Aqueous zinc ion battery electrolyte containing silane additive as well as preparation method and application of aqueous zinc ion battery electrolyte

By using silane additives to regulate the double layer structure of the zinc negative electrode interface in aqueous zinc ion batteries, the problems of dendrites growth and hydrogen evolution reaction are solved, the circulation time of zinc negative electrode is extended, and the battery performance is improved, and the stability is achieved and reversibility.

CN118943521APending Publication Date: 2024-11-12CHANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411038182.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

There are problems with dendrite growth and hydrogen evolution reactions in aqueous zinc ion batteries, which lead to passivation and side reactions on the surface of zinc negative electrodes, affecting the cycle performance and life of the battery.

Method used

Add silane additives, such as dimethyldiethoxysilane and methylsilanetriol, to the electrolyte solution of the aqueous zinc ion battery, to regulate the double layer structure of the zinc negative electrode interface, and to control the concentration of additives, inhibit dendrites' growth React with hydrogen evolution to improve the deposition method of zinc ions.

Benefits of technology

It effectively extends the cycle time of zinc negative electrode, improves the device life and cycle stability of aqueous zinc ion batteries, significantly improves battery performance, and has a small usage and low production cost, making it suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943521A_ABST
    Figure CN118943521A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of aqueous zinc ion batteries, and particularly relates to an aqueous zinc ion battery electrolyte containing silane additives and a preparation method and application of the aqueous zinc ion battery electrolyte. The aqueous zinc ion battery electrolyte containing the silane additives is prepared from soluble zinc salt, the silane additives and chromatographic water, wherein the silane additives comprise dimethyl diethoxy silane, dimethyl dimethoxy silane, methylsilanetriol, dimethyl silane glycol and the like. When the aqueous zinc ion battery electrolyte containing the silane additive is applied to a battery, the aqueous zinc ion battery electrolyte is adsorbed on the surface of an electrode and regulates and controls a double electrode layer at a zinc negative electrode interface by virtue of the zinc-loving characteristic of the silane additive, so that the cycle time of a zinc negative electrode is effectively prolonged, the service life of an aqueous zinc ion battery device is prolonged, the usage amount of the additive is small, and the preparation cost is low; the preparation method is simple and suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of aqueous zinc ion batteries, and in particular relates to an aqueous zinc ion battery electrolyte containing a silane additive, and a preparation method and application thereof. Background Art

[0002] With the depletion of fossil fuel resources, a serious problem has arisen: energy shortage. Therefore, there is a more urgent need for the development, utilization and storage of renewable energy. Large-scale storage of renewable energy has always been a problem that has troubled people. Using battery systems for storage is an effective solution, but traditional lithium batteries have high costs, serious pollution, and flammability and explosion, which limits their application in large-scale energy storage. Aqueous zinc-ion batteries have attracted widespread attention due to their cost-effectiveness and inherent safety. However, problems such as passivation, dendrites, hydrogen evolution reactions, and other parasitic reactions hinder the practical application of metallic zinc in aqueous electrolytes.

[0003] Modifying the electrolyte by adding additives has been proven to be an effective means to reduce side reactions and inhibit dendrite growth. In the electrochemical reaction at the zinc anode-electrolyte interface, the desolvation / deposition process has always played an important role, and the desolvation / deposition process is determined by the chemical structure and properties of the double layer. In traditional zinc sulfate electrolytes, the coordinated water in the solvation structure of zinc ions in the double layer receives electrons during the desolvation and zinc plating process. This process causes the hydrogen evolution side reaction at the zinc anode interface, increasing the OH at the interface. - The concentration of zinc anode is increased, and then alkaline sulfide byproducts are formed, which passivates the surface of zinc anode. In addition, under the repulsive force of the double layer, the two-dimensional random diffusion of zinc ions leads to the extensive growth of zinc dendrites. Therefore, reconstructing the double layer structure of zinc anode and adjusting the electrode / electrolyte interface environment can effectively improve the battery life and cycle performance.

[0004] However, how to choose the right additive to effectively regulate the double layer remains a big challenge. In previous studies, the effects of slight changes in the adsorption form of additives on the double layer structure of the zinc negative electrode interface are often overlooked. However, the concentration changes of adsorbed additives have a significant effect on the double layer, which directly affects the performance of the entire battery. Excessive addition of electrolyte additives may cause excessive adsorption of molecules on the double layer, potentially causing an increase in overpotential. This increase will have a negative impact on the transport kinetics of zinc ions and hinder the rapid deposition of zinc ions. On the contrary, insufficient amounts of additives may fail to establish an effective isolation layer, thereby failing to effectively protect the zinc negative electrode.

[0005] Therefore, selecting suitable adsorption additives, precisely controlling the concentration of adsorption additives, and regulating to obtain a suitable zinc negative electrode double-layer interface can effectively address the problems of hydrogen evolution side reactions and dendrite growth currently faced by aqueous zinc-ion batteries. Summary of the invention

[0006] In view of the above-mentioned shortcomings that currently exist, the present invention provides an aqueous zinc ion battery electrolyte containing a silane additive, and a preparation method and application thereof. The present invention adds a silane additive to an aqueous electrolyte containing a zinc salt solute to prepare an aqueous composite electrolyte, utilizes the zinc-philic properties of silane additives such as dimethyldiethoxysilane and methylsilanetriol to regulate the double electric layer at the zinc negative electrode interface, studies the difference between the chemical environment of the double electric layer at the zinc negative electrode interface and the chemical environment of the solution, and regulates the double electric layer interface of the zinc negative electrode by controlling the concentration of the additive, thereby effectively inhibiting zinc dendrite growth and interface side reactions, extending the cycle time of the zinc negative electrode, and improving the device life of the aqueous zinc ion battery.

[0007] The object of the present invention is to provide an aqueous zinc ion battery electrolyte containing a silane additive and a preparation method thereof, in view of the problems of dendrite growth and hydrogen evolution reaction that are common in aqueous zinc ion batteries. The aqueous zinc ion battery electrolyte containing a silane additive is composed of a soluble zinc salt, a silane additive, and chromatographic water, and the preparation method thereof comprises the following steps:

[0008] Step 1: Add soluble zinc salt to chromatographic water to prepare an aqueous zinc salt electrolyte;

[0009] Step 2: After the pH value of the aqueous zinc salt electrolyte is stabilized, add a silane additive, mix well, and let stand to obtain a stable aqueous zinc ion battery electrolyte containing a silane additive.

[0010] Further, the soluble zinc salt is selected from one or a combination of two or more of zinc sulfate, zinc chloride, zinc nitrate, zinc acetate, zinc trifluoromethanesulfonate, zinc perchlorate, zinc trifluoromethanesulfonyl imide, and zinc tetrafluoroborate. In the present invention, zinc sulfate is preferred.

[0011] Furthermore, in the aqueous zinc ion battery electrolyte containing silane additives, the concentration of soluble zinc salt is 0.2-4 mol / kg. In the present invention, the preferred concentration of soluble zinc salt is 3 mol / kg.

[0012] Furthermore, the silane additive is any one of dimethyldiethoxysilane, dimethyldimethoxysilane, diethyldiethoxysilane, methylsilanetriol, dimethylsilanediol, triisopropylsilane, triethylsilane, triethylsilanol, and triethoxysilane.

[0013] Preferably, the silane additive is any one of dimethyldiethoxysilane, dimethyldimethoxysilane, methylsilanetriol and dimethylsilanediol.

[0014] Further, in the aqueous composite electrolyte of the silane additive, the concentration of the silane additive is 0.05-0.5m (m: mol / kg). Different silane additives have different optimal addition concentrations due to the differences in some functional groups on their molecules. With reference to Examples 1-3, the optimal concentration of the silane additive when dimethyldiethoxysilane is 0.1mol / kg, and the optimal concentration when the silane additive is dimethyldimethoxysilane, dimethylsilanediol or methylsilanetriol is 0.2mol / kg.

[0015] The present invention applies the aqueous zinc ion battery electrolyte containing silane additives to a battery, wherein the battery is a symmetrical battery assembled from the aqueous zinc ion battery electrolyte containing silane additives and a commercial zinc sheet; or a half-battery assembled from the aqueous zinc ion battery electrolyte containing silane additives and a commercial current collector; or the aqueous zinc ion battery electrolyte containing silane additives is the electrolyte, the commercial zinc sheet is used as the negative electrode, and NH4V4O 10 / MnO2 or VO2 is used as the positive electrode to assemble the obtained aqueous zinc ion battery.

[0016] Furthermore, the commercial current collector is selected from any one of titanium foil, copper foil, nickel foil, stainless steel mesh, copper mesh, nickel mesh, foam copper, and foam nickel.

[0017] After testing, the above-mentioned aqueous zinc-ion battery electrolyte containing silane additives can significantly prolong the stable cycle time of the zinc negative electrode; according to its functions and effects, the above-mentioned aqueous zinc-ion battery electrolyte containing silane additives can improve the cycle stability of the aqueous zinc-ion battery and the reversibility of the zinc negative electrode.

[0018] The invention has the advantages that by adding an appropriate amount of the silane additive, it can be adsorbed on the surface of the zinc negative electrode to regulate the double electric layer of the zinc negative electrode interface, effectively reducing the contact between water and the zinc negative electrode, and reducing the hydrogen evolution side reaction at the interface. At the same time, the additive improves the diffusion mode of zinc ions at the zinc negative electrode interface, and changes from 2D diffusion to 3D diffusion, which is conducive to the uniform migration and deposition of zinc ions on the negative electrode surface, thereby inhibiting the formation and growth of zinc dendrites, greatly extending the cycle time of the zinc negative electrode, and improving the device life of the aqueous zinc ion battery. The symmetrical battery cycle exceeds 6000h, and the full battery cycle is close to 2000 circles, which effectively improves the performance of the aqueous zinc ion battery. The effect is significantly better than the current small molecule organic matter and polymer additives. And the additive is used in a small amount and is easy to use.

[0019] The present invention is characterized by:

[0020] (1) The electrolyte is modified by silane additives, the amount of additives used is small, the preparation cost is low, the preparation method is simple, and it is suitable for large-scale production.

[0021] (2) The silane additive introduced into the electrolyte of the present invention, by virtue of its zinc affinity, is adsorbed on the electrode surface, regulates the double electric layer at the zinc negative electrode interface, effectively reduces the contact between water and the electrode, reduces the hydrogen evolution side reaction, and improves the reversibility of the zinc negative electrode.

[0022] (3) The electron-rich groups in the silane additives introduced into the electrolyte of the present invention can participate in the solvation structure of zinc ions in the electrolyte, reduce the amount of coordinated water in the solvation sheath structure of zinc ions, increase the zinc deposition overpotential, and make zinc deposited in smaller grains and deposited more evenly on the electrode surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The scanning electron microscope image of the zinc negative electrode of a zinc-zinc symmetrical battery made with an electrolyte containing a silane additive (dimethyldiethoxysilane 0.1 mol / kg) after 50 cycles of charge and discharge;

[0024] Figure 2 This is a scanning electron microscope image of the zinc negative electrode of a zinc-zinc symmetrical battery made with an electrolyte without additives after 50 cycles of charge and discharge;

[0025] Figure 3 The time-voltage curves of zinc-zinc symmetric batteries prepared with electrolytes containing silane additives (dimethyldiethoxysilane 0.1 mol / kg) and electrolytes without additives;

[0026] Figure 4 The Tafel curves of the three-electrode system prepared by the electrolyte containing silane additives (dimethyldiethoxysilane 0.1 mol / kg) and the electrolyte without additives;

[0027] Figure 5 The chronoamperometric curves of zinc-zinc symmetric batteries prepared with electrolytes containing silane additives (dimethyldiethoxysilane 0.1 mol / kg) and electrolytes without additives;

[0028] Figure 6 The specific capacity decay and coulombic efficiency diagram of zinc-VO2 full battery made of electrolyte containing silane additives (dimethyldiethoxysilane 0.1 mol / kg) and electrolyte without additives;

[0029] Figure 7 The time-voltage curve of the zinc-zinc symmetric battery prepared with electrolyte containing different concentrations of silane additives (dimethyldiethoxysilane);

[0030] Figure 8 The coulombic efficiency test of zinc-copper asymmetric battery prepared with electrolyte containing different concentrations of silane additives (dimethyldiethoxysilane);

[0031] Fig. 9 The time-voltage curves of zinc-zinc symmetric batteries containing electrolytes with different concentrations of silane additives (dimethyldimethoxysilane) and electrolytes without silane additives;

[0032] Fig.10 The time-voltage curves of zinc-zinc symmetric batteries prepared with electrolytes containing different concentrations of silane additives (dimethylsilanediol) and electrolytes without silane additives;

[0033] Fig.11 The time-voltage curves of zinc-zinc symmetric batteries prepared with electrolytes containing different concentrations of silane additives (methylsilanetriol) and electrolytes without silane additives. DETAILED DESCRIPTION

[0034] To make the present invention easier to understand, the present invention is further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. Unless otherwise defined, the professional terms used below are consistent with the meanings understood by professional and technical personnel in the field; unless otherwise specified, the raw materials and reagents involved in this article can be purchased from the market or prepared by known methods.

[0035] Among them, "ZSO" in the drawings of the present application is an aqueous solution of zinc sulfate (also known as: aqueous zinc salt electrolyte); "3m ZSO" in the drawings of the present application is an aqueous solution of zinc sulfate, and the concentration of zinc sulfate salt is 3 mol / kg; "DDS" in the drawings of the present application is an aqueous zinc ion battery electrolyte containing a silane additive, and the silane additive is dimethyldiethoxysilane; "0.1m DDS" in the drawings of the present application is an aqueous zinc ion battery electrolyte containing a silane additive, and the silane additive is dimethyldiethoxysilane, and the concentration of dimethyldiethoxysilane is 0.1 mol / kg;

[0036] Embodiment 1:

[0037] The aqueous zinc ion battery electrolyte of the present embodiment is specifically composed of chromatographic water, zinc sulfate and dimethyldiethoxysilane. Its preparation method is as follows: weigh 0.53841g of zinc sulfate monohydrate, place it in 0.946g of chromatographic water, and ultrasonicate at room temperature for 20min to obtain a 3m (m: mol / kg) zinc sulfate solution. By weighing 0.014828g of dimethyldiethoxysilane, adding it to the prepared 3m zinc sulfate solution, ultrasonicate at room temperature for 30min, an electrolyte containing 0.1m dimethyldiethoxysilane additive is obtained.

[0038] The electrolyte containing silane additives and the electrolyte without additives obtained in this example were applied to a zinc-zinc symmetrical battery and the electrolyte was charged at 5 mA / cm 2 The charge and discharge were carried out at a current density of 1.547 W / m and a charge and discharge cycle time of 12 min. After 50 cycles, the dendrite growth on the surface of the zinc electrode was observed using a scanning electron microscope.

[0039] The electron microscopy results are as follows Figure 1 and Figure 2 As shown, Figure 1 This is a scanning electron microscope image of the zinc negative electrode of a zinc ion battery electrolyte containing silane additives. Figure 2 This is a scanning electron microscope image of the zinc negative electrode of the zinc ion battery electrolyte without additives. The results show that the surface of the zinc sheet using the zinc ion battery electrolyte containing additives is flat and uniform, and there are no obvious dendrites; while in the comparative experiment, a large number of dendrites can be clearly observed on the surface of the zinc sheet using the zinc ion battery electrolyte without additives.

[0040] The electrolyte containing silane additives and the electrolyte without additives obtained in this example were applied to a zinc-zinc symmetrical battery to perform constant current charge and discharge tests. The current density was 0.5 mA / cm 2 , time is 1h, observe the voltage curve.

[0041] The results are as follows Figure 3 As shown, the zinc-zinc symmetric battery containing the electrolyte containing silane additives has a longer cycle life.

[0042] The electrolyte containing silane additives and the electrolyte without additives obtained in this example were applied to a three-electrode system with zinc foil as the working electrode, platinum sheet as the counter electrode, and Ag / AgCl electrode (0.197V vs. SHE) as the reference electrode. -1 The Tafel diagram is measured by band scanning.

[0043] The results are as follows Figure 4As shown in Figure 2, after adding silane additives, the corrosion potential of the electrolyte increased from -0.985 V to -0.956 V (vs. Ag / AgCl), and the corrosion current increased from 9.50 mA cm -2 Down to 2.88 mA cm -2 . It shows that the addition of silane additives effectively inhibits the corrosion of zinc negative electrode.

[0044] The electrolyte containing silane additives and the electrolyte without additives obtained in this example were applied to a zinc-zinc symmetrical battery, and a chronoamperometric curve at a fixed overpotential of -150 mV was obtained on an electrochemical workstation.

[0045] The results are as follows Figure 5 As shown, it can be clearly observed that the current density of zinc electrodeposition in the electrolyte before the addition of additives continued to increase. This trend can be attributed to the "tip effect" caused by the inhomogeneous electric field. Subsequently, zinc deposition occurred at the tip of the original irregular crystal nucleus, minimizing the surface energy and ultimately initiating the formation of uncontrollable dendrites. In contrast, in the electrolyte after the addition of additives, the current response of zinc electrodeposition remained stable after a transient increase in current density for 48 seconds. This behavior can be attributed to limited two-dimensional diffusion, which promotes the formation of a uniform and dense zinc deposition layer.

[0046] The electrolyte containing silane additives and the electrolyte without additives obtained in this example were applied to zinc-vanadium dioxide full batteries to test the cycle stability of the full batteries.

[0047] The results are as follows Figure 6 As shown, in 3Ag -1 Under the same conditions, the zinc-VO2 full battery containing silane additive electrolyte also showed more than 2000 stable cycles, with a capacity retention rate of more than 80%, while the zinc-VO2 full battery without additive electrolyte had a rapid capacity decay until failure after 209 cycles, which shows that silane additives can effectively improve the cycle stability of the whole battery.

[0048] Embodiment 2:

[0049] The aqueous zinc ion battery electrolyte of this example is specifically composed of chromatographic water, zinc sulfate and dimethyldiethoxysilane. Its preparation method is as follows: weigh 0.53841g of zinc sulfate monohydrate, place it in 0.946g of chromatographic water, and ultrasonicate at room temperature for 20min to obtain a 3m (m: mol / kg) zinc sulfate solution. By weighing 0.007414g, 0.029656g and 0.07414g of dimethyldiethoxysilane respectively, and adding them to the prepared 3m zinc sulfate solution, ultrasonicate at room temperature for 30min, an electrolyte containing 0.05m, 0.2m and 0.5m dimethyldiethoxysilane additives is obtained.

[0050] The electrolytes containing different concentrations of silane additives and the electrolytes without additives obtained in this example were applied to zinc-zinc symmetrical batteries to perform constant current charge and discharge tests at a current density of 5 mA / cm 2 , time is 1h, observe the voltage curve.

[0051] The results are as follows Figure 7 As shown, the battery containing 0.1m silane additives has the longest cycle life, which indicates that the appropriate additive concentration can improve the cycle life of the battery.

[0052] The electrolytes containing silane additives of different concentrations and the electrolytes without additives obtained in this example were applied to zinc-copper asymmetric batteries to perform coulombic efficiency tests.

[0053] The results are as follows Figure 8 As shown in the figure, the battery containing 0.1m silane additives has the highest average coulombic efficiency and the longest cycle life. This appropriate additive concentration can improve the reversibility of the zinc negative electrode.

[0054] The electrolytes containing silane additives of different concentrations and the electrolytes without additives obtained in this example were applied to zinc-vanadium dioxide full batteries to test the cycle stability of the full batteries.

[0055] The results are shown in Table 1. Appropriate additive concentration can improve the full battery performance and capacity retention.

[0056] Table 1 Cycling performance of full batteries containing different concentrations of silane additives

[0057]

[0058] Embodiment 3:

[0059] The aqueous zinc ion battery electrolyte of the present embodiment is specifically composed of chromatographic water, zinc sulfate and dimethyldimethoxysilane, diethyldiethoxysilane, methylsilanetriol, dimethylsilanediol, triisopropylsilane, triethylsilane, triethylsilanol, triethoxysilane. Its preparation method is as follows: weigh 0.53841g of zinc sulfate monohydrate, place it in 0.946g of chromatographic water, ultrasonicate at room temperature for 20min, and obtain 3m (m: mol / kg) zinc sulfate solution. By weighing different masses of dimethyldimethoxysilane, diethyldiethoxysilane, methylsilanetriol, dimethylsilanediol, triisopropylsilane, triethylsilane, triethylsilanol, triethoxysilane respectively, and adding it to the prepared 3m zinc sulfate solution, ultrasonicate at room temperature for 30min, an electrolyte containing silane additives containing 0.05-0.5m is obtained.

[0060] The electrolytes with different concentrations of additives prepared by using different silane additives obtained in this example and the electrolytes without additives were applied to zinc-zinc symmetrical batteries to perform constant current charge and discharge tests. The current density was 1 mA / cm 2 , time is 1h, observe the voltage curve.

[0061] The results are as follows Fig. 9 , 10 As shown in Figure 11, the zinc-zinc symmetric battery containing a zinc-ion battery electrolyte with a silane additive has a longer cycle life.

[0062] The electrolytes with different concentrations of additives prepared by using different silane additives obtained in this example and the electrolytes without additives were applied to zinc-vanadium dioxide full batteries to test the cycle stability of the full batteries.

[0063] The results are shown in Table 2, which indicate that the zinc-vanadium dioxide full battery containing a zinc ion battery electrolyte containing a silane additive can improve the full battery performance and capacity retention rate.

[0064] Table 2 Cycling performance of zinc-vanadium dioxide full batteries assembled with electrolytes containing different concentrations of additives prepared with different silane additives and electrolytes without additives

[0065]

[0066] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. An aqueous zinc ion battery electrolyte containing a silane additive, It is characterized in that The aqueous zinc ion battery electrolyte consists of a soluble zinc salt, a silane additive, and chromatographic water; The silane additive is any one of dimethyldiethoxysilane, dimethyldimethoxysilane, diethyldiethoxysilane, methylsilanetriol, dimethylsilanediol, triisopropylsilane, triethylsilane, triethylsilanol and triethoxysilane.

2. The aqueous zinc ion battery electrolyte containing silane additives according to claim 1, It is characterized in that The soluble zinc salt is at least one selected from zinc sulfate, zinc chloride, zinc nitrate, zinc acetate, zinc trifluoromethanesulfonate, zinc perchlorate, zinc trifluoromethanesulfonyl imide, and zinc tetrafluoroborate; The concentration of the soluble zinc salt in the aqueous zinc ion battery electrolyte is 0.2-4 mol / kg.

3. The aqueous zinc ion battery electrolyte containing silane additives according to claim 1, It is characterized in that The concentration of the silane additive in the aqueous zinc ion battery electrolyte is 0.05-0.5 mol / kg.

4. A method for preparing an aqueous zinc ion battery electrolyte containing a silane additive according to any one of claims 1 to 3, It is characterized in that The steps include: Step (1): adding a soluble zinc salt to chromatographic water to prepare an aqueous zinc salt electrolyte; Step (2): After the pH value of the aqueous zinc salt electrolyte is stabilized, a silane additive is added, mixed evenly, and allowed to stand to obtain a stable aqueous zinc ion battery electrolyte containing a silane additive.

5. Use of the aqueous zinc ion battery electrolyte containing silane additives according to any one of claims 1 to 3 in a battery.

6. The use according to claim 5, It is characterized in that The battery is a symmetrical battery assembled from an aqueous zinc ion battery electrolyte containing silane additives and a commercial zinc sheet, a half-cell assembled from an aqueous zinc ion battery electrolyte containing silane additives and a commercial current collector, or an aqueous zinc ion battery assembled from an aqueous zinc ion battery electrolyte containing silane additives as an electrolyte and commercial zinc sheets as a negative electrode and a positive electrode.

7. The use according to claim 6, It is characterized in that The commercial current collector is selected from any one of titanium foil, copper foil, nickel foil, stainless steel mesh, copper mesh, nickel mesh, foam copper, and foam nickel; The positive electrode is NH 4 V 4 O 10 / MnO 2 or VO 2 .