Electrothermal film with low resistance dispersion and manufacturing method thereof

By using a combination of ceramic matrix layer and ruthenium dioxide and silica in the electric heating film, the problem of conductive chain instability caused by high-temperature sintering of silver powder is solved, and the consistency of resistance value of the electric heating film and production reliability are achieved.

CN118945912APending Publication Date: 2024-11-12SHANGHAI SHUXIN ELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411088401.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The irregular shrinkage of the silver powder during the high-temperature sintering of the existing electric heating films leads to unstable conductive chains and the resistance value cannot be adjusted, resulting in difficulty in production and low yield.

Method used

Ceramics are used as the substrate layer, and ruthenium dioxide and silica are added to the conductive heating layer to form a stable conductive chain through high temperature sintering to control the consistency of the resistance value.

Benefits of technology

The electric heating film resistance discrete is reduced, the resistance value consistency is ensured, and the production reliability and yield rate are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118945912A_ABST
    Figure CN118945912A_ABST
Patent Text Reader

Abstract

The invention discloses an electrothermal film with low resistance dispersion and a manufacturing method thereof, and relates to the technical field of electrothermal film manufacturing. The electrothermal film with low resistance dispersion comprises a substrate layer, a conductive heating layer is filled outside the substrate layer, a thick-film resistance paste layer is coated outside the conductive heating layer, a cut-off layer is arranged outside the conductive heating layer, a wire is arranged between the cut-off layer and the conductive heating layer, and the thick-film resistance paste layer is coated outside the thick-film resistance paste layer. And the guide layer, the cut-off layer and the conductive heating layer are communicated with the substrate layer in the thick-film resistor paste layer through one end of the packaging layer and are sealed. The conductive phases ruthenium dioxide and silicon dioxide are added on the original basis, the conductive phases are stable and low in shrinkage degree in the high-temperature sintering process, meanwhile, the particles are interspersed among the silver particles, irregular shrinkage of silver in the high-temperature sintering process is prevented, a stable conductive chain is formed, and therefore the purpose of controlling the consistency of the resistance value of the electrothermal film is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electric heating film manufacturing, in particular to an electric heating film with low resistance dispersion and a manufacturing method thereof. Background Art

[0002] The electric film heating system is different from the point heating system represented by radiators, air conditioners, and radiators, and the line heating system represented by heating cables. It is a low-carbon heating high-tech product developed using modern aerospace technology in the field of surface heating.

[0003] The principle of electric heating film heating is that under the action of the electric field, the carbon molecules in the heating element produce "Brownian motion", and violent friction and collision occur between the carbon molecules. The heat energy generated is transmitted to the outside in the form of far-infrared radiation and convection, and the conversion rate of electric energy to heat energy is as high as more than 98%. The action of carbon molecules causes the surface of the system to heat up rapidly. When the electric heating film heating system is installed on the wall (ground), the heat energy will be continuously and evenly transmitted to every corner of the room. The reason why the electric heating film can quickly heat up the space is that its 100% of the electrical energy input is effectively converted into more than 66% of far-infrared radiation energy and 33% of convection heat energy. The electric heating film has a broad development prospect because it meets the policy orientation of emission reduction and low carbon.

[0004] In the process of making electric heating films, the prior art mainly adds chitosan derivatives to achieve uniform dispersion of conductive fillers and high component compatibility of the products, thereby solving the problems of low conductive efficiency of the electric heating film caused by uneven distribution and agglomeration of conductive fillers in the slurry and low component compatibility caused by adding dispersants and thickeners in the related art.

[0005] In the above-mentioned method for preparing the electric heating film, the resistor paste is mainly composed of silver powder, palladium powder, glass powder and added chitosan derivatives. Since the silver powder shrinks uncontrollably under high-temperature sintering and cannot form a stable conductive chain, the above-mentioned electric heating film product cannot adjust the resistance value, resulting in production difficulties and low yield. Summary of the invention

[0006] In view of the deficiencies of the prior art, the present invention provides an electric heating film with low resistance dispersion and a manufacturing method thereof, which solves the problems raised in the above-mentioned background technology.

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions: an electric heating film with low resistance dispersion and a manufacturing method thereof, comprising a base layer, the outside of the base layer is filled with a conductive heating layer, the outside of the conductive heating layer is coated with a thick film resistor slurry layer, the area of ​​the thick film resistor slurry layer is larger than the conductive heating layer, the area of ​​the conductive heating layer is larger than the base layer, a cutoff layer is arranged outside the conductive heating layer, a wire is arranged between the cutoff layer and the conductive heating layer, the guide, the cutoff layer and the conductive heating layer are connected to the base layer inside the thick film resistor slurry layer through one end of the packaging layer and are sealed.

[0008] A further improvement of the technical solution of the present invention is that the thick film resistor slurry layer is composed of ruthenium dioxide, silver, silicon dioxide, Pd, glass powder, other oxides and a carrier.

[0009] A further improvement of the technical solution of the present invention is that the surface of the base layer is dense and has a smooth and bright surface state, and the material of the base layer is ceramic, and the dielectric loss tangent of the base layer is positive.

[0010] Regarding the selection of the substrate, the surface of the substrate should not have visible damage, bubbles, cracks, spots, etc. The reason why this electric heating film uses ceramic as the substrate is that the ceramic surface has uneven particles, and the unevenness is relatively fine and uniform, with an unevenness of about 2-3mm. In addition, the ceramic surface has high cleanliness and is easy to clean. It is insoluble in the film to produce pinholes, so the resistor is not prone to short circuit and high resistance.

[0011] The further improvement of the technical solution of the present invention is:

[0012] The present invention also provides a method for manufacturing an electric heating film with low resistance dispersion, which is characterized by comprising the following specific steps:

[0013] S1: Substrate pretreatment: select a ceramic tube as the substrate of the electric heating film, scrub the ceramic tube with anhydrous ethanol or acetone, then wash it with deionized water, and place it in a drying oven for 30 minutes for drying;

[0014] S2: Preparation of electric heating film solution; add 4-10 parts of ruthenium dioxide, 53-72 parts of silver, 1-5 parts of silicon dioxide, 1 part of Pd, 8-22 parts of glass powder, 1-2 parts of other oxides, and 12-36 parts of organic carrier according to the following weight ratio, pour into a beaker and mix, add acid and alcohol, stir evenly, and set aside;

[0015] S3: coating; the electric heating film solution prepared in S2 is vaporized into smoke at 400-700°C. When the steam passes through the heated substrate, it undergoes a hydrolysis reaction with the substrate surface to form an electric heating film. During the coating process, the ceramic tube substrate rotates at a speed of 3-10r / min.

[0016] S4: annealing treatment: annealing the substrate formed in S3 at 200-400°C for 15-20 minutes, then cooling down and allowing to cool naturally;

[0017] S5: Assemble electrodes; use a brush method to apply conductive silver paste on both ends of the electric heating film, and then bake it at 500°C. The silver paste gradually decomposes into a white silver layer under high temperature, and after it firmly penetrates the surface of the electric heating film to form a silver electrode, it is connected to the wire on the motor by mechanical crimping.

[0018] A further improvement of the technical solution of the present invention is that the organic carrier in S2 includes but is not limited to terpineol, butyl carbitol acetate, ethylene glycol ethyl ether acetate, tributyl citrate, dibutyl phthalate and lecithin.

[0019] A further improvement of the technical solution of the present invention is that a surfactant, a plasticizer, a fluidity control agent and a diluent are added during the mixing process in the beaker in S2.

[0020] A further improvement of the technical solution of the present invention is that other oxides in S2 include but are not limited to Mn, Nd and Sb.

[0021] A further improvement of the technical solution of the present invention is that the surface area coverage rate of Ru atoms and Si atoms in the electrothermal film embryo prepared in S4 is greater than 62%.

[0022] Beneficial Effects

[0023] The present invention provides an electric heating film with low resistance dispersion and a manufacturing method thereof. Compared with the prior art, the present invention has the following beneficial effects:

[0024] The electric heating film with low resistance dispersion and its manufacturing method are designed by redesigning the resistor formula, adding a new conductive phase of ruthenium dioxide and introducing a certain amount of silicon dioxide. The above measures are used to control the problem of large resistance dispersion of electric heating film products in the production process. Because the new conductive phases of ruthenium dioxide and silicon dioxide are stable and have a slight shrinkage during high-temperature sintering, these particles are interspersed between silver particles to prevent irregular shrinkage of silver during high-temperature sintering, forming a stable conductive chain, thereby achieving the consistency of controlling the resistance value of the electric heating film. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The structure cross-sectional view of the electric heating film with low resistance dispersion and the electric heating film in the manufacturing method thereof;

[0026] Figure 2 The characteristic curve diagram of the resistance dispersion of the products manufactured in the second embodiment and the third embodiment of the electric heating film with low resistance dispersion and the manufacturing method thereof;

[0027] Figure 3 The resistance dispersion characteristic curve diagram of the electric heating film with low resistance dispersion and the manufacturing method thereof after introducing different amounts of ruthenium dioxide in Example 2 and Example 4;

[0028] Figure 4 The resistance dispersion characteristic curve diagram of the electric heating film with low resistance dispersion and the manufacturing method thereof after introducing different amounts of silicon dioxide in Example 2;

[0029] Figure 5 A schematic diagram of manufacturing an electric heating film with low resistance dispersion and a manufacturing method thereof;

[0030] Figure 6 A manufacturing flow chart of an electric heating film with low resistance dispersion and a manufacturing method thereof

[0031] In the figure: 1. substrate layer; 2. conductive heating layer; 3. thick film resistor slurry layer; 4. cut-off layer; 5. wire; 6. packaging layer. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Reference Figure 1-Figure 6 , the present invention provides 6 technical solutions:

[0034] Embodiment 1:

[0035] An electric heating film with low resistance dispersion comprises a base layer, the outside of the base layer is filled with a conductive heating layer, the outside of the conductive heating layer is coated with a thick film resistor slurry layer, the area of ​​the thick film resistor slurry layer is larger than the conductive heating layer, the area of ​​the conductive heating layer is larger than the base layer, a cut-off layer is arranged outside the conductive heating layer, a wire is arranged between the cut-off layer and the conductive heating layer, the guide, the cut-off layer and the conductive heating layer are connected to the base layer inside the thick film resistor slurry layer through one end of the packaging layer and are sealed.

[0036] The thick film resistor paste layer is composed of ruthenium dioxide, silver, silicon dioxide, Pd, glass powder, other oxides and a carrier.

[0037] The surface of the base layer is dense and has a smooth and clean surface state, and the material of the base layer is ceramic, and the dielectric loss tangent of the base layer is positive.

[0038] The substrate should not have visible damage, bubbles, cracks, spots, etc. on its surface. The reason why this electric heating film uses ceramic as the substrate is that the ceramic surface has uneven particles, and the unevenness is relatively fine and uniform, with an unevenness of about 2-3mm. In addition, the ceramic surface has high cleanliness and is easy to clean. It is not soluble in the film to produce pinholes, so the resistor is not easy to produce short circuit and high resistance.

[0039] A method for manufacturing an electric heating film with low resistance dispersion comprises the following steps:

[0040] S1: Substrate pretreatment: select a ceramic tube as the substrate of the electric heating film, scrub the ceramic tube with anhydrous ethanol or acetone, then wash it with deionized water, and place it in a drying oven for 30 minutes for drying;

[0041] S2: Preparation of electric heating film solution; add 4-10 parts of ruthenium dioxide, 53-72 parts of silver, 1-5 parts of silicon dioxide, 1 part of Pd, 8-22 parts of glass powder, 1-2 parts of other oxides, and 12-36 parts of organic carrier according to the following weight ratio, pour into a beaker and mix, add acid and alcohol, stir evenly, and set aside;

[0042] In this embodiment, conductive phase ruthenium dioxide and silicon dioxide are added to the original basis, which is stable during high-temperature sintering and has a slight shrinkage. At the same time, these particles are interspersed between silver particles to prevent the irregular shrinkage of silver during high-temperature sintering, ensuring that a stable conductive chain can be formed, thereby achieving the consistency of controlling the resistance value of the electric heating film;

[0043] The oxides include Mn, Nd, Sb, etc.

[0044] S3: coating; the electric heating film solution prepared in S2 is vaporized into smoke at 400-700°C. When the steam passes through the heated substrate, it undergoes a hydrolysis reaction with the substrate surface to form an electric heating film. During the coating process, the ceramic tube substrate rotates at a speed of 3-10r / min.

[0045] S4: annealing treatment: annealing the substrate formed in S3 at 200-400°C for 15-20 minutes, then cooling down and allowing to cool naturally;

[0046] S5: Assemble electrodes; use a brush method to apply conductive silver paste on both ends of the electric heating film, and then bake it at 500°C. The silver paste gradually decomposes into a white silver layer under high temperature, and after it firmly penetrates the surface of the electric heating film to form a silver electrode, it is connected to the wire on the motor by mechanical crimping.

[0047] The organic carrier in S2 includes, but is not limited to, terpineol, butyl carbitol acetate, ethylene glycol ethyl ether acetate, tributyl citrate, dibutyl phthalate and lecithin.

[0048] During the mixing process in the beaker in S2, surfactants, plasticizers, fluidity control agents and diluents are added; the film layer of the slurry is in a condensed state before sintering, and the carrier in the film layer is softened and melted by heat in the initial sintering stage, which is prone to secondary flow, causing cracks in the film layer after sintering. For this reason, a fluidity control agent is added to the slurry to control the secondary flow.

[0049] Other oxides in S2 include but are not limited to Mn, Nd and Sb.

[0050] The surface area coverage rate of Ru atoms and Si atoms in the electrothermal film embryo prepared in S4 is greater than 62%.

[0051] Embodiment 2:

[0052] Based on Example 1:

[0053] A method for manufacturing an electric heating film with low resistance dispersion comprises the following specific steps:

[0054] S1: Substrate pretreatment: select a ceramic tube as the substrate of the electric heating film, scrub the ceramic tube with anhydrous ethanol or acetone, then wash it with deionized water, and place it in a drying oven for 30 minutes for drying;

[0055] S2: Preparation of electric heating film solution; add 6 parts of ruthenium dioxide, 53 parts of silver, 3 parts of silicon dioxide, 1 part of Pd, 13 parts of glass powder, 2 parts of other oxides, and 22 parts of organic carrier according to the following weight ratio, pour into a beaker and mix, add acid and alcohol, stir evenly, and set aside;

[0056] S3: coating; the electric heating film solution prepared in S2 is vaporized into smoke at 550°C. When the steam passes through the heated substrate, it undergoes a hydrolysis reaction with the substrate surface to form an electric heating film. During the coating process, the rotation speed of the ceramic tube substrate is 5r / min.

[0057] S4: annealing treatment: annealing the substrate formed in S3 at 320°C for 18 minutes, then cooling down and allowing to cool naturally;

[0058] S5: Assemble electrodes; use a brush method to apply conductive silver paste on both ends of the electric heating film, and then bake it at 500°C. The silver paste gradually decomposes into a white silver layer under high temperature, and after it firmly penetrates the surface of the electric heating film to form a silver electrode, it is connected to the wire on the motor by mechanical crimping.

[0059] Embodiment three:

[0060] Based on Example 1:

[0061] The present invention also provides a method for manufacturing an electric heating film, comprising the following specific steps:

[0062] S1: Substrate pretreatment: select a ceramic tube as the substrate of the electric heating film, scrub the ceramic tube with anhydrous ethanol or acetone, then wash it with deionized water, and place it in a drying oven for 30 minutes for drying;

[0063] S2: Preparation of electric heating film solution; add 60 parts of silver, 1 part of Pd, 13 parts of glass powder, 2 parts of other oxides, and 24 parts of organic carrier according to the following weight ratio, pour into a beaker and mix, add acid and alcohol, stir evenly, and set aside;

[0064] S3: coating; the electric heating film solution prepared in S2 is vaporized into smoke at 550°C. When the steam passes through the heated substrate, it undergoes a hydrolysis reaction with the substrate surface to form an electric heating film. During the coating process, the rotation speed of the ceramic tube substrate is 5r / min.

[0065] S4: annealing treatment: annealing the substrate formed in S3 at 320°C for 18 minutes, then cooling down and allowing to cool naturally;

[0066] S5: Assemble electrodes; use a brush method to apply conductive silver paste on both ends of the electric heating film, and then bake it at 500°C. The silver paste gradually decomposes into a white silver layer under high temperature, and after it firmly penetrates the surface of the electric heating film to form a silver electrode, it is connected to the wire on the motor by mechanical crimping.

[0067] Embodiment 4:

[0068] Based on Example 1:

[0069] A method for manufacturing an electric heating film with low resistance dispersion comprises the following specific steps:

[0070] S1: Substrate pretreatment: select a ceramic tube as the substrate of the electric heating film, scrub the ceramic tube with anhydrous ethanol or acetone, then wash it with deionized water, and place it in a drying oven for 30 minutes for drying;

[0071] S2: Preparation of electric heating film solution; add 10 parts of ruthenium dioxide, 56 parts of silver, 1.5 parts of silicon dioxide, 1 part of Pd, 20 parts of glass powder, 1.5 parts of other oxides, and 30 parts of organic carrier according to the following weight ratio, pour into a beaker and mix, add acid and alcohol, stir evenly, and set aside;

[0072] S3: coating; the electric heating film solution prepared in S2 is vaporized into smoke at 550°C. When the steam passes through the heated substrate, it undergoes a hydrolysis reaction with the substrate surface to form an electric heating film. During the coating process, the rotation speed of the ceramic tube substrate is 5r / min.

[0073] S4: annealing treatment: annealing the substrate formed in S3 at 320°C for 18 minutes, then cooling down and allowing to cool naturally;

[0074] S5: Assemble electrodes; use a brush method to apply conductive silver paste on both ends of the electric heating film, and then bake it at 500°C. The silver paste gradually decomposes into a white silver layer under high temperature, and after it firmly penetrates the surface of the electric heating film to form a silver electrode, it is connected to the wire on the motor by mechanical crimping.

[0075] Embodiment five;

[0076] On the basis of Example 1: S1: substrate pretreatment; a ceramic tube is selected as the substrate of the electric heating film, the ceramic tube is scrubbed with anhydrous ethanol or acetone, then washed with deionized water, and placed in a drying oven for 30 minutes for drying;

[0077] S2: Preparation of electric heating film solution; add 6 parts of ruthenium dioxide, 54 parts of silver, 1 part of Pd, 13 parts of glass powder, 2 parts of other oxides, and 24 parts of organic carrier according to the following weight ratio, pour into a beaker and mix, add acid and alcohol, stir evenly, and set aside;

[0078] S3: coating; the electric heating film solution prepared in S2 is vaporized into smoke at 550°C. When the steam passes through the heated substrate, it undergoes a hydrolysis reaction with the substrate surface to form an electric heating film. During the coating process, the rotation speed of the ceramic tube substrate is 5r / min.

[0079] S4: annealing treatment: annealing the substrate formed in S3 at 320°C for 18 minutes, then cooling down and allowing to cool naturally;

[0080] S5: Assemble electrodes; use a brush method to apply conductive silver paste on both ends of the electric heating film, and then bake it at 500°C. The silver paste gradually decomposes into a white silver layer under high temperature, and after it firmly penetrates the surface of the electric heating film to form a silver electrode, it is connected to the wire on the motor by mechanical crimping.

[0081] Embodiment six:

[0082] The performance test of the electric heating film was carried out on Example 2 and Example 3;

[0083] The electric heating film obtained by adding conductive phase ruthenium dioxide and silicon dioxide in Example 1 and the electric heating film obtained by not adding conductive phase ruthenium dioxide and silicon dioxide in Example 2 are based on the sample substrate being ceramic and the film forming temperature being 550°C. The schematic diagram of the resistance dispersion detection is as shown in the attached figure. Figure 2 As shown;

[0085] The electric heating films obtained by adding different amounts of conductive phase ruthenium dioxide and silicon dioxide in Example 2 and Example 4 were measured based on the sample substrate being a ceramic and the film forming temperature being 550°C. 4-10 groups of control experiments were conducted according to Example 4. A curve of the change of resistance with the amount of ruthenium dioxide added was obtained according to the obtained results, as shown in the attached figure. Figure 3 As shown:

[0087] From the attached Figure 3 It is shown that as the concentration of ruthenium dioxide increases, the mobility of the electric heating film also increases slightly, thereby increasing the conductivity and resistance. When the ruthenium dioxide content is greater than 10%, the number of carriers basically no longer changes, and ruthenium dioxide changes from substitutional to interstitial, which reduces the electron mobility, increases the conductivity, increases the resistance, and increases the dispersion of its resistance value accordingly.

[0088] The second embodiment and the fourth embodiment were compared with the fifth embodiment, and the average resistance error of the fifth embodiment> the fourth embodiment> the second embodiment was obtained. The second embodiment was compared with the fifth embodiment, and it was found that the difference between the fifth embodiment and the second embodiment was that no silicon dioxide was added to the fifth embodiment. Therefore, the second embodiment was used as the basic amount, and different amounts of silicon dioxide were added to measure the average resistance error, as shown in the attached figure. Figure 4 As shown:

[0090] As can be seen from the figure, adding 1-5 parts of silicon dioxide based on a certain amount of ruthenium dioxide can further reduce the dispersion of resistance. Ruthenium dioxide and silicon dioxide prevent the irregular shrinkage of silver during high-temperature sintering, ensuring the formation of a stable conductive chain, thereby achieving the consistency of controlling the resistance value of the electric heating film.

[0091] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art, and the model parameters of each electrical appliance are not specifically limited, and conventional equipment can be used.

[0092] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0093] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An electric heating film with low resistance dispersion, comprising a substrate layer, characterized in that: The outside of the base layer is filled with a conductive heating layer, the outside of the conductive heating layer is coated with a thick film resistor slurry layer, the area of ​​the thick film resistor slurry layer is larger than the conductive heating layer, the area of ​​the conductive heating layer is larger than the base layer, a cut-off layer is arranged outside the conductive heating layer, a wire is arranged between the cut-off layer and the conductive heating layer, the guide, the cut-off layer and the conductive heating layer are connected to the base layer inside the thick film resistor slurry layer through one end of the packaging layer and are sealed.

2. The electric heating film with low resistance dispersion and the manufacturing method thereof according to claim 1, characterized in that: The thick film resistor paste layer is composed of ruthenium dioxide, silver, silicon dioxide, Pd, glass powder, other oxides and a carrier.

3. The electric heating film with low resistance dispersion and the manufacturing method thereof according to claim 1, characterized in that: The surface of the base layer is dense and has a smooth and clean surface state, and the material of the base layer is ceramic, and the dielectric loss tangent of the base layer is positive.

4. A method for manufacturing an electric heating film with low resistance dispersion, characterized in that: The specific steps include: S1: Substrate pretreatment: select a ceramic tube as the substrate of the electric heating film, scrub the ceramic tube with anhydrous ethanol or acetone, then wash it with deionized water, and place it in a drying oven for 30 minutes for drying; S2: Preparation of electric heating film solution; Add 4-10 parts of ruthenium dioxide, 53-72 parts of silver, 1-5 parts of silicon dioxide, 1 part of Pd, 8-22 parts of glass powder, 1-2 parts of other oxides, and 12-36 parts of organic carrier according to the following weight ratio, pour into a beaker and mix, add acid and alcohol, stir evenly, and set aside; S3: coating; the electric heating film solution prepared in S2 is vaporized into smoke at 400-700°C. When the steam passes through the heated substrate, it undergoes a hydrolysis reaction with the substrate surface to form an electric heating film. During the coating process, the ceramic tube substrate rotates at a speed of 3-10r / min. S4: annealing treatment: annealing the substrate formed in S3 at 200-400°C for 15-20 minutes, then cooling down and allowing to cool naturally; S5: assembling electrodes; The two ends of the electric heating film are coated with conductive silver paste using a brush method, and then baked at 500°C. The silver paste is gradually decomposed into a white silver layer under high temperature. After it firmly penetrates the surface of the electric heating film to form a silver electrode, the wires are connected to the motor using mechanical crimping.

5. The method for manufacturing an electric heating film with low resistance dispersion according to claim 4, characterized in that: The organic carrier in S2 includes, but is not limited to, terpineol, butyl carbitol acetate, ethylene glycol ethyl ether acetate, tributyl citrate, dibutyl phthalate and lecithin.

6. The method for manufacturing an electric heating film with low resistance dispersion according to claim 4, characterized in that: During the mixing process in the beaker in S2, a surfactant, a plasticizer, a flow control agent and a diluent are added.

7. The method for manufacturing an electric heating film with low resistance dispersion according to claim 4, characterized in that: Other oxides in S2 include but are not limited to Mn, Nd and Sb.

8. The method for manufacturing an electric heating film with low resistance dispersion according to claim 4, characterized in that: The surface area coverage rate of Ru atoms and Si atoms in the electrothermal film embryo prepared in S4 is greater than 62%.