Composite diaphragm as well as preparation method and application thereof
By modifying the multi-layer nanofiber layer on the lithium-ion battery separator, the problems of insufficient thermal stability and electrolyte infiltration are solved, high breathability and pole adhesiveness are achieved, and battery performance and safety are significantly improved. .
Patent Information
- Application Number
- CN202411426258.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional lithium-ion battery separators have problems such as poor thermal stability, low electrolyte wetting, insufficient adhesion and easy ceramic layer to fall off, resulting in battery safety hazards and insufficient performance.
The composite separator including a base film and at least three nanofiber layers modified on the surface of the base film are prepared by electrospinning process, and the heat resistance, adhesion and breathability of the separator are improved using PVDF and aramid nanofiber layers. It forms high porosity and high electrolyte wetting.
It significantly improves the heat resistance of the diaphragm, the electrolyte wetting property and the adhesiveness of the electrode sheet, extends the battery life, and improves battery safety and market competitiveness.
Smart Images

Figure CN118943665A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a composite diaphragm and a preparation method and application thereof, belonging to the technical field of lithium-ion batteries. Background Art
[0002] Traditional polyolefin diaphragms have large thermal shrinkage, which leads to battery short circuits and frequent lithium battery safety accidents. In order to improve the thermal stability of the diaphragm, ceramic coating diaphragm technology is usually used to coat a ceramic layer on the surface of the polyolefin diaphragm to improve the thermal stability of the diaphragm. However, ceramic diaphragms have problems such as poor lyophilicity, low ionic conductivity, poor adhesion to the pole piece, easy detachment of the ceramic layer, and easy pore clogging by ceramic particles. Moreover, ceramic particles have strong water absorption, which can easily cause quality risks such as rapid battery cycle decay. In addition, the high specific gravity of ceramics is not conducive to the lightweighting of large power batteries.
[0003] The full name of aramid is "poly (p-phenylene isophthalamide)", which has excellent properties such as ultra-high strength, high modulus, high temperature resistance, acid and alkali resistance, and light weight. Its thermal decomposition temperature can reach 400-430°C. As a diaphragm coating for lithium-ion batteries, it can greatly improve the heat resistance and safety performance of the battery. However, at present, the phase inversion method is usually used to prepare aramid coated diaphragms. The diaphragm prepared by this method has the problem of pore blocking, the air permeability of the diaphragm is significantly increased, and the coating formed by the aramid slurry has poor adhesion to the base film and is easy to fall off. Therefore, how to apply aramid to the lithium-ion battery diaphragm coating liquid to greatly improve the heat resistance stability and heat shrinkage rate of the lithium battery diaphragm, improve battery performance, extend service life, and enhance market competitiveness is a problem that needs to be solved urgently. Summary of the invention
[0004] In view of the deficiencies in the prior art, one of the objects of the present invention is to provide a composite diaphragm having good high temperature resistance, high wettability, thin thickness, low resistance and high air permeability.
[0005] The second object of the present invention is to provide a method for preparing a composite diaphragm, which is easy to control and can produce a diaphragm material with high quality, reducing battery quality risks and effectively improving battery safety.
[0006] The third object of the present invention is to provide application of the composite diaphragm in lithium ion batteries.
[0007] The present invention adopts the following technical scheme: a composite diaphragm and a preparation method and application thereof. The composite diaphragm comprises a base membrane and at least three nanofiber layers modified on the surface of the base membrane. The first nanofiber layer is a PVDF nanofiber layer, the second nanofiber layer is an aramid nanofiber layer, and the third nanofiber layer is a PVDF nanofiber layer.
[0008] The base film includes a PP film and a PE film, and the thickness of the base film is 4-8 μm.
[0009] Preferably, the thickness of the first nanofiber layer is 1-2µm, the thickness of the second nanofiber layer is 3-8µm, and the thickness of the third nanofiber layer is 1-2µm. Preferably, the diameter of the nanofibers is 200-600nm, and the thickness of the composite membrane is 9-20µm.
[0010] The nanofiber layers are all prepared by an electrostatic spinning process.
[0011] The composite diaphragm of the present invention is provided with a base membrane and at least three nanofiber layers for modifying the surface of the base membrane. The base membrane provides sufficient mechanical strength for the composite diaphragm, the first nanofiber layer provides adhesion for the base membrane and the second nanofiber layer, improves the peel strength, and integrates the base membrane with the spinning composite functional layer; the second nanofiber layer provides sufficient thermal stability for the composite diaphragm, significantly improves the heat resistance of the diaphragm; the third nanofiber layer provides extremely high electrode sheet adhesion for the composite diaphragm, significantly improves the hardness of the battery, reduces the interface resistance of the battery, and improves the battery performance. The electrospinning preparation process gives the diaphragm an extremely high porosity, thereby giving the diaphragm high air permeability. In addition, the second nanofiber layer used in the present invention has a good interaction with the electrolyte, thereby giving the composite diaphragm extremely high electrolyte wettability and liquid retention rate.
[0012] The present application also provides a method for preparing the composite diaphragm, the method comprising the following steps: (1) PVDF is added to polar solvent 1, stirred and dissolved to prepare spinning solution 1. Aramid and a cosolvent are added to polar solvent 2, stirred and dissolved to prepare spinning solution 2.
[0013] (2) Add the spinning solution 1 into the syringe and perform electrospinning at an appropriate voltage, receiving distance and extrusion speed, with the receiving end being the base membrane.
[0014] (3) Add the spinning solution 2 into the syringe and perform electrospinning at an appropriate voltage, receiving distance and extrusion speed, with the receiving end being the diaphragm obtained in step (2).
[0015] (4) Add the spinning solution 1 into the syringe and perform electrospinning at an appropriate voltage, receiving distance and extrusion speed, with the receiving end being the diaphragm obtained in step (3).
[0016] (5) The diaphragm in the previous step is post-treated under appropriate temperature and pressure conditions to obtain a composite diaphragm.
[0017] Preferably, in the above step (1), the polar solvent 1 and the polar solvent 2 are independently selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide, and the co-solvent is selected from at least one of lithium chloride, calcium chloride, and magnesium chloride.
[0018] Preferably, in the above step (1), the concentration of the spinning solution 1 is 13-25wt%, the concentration of the spinning solution 2 is 8-20wt%, and the concentration of the co-solvent is 4-12wt%.
[0019] Preferably, in the above steps (2 / 3 / 4), the electrospinning voltage is set to 15-30 kV, the spinning solution extrusion speed is 0.5-3 ml / h, and the receiving distance is 8-25 cm.
[0020] Preferably, in the above step (5), the post-treatment method is: hot pressing the composite film at 80-120° C. and 5-15 MPa for 3-15 min.
[0021] The present invention uses aramid and PVDF with high thermal stability to jointly modify a polyolefin separator, which can fully improve the thermal shrinkage performance and electrolyte wettability of the separator, while integrating the separator, improving the peel strength, and improving the hardness of the assembled battery.
[0022] The third purpose of the present application is to provide an application of a composite diaphragm for use in lithium-ion batteries, wherein the prepared diaphragm has excellent performance in lithium-ion batteries.
[0023] Compared with the prior art, the composite diaphragm provided in this application has the following advantages: 1. The aramid modified polyolefin separator used in this application can significantly improve the heat resistance and electrolyte wettability of the polyolefin separator, thereby improving battery safety and rate performance.
[0024] 2. This application uses a first nanofiber layer of PVDF to modify the polyolefin membrane and a second nanofiber layer of aramid interface, and through hot pressing treatment, can significantly improve the poor compatibility between aramid and polyolefin membranes, and the resulting composite membrane has good compatibility and strong adhesion.
[0025] 3. In the present application, an electrospinning process is used to prepare a composite diaphragm, and nano-scale filamentous materials are cross-linked to form a functional layer, resulting in high porosity and high ion permeability. Compared with the phase inversion method, it will not block the pores of the basement membrane, thereby giving the diaphragm high air permeability.
[0026] 4. This application uses a third nanofiber layer of PVDF to modify the interface between the second nanofiber layer of aramid and the electrode, and through hot pressing treatment, gives the composite diaphragm extremely high electrode adhesion, significantly improves the battery hardness, reduces the battery interface resistance, and improves battery performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a battery performance diagram of the separator in Example 1 of the present invention and Comparative Examples 1 to 3. DETAILED DESCRIPTION
[0028] The present application is described in detail below in conjunction with embodiments, but the present application is not limited to the following embodiments.
[0029] Example 1 A composite diaphragm and a preparation method and application thereof, comprising the following steps: (1) Add 1.3 g of PVDF to 8.7 g of N,N-dimethylformamide, stir and dissolve to prepare spinning solution 1. Add 1.0 g of aramid and 0.4 g of lithium chloride as a co-solvent to 8.6 g of N,N-dimethylformamide, stir and dissolve to prepare spinning solution 2.
[0030] (2) The spinning solution 1 was added into the syringe, and electrospinning was performed at a voltage of 22 kV, a spinning solution extrusion speed of 1.2 ml / h, and a receiving distance of 8 cm, with the receiving end being the base membrane.
[0031] (3) Add the spinning solution 2 into the syringe and perform electrospinning at a voltage of 18 kV, a spinning solution extrusion rate of 0.8 ml / h, and a receiving distance of 8 cm. The receiving end is the diaphragm obtained in step (2).
[0032] (4) Spinning solution 1 is added into a syringe at a voltage of 22 kV, a spinning solution extrusion rate of 1.2 ml / h, and a receiving distance of 8 cm. The receiving end is the diaphragm obtained in step (3).
[0033] (5) The diaphragm prepared in the previous step is hot pressed at 100°C and 5 MPa for 15 min to obtain a composite diaphragm.
[0034] The base film used in this embodiment is a PE base film with a thickness of 4 μm. The diameters of the first, second and third nanofibers are 200 nm, 300 nm and 200 nm respectively, the thicknesses of the first, second and third nanofiber layers are 1 μm, 3 μm and 1 μm respectively, and the final composite membrane thickness is 9 μm.
[0035] Example 2 A composite diaphragm and a preparation method and application thereof, comprising the following steps: (1) Add 2 g of PVDF to 8 g of N,N-dimethylacetamide, stir and dissolve to prepare spinning solution 1. Add 0.8 g of meta-aramid and 0.6 g of calcium chloride as a co-solvent to 8.6 g of N,N-dimethylformamide, stir and dissolve to prepare spinning solution 2.
[0036] (2) The spinning solution 1 was added into the syringe, and electrospinning was performed at a voltage of 15 kV, a spinning solution extrusion rate of 0.5 ml / h, and a receiving distance of 12 cm, with the receiving end being the base membrane.
[0037] (3) Add spinning solution 2 into the syringe and perform electrospinning at a voltage of 18 kV, a spinning solution extrusion rate of 0.9 ml / h, and a receiving distance of 12 cm. The receiving end is the diaphragm obtained in step (2).
[0038] (4) Spinning solution 1 is added into a syringe at a voltage of 15 kV, a spinning solution extrusion rate of 0.5 ml / h, and a receiving distance of 12 cm. The receiving end is the diaphragm obtained in step (3).
[0039] (5) The diaphragm prepared in the previous step is hot pressed at 120°C and 10 MPa for 10 min to obtain a composite diaphragm.
[0040] The base film used in this embodiment is a PE base film with a thickness of 8 μm. The diameters of the first, second and third nanofibers are 300 nm, 600 nm and 300 nm respectively, the thicknesses of the first, second and third nanofiber layers are 2 μm, 8 μm and 2 μm respectively, and the final composite membrane thickness is 20 μm.
[0041] Example 3 A composite diaphragm and a preparation method and application thereof, comprising the following steps: (1) Add 2.5 g of PVDF to 7.5 g of dimethyl sulfoxide and stir to dissolve to prepare spinning solution 1. Add 2 g of meta-aramid and 1.2 g of magnesium chloride as a co-solvent to 6.8 g of N,N-dimethylformamide and stir to dissolve to prepare spinning solution 2.
[0042] (2) The spinning solution 1 was added into the syringe, and electrospinning was performed at a voltage of 22 kV, a spinning solution extrusion rate of 3 ml / h, and a receiving distance of 25 cm, with the receiving end being the base membrane.
[0043] (3) Add spinning solution 2 into a syringe and perform electrospinning at a voltage of 30 kV, a spinning solution extrusion rate of 0.9 ml / h, and a receiving distance of 25 cm. The receiving end is the diaphragm obtained in step (2).
[0044] (4) Spinning solution 1 is added into a syringe at a voltage of 22 kV, a spinning solution extrusion rate of 3 ml / h, and a receiving distance of 25 cm. The receiving end is the diaphragm obtained in step (3).
[0045] (5) The diaphragm prepared in the previous step was hot pressed at 80°C and 15 MPa for 3 min to obtain a composite diaphragm.
[0046] The base film used in this embodiment is a PP base film with a thickness of 6 μm. The diameters of the first, second and third nanofibers are 300 nm, 600 nm and 300 nm respectively, the thicknesses of the first, second and third nanofiber layers are 1.5 μm, 5 μm and 1.5 μm respectively, and the final composite membrane thickness is 14 μm.
[0047] Comparative Example 1 Comparative Example 1 is a commercial aramid coated diaphragm with a specification of 7+2 and a thickness of 9 μm, and the manufacturer is Hebei Jinli New Energy Technology Co., Ltd.
[0048] Comparative Example 2 Comparative Example 2 is a commercial ceramic coated diaphragm with a specification of 7+3 and a thickness of 10 μm, and the manufacturer is Enjie New Energy Co., Ltd.
[0049] Comparative Example 3 Comparative Example 3 is a commercial PE base film with a thickness of 9 μm, and the manufacturer is Enjie New Energy Co., Ltd.
[0050] Performance Test 1: The diaphragms obtained in Example 1 and Comparative Examples 1 to 3 were tested for heat shrinkage, air permeability, electrolyte wettability and peel strength. The specific test methods are as follows. The test results are shown in Table 1.
[0051] Thermal shrinkage rate: Cut the diaphragm into 100×100mm film samples, measure their longitudinal and transverse lengths, put them into a vacuum oven and bake them for 1h respectively, take out the diaphragm samples, cool them to room temperature, measure their longitudinal and transverse lengths again, calculate the thermal shrinkage rate, and characterize the heat resistance of the diaphragm. Test them at three temperatures of 105℃, 120℃ and 150℃ respectively.
[0052] Air permeability: Use a membrane air permeability tester to test the air permeability of the composite membrane.
[0053] Electrolyte Wettability: The electrolyte wettability uses electrolyte solvent (ethylene carbonate and dimethyl carbonate, with a mass ratio of 1:1) as the test object to test the liquid absorption rate.
[0054] Peel strength: The coated surface of the composite diaphragm is bonded with tape to prepare a sample. The base film and the tape are fixed with a universal testing machine respectively, and peeled off from the adhesive opening at a specified rate. In this way, the coating and the base film are gradually separated along the length of the adhered surface. The force value when the coating and the base film are separated is automatically obtained by the testing machine, and the peel force between the diaphragm coating and the base film is calculated.
[0055] Table 1 Heat shrinkage, air permeability and peel strength of the diaphragm in Example 1 of the present invention and Comparative Examples 1-3
[0056] The separators in the examples and comparative examples are assembled into soft-pack batteries, the positive electrode uses 811 electrode sheets, and the negative electrode uses graphite negative electrode. The positive electrode sheet, separator, negative electrode sheet, and separator are stacked in sequence to form a "sandwich" structure to form a battery cell that can be packaged. The test rate curve is as follows: Figure 1 shown.
[0057] As can be seen from Table 1, the heat resistance of the diaphragm provided in Example 1 is much higher than that of Comparative Example 3, indicating that the nanofiber layer significantly improves the thermal stability of the diaphragm. The air permeability of the diaphragm provided in Example 1 is much higher than that of Comparative Example 1 and Comparative Example 2, indicating that compared with commercial aramid coated diaphragms and commercial ceramic coated diaphragms, the air permeability of the composite diaphragm in the present application is extremely high. The peeling force between the coating and the base film of the diaphragm provided in Example 1 is higher than that of Comparative Example 1, indicating that the adhesion between the nanofiber layer and the base film is good. It can be seen from the electrolyte wettability experiment that compared with Comparative Example 1 and Comparative Example 2, the electrolyte wettability of the diaphragm provided in Example 1 is significantly improved than that of the aramid coated diaphragm provided in Comparative Example 1, the ceramic coated diaphragm provided in Comparative Example 2, and the PE base film provided in Comparative Example 3, indicating that the spinning layer structure and composition can significantly improve the wettability of the diaphragm to the electrolyte. Combined with the analysis of Table 1, it can be obtained that the composite diaphragm provided by the present invention has high electrolyte wettability, thermal stability and air permeability, and the coating and the base film have good adhesion.
[0058] Depend on Figure 1 It can be seen that the ceramic coated diaphragm in Comparative Example 2 has no significant change in rate performance compared to the traditional PE-based membrane in Comparative Example 3. The aramid coated diaphragm in Comparative Example 1 has significantly improved rate performance compared to the PE-based membrane in Comparative Example 3. The rate performance of the composite membrane in Example 1 is significantly improved. This is because the components of the composite functional layer used in this application have good compatibility with the electrolyte, which makes the composite diaphragm have an extremely high liquid absorption rate. In addition, the composite functional layer is prepared by an electrospinning process to form a porous structure, which further significantly improves the wettability and liquid retention rate of the electrolyte. At the same time, the third nanofiber layer significantly improves the bonding force between the diaphragm and the electrode, thereby reducing the interface resistance and improving the battery performance.
[0059] The above are only some of the embodiments of the invention, and do not constitute any formal limitation on the present application. All raw material ratios, upper and lower limits of working conditions and interval values in the preparation process of the present application can realize the present application, and the embodiments are not listed one by one here. Any person familiar with this profession, without departing from the technical solution of the present application, can make some changes or modifications to the equivalent embodiments of the decoration by using the above technical content. However, any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present application without departing from the content of the technical solution of the present application are still within the scope of the technical solution of the present application.
Claims
1. A composite diaphragm, characterized in that: The composite membrane comprises a base membrane and at least three nanofiber layers modified on the surface of the base membrane; the first nanofiber layer is a PVDF nanofiber layer, the second nanofiber layer is an aramid nanofiber layer, and the third nanofiber layer is a PVDF nanofiber layer.
2. The composite diaphragm according to claim 1, characterized in that: The base film includes a PP film and a PE film, and the thickness of the base film is 4-8 μm.
3. The composite diaphragm according to claim 1, characterized in that: The thickness of the first nanofiber layer is 1-2µm, the thickness of the second nanofiber layer is 3-8µm, and the thickness of the third nanofiber layer is 1-2µm; the diameters of the nanofibers are all 200-600nm, and the thickness of the composite membrane is 9-20µm.
4. The composite diaphragm according to claim 1, characterized in that: The nanofiber layers are all prepared by an electrostatic spinning process.
5. A method for preparing a composite diaphragm, characterized in that: The following steps are involved: (1) adding PVDF to polar solvent 1, stirring and dissolving, to prepare spinning solution 1; adding aramid and cosolvent to polar solvent 2, stirring and dissolving, to prepare spinning solution 2; (2) Adding the spinning solution 1 into the syringe, and performing electrospinning at an appropriate voltage, receiving distance and extrusion speed, with the receiving end being the base film; (3) Adding the spinning solution 2 into the syringe, and performing electrospinning at an appropriate voltage, receiving distance and extrusion speed, the receiving end being the diaphragm obtained in step (2); (4) Adding the spinning solution 1 into the syringe, and performing electrospinning at an appropriate voltage, receiving distance and extrusion speed, the receiving end being the diaphragm obtained in step (3); (5) The diaphragm in the previous step is post-treated under appropriate temperature and pressure conditions to obtain a composite diaphragm.
6. The method for preparing the composite diaphragm according to claim 5, characterized in that: In the step (1), the polar solvent 1 or the polar solvent 2 is independently selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide, and the co-solvent is selected from at least one of lithium chloride, calcium chloride, and magnesium chloride.
7. The method for preparing a composite diaphragm according to claim 5, characterized in that: In the step (1), the concentration of the spinning solution 1 is 13-25wt%, the concentration of the spinning solution 2 is 8-20wt%, and the concentration of the co-solvent is 4-12wt%.
8. The method for preparing a composite diaphragm according to claim 5, characterized in that: In the steps (2), (3) and (4), the electrospinning voltage is set to 15-30 kV, the spinning solution extrusion speed is 0.5-3 ml / h, and the receiving distance is 8-25 cm.
9. The method for preparing a composite diaphragm according to claim 5, characterized in that: In the step (5), the post-treatment method is: hot pressing the composite film at 80-120° C. and 5-15 MPa for 3-15 min.
10. Use of the composite diaphragm according to any one of claims 1 to 4 or the composite diaphragm obtained by the preparation method according to any one of claims 5 to 9 in a lithium ion battery.
Citation Information
Patent Citations
Lithium-ion battery separator subjected to composite coating treatment and preparation method thereof
CN106252565A
Environment-friendly high-magnification coated diaphragm
CN113675534A
Compound lithium ion battery diaphragm of aramid fiber
CN208522020U
Composite lithium ion battery diaphragm and lithium ion battery
CN210778776U
Lithium ion battery separator having high temperature-resistant coating and preparation method therefor
WO2020155001A1
Cited By
Composite fiber diaphragm for alkaline electrolytic cell and preparation method of composite fiber diaphragm
CN119663370A