the present invention provides a method for assembling a lithium ion battery, wherein the method comprises the following steps: (1) preparing a bare cell according to the method described in the first aspect of the present invention; (2) The bare cell is subjected to tab welding, film coating, packaging and liquid injection to obtain a lithium-ion battery.
[0040] In a preferred embodiment of the present invention, the welding method of the tab welding is selected from ultrasonic welding, and the operating conditions of the ultrasonic welding include: the positive electrode welding energy is 100J-500J, preferably 200J-400J; the welding pressure is 800N-1200N, preferably 900N-1100N; the ultrasonic amplitude is 20μm-80μm, preferably 40μm-60μm; the negative electrode welding energy is 150J-750J, preferably 350J-550J; the welding pressure is 1000N-2000N, preferably 1300N-1700N; the ultrasonic amplitude is 30μm-100μm, preferably 50μm-70μm.
[0041] In a preferred embodiment of the present invention, the present invention does not specifically limit the coating, and the coating can be performed by conventional operations in the art. In practice, the coating operation can be to coat the outer periphery of the battery cell after the tab welding is completed with a layer of Mylar film.
[0042] In a preferred embodiment of the present invention, the packaging method is selected from laser welding, wherein the operating conditions of the laser welding include: welding power of 600W-1200W, preferably 800W-1000W; defocus of -3mm to 3mm, preferably 1mm-2mm; welding rate of 70mm / s-110mm / s, preferably 70mm / s-90mm / s.
[0043] In a preferred embodiment of the present invention, the operating conditions of the injection include: the injection pressure is 200kPa-800kPa, preferably 300kPa-600kPa; the number of injection cycles is 2 times to 10 times, preferably 5 times to 7 times; the vacuum degree is -60kPa to -100kPa, preferably -80kPa to -95kPa.
[0044] The present invention will be described in detail below through examples.
[0045] Positive electrode: first bake at 120℃ for 16h, detect the moisture value to be 180ppm, then perform laser die-cutting.
[0046] Negative electrode sheet: first bake at 95℃ for 20h, detect the moisture value to be 165ppm, then perform laser die-cutting.
[0047] The oven is a tunnel type oven, and a plurality of upper rollers and a plurality of lower rollers are arranged in the oven.
[0048] The diaphragm is a PE diaphragm. In addition, unless otherwise specified, various raw materials or components used in the assembly method of the lithium ion battery of the present invention can be purchased commercially or prepared according to conventional methods in the technical field.
[0049] Example 1 (1) The separator (197 mm in width and 13 μm in thickness) passes through the oven along a zigzag route under the action of traction to obtain a dried separator with an initial temperature of 90°C; the dried separator leaving the oven is directly wound with the positive electrode sheet and the negative electrode sheet, and after winding, it is shaped at room temperature to obtain a bare battery cell; Among them, along the circumferential direction of the roller, the arc formed by the contact area between the diaphragm and the roller corresponds to the center angle α of the roller, which is 180°; in the zigzag route, L1=900mm, L21=350mm, L22=350mm; the traction force is 300gf, the traction speed is 1200mm / s, the drying temperature is 95℃, and the drying time is 40s; the shaping pressure is 2t, and the shaping time is 5s; (2) welding the tabs of the battery cell, coating, packaging and injecting liquid to obtain a lithium-ion battery; Among them, the pole ear welding adopts an ultrasonic welding machine, the positive electrode welding energy is 300J, the welding pressure is 1000N, and the ultrasonic amplitude is 50μm; the negative electrode welding energy is 450J, the welding pressure is 1500N, and the ultrasonic amplitude is 60μm; The packaging adopts a laser welding machine with a welding power of 900W, a defocus of +1.5mm, and a welding rate of 80mm / s; The injection is carried out using an injection machine, the injection pressure is 480 kPa, the injection cycle number is 6 times, and the vacuum degree is -90 kPa.
[0050] Example 2 (1) The separator (180 mm in width and 12 μm in thickness) passes through the oven along a zigzag route under the action of traction to obtain a dried separator with an initial temperature of 100°C; the dried separator leaving the oven is directly wound with the positive electrode sheet and the negative electrode sheet, and after winding, it is shaped at room temperature to obtain a bare battery cell; Among them, along the circumferential direction of the roller, the arc formed by the contact area between the diaphragm and the roller corresponds to the center angle α of the roller, which is 120°; in the zigzag route, L1=1000mm, L21=300mm, L22=300mm; the traction force is 300gf, the traction speed is 800mm / s, the drying temperature is 110℃, and the drying time is 50s; the shaping pressure is 3t, and the shaping time is 7s; (2) welding the tabs of the bare cell, coating, packaging and injecting liquid to obtain a lithium-ion battery; Among them, the pole ear welding adopts an ultrasonic welding machine, the positive electrode welding energy is 200J, the welding pressure is 900N, and the ultrasonic amplitude is 40μm; the negative electrode welding energy is 350J, the welding pressure is 1300N, and the ultrasonic amplitude is 50m; The packaging adopts a laser welding machine with a welding power of 800W, a defocus of +1mm, and a welding rate of 70mm / s; The injection is carried out using an injection machine, the injection pressure is 300kPa, the injection cycle number is 5 times, and the vacuum degree is -80kPa.
[0051] Example 3 (1) The diaphragm (width 330 mm, thickness 16 mm) passes through the oven along a zigzag route under the action of traction to obtain a dried diaphragm with an initial temperature of 80°C; the dried diaphragm leaving the oven is directly wound with the positive electrode sheet and the negative electrode sheet, and after winding, it is shaped at room temperature to obtain a bare battery cell; Among them, along the circumferential direction of the roller, the arc formed by the contact area between the diaphragm and the roller corresponds to the center angle α of the roller, which is 150°; in the zigzag route, L1=800mm, L21=500mm, L22=500mm; the traction force is 200 gf, the traction speed is 1600mm / s, the drying temperature is 90℃, and the drying time is 30s; the shaping pressure is 2t, and the shaping time is 4s; (2) welding the tabs of the battery cell, coating, packaging and injecting liquid to obtain a lithium-ion battery; Among them, the pole ear welding adopts an ultrasonic welding machine, the positive electrode welding energy is 400J, the welding pressure is 1100N, and the ultrasonic amplitude is 60μm; the negative electrode welding energy is 550J, the welding pressure is 1700N, and the ultrasonic amplitude is 70μm; The packaging adopts a laser welding machine with a welding power of 1000W, a defocus of +2mm, and a welding rate of 90mm / s; The injection is carried out using an injection machine, the injection pressure is 600kPa, the injection cycle number is 7 times, and the vacuum degree is -95kPa.
[0052] Example 4 (1) Under the action of traction, the diaphragm (505 mm in width and 18 mm in thickness) passes through the oven along a zigzag route to obtain a dried diaphragm with an initial temperature of 115°C; the dried diaphragm leaving the oven is directly wound with the positive electrode sheet and the negative electrode sheet, and after winding, it is shaped at room temperature to obtain a bare battery cell; Among them, along the circumferential direction of the roller, the arc formed by the contact area between the diaphragm and the roller corresponds to the center angle α of the roller, which is 100°; in the zigzag route, L1=1100mm, L21=250mm, L22=250mm; the traction force is 160 gf, the traction speed is 1800mm / s, the drying temperature is 125℃, and the drying time is 15s; the shaping pressure is 1t, and the shaping time is 3s; (2) welding the tabs of the bare cell, coating, packaging and injecting liquid to obtain a lithium-ion battery; Among them, the pole ear welding adopts an ultrasonic welding machine, the positive electrode welding energy is 150J, the welding pressure is 850N, and the ultrasonic amplitude is 30μm; the negative electrode welding energy is 250J, the welding pressure is 1150N, and the ultrasonic amplitude is 40μm; The packaging uses a laser welding machine with a welding power of 700W, a defocus of -1mm, and a welding rate of 100mm / s; The injection is carried out using an injection machine, the injection pressure is 250kPa, the injection cycle number is 4 times, and the vacuum degree is -70kPa.
[0053] Example 5 (1) The separator (width 80 mm, thickness 10 mm) passes through the oven along a zigzag route under the action of traction to obtain a dried separator with an initial temperature of 60°C; the dried separator leaving the oven is directly wound with the positive electrode sheet and the negative electrode sheet, and after winding, it is shaped at room temperature to obtain a bare battery cell; Among them, along the circumferential direction of the roller, the arc formed by the contact area between the diaphragm and the roller corresponds to the center angle α of the roller, which is 170°; in the zigzag route, L1=700mm, L21=600mm, L22=600mm; the traction force is 350gf, the traction speed is 300mm / s, the drying temperature is 85℃, and the drying time is 55s; the shaping pressure is 4t, and the shaping time is 9s; (2) welding the tabs of the bare cell, coating, packaging and injecting liquid to obtain a lithium-ion battery; Among them, the pole ear welding adopts an ultrasonic welding machine, the positive electrode welding energy is 450J, the welding pressure is 1200N, and the ultrasonic amplitude is 70μm; the negative electrode welding energy is 650J, the welding pressure is 1900N, and the ultrasonic amplitude is 80μm; The packaging uses a laser welding machine with a welding power of 1100W, a defocus of 3mm, and a welding rate of 110mm / s; The injection is carried out using an injection machine, the injection pressure is 700 kPa, the injection cycle number is 9 times, and the vacuum degree is -60 kPa.
[0054] Example 6 The same as Example 3, except that the drying temperature is 70°C and the initial temperature of the drying diaphragm during the winding process is 60°C.
[0055] Example 7 The same as Example 1, except that: along the circumferential direction of the roller, the arc formed by the contact area between the diaphragm and the roller corresponds to the central angle α of the roller, which is 90°. In the zigzag line route, L1=650mm, L21=920mm, and L22=920mm.
[0056] Example 8 Compared with Example 3, the difference is that the diaphragm passes through the oven in a straight line, the pulling speed is 500 mm / s, and along the circumferential direction of the roller, the center angle α of the roller corresponding to the arc formed by the contact area between the diaphragm and the roller is 0°.
[0057] Comparative Example 1 The same as Example 1, except that the separator is not dried before winding, and the battery cell is baked after packaging. The operating conditions of the battery cell baking are: baking temperature of 95° C., baking time of 20 h, and vacuum pressure of 100 Pa.
[0058] Comparative Example 2 Compared with Example 2, the difference is that the dried diaphragm leaving the oven is cooled to room temperature before being wound with the positive electrode sheet and the negative electrode sheet.
[0059] Comparative Example 3 Compared with Example 3, the difference is that the drying temperature is 40°C and the initial temperature of the drying separator during the winding process is 35°C.
[0060] Comparative Example 4 Compared with Example 2, the difference is that the drying temperature is 150°C, and the initial temperature of the drying separator during the winding process is 135°C.
[0061] Test Example 1 The lithium-ion batteries prepared in Examples 1-8 and Comparative Examples 1-4 were charged to full charge and then disassembled at a dew point of -30°C. The total number of negative electrode sheets of the battery cell was defined as A1, the number of deformed negative electrode sheets was defined as A2, and the deformation rate was defined as A2 / A1. The test results are shown in Table 1. The "deformation" here refers to the presence of wrinkles and protrusions running through the width direction of the negative electrode sheet (such as Figure 6 As shown in the figure), the negative electrode layer with such "deformation" is regarded as a "deformed layer".
[0062] Among them, taking Examples 1-8 and Comparative Examples 1-4 as examples, Figure 5 This is a deformation test result diagram of the lithium-ion battery prepared in Example 1. Figure 6 This is a deformation test result diagram of the lithium-ion battery prepared in Comparative Example 2. Figure 5 and Figure 6 It can be seen that the lithium ion battery prepared in Example 1 has no obvious wrinkles after disassembly, while the lithium ion battery prepared in Comparative Example 2 has obvious wrinkles after disassembly.
[0063] Table 1 Test subjects Deformation rate Example 1 2.0% Example 2 4.0% Example 3 4.0% Example 4 6.0% Example 5 5.0% Example 6 5.0% Example 7 4.0% Example 8 7.0% Comparative Example 1 15.0% Comparative Example 2 12.0% Comparative Example 3 13.0% Comparative Example 4 18.0% As can be seen from Table 1, the lithium-ion battery assembly method provided in the present invention directly winds the dried separator with the initial temperature with the positive electrode sheet and the negative electrode sheet, so that the deformation rate of the lithium-ion battery can be less than 7%.
[0064] By comparing Example 2 with Comparative Example 2, it can be seen that the diaphragm has a certain temperature during winding, which can improve the shaping effect and significantly reduce the deformation rate of the lithium-ion battery. By comparing Example 3 with Comparative Example 3, and Example 2 with Comparative Example 4, it can be seen that if the initial temperature of drying the diaphragm is too high or too low, it is not conducive to reducing the deformation rate of the lithium-ion battery.
[0065] Test Example 2 Referring to the methods in Examples 1-8 and Comparative Examples 2-4, a diaphragm having an initial moisture content of 1000 ppm was dried, and then the moisture content and thermal shrinkage of the diaphragm after drying were measured.
[0066] (1) Test method for moisture content in dried diaphragm after drying: 1. Sampling: After the diaphragm leaves the oven, immediately cut a 1-meter diaphragm sample and vacuum-seal the diaphragm sample with an aluminum-plastic bag; 2. Test: Cut a test sample weighing 1±0.2g from the above-mentioned diaphragm sample, test it with a Karl Fischer moisture tester, and bake it at 150°C. The baking cutoff condition adopts the drift value cutoff, and the drift value is less than or equal to 1 mg per 90s; 3. Data processing: Test three parallel samples and record the average value.
[0067] (2) Thermal shrinkage measurement method: Before baking, test the width W1 of the separator. After baking, wait for 60 seconds and test the width W2 of the separator at the same position on the same roll. The shrinkage rate = W1-W2 / W1. The test tool is a film ruler. The test results are shown in Table 2. The width of the separator is the TD direction.
[0068] Table 2 Initial moisture value / ppm Moisture content after drying / ppm Thermal shrinkage / % Example 1 1000 158 0.14% Example 2 1000 140 0.20% Example 3 1000 183 0.13% Example 4 1000 260 0.12% Example 5 1000 247 0.12% Example 6 1000 285 0.08% Example 7 1000 160 0.17% Example 8 1000 185 0.20% Comparative Example 1 1000 120 0.32% Comparative Example 2 1000 145 0.19% Comparative Example 3 1000 699 0.00% Comparative Example 4 1000 131 0.51% As can be seen from Table 2, the lithium-ion battery assembly method provided in the present invention can not only significantly reduce the thermal shrinkage rate of the diaphragm, but also significantly improve the drying effect of the diaphragm by optimizing the path of the diaphragm passing through the drying area and / or the specific operating conditions of the oven.
[0069] It can be seen from comparative examples 1, 6, 3 and 4 that the drying temperature has a significant effect on the drying effect and thermal shrinkage of the diaphragm. Within the drying temperature range defined in the present invention, the dried diaphragm can have both low moisture content and low thermal shrinkage.
[0070] It can be seen from comparative examples 1 and 7 that, in the zigzag route, the forward direction of the diaphragm is controlled so that the vertical distance L1 between the adjacent highest running points and the lowest running points is larger than the horizontal distance L21 between the two adjacent highest running points and the horizontal distance L22 between the two adjacent lowest running points. This can increase the contact area between the diaphragm and the roller, thereby helping to reduce the thermal shrinkage rate of the diaphragm during the drying process.
[0071] It can be seen from Comparative Examples 1 and 8 that, compared with passing through the drying area along a straight line, the diaphragm passing through the drying area along a zigzag route is helpful to suppress the thermal shrinkage of the diaphragm.
[0072] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a bare battery cell, It is characterized in that The method comprises the following steps: winding a dried separator, a positive electrode sheet and a negative electrode sheet to obtain a bare battery cell; wherein the initial temperature of the dried separator during the winding process is 45° C.-120° C.
2. The preparation method according to claim 1, in, The initial temperature of the drying diaphragm during the winding process is 80°C-100°C.
3. The preparation method according to claim 1 or 2, in, The method further comprises: first drying the diaphragm to obtain a dried diaphragm with an initial temperature of 45°C-120°C, preferably 80°C-100°C, and then directly winding the dried diaphragm with the positive electrode sheet and the negative electrode sheet to obtain the bare battery cell; The drying process includes: the membrane passes through a drying area along a zigzag route under the action of traction to undergo drying process. Preferably, the membrane passes through a drying area along a zigzag route under the action of the traction force of the winding to undergo a drying process.
4. The preparation method according to claim 3, in, In the zigzag route, along the advancing direction of the diaphragm, the distance between the adjacent highest running point and the lowest running point in the vertical direction is L1, the distance between the two adjacent highest running points in the horizontal direction is L21, and the distance between the two adjacent lowest running points in the horizontal direction is L22, wherein L1>L21 and L1>L22; and / or, The L1 is 600mm-1200mm, preferably 800mm-1000mm; the L21 and L22 are each 150mm-1000mm, preferably 300mm-500mm; Preferably, L21 and L22 are the same.
5. The preparation method according to any one of claims 3 to 4, in, The operating conditions of the drying treatment include: a pulling force of 120gf-400gf, preferably 200gf-300gf; a pulling speed of 300mm / s-2000mm / s, preferably 800mm / s-1600mm / s; preferably, a drying temperature of the drying area of 60°C-130°C, preferably 90°C-120°C; a drying time of 10s-60s, preferably 30s-50s; and / or, Along the circumferential direction of the roller, the center angle of the roller corresponding to the arc formed by the contact area between the diaphragm and the roller is above 60°, preferably 60-180°, and more preferably 120-180°.
6. The preparation method according to any one of claims 3 to 5, in, The operating conditions of the drying treatment also include: the width of the diaphragm is 60 mm-600 mm, preferably 180 mm-330 mm; the thickness of the diaphragm is 7 μm-20 μm, preferably 12 μm-16 μm.
7. The preparation method according to any one of claims 1 to 6, in, The moisture value of the positive electrode sheet is ≤200ppm, and the moisture value of the negative electrode sheet is ≤200ppm; and / or, The method further comprises: performing shaping treatment after winding to obtain a bare battery cell; Preferably, the pressure of the shaping treatment is 1t-5t, preferably 2t-3t; the time of the shaping treatment is 2s-10s, preferably 4s-7s.
8. A method for assembling a lithium-ion battery, It is characterized in that The method comprises the following steps: (1) Preparing a bare cell according to the method according to any one of claims 1 to 7; (2) The bare cell is subjected to tab welding, film coating, packaging and liquid injection to obtain a lithium-ion battery.
9. The assembly method according to claim 8, in, The welding method of the tab welding is selected from ultrasonic welding; preferably, the operating conditions of the ultrasonic welding include: positive electrode welding energy is 100J-500J, preferably 200J-400J; welding pressure is 800N-1200N, preferably 900N-1100N; ultrasonic amplitude is 20μm-80μm, preferably 40μm-60μm; negative electrode welding energy is 150J-750J, preferably 350J-550J; welding pressure is 1000N-2000N, preferably 1300N-1700N; ultrasonic amplitude is 30μm-100μm, preferably 50μm-70μm; and / or, The packaging method is selected from laser welding; preferably, the operating conditions of the laser welding include: welding power of 600W-1200W, preferably 800W-1000W; defocusing amount of -3mm to 3mm, preferably 1mm-2mm; welding rate of 70mm / s-110mm / s, preferably 70mm / s-90mm / s; and / or, The injection pressure is 200kPa-800kPa, preferably 300kPa-600kPa; the injection cycle times are 2-10 times, preferably 5-7 times; the vacuum degree is -100kPa to -60kPa, preferably -95kPa to -80kPa.
10. A lithium ion battery prepared by the method according to any one of claims 8 to 9.