Battery composite diaphragm as well as preparation method and application thereof
By using coaxial electrospinning method to prepare the core-shell structure coating on the lithium-ion battery separator, the problem of the separator being easily shrinkable at high temperature is solved, the thermal stability, mechanical strength and safety performance of the battery are improved, and suitable for hybrid power High demands for vehicles.
Patent Information
- Application Number
- CN202411118451.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing lithium-ion battery separators are prone to shrink at high temperatures, affecting thermal stability, mechanical strength and flame retardant performance, resulting in insufficient battery safety performance.
Coaxial electrospinning method is used to prepare functional coatings on the substrate layer. The coating consists of high-temperature resistant polymer material as a core layer and a shell layer composed of ceramic material and adhesive to form a core-shell structure to enhance the mechanical stability of the diaphragm. and electrolyte wetting properties.
It significantly improves the thermal stability, mechanical strength and ionic conductivity of the diaphragm, enhances the safety performance of the battery, and is suitable for high-demand applications such as hybrid vehicles.
Smart Images

Figure CN118943648A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery separator technology, and more specifically to a battery composite separator, its preparation method, and its application. Background Technology
[0002] The separator is a crucial component of lithium-ion batteries, significantly impacting their electrochemical and safety performance. Currently, commercially available separators are primarily made of polyolefins, with polyethylene and polypropylene being widely used. However, polyethylene and polypropylene have melting points of 132°C and 165°C, respectively, and are prone to shrinkage at high temperatures, affecting the separator's thermal stability, mechanical strength, and flame retardant properties, thus posing a significant threat to battery safety. Summary of the Invention
[0003] This application provides a battery composite separator, its preparation method, and its application, which can effectively improve the thermal stability and mechanical strength of the separator, and effectively improve the ionic conductivity and safety performance of the battery.
[0004] This application provides a battery composite separator, including a substrate layer and a functional coating coated on at least one surface of the substrate layer, the functional coating including coaxial electrospun fibers; the coaxial electrospun fibers include a core layer and a shell layer wrapped on the core layer, the material forming the core layer includes a high-temperature resistant polymer material, and the material forming the shell layer includes a ceramic material and an adhesive.
[0005] In some alternative embodiments, the mass ratio of the ceramic material to the adhesive in the shell is 1:0.02 to 1:0.1.
[0006] In some alternative embodiments, the adhesive includes at least one of polyurethane, silicone rubber, polyacrylate, polyamide, and polyether.
[0007] In some alternative embodiments, the ceramic material includes at least one of boehmite, alumina, and silicon dioxide.
[0008] In some optional embodiments, the high-temperature resistant polymer material includes at least one of polyimide, polyarylethersulfone ketone, polyetherimide, polyphenylene sulfone, and polyisophthalamide.
[0009] In some alternative embodiments, the coaxial electrospun fibers form a porous network structure in the functional coating.
[0010] This application provides a method for preparing a battery composite separator, which includes the following steps:
[0011] The high-temperature resistant polymer material is dissolved in a solvent according to a preset ratio and stirred and mixed evenly to obtain the core layer spinning solution.
[0012] The adhesive and ceramic material are dissolved in a solvent according to a preset ratio and stirred to obtain a shell spinning solution.
[0013] Using the core spinning solution and the shell spinning solution as electrospinning solutions, coaxial electrospinned fibers are prepared on at least one surface of the substrate layer by coaxial electrospinning.
[0014] After vacuum drying of the substrate layer coated with the coaxial electrospun fibers, it is hot-pressed under preset conditions to form a functional coating, thereby obtaining the diaphragm.
[0015] In some optional embodiments, at least one of the conditions (1)-(5) is satisfied when the functional coating is prepared:
[0016] (1) In the core spinning solution, the mass percentage of the high-temperature resistant polymer material is 5 wt.%-20 wt.%.
[0017] (2) In the shell spinning solution, the total mass percentage of the ceramic material and the adhesive is 10 wt.% to 30 wt.%.
[0018] (3) The coaxial electrospinning method includes preparing the functional coating by using a transmitter and a receiver in conjunction under the action of an electric field. The voltage of the electric field is 20kV-30kV, the rotation speed of the receiver is 200rpm-400rpm, the distance between the transmitter and the receiver is 15cm-30cm, the injection rate of the core spinning solution is 0.1mL / h-1.0mL / h, and the injection rate of the shell spinning solution is 0.1mL / h-1.0mL / h.
[0019] (4) The thickness of the functional coating is d2, and the value range of d2 is 0.5μm≤d2≤10μm;
[0020] (5) The mass ratio of the ceramic material to the adhesive is 1:0.02-1:0.1.
[0021] In some optional embodiments, the preset conditions during hot pressing include hot pressing temperature and hot pressing pressure, wherein the hot pressing temperature ranges from 40℃ to 100℃ and the hot pressing pressure ranges from 5MPa to 20MPa.
[0022] This application provides a secondary battery, including the battery composite separator as described above or the battery composite separator prepared by the preparation method described above.
[0023] The battery composite separator according to the above embodiments includes a substrate layer and a functional coating coated on at least one surface of the substrate layer. The functional coating includes coaxial electrospun fibers. The coaxial electrospun fibers include a core layer and a shell layer wrapped around the core layer. The material forming the core layer includes a high-temperature resistant polymer material, and the material forming the shell layer includes a ceramic material and an adhesive. Because the functional coating uses a high-temperature resistant polymer material as the core layer, the core layer can endow the separator with excellent mechanical stability, high temperature resistance and flame retardant properties. The shell layer uses a ceramic adhesive system composed of ceramic materials and adhesives, which can endow the separator with excellent electrolyte wettability, mechanical properties and thermal stability. The excellent electrolyte wettability can improve the ionic conductivity of the separator. Since the functional coating is prepared by coaxial electrospinning, this method can produce polymer fibers with nanoscale diameter. The polymer fibers with excellent mechanical properties, thermal stability, flame retardant properties and high ionic conductivity are attached to the substrate layer, so that the separator has the above properties and excellent electrochemical performance. The battery made from this separator can be directly used in hybrid vehicles, which greatly improves the safety performance of the battery. Attached Figure Description
[0024] Figure 1 This is a schematic diagram of the structure of the battery composite separator in one embodiment;
[0025] Figure 2 This is a schematic diagram of the battery composite separator in another embodiment;
[0026] Figure 3 This is a schematic diagram of the structure of the functional coating in one embodiment.
[0027] Wherein: 100, substrate layer; 200, functional coating; 210, coaxial electrospun fiber; 210a, core layer; 210b, shell layer. Detailed Implementation
[0028] The present application will now be described in further detail with reference to the accompanying drawings and specific embodiments. Similar elements in different embodiments are referred to by related similar element reference numerals. In the following embodiments, many details are described to facilitate a better understanding of the present application. However, those skilled in the art will readily recognize that some features may be omitted in different situations, or may be replaced by other elements, materials, or methods. In some cases, certain operations related to the present application are not shown or described in the specification. This is to avoid obscuring the core parts of the present application with excessive description. For those skilled in the art, detailed description of these related operations is not necessary; they can fully understand the related operations based on the description in the specification and general technical knowledge in the art.
[0029] Furthermore, the features, operations, or characteristics described in the specification can be combined in any suitable manner to form various embodiments, and the operational steps involved in each embodiment can also be rearranged or adjusted in a manner that is obvious to those skilled in the art. Therefore, the specification and drawings are only for clearly describing a particular embodiment and do not imply that they represent the necessary components and / or order.
[0030] The serial numbers assigned to components in this document, such as "first" and "second," are used only to distinguish the described objects and have no sequential or technical meaning. The terms "connection" and "linkage" used in this application, unless otherwise specified, include both direct and indirect connections (linkages).
[0031] In this application, the term "secondary battery" refers to a battery that can be recharged after discharge to reactivate its active materials and continue to be used. These batteries typically utilize the reversibility of chemical reactions; that is, once a chemical reaction converts into electrical energy, electrical energy can be used to repair the chemical system, and then the chemical reaction can be converted back into electrical energy. Common secondary batteries include, but are not limited to, nickel-metal hydride batteries, nickel-cadmium batteries, lead-acid (or lead-acid) batteries, lithium-ion batteries, polymer lithium-ion batteries, and sodium-ion batteries.
[0032] In this application, the "battery composite separator" is an important component of a secondary battery cell. The battery composite separator is a thin film used during electrolysis to separate the positive and negative electrodes, preventing direct reaction and energy loss. The performance of the battery composite separator determines the battery's interface structure, internal resistance, and other characteristics, directly affecting the battery's capacity, cycle life, and safety performance. A high-performance battery composite separator plays a crucial role in improving the overall performance of the battery.
[0033] Please see Figures 1 to 3 This application discloses a battery composite separator, including a substrate layer 100 and a functional coating 200 coated on at least one surface of the substrate layer 100. The functional coating 200 includes coaxial electrospun fibers 210. The coaxial electrospun fibers 210 include a core layer 210a and a shell layer 210b wrapped around the core layer 210a. The material forming the core layer 210a includes a high-temperature resistant polymer material, and the material forming the shell layer 210b includes a ceramic material and an adhesive.
[0034] It is understood that the aforementioned at least one surface includes a functional coating 200 (such as...) disposed on one of the surfaces of the substrate layer 100. Figure 1 As shown), functional coatings 200 can also be provided on both surfaces of the substrate layer 100 (e.g., as shown). Figure 2 (As shown).
[0035] Since the functional coating 200 uses a high-temperature resistant polymer material as the core layer 210a, the high-temperature resistant polymer material has high heat resistance and flame retardancy, which makes the prepared composite nanofibers have good thermal stability and self-extinguishing properties. This gives the separator excellent mechanical stability, high temperature resistance and flame retardancy, which is beneficial to improving the safety performance of the battery.
[0036] Since the core layer 210a uses a ceramic adhesive system composed of ceramic materials and an adhesive as the shell layer 210b, the ceramic material enhances the mechanical stability and heat resistance of the functional coating 200, while also improving the overall moisture absorption and retention of the membrane, facilitating efficient lithium ion transfer and increasing the ionic conductivity of the membrane. The adhesive effectively connects the ceramic materials and adheres to the surface of the fibers in the core layer 210a. The adhesive has high elasticity, which effectively improves the mechanical stability of the composite membrane (including tensile deformation and puncture strength). By using the ceramic adhesive system as the shell layer 210b, the shell layer 210b imparts excellent electrolyte wettability, mechanical properties, and thermal stability to the membrane. Excellent electrolyte wettability enhances the ionic conductivity of the membrane. The ceramic material uses ceramic particles, giving the functional coating 200 a certain particle size, which effectively ensures the membrane's permeability.
[0037] Because the functional coating 200 includes coaxial electrospun fibers 210, which are polymer fibers with nanoscale diameters (such as... Figure 3 As shown, polymer fibers with excellent mechanical properties, thermal stability, flame retardancy and high ionic conductivity are attached to the substrate layer 100, so that the diaphragm has the above properties. At the same time, the shell layer 210b material can be varied to improve the adaptability of the diaphragm.
[0038] Because the core-shell structured polymer fibers obtained by using high heat-resistant polymer materials and ceramic adhesive systems can control the coating thickness while ensuring that various material systems are evenly distributed on the substrate layer 100, avoiding uneven distribution of multiple uniaxial fiber materials, thereby improving the stability and uniformity of the diaphragm performance.
[0039] The core-shell structured polymer fiber obtained by utilizing high heat-resistant polymer materials and ceramic adhesive systems gives the resulting separator good mechanical stability, thermal stability, flame retardancy, and moisture absorption and retention. This improves the electrolyte affinity of the separator, reduces the contact angle, and effectively controls costs. The battery made from it has better cycle stability and rate performance, and can reduce the occurrence of thermal runaway. Lithium-ion batteries made from this separator can be directly used in hybrid vehicles, greatly improving battery safety performance.
[0040] In some alternative embodiments, one or more coaxial electrospun fibers 210 are bonded together by an adhesive in the shell 210b to form a porous network structure. Because the coaxial electrospun fibers 210 are bonded together to form a porous network, the functional coating 200 exhibits good mechanical properties.
[0041] In some optional embodiments, the mass ratio of ceramic material to adhesive in shell layer 210b is 1:0.02-1:0.1. For example, the mass ratio of ceramic material to adhesive can be 1:0.02, 1:0.03, 1:0.04, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09, or 1:0.1, or any combination of the above values. Using this mass ratio effectively controls the prepared diaphragm to have both good mechanical stability and electrolyte wettability. When the mass ratio of ceramic to adhesive is greater than this range, i.e., the content of ceramic material is higher, the air permeability of the diaphragm increases, thereby reducing the air permeability of the diaphragm and affecting the ionic conductivity of the diaphragm. When it is less than this range, the integrity of the adhesion between the functional coating 200 and the substrate layer 100 is poor, and the heat resistance of the functional coating 200 is also poor, affecting the mechanical properties and thermal stability of the diaphragm.
[0042] In some alternative embodiments, the adhesive includes at least one of polyurethane, silicone rubber, polyacrylate, polyamide, and polyether.
[0043] In some alternative embodiments, the ceramic material includes at least one of boehmite, alumina, and silicon dioxide.
[0044] In some alternative embodiments, the high-temperature resistant polymer material includes at least one of polyimide, polyarylethersulfone ketone, polyetherimide, polyphenylene sulfone, and polyisophthalamide.
[0045] In some optional embodiments, the thickness of the substrate layer 100 is d1, and the value of d1 is in the range of 3μm ≤ d1 ≤ 36μm. For example, the thickness d1 of the substrate layer 100 can be 3μm, 4μm, 5μm, 6μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, or 36μm, or any combination of the above values. The thickness of the functional coating 200 is d2, and the value of d2 is in the range of 0.5μm ≤ d2 ≤ 10μm. For example, the thickness d2 of the functional coating 200 can be 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 2μm, 3μm, 4μm, 5μm, or 10μm, or any combination of the above values.
[0046] This application also provides a method for preparing a battery composite separator, which includes the following steps:
[0047] The high-temperature resistant polymer material is dissolved in a solvent according to a preset ratio and stirred and mixed evenly to obtain the core layer spinning solution.
[0048] The adhesive and ceramic material are dissolved in a solvent according to a preset ratio and stirred until uniform to obtain a shell spinning solution. The mass ratio of ceramic material to adhesive is 1:0.02-1:0.1.
[0049] Using the core spinning solution and the shell spinning solution as electrospinning solutions, coaxial electrospun fibers 210 are prepared on at least one surface of the substrate layer 100 by coaxial electrospinning.
[0050] After vacuum drying, the substrate layer 100 coated with coaxial electrospun fibers 210 is hot-pressed under preset conditions to form a functional coating 200 and obtain a diaphragm.
[0051] It should be further explained that the coaxial electrospinning method produces coaxial electrospinning fiber 210, and the functional coating 200 is formed by laying or stacking multiple coaxial electrospinning fibers 210. The coaxial electrospinning fiber 210 gives the functional coating 200 a good liquid absorption and retention rate.
[0052] It should be further explained that coaxial electrospinning is a special electrospinning technology that allows solutions of different properties to be injected into two coaxial capillaries, thereby preparing nanofibers with specific structures. The basic principle of this technology is that, under the action of an electric field, the solutions in two coaxial capillaries with different inner diameters (one being the core layer solution 210a, and the other the shell layer solution 210b) converge at the nozzle end and solidify into composite nanofibers. When coating the composite nanofibers onto the substrate layer 100, the two capillaries act as emitters, and a rotating cylinder acts as a receiver. The substrate layer 100 is covered on the rotating cylinder, with one surface facing the emitter. By rotating the rotating cylinder, the composite nanofibers are fully and uniformly coated at different positions on the surface of the substrate layer 100, thus preparing a diaphragm. When it is necessary to coat the composite nanofibers onto both surfaces of the substrate layer 100, coating, drying, and hot-pressing can be completed on one surface, and then the coating can be performed on the other surface facing the emitter.
[0053] Furthermore, the solvent is a highly volatile solvent, including dimethylacetamide. During the preparation of the functional coating 200, the solvent can evaporate, thereby forming a functional coating 200 on the surface of the substrate layer 100, including a core layer 210a formed of a high-temperature resistant polymer material and a shell layer 210b formed of a ceramic material and an adhesive.
[0054] In some alternative embodiments, the mass percentage of the heat-resistant polymer material in the core spinning solution is 5 wt.% to 20 wt.%, for example, the mass percentage of the heat-resistant polymer material is 5 wt.%, 5 wt.%, 6 wt.%, 7 wt.%, 8 wt.%, 9 wt.%, 10 wt.%, 15 wt.%, or 20 wt.%, or any combination of the above values.
[0055] In some alternative embodiments, the total mass percentage of ceramic material and adhesive in the shell spinning solution (or the solid content in the shell 210b spinning solution) is 10 wt.% to 30 wt.%, for example, the mass percentage of ceramic material and adhesive is 10 wt.%, 11 wt.%, 12 wt.%, 13 wt.%, 14 wt.%, 15 wt.%, 20 wt.%, 25 wt.%, or 30 wt.%, or any combination of the above values.
[0056] In some optional embodiments, the coaxial electrospinning method includes fabricating a functional coating 200 using a transmitter and receiver in conjunction under the action of an electric field. The voltage of the electric field is 20kV-30kV, for example, 20kV, 21kV, 22kV, 23kV, 24kV, 25kV, 26kV, 27kV, 28kV, 29kV, or 30kV, or any combination thereof. Controlling the voltage of the electric field can effectively ensure the morphology and diameter of the prepared composite nanofibers, thereby facilitating filamentation and bonding of the composite nanofibers, and effectively improving the mechanical properties of the membrane.
[0057] In some alternative embodiments, the receiver rotation speed is 200 rpm to 400 rpm, for example, the receiver rotation speed is 200 rpm, 240 rpm, 260 rpm, 270 rpm, 300 rpm, 340 rpm, 350 rpm, 360 rpm, 390 rpm or 400 rpm, or any combination of the above values.
[0058] In some alternative embodiments, the distance between the transmitter and the receiver is 15cm-30cm, for example, the distance between the transmitter and the receiver is 15cm, 16cm, 17cm, 18cm, 19cm, 20cm, 21cm, 22cm, 23cm, 24cm, 25cm, 26cm, 27cm, 28cm, 29cm or 30cm, or any combination of the above values.
[0059] In some optional embodiments, the injection rate of the core spinning solution is 0.1 mL / h to 1.0 mL / h, for example, the injection rate of the core spinning solution is 0.1 mL / h, 0.2 mL / h, 0.3 mL / h, 0.4 mL / h, 0.5 mL / h, 0.6 mL / h, 0.7 mL / h, 0.8 mL / h, 0.9 mL / h, or 1.0 mL / h, or any range of the above values. The injection rate of the shell spinning solution is 0.1 mL / h to 1.0 mL / h. For example, the injection rate of the shell spinning solution is 0.1 mL / h, 0.2 mL / h, 0.3 mL / h, 0.4 mL / h, 0.5 mL / h, 0.6 mL / h, 0.7 mL / h, 0.8 mL / h, 0.9 mL / h, or 1.0 mL / h, or any range of the above values. Controlling the injection rates of the core-layer spinning solution and the shell-layer spinning solution can effectively ensure the morphology and diameter of the prepared composite nanofibers, thereby facilitating filamentation and composite nanofiber bonding, and effectively improving the mechanical properties of the membrane. Preferably, the injection rates of the core-layer spinning solution and the shell-layer spinning solution are the same.
[0060] In some optional embodiments, the preset conditions for hot pressing include hot pressing temperature and hot pressing pressure. The hot pressing temperature ranges from 40℃ to 100℃, for example, 40℃, 50℃, 60℃, 70℃, 80℃, 90℃, or 100℃, or any combination thereof. The hot pressing pressure ranges from 5MPa to 20MPa, for example, 5MPa, 6MPa, 7MPa, 8MPa, 9MPa, 10MPa, 15MPa, or 20MPa, or any combination thereof. Hot pressing can improve the mechanical strength of the prepared functional coating 200. Since the composite nanofibers prepared by coaxial electrospinning are often relatively loose and the bonding force between the fibers is weak, resulting in insufficient mechanical strength, hot pressing allows the originally loose fibers to come into close contact and form bonding points, thereby effectively reducing the phenomenon of fiber slippage under stress. This can significantly improve the tensile strength and elongation at break of the functional coating 200. At the same time, hot pressing can also improve the bonding force between the functional coating 200 and the substrate layer 100, effectively improving the mechanical properties of the diaphragm.
[0061] In addition, this application also provides a secondary battery, including the battery composite separator described above or the battery composite separator prepared by the above preparation method.
[0062] To facilitate the explanation of the beneficial effects of this application, the following specific embodiments are also provided.
[0063] Example 1
[0064] This embodiment provides a secondary battery composite separator comprising coaxial electrospun fibers 210, wherein the coaxial electrospun fibers 210 have a polyimide core layer 210a and a polyurethane and alumina shell layer 210b. In this embodiment, the mass ratio of ceramic material to adhesive in the ceramic material and adhesive system is 1:0.07, and the selected high-temperature resistant polymer material is polyimide.
[0065] The coaxial electrospun composite separator for secondary batteries described above is prepared by the following steps:
[0066] Step 1: Add 10.24 mL of dimethylacetamide to 18 g of 25% polyimide emulsion and stir at room temperature for 10 hours to obtain the core spinning solution;
[0067] Step 2: Prepare polyurethane and aluminum oxide according to the ratio. Dissolve 0.46g of polyurethane in 32.45mL of dimethylformamide solvent and stir at 45℃ for 4 hours. Then, add 6.2g of nano aluminum oxide to the above solution, ultrasonically disperse for 30 minutes, and stir at room temperature for 10 hours to obtain a uniform and stable shell spinning solution with a solid content of 16.9wt.%.
[0068] Step 3: Slowly add 5 mL of the core spinning solution from Step 1 to a 10 mL syringe, and slowly add 5 mL of the shell spinning solution from Step 2 to a 10 mL syringe. Connect the two spinning solutions to the core layer 210a and shell layer 210b of the coaxial spinning needle, which serves as the emitter, respectively. Maintain the injection rate of the core spinning solution at 7.1 μL / min, and the injection rate of the shell spinning solution at 7.1 μL / min. A surface covered by the substrate layer 100... A rotating cylinder is used as a receiver at a speed of 360 rpm, and a spinning distance of 20 cm is set between the syringe tip and the receiver. The injection volume of the core layer 210a and the shell layer 210b is 4.2 mL. The spinning solution is passed through the spinneret and the fibers are stretched by a high voltage electrostatic field with a voltage of 20 kV. After the solvent evaporates, a coaxial electrospun composite film of polyimide core and polyurethane ceramic shell layer 210b is obtained on a 9 μm thick polypropylene substrate layer 100.
[0069] Step 4: Place the coaxial electrospun composite membrane obtained in Step 3 in a vacuum oven at 80°C for 10 hours. After taking it out, hot press it at 80°C and 10MPa for 30 minutes to obtain a dried coaxial electrospun composite membrane with polyimide core, polyurethane and polyurethane ceramic shell 210b.
[0070] It should be noted that the injection rates of the core spinning solution and the shell spinning solution mentioned in this article refer to the rate at which the syringe injects liquid into the coaxial spinning needle. The injection volume is the amount of spinning solution used to complete one spinning cycle of the core spinning solution and the shell spinning solution.
[0071] Example 2
[0072] This embodiment provides a secondary battery composite separator including coaxial electrospun fibers 210. The coaxial electrospun fibers 210 have polyimide as the core layer 210a and polyurethane and alumina as the shell layer 210b. The difference from Embodiment 1 is that the mass ratio of ceramic material to adhesive in the ceramic material and adhesive system is different. In this embodiment, the mass ratio of ceramic material to adhesive is 1:0.03, the solid content in the shell spinning solution is 18 wt.%, and the high-temperature resistant polymer material of the core layer 210a is polyetherimide.
[0073] Example 3
[0074] This embodiment provides a secondary battery composite separator including coaxial electrospun fibers 210. The coaxial electrospun fibers 210 have polyimide as the core layer 210a and polyurethane and aluminum oxide as the shell layer 210b. The difference from Embodiment 1 is that the injection rates of the core layer spinning solution and the shell layer spinning solution are different. The injection rate of the core layer spinning solution is maintained at 5.6 μL / min, and the injection rate of the shell layer spinning solution is also maintained at 5.6 μL / min. The electric field voltage is different, which is 18 kV.
[0075] Comparative Example 1
[0076] The diaphragm in this comparative example is a microporous membrane without the above-mentioned functional coating 200. The diaphragm is prepared directly from the substrate layer 100 in the above-mentioned composite diaphragm, that is, the diaphragm is a 9μm thick polypropylene porous membrane.
[0077] Comparative Example 2
[0078] In this comparative example, the membrane was prepared by directly coating the raw materials used to prepare the functional coating 200 onto the surface of the substrate layer 100 after mixing them.
[0079] Specifically, polyimide, aluminum oxide particles, and polyurethane were added to dimethylformamide solvent in a mass ratio of 1:1:0.07 to obtain a slurry with a solid content of 18wt%. The obtained slurry was then coated directly onto a 9μm thick polypropylene substrate using a gravure coating method. The coating amount was the same as that of electrospinning (area density of the coating).
[0080] Comparative Example 3
[0081] This comparative example involves directly preparing an electrospun composite film on the substrate layer 100 using the core layer spinning solution. The method for preparing the electrospun composite film on the substrate layer 100 using the core layer spinning solution is the same as in Example 1.
[0082] The above-mentioned electrospun composite film is prepared by the following steps:
[0083] Step 1: Add 10.24 mL of dimethylacetamide to 18 g of 25% polyimide emulsion and stir at room temperature for 10 hours to obtain a polyimide spinning solution;
[0084] Step 2: Take 5 mL of the polyimide spinning solution from Step 1 and slowly add it into a 10 mL syringe. The injection rate is maintained at 7.1 μL / min. A rotating cylinder covered with a 9 μm substrate layer 100 is used as the receiver, with a rotation speed of 360 rpm. A spinning distance of 20 cm is set between the syringe tip and the receiver. The injection volume of polyimide spinning solution is 4.2 mL. The spinning solution passes through the spinneret and is stretched into fibers under the action of a high-voltage electrostatic field, where the electric field voltage used is 20 kV. After the solvent evaporates, a polyimide core electrospun composite film is obtained on the 9 μm thick polypropylene substrate layer 100.
[0085] Step 3: Place the polyimide core electrospun composite membrane obtained in Step 2 in a vacuum oven at 80°C for 10 hours. After taking it out, hot press it at 80°C and 10MPa for 30 minutes to obtain the dried polyimide core electrospun composite membrane.
[0086] Comparative Example 4
[0087] This comparative example involves directly preparing an electrospun composite film on the substrate layer 100 using the shell spinning solution prepared in Example 1. The method for forming the electrospun composite film on the substrate layer 100 using the shell spinning solution is the same as in Example 1.
[0088] The above-mentioned electrospun composite film is prepared by the following steps:
[0089] Step 1: Prepare polyurethane and aluminum oxide according to the ratio of 1:0.07. Dissolve 0.46g of polyurethane in 32.45mL of dimethylformamide solvent and stir at 45℃ for 4 hours. Then, add 6.2g of nano aluminum oxide to the above solution, ultrasonically disperse for 30 minutes, and stir at room temperature for 10 hours to obtain a uniform and stable ceramic adhesive spinning solution with a solid content of 16.9wt.%.
[0090] Step 2: Take 5 mL of the ceramic adhesive spinning solution from Step 1 and slowly add it into a 10 mL syringe. The injection rate is maintained at 7.1 μL / min. A rotating cylinder covered with a 9 μm substrate layer 100 is used as the receiver, with a rotation speed of 360 rpm. A spinning distance of 20 cm is set between the syringe tip and the receiver. The injection volume of the ceramic adhesive spinning solution is 4.2 mL. The spinning solution passes through the spinneret and is stretched into fibers under the action of a high-voltage electrostatic field, where the electric field voltage used is 20 kV. After the solvent evaporates, a ceramic adhesive electrospun composite film is obtained on the 9 μm thick polypropylene substrate layer 100.
[0091] Step 3: Place the ceramic adhesive electrospun composite membrane obtained in Step 2 in a vacuum oven at 80°C for 10 hours. After taking it out, hot press it at 80°C and 10MPa for 30 minutes to obtain the dried ceramic adhesive electrospun composite membrane.
[0092] The membranes prepared in Examples 1 to 3, and Comparative Examples 1 to 4, were tested to determine their basic physicochemical properties, including ionic conductivity, liquid absorption rate, puncture strength, and heat shrinkage properties. At least 10 data points were collected for each test, and the average of these 10 data points was used as the final test result for comparison. Specifically:
[0093] The method for testing the ionic conductivity of the membrane is as follows: The ionic conductivity is tested using electrochemical impedance spectroscopy. The membrane is wetted with electrolyte, the electrolyte on the membrane surface is removed, and the membrane is sandwiched between identical stainless steel sheets to form a button cell. Impedance spectra are measured within a scanning frequency range of 0.1 Hz to 100,000 Hz. The intersection of the impedance spectrum with the horizontal axis in the high-frequency region represents the bulk resistance (R) of the membrane, and the ionic conductivity (σ) can be calculated using a formula.
[0094] Test of diaphragm liquid absorption rate: The liquid absorption rate of the diaphragm is tested by weighing, that is, by weighing the diaphragm before and after liquid absorption, and comparing the weights to obtain the liquid absorption rate of the diaphragm.
[0095] Puncture strength test of the separator: The battery separator is laid flat in the clamp of the MTL (PC) tensile testing machine and clamped. Puncture is performed at a rate of (100+10) mm / min. After completion, the sample is removed and the thickness is tested at 4 points around the needle hole in accordance with the provisions of GB / T6672-2001. The average value is taken and the puncture strength is calculated according to the formula.
[0096] Thermal shrinkage test of the diaphragm: The test method is in accordance with GB / T 12027-2004. Take three samples with a size greater than or equal to 100mm × 100mm and measure their dimensions before heating. Place the samples between A4 sheets of paper in a 150℃ oven for 30 minutes. Remove them and measure their dimensions in the MD and TD directions after heating. Calculate the thermal shrinkage according to the formula. MD (main direction) refers to the shrinkage rate of the diaphragm in the main direction of the mold, while TD (transverse direction) refers to the shrinkage rate of the diaphragm in the transverse direction of the mold.
[0097] The specific test results are shown in Table 1 below.
[0098] Table 1
[0099]
[0100] Based on the test results of the embodiments and comparative examples in the table above, it can be seen that the composite diaphragm prepared by coating the core-shell structure polymer fiber obtained by the high heat-resistant polymer material and ceramic adhesive system onto the substrate layer 100 has good mechanical properties, thermal stability, ionic conductivity and liquid absorption rate.
[0101] A comparison of the data from Example 1 and Example 2 shows that increasing the specific gravity of ceramic materials is beneficial to improving the ionic conductivity of the diaphragm.
[0102] A comparison of the data from Examples 1 and 3 shows that, in the preparation of coaxial electrospun composite membranes, the higher the injection rate of the core layer spinning solution and the shell layer spinning solution, the lower the bonding of the resulting composite fiber filaments, resulting in high fiber bulkiness and high liquid absorption rate, thereby reducing its mechanical strength. Appropriately controlling the injection rate of the core layer spinning solution and the shell layer spinning solution is beneficial to improving the liquid absorption rate, ionic conductivity, mechanical strength, and thermal stability of the membrane.
[0103] The data from Example 1 and Comparative Example 2 show that the functional coating 200 prepared by coaxial electrospinning can effectively improve the ionic conductivity, liquid absorption rate, mechanical puncture strength and thermal stability of the diaphragm.
[0104] Comparison of data from Comparative Examples 3 and 4 shows that the coaxial electrospun composite separator prepared by combining the core layer 210a and shell layer 210b, with a high heat-resistant polymer material as the core and a ceramic adhesive system as the shell, can greatly improve the ionic conductivity, liquid absorption rate, high temperature resistance and mechanical puncture strength of the separator, thus greatly improving the safety of the battery.
[0105] The above examples illustrate this application only to aid understanding and are not intended to limit its scope. Those skilled in the art to which this application pertains can make various simple deductions, modifications, or substitutions based on the ideas presented.
Claims
1. A battery composite separator, characterized in that: It comprises a substrate layer and a functional coating coated on at least one surface of the substrate layer, wherein the functional coating comprises coaxial electrospun fibers; the coaxial electrospun fibers comprise a core layer and a shell layer wrapped around the core layer, wherein the material forming the core layer comprises a high temperature resistant polymer material, and the material forming the shell layer comprises a ceramic material and an adhesive.
2. The battery composite separator according to claim 1, characterized in that: In the shell layer, the mass ratio of the ceramic material to the adhesive is 1:0.02-1:0.
1.
3. The battery composite separator according to claim 1, characterized in that: The adhesive includes at least one of polyurethane, silicone rubber, polyacrylate, polyamide and polyether.
4. The battery composite separator according to claim 1, characterized in that: The ceramic material includes at least one of boehmite, aluminum oxide and silicon dioxide.
5. The battery composite separator according to claim 1, characterized in that: The high temperature resistant polymer material includes at least one of polyimide, polyarylethersulfoneketone, polyetherimide, polyphenylsulfone and poly(metaphenylene isophthalamide).
6. The battery composite separator according to claim 1, characterized in that: In the functional coating, the coaxial electrospun fibers form a porous network structure.
7. A method for preparing a battery composite diaphragm, used for preparing the battery composite diaphragm according to any one of claims 1 to 6, characterized in that: The following steps are involved: Dissolving the high temperature resistant polymer material in a solvent according to a preset ratio, stirring and mixing to obtain a core layer spinning solution; Dissolving the adhesive and the ceramic material in a solvent according to a preset ratio, stirring and mixing evenly to obtain a shell spinning solution; Using the core layer spinning solution and the shell layer spinning solution as electrospinning solutions, and preparing coaxial electrospinning fibers on at least one surface of the substrate layer by a coaxial electrospinning method; The substrate layer coated with the coaxial electrospun fibers is vacuum dried and then hot-pressed under preset conditions to form a functional coating to obtain the diaphragm.
8. The method for preparing a battery composite separator according to claim 7, characterized in that: When preparing the functional coating, at least one of the conditions (1) to (5) is met: (1) In the core layer spinning solution, the mass percentage of the high temperature resistant polymer material is 5wt.%-20wt.%; (2) In the shell spinning solution, the total mass percentage of the ceramic material and the adhesive is 10wt.%-30wt.%; (3) The coaxial electrospinning method comprises preparing the functional coating by using a transmitter and a receiver in combination under the action of an electric field, wherein the voltage of the electric field is 20 kV-30 kV, the rotation speed of the receiver is 200 rpm-400 rpm, the distance between the transmitter and the receiver is 15 cm-30 cm, the injection rate of the core layer spinning solution is 0.1 mL / h-1.0 mL / h, and the injection rate of the shell layer spinning solution is 0.1 mL / h-1.0 mL / h; (4) The thickness of the functional coating is d2, and the value range of d2 is 0.5 μm ≤ d2 ≤ 10 μm; (5) The mass ratio of the ceramic material to the adhesive is 1:0.02-1:0.
1.
9. The method for preparing a battery composite separator according to claim 7, characterized in that: The preset conditions during hot pressing include hot pressing temperature and hot pressing pressure. The hot pressing temperature has a value range of 40° C.-100° C., and the hot pressing pressure has a value range of 5 MPa-20 MPa.
10. A secondary battery, characterized in that: The invention comprises a battery composite separator according to any one of claims 1 to 6 or a battery composite separator prepared by the preparation method according to any one of claims 7 to 9.
Citation Information
Patent Citations
Nanometer fiber lithium ion battery diaphragm material with composite structure and preparation method of nanometer fiber lithium ion battery diaphragm material
CN102629679A
Battery diaphragm, preparation method thereof and lithium ion battery
CN109473603A
Coaxial electrostatic spinning diaphragm for lithium ion battery and preparation method of coaxial electrostatic spinning diaphragm
CN116315427A