Method for producing patterned film substrate, and fluorine-containing copolymer
By using specific fluorine-containing copolymers on the patterned film substrate and heating to restore liquid repellency after cleaning, the problem of decreasing liquid repellency in the dam is solved, and the dual maintenance of lyophilicity and liquid repellency of the patterned film is achieved, improving the The pattern formation effect of the inkjet method is achieved.
Patent Information
- Application Number
- CN202411073072.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2018-05-23
- Filing Date
- 2019-05-23
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, after UV ozone cleaning or oxygen plasma cleaning, the liquid repellency of the dam will decrease, resulting in the problem of ink crossing or dissolving the dam in ink.
UV ozone cleaning or oxygen plasma cleaning is performed using a patterned film containing a specific fluorine-containing copolymer, and the liquid repellency is restored by heating. A specific fluorine-containing copolymer structure is used to make the surface free energy small by heating after cleaning. Move to restore hydrophobicity.
The lyophilicity of the concave substrate surface of the pattern film is effectively maintained, and the liquid repellency is restored by heating after cleaning, preventing ink from crossing or dissolving the dam, and improving the pattern formation accuracy and stability in the inkjet method.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
[0001] The present invention is a divisional application of the Chinese patent application with application number 201980034689.0, application date May 23, 2019, and invention name “Method for manufacturing patterned film substrate and fluorinated copolymer”. This application claims the priority of Japanese patent application No. 2018-098679 filed in Japan on May 23, 2018. Technical Field
[0002] The present application relates to a method for manufacturing a patterned film substrate and a fluorinated copolymer. The method for manufacturing a patterned film substrate in the present application can be used, for example, in the manufacture of a display element based on an inkjet method. As a display element, for example, an organic electroluminescent display (hereinafter, an organic EL display), a micro light emitting diode display (hereinafter, a micro LED display) or a quantum dot display can be listed. Background Art
[0003] It is well known to manufacture display elements such as organic EL displays, micro LED displays or quantum dot displays using an inkjet method.
[0004] As methods for manufacturing these display elements using an inkjet method, there can be listed: a method of dripping droplets of ink onto concave portions of a pattern formed on a substrate in the form of projections and recesses of the film through a nozzle and solidifying the resultant; or a method of dripping droplets of ink onto a pattern film pre-formed on a substrate as a lyophilic portion and a lyophobic portion, thereby causing the ink to adhere to the lyophilic portion, wherein the lyophilic portion is a portion that wets with ink and the lyophobic portion is a portion that repels ink.
[0005] In the method of dripping ink droplets to the depressions (concave parts) of the pattern film with concave and convex parts through a nozzle to solidify them, in order to prepare such a pattern film, the following methods can be used: a photolithography method in which a pattern consisting of an exposed part and an unexposed part is formed by exposing the surface of the resist film formed on the substrate in a patterned manner, dissolving any part in a developer, and forming concave and convex parts on the resist film; or an imprinting method in which a pattern film with concave and convex parts is formed on the substrate using a printing technique. In such a pattern film with concave and convex parts, the substrate surface of the concave parts is preferably exposed, and the exposed substrate surface is preferably lyophilic.
[0006] In the inkjet method, the convex parts of the pattern film having concavoconvexities are called banks. When ink is dropped into the concave parts of the pattern film by inkjet, the banks function as a barrier to prevent the mixing of ink.
[0007] For example, Patent Document 1 discloses a composition for an organic EL element used as ink in the manufacture of an organic EL display using an inkjet method. Patent Document 1 also describes that a bank is previously manufactured on a substrate, and an ink (composition for an organic EL element) for forming a light-emitting layer is dripped to manufacture a display element for an organic EL display.
[0008] Patent Document 2 discloses a method for manufacturing a color filter for liquid crystal, characterized in that a photosensitive compound layer is formed on a light-shielding portion on a light-transmitting substrate on which a light-shielding portion is formed by photolithography, and then an inkjet recording device is used to eject ink so that a colorant is arranged on the light-transmitting portion, wherein the photosensitive compound layer contains a surface tension or a critical surface tension of 2.5×10 -2 [N / m] or less. Patent Document 2 also states that when ink is dripped into the concave portion of the pattern film by inkjet, the photosensitive compound layer forming the dam contains a fluorine-based polymer or a fluorine-based surfactant, thereby improving the liquid repellency of the dam and preventing the ink from crossing the dam and invading the adjacent concave portion.
[0009] Patent document 3 discloses a lyophobic resist composition for obtaining a pattern consisting of a lyophobic region and a lyophilic region by photolithography. Patent document 3 also states that by using the lyophobic resist composition, a lyophobic-lyophilic pattern having a clear ink wetting contrast can be formed on a substrate by an inkjet method, and that when ink is dripped into a concave portion of a pattern film by an inkjet method, the surface of the substrate as the concave portion is made lyophilic and the surface of the dam is made lyophobic.
[0010] Patent Document 4 discloses a patterning substrate for inkjet method, which has a thin film on which a bank of a predetermined height and a coated area separated by the bank are formed. Patent Document 4 also states that the coated area as a concave portion is lyophilic, and the bank as a convex portion is lyophobic.
[0011] Patent Document 5 discloses a positive photosensitive resin composition that can form an image having high hydrophobicity and oleophobicity on the surface of a cured film. Patent Document 5 also states that the positive photosensitive resin composition is suitable for use as an interlayer insulating film in a liquid crystal display or an EL display, a light shielding material or a spacer material corresponding to an inkjet method.
[0012] In addition, Patent Documents 4 and 5 also record that when a pattern film is formed on a substrate by photolithography, the substrate surface as the concave portion of the pattern film is contaminated by organic matter, and when a pattern film is formed by an imprinting method, film residue occurs in the concave portion of the pattern film. Due to these defects, the concave portion of the pattern film becomes hydrophobic, so a hydrophilic treatment is performed on a substrate with a pattern film using a hydrophilic ink to make the concave portion of the pattern film hydrophilic. When the hydrophilic treatment is performed, the concave portion of the pattern film does not repel ink during inkjet printing, and ink can be dripped onto the substrate with the pattern film well.
[0013] Patent Document 4 also describes that by bringing a pattern film-attached substrate into contact with oxygen plasma gas and fluorine plasma gas, the substrate surface as the concave portion of the pattern film is made hydrophilic and the bank of the convex portion is made hydrophobic.
[0014] According to the positive photosensitive resin composition described in Patent Document 5, a substrate with a patterned film can be obtained in which the surface of the patterned film as a bank remains highly liquid-repellent after UV ozone cleaning during the hydrophilization treatment.
[0015] Prior art literature
[0016] Patent Literature
[0017] Patent Document 1: Japanese Patent Application Laid-Open No. 11-54270
[0018] Patent Document 2: Japanese Patent Application Laid-Open No. 10-197715
[0019] Patent Document 3: Japanese Patent Application Publication No. 2012-220860
[0020] Patent Document 4: Japanese Patent Application Publication No. 2000-353594
[0021] Patent Document 5: International Publication No. 2017 / 126610 Summary of the invention
[0022] 1. Technical issues to be resolved
[0023] As described in Patent Documents 4 and 5, in order to improve the lyophilicity of the substrate surface serving as the concave portion of the pattern film, when the substrate with the pattern film is subjected to UV ozone cleaning or oxygen plasma cleaning, the lyophobicity of the dam will decrease after cleaning, and when ink is dripped into the concave portion of the pattern film by an inkjet method, there is a problem of the ink crossing over the dam or the dam dissolving in the ink.
[0024] The present application provides a method for manufacturing a substrate with a pattern film that solves the above problems. In addition, the present application provides a novel fluorine-containing copolymer contained in the above pattern film.
[0025] (II) Technical solution
[0026] The inventors of the present application conducted in-depth research to solve the above-mentioned problems, and found that when a patterned film substrate containing a specific fluorinated copolymer is subjected to UV ozone cleaning or oxygen plasma cleaning, the liquid repellency of the patterned film will temporarily decrease, but the liquid repellency can be restored (the liquid repellency is restored) by subsequent heating.
[0027] For pattern films containing specific fluorinated copolymers, after UV ozone cleaning or oxygen plasma cleaning, it is observed that the lyophobicity to water and anisole used as an ink solvent in the inkjet method decreases, but by heating the pattern film, the decreased lyophobicity to water and anisole will be restored (see Table 2 and Table 3 of [Examples] of this specification). Similarly, for pattern films containing specific fluorinated copolymers, after UV ozone cleaning or oxygen plasma cleaning, it is observed that the lyophobicity to propylene glycol monomethyl ether acetate (PGMEA) and xylene decreases, but by heating the pattern film, the decreased lyophobicity to PGMEA and xylene will be restored (see Table 4 and Table 5 of [Examples] of this specification). In this way, the inventors of the present application unexpectedly found that for pattern films containing specific fluorinated copolymers, the lyophobicity is significantly restored by heating after UV cleaning.
[0028] It is speculated that the reason why the liquid repellency is restored by heating is that the membrane surface is oxidized and becomes liquid-philic by UV ozone cleaning or oxygen plasma cleaning, but because a special fluorinated copolymer that can inhibit the cleavage of the polymer main chain is used, the fluoroalkyl part with small surface free energy moves to the membrane surface due to the molecular movement caused by heating.
[0029] In the present application, UV ozone cleaning refers to a method of removing organic pollutants by irradiating a substrate with a patterned film with ultraviolet rays to break the chemical bonds of organic pollutants attached to the patterned film and the recessed portions of the substrate with the patterned film, and chemically bonding the active oxygen separated from the ozone generated by the ultraviolet irradiation with the organic pollutants to decompose them into volatile substances such as carbon dioxide and water. As an ultraviolet irradiation device, a low-pressure mercury lamp is generally used.
[0030] Oxygen plasma cleaning is a method of applying high pressure to a gas containing oxygen molecules to dissociate the oxygen molecules to generate active oxygen, thereby decomposing organic pollutants attached to the surface of the patterned film substrate into volatile substances such as carbon dioxide and water and removing them.
[0031] Inventions 1 to 17 are disclosed below.
[0032] [Invention 1]
[0033] A method for manufacturing a patterned film substrate, comprising:
[0034] A cleaning process of performing UV ozone cleaning or oxygen plasma cleaning on a patterned film substrate to obtain a first patterned film substrate, wherein the patterned film substrate is a patterned film substrate having a pattern formed on a substrate, the pattern film containing a fluorine-containing copolymer, and the fluorine-containing copolymer simultaneously contains a repeating unit represented by formula (A) and a repeating unit represented by formula (C); and
[0035] A heating step of heating the first patterned film substrate to obtain a second patterned film substrate.
[0036] [Chemical formula 1]
[0037]
[0038] In the formula, R 1 , R 3 Each independently represents a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group are optionally substituted by fluorine atoms. Q represents a fluoroalkyl group having 1 to 20 carbon atoms, which optionally has a hydrogen atom, an oxygen atom or a nitrogen atom. X represents a single bond or a divalent group. Z represents an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups are optionally substituted by fluorine atoms, oxygen atoms or nitrogen atoms. O represents an oxygen atom.
[0039] [Invention 2]
[0040] The production method according to Invention 1, wherein the fluorinated copolymer contains a repeating unit represented by formula (A), a repeating unit represented by formula (B), and a repeating unit represented by formula (C) simultaneously.
[0041] [Chemical formula 2]
[0042]
[0043] In the formula, R 1 , R 2 , R 3 Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group are optionally substituted by fluorine atoms. Q is a fluoroalkyl group having 1 to 20 carbon atoms, which optionally has a hydrogen atom, an oxygen atom or a nitrogen atom. X and Y are each independently a single bond or a divalent group. Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups are optionally substituted by fluorine atoms, oxygen atoms or nitrogen atoms. O is an oxygen atom and H is a hydrogen atom.
[0044] [Invention 3]
[0045] In the manufacturing method according to the invention 1 or 2, in the heating step, the first patterned film substrate is heated at a temperature of 50° C. to 350° C. for 10 seconds or more.
[0046] [Invention 4]
[0047] The manufacturing method according to any one of Inventions 1 to 3, wherein the second patterned film substrate is a substrate for forming a display element by an inkjet method.
[0048] [Invention 5]
[0049] The production method according to any one of Inventions 1 to 4, wherein Q in the repeating unit represented by formula (A) is a fluoroalkyl group having 3 to 10 carbon atoms, and X is a carbonyl group.
[0050] [Invention 6]
[0051] The production method according to Invention 5, wherein Q in the repeating unit represented by the formula (A) is a perfluorohexylethyl group and X is a carbonyl group.
[0052] [Invention 7]
[0053] The production method according to Invention 5, wherein Q in the repeating unit represented by the formula (A) is a hexafluoroisopropyl group and X is a carbonyl group.
[0054] [Invention 8]
[0055] The production method according to any one of Inventions 1 to 4, wherein the repeating unit represented by the formula (A) is a repeating unit represented by the formula (A-1).
[0056] [Chemical formula 3]
[0057]
[0058] In formula (A-1), R 4 , R 5 Each independently represents a hydrogen atom, a fluorine atom or an alkyl group having 1 to 3 carbon atoms, wherein a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted with fluorine atoms. O represents an oxygen atom, H represents a hydrogen atom, and F represents a fluorine atom.
[0059] [Invention 9]
[0060] A production method as described in any one of Inventions 2 to 4, wherein Q possessed by the repeating unit represented by formula (A) is a hexafluoroisopropyl group and X is a carbonyl group; and Y possessed by the repeating unit represented by formula (B) is a p-phenylene group or a carboxyethylene group.
[0061] [Invention 10]
[0062] A production method as described in any one of Inventions 2 to 4, wherein Q possessed by the repeating unit represented by formula (A) is hexafluoroisopropyl and X is a carbonyl group; Y possessed by the repeating unit represented by formula (B) is p-phenylene or carboxyethylene; and Z possessed by the repeating unit represented by formula (C) is an alkoxy group, a carboxyl group, an acetoxy group or a bistrifluoromethylvinyl group.
[0063] [Invention 11]
[0064] The production method according to any one of Inventions 2 to 4, wherein Z in the repeating unit represented by the formula (C) is a bistrifluoromethylvinyl group.
[0065] [Invention 12]
[0066] A production method as described in any one of Inventions 2 to 4, wherein Q possessed by the repeating unit represented by formula (A) is a fluoroalkyl group having 3 to 10 carbon atoms, and X is a carbonyl group; Y possessed by the repeating unit represented by formula (B) is a p-phenylene group, a p-phenylenecarbonyl group or a p-phenylenehexafluoroisopropylidene group; and Z possessed by the repeating unit represented by formula (C) is a bistrifluoromethylvinyl group.
[0067] [Invention 13]
[0068] A fluorinated copolymer comprising a repeating unit represented by the following formula (A) and a repeating unit represented by the following formula (C).
[0069] [Chemical formula 4]
[0070]
[0071] In the formula, R 1 , R 3 Each independently represents a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group are optionally substituted by fluorine atoms. Q represents a fluoroalkyl group having 1 to 20 carbon atoms, which optionally has a hydrogen atom, an oxygen atom or a nitrogen atom. X represents a single bond or a divalent group. Z represents an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups are optionally substituted by fluorine atoms, oxygen atoms or nitrogen atoms. O represents an oxygen atom.
[0072] [Invention 14]
[0073] The fluorinated copolymer according to Invention 13, wherein Q in the repeating unit represented by formula (A) is a fluoroalkyl group having 3 to 10 carbon atoms, X is a carbonyl group, and Z in the repeating unit represented by formula (C) is a bistrifluoromethylvinyl group.
[0074] [Invention 15]
[0075] A fluorinated copolymer comprising a repeating unit represented by the following formula (A), a repeating unit represented by the following formula (B), and a repeating unit represented by the following formula (C).
[0076] [Chemical formula 5]
[0077]
[0078] In the formula, R 1 , R 2 , R 3 Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group are optionally substituted by fluorine atoms. Q is a fluoroalkyl group having 1 to 20 carbon atoms, which optionally has a hydrogen atom, an oxygen atom or a nitrogen atom. X and Y are each independently a single bond or a divalent group. Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups are optionally substituted by fluorine atoms, oxygen atoms or nitrogen atoms. O is an oxygen atom and H is a hydrogen atom.
[0079] [Invention 16]
[0080] The fluorinated copolymer according to Invention 15, wherein Q in the repeating unit represented by formula (A) is hexafluoroisopropyl and X is carbonyl; Y in the repeating unit represented by formula (B) is carboxyethylene; R in the repeating unit represented by formula (C) is 3 is a hydrogen atom or a methyl group, and Z is an alkylcarbonyloxy group having 1 to 4 carbon atoms.
[0081] [Invention 17]
[0082] The fluorinated copolymer according to Invention 15, wherein Q in the repeating unit represented by formula (A) is a fluoroalkyl group having 3 to 10 carbon atoms, and X is a carbonyl group; Y in the repeating unit represented by formula (B) is a p-phenylene group, a p-phenylenecarbonyl group or a p-phenylenehexafluoroisopropylidene group; R in the repeating unit represented by formula (C) is 3 is a hydrogen atom or a methyl group, and Z is a bistrifluoromethylvinyl group.
[0083] (III) Beneficial effects
[0084] As long as the manufacturing method of the patterned film substrate of the present application is used, the lyophilicity of the substrate surface serving as the concave portion of the pattern film can be maintained at all times, while the pattern film can be made sufficiently lyophobic. Even after the surface of the pattern film is subjected to UV ozone cleaning or oxygen plasma cleaning, the lyophobicity of the pattern film can be restored by heating the pattern film. DETAILED DESCRIPTION
[0085] The present invention is not limited to the following embodiments. It should be understood that appropriate changes and improvements to the following embodiments based on the general knowledge of those skilled in the art without departing from the scope of the present application fall within the scope of the present invention.
[0086] 1. Heat treatment after UV ozone cleaning or oxygen plasma cleaning
[0087] The method for manufacturing a patterned film substrate in the present application comprises: a cleaning step of performing UV ozone cleaning or oxygen plasma cleaning on the patterned film substrate to obtain a first patterned film substrate; and a heating step of heating the first patterned film substrate to obtain a second patterned film substrate.
[0088] The heating temperature in the heating step is preferably 50° C. to 350° C., more preferably 100° C. to 300° C., and even more preferably 150° C. to 250° C. If the heating temperature is lower than 50° C., it is difficult to obtain the following effect: the liquid repellency of the patterned film substrate that has decreased after UV ozone cleaning or oxygen plasma cleaning is restored to the same level as before UV ozone cleaning or oxygen plasma cleaning.
[0089] The upper limit of the heating time is not particularly limited, but it is preferably adjusted according to the heat resistance of the photoresist used in the pattern formation of the patterned film substrate. Although the upper limit is not particularly limited, it is substantially less than 1 hour. About the lower limit, it is preferably more than 10 seconds, more preferably more than 30 seconds. If the heating time is less than 10 seconds, it is difficult to obtain the following effect: the lyophobicity of the patterned film substrate that has decreased after UV ozone cleaning or oxygen plasma cleaning is restored to the same degree as before UV ozone cleaning or oxygen plasma cleaning.
[0090] As the heating method, a commonly used heating device can be used, for example, a hot plate or an oven.
[0091] The heating environment may be in nitrogen or under reduced pressure, but is preferably in atmospheric air (at normal pressure (101.325 kPa) because a commercially available heating device can be used.
[0092] According to the manufacturing method of the patterned film substrate of the present application, by heating the patterned film substrate with a patterned film formed on the substrate after UV ozone cleaning or oxygen plasma cleaning, when ink droplets are dripped into the concave part of the patterned film of the patterned film substrate by inkjet method, problems such as the ink crossing over the dam or the dam dissolving into the ink can be suppressed, and the patterned film includes a fluorinated copolymer having specific repeating units.
[0093] 2. Fluorinated copolymers
[0094] In the method for manufacturing a patterned film substrate of the present application, the patterned film substrate is obtained by forming a patterned film having a pattern on a substrate. The patterned film contains a fluorinated copolymer. The fluorinated copolymer contains both a repeating unit represented by formula (A) and a repeating unit represented by formula (C).
[0095] [Fluorinated copolymer containing both a repeating unit represented by the formula (A) and a repeating unit represented by the formula (C)]
[0096] In the method for producing a patterned film substrate of the present application, the fluorinated copolymer contains both a repeating unit represented by the following formula (A) (hereinafter sometimes referred to as repeating unit (A)) and a repeating unit represented by the following formula (C) (hereinafter sometimes referred to as repeating unit (C)).
[0097] [Chemical formula 6]
[0098]
[0099] In the formula, R 1 , R 3 Each independently represents a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group are optionally substituted by fluorine atoms. Q represents a fluoroalkyl group having 1 to 20 carbon atoms, which optionally has a hydrogen atom, an oxygen atom or a nitrogen atom. X represents a single bond or a divalent group. Z represents an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups are optionally substituted by fluorine atoms, oxygen atoms or nitrogen atoms. O represents an oxygen atom.
[0100] Preferably, Q in the repeating unit represented by formula (A) is a fluoroalkyl group having 3 to 10 carbon atoms, X is (-C(=O)-), and Z in the repeating unit represented by formula (C) is a trifluoromethylvinyl group (-CH=C(CF 3 ) 2 ).
[0101] The following combinations of repeating units (A) and repeating units (C) are preferred.
[0102] [Chemical formula 7]
[0103]
[0104] [Chemical formula 8]
[0105]
[0106] <Content ratio of repeating unit>
[0107] The content of the repeating unit (A) based on the total amount of the repeating units (A) and (C) contained in the fluorinated copolymer is preferably 5% to 80%, more preferably 10% to 60%, in mol%.
[0108] The content of the repeating unit (C) based on the total amount of the repeating units (A) and (C) contained in the fluorinated copolymer is preferably 3% to 90%, more preferably 5% to 80%, in mol%.
[0109] In order to improve the solubility in organic solvents, the adhesion or hardness with the substrate during film formation, the above-mentioned fluorinated copolymer may also contain repeating units other than repeating units (A) and (C) as required. In terms of mol%, the content of repeating units other than repeating units (A) and (C) is preferably 50% or less, more preferably 30% or less relative to the total amount of repeating units (A) and (C). If it is greater than 50%, there is a tendency to be difficult to obtain liquid repellency.
[0110] [A fluorinated copolymer containing a repeating unit represented by the following formula (A), a repeating unit represented by the following formula (B), and a repeating unit represented by the following formula (C)]
[0111] In the method for producing a patterned film substrate of the present application, the fluorinated copolymer preferably contains a repeating unit represented by the following formula (A), a repeating unit represented by the formula (B) (hereinafter sometimes referred to as repeating unit (B)), and a repeating unit represented by the formula (C).
[0112] [Chemical formula 9]
[0113]
[0114] In the formula, R 1 , R 2 , R 3Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group are optionally substituted by fluorine atoms. Q is a fluoroalkyl group having 1 to 20 carbon atoms, which optionally has a hydrogen atom, an oxygen atom or a nitrogen atom. X and Y are each independently a single bond or a divalent group. Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups are optionally substituted by fluorine atoms, oxygen atoms or nitrogen atoms. O is an oxygen atom and H is a hydrogen atom.
[0115] In the above fluorinated copolymer, it is preferred that: Q in the repeating unit represented by the formula (A) is hexafluoroisopropyl (—CH(CF 3 ) 2 ), X is a carbonyl group (-C(=O)-), and Y in the repeating unit represented by the formula (B) is a carboxyethylene group (-C(=O)-O-CH 2 CH 2 -), the repeating unit represented by the formula (C) has R 3 is a hydrogen atom or a methyl group, and Z is an alkylcarbonyloxy group having 1 to 4 carbon atoms.
[0116] The following combinations of repeating unit (A), repeating unit (B) and repeating unit (C) are preferred.
[0117] [Chemical formula 10]
[0118]
[0119] In the above fluorinated copolymer, Q in the repeating unit represented by the formula (A) is a fluoroalkyl group having 3 to 10 carbon atoms, X is a carbonyl group (-C(=O)-), and Y in the repeating unit represented by the formula (B) is a p-phenylene group (-C 6 H 4 -), p-phenylenecarbonyl (-C 6 H 4 -C(=O)-) or p-phenylene hexafluoroisopropylidene (-C 6 H 4 -C(CF 3 ) 2 -), the repeating unit represented by the formula (C) has R 3 is a hydrogen atom or a methyl group, Z is a bistrifluoromethylvinyl group (-CH=C(CF 3 ) 2 ).
[0120] The following combinations of repeating unit (A), repeating unit (B) and repeating unit (C) are preferred.
[0121] [Chemical formula 11]
[0122]
[0123] [Chemical formula 12]
[0124]
[0125] [Chemical formula 13]
[0126]
[0127] [Chemical formula 14]
[0128]
[0129] <Content ratio of repeating unit>
[0130] The content of the repeating unit (A) based on the total amount of the repeating units (A), (B) and (C) contained in the fluorinated copolymer is preferably 5% to 80%, more preferably 10% to 60%, in mol%.
[0131] The content of the repeating unit (B) based on the total amount of the repeating units (A), (B) and (C) contained in the fluorinated copolymer is preferably 10% to 85%, more preferably 20% to 70%, in mol%.
[0132] The content of the repeating unit (C) based on the total amount of the repeating units (A), (B) and (C) contained in the fluorinated copolymer is preferably 3% to 90%, more preferably 5% to 80%, in mol%.
[0133] In order to improve the solubility in organic solvents, the adhesion to the substrate during film formation or the hardness, the fluorinated copolymer may contain repeating units other than repeating units (A), (B) and (C) as needed. The content of repeating units other than repeating units (A), (B) and (C) is preferably 50% or less, more preferably 30% or less relative to the total amount of repeating units (A), (B) and (C). If it is greater than 50%, it is difficult to obtain liquid repellency.
[0134] [Molecular weight of fluorinated copolymer]
[0135] In the method for manufacturing a patterned film substrate of the present application, the number average molecular weight Mn of the fluorinated copolymer contained in the patterned film is preferably 1,000 or more and 100,000 or less, more preferably 3,000 or more and 60,000 or less. In addition, the molecular weight distribution Mw / Mn defined by the ratio of the number average molecular weight Mn to the weight average molecular weight Mw is preferably 1 or more and 4 or less, more preferably 1 or more and 2.5 or less.
[0136] If the number average molecular weight Mn is 1,000 or more, the hardness of the pattern film containing the fluorinated copolymer is appropriate, and it is also easy to form a film of the desired thickness, so it is preferred. In addition, it is also preferred from the perspective of easy formation of a fine pattern consisting of a lyophobic portion and a lyophilic portion, and pattern durability. If the number average molecular weight Mn is 100,000 or less, when preparing a pattern-forming composition containing a fluorinated copolymer on a substrate, the fluorinated copolymer is easy to dissolve in a solvent, easy to apply, and is not easy to crack after film formation, so it is preferred.
[0137] The number average molecular weight Mn and weight average molecular weight Mw of the polymer are measured by using a high-speed gel permeation chromatograph (hereinafter sometimes referred to as GPC; manufactured by TOSOH CORPORATION, model HLC-8320GPC), connecting an ALPHA-M column and an ALPHA-2500 column (both manufactured by TOSOH CORPORATION) in series, and using tetrahydrofuran (THF) as a developing solvent. A detector for measuring a refractive index difference can be used as a detector.
[0138] 3. Repeating Unit
[0139] Hereinafter, the repeating unit (A), the repeating unit (B) and the repeating unit (C) contained in the fluorinated copolymer will be described.
[0140] [Repeating unit (A)]
[0141] [Chemical formula 15]
[0142]
[0143] In the formula, R 1 is a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, wherein a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted by fluorine atoms. Q is a fluoroalkyl group having 1 to 20 carbon atoms, which may have a hydrogen atom, an oxygen atom or a nitrogen atom. X is a single bond or a divalent group. O is an oxygen atom.
[0144] R 1 Examples include a hydrogen atom, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a fluorine atom, a trifluoromethyl group, a trifluoroethyl group, a trifluoropropyl group, a 1,1,1,3,3,3-hexafluoroisopropyl group (-C(CF3 ) 2 H) or heptafluoroisopropyl. Particularly preferred are hydrogen atom, fluorine atom or methyl group.
[0145] Q is preferably a fluoroalkyl group having 3 to 10 carbon atoms, and examples thereof include trifluoromethyl, trifluoroethyl, trifluoropropyl, 1,1,1,3,3,3-hexafluoroisopropyl (-C(CF 3 ) 2 H), heptafluoroisopropyl, pentafluoropropyl, perfluorobutylethyl, perfluorohexylethyl, perfluorooctylethyl, 1,2,2,3,3,4,4,5-octafluorocyclopentylmethyl, perfluorocyclopentyl, perfluorocyclohexyl or perfluoroadamantyl. Perfluorohexylethyl or hexafluoroisopropyl is particularly preferred.
[0146] X is a single bond or a divalent group, and the hydrogen atoms contained in the divalent group are optionally substituted by fluorine atoms. The divalent group is preferably a divalent group having 2 to 10 carbon atoms, and a methylene group, an alkylene group having 2 to 10 carbon atoms, an alkenylene group having 2 to 10 carbon atoms, a divalent aromatic group having 6 to 10 carbon atoms, or a divalent alicyclic hydrocarbon group having 4 to 10 carbon atoms can be listed. An ether bond (-O-), a carbonyl group (-C(=O)-), a carboxyl group (-C(=O)-O-) or an oxycarbonyl group (-OC(=O)-) can also be contained inside the alkylene or alkenylene group. If the aliphatic chain in the divalent group is a long chain, the liquid repellency decreases, so a single bond, a carbonyl group (-C(=O)-), an oxyethylene group (-O-CH 2 -CH 2 -), carboxyethylene (-C(=O)-O-CH 2 -CH 2 -), carboxyphenylene (-C(=O)-OC 6 H 4 -), phenylene (-C 6 H 4 -) or phenylene hexafluoroisopropylidene (-C 6 H 4 -C(CF 3 ) 2 -) A carbonyl group is particularly preferred.
[0147] Furthermore, as the repeating unit (A), a structure represented by formula (A-1) is also preferably mentioned.
[0148] [Chemical formula 16]
[0149]
[0150] In formula (A-1), R 4 , R 5Each independently represents a hydrogen atom, a fluorine atom or an alkyl group having 1 to 3 carbon atoms, wherein a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted with fluorine atoms. O represents an oxygen atom, H represents a hydrogen atom, and F represents a fluorine atom.
[0151] [Repeating unit (B)]
[0152] [Chemical formula 17]
[0153]
[0154] In the formula, R 2 is a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, wherein a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted with fluorine atoms. Y is a single bond or a divalent group. O is an oxygen atom, and H is a hydrogen atom.
[0155] R 2 Preferred examples include a hydrogen atom, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a fluorine atom, a trifluoromethyl group, a trifluoroethyl group, a trifluoropropyl group, a 1,1,1,3,3,3-hexafluoroisopropyl group (-C(CF 3 ) 2 H) or heptafluoroisopropyl. Particularly preferred are hydrogen atom, fluorine atom or methyl group.
[0156] Y is a single bond or a divalent group, and the divalent group is preferably a divalent group having 2 to 10 carbon atoms, and examples thereof include a methylene group, an alkylene group having 2 to 10 carbon atoms, an alkenylene group having 2 to 10 carbon atoms, an arylene group having 6 to 10 carbon atoms, or a divalent alicyclic hydrocarbon group having 4 to 10 carbon atoms. An ether bond (-O-), a carbonyl group (-C(=O)-), a carboxyl group (-C(=O)-O-), or an oxycarbonyl group (-OC(=O)-) may be contained inside the alkylene group or the alkenylene group. If the aliphatic chain in the divalent group is long, the liquid repellency decreases, and therefore, a single bond, a carbonyl group (-C(=O)-), an oxyethylene group (-O-CH 2 -CH 2 -), carboxyethylene (-C(=O)-O-CH 2 -CH 2 -), carboxyphenylene (-C(=O)-OC 6 H 4 -), phenylene (-C 6 H 4 -) or phenylene hexafluoroisopropylidene (-C 6 H 4 -C(CF 3 ) 2 -) Particularly preferred is p-phenylene or carboxyethylene.
[0157] [Repeating unit (C)]
[0158] [Chemical formula 18]
[0159]
[0160] In the formula, R 3 is a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group may be substituted with fluorine atoms. Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms in these groups may be substituted with fluorine atoms, oxygen atoms or nitrogen atoms.
[0161] R 3 Preferred examples include a hydrogen atom, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a fluorine atom, a trifluoromethyl group, a trifluoroethyl group, a trifluoropropyl group, a 1,1,1,3,3,3-hexafluoroisopropyl group (-C(CF 3 ) 2 H) or heptafluoroisopropyl. Particularly preferred are hydrogen atom, fluorine atom or methyl group.
[0162] Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms, or a carboxyl group, and the hydrogen atoms in these groups are optionally substituted with fluorine atoms, oxygen atoms, or nitrogen atoms. Z is particularly preferably bistrifluoromethylvinyl (-CH=C(CF 3 ) 2 ).
[0163] 4. Synthesis of fluorinated copolymers
[0164] 4-1. Monomer
[0165] The following lists the monomer (A1) that provides the repeating unit (A), the monomer (B1) that provides the repeating unit (B), and the monomer (C1) that provides the repeating unit (C).
[0166] The fluorinated copolymer containing both repeating units (A) and (C) can be obtained by copolymerizing the monomer (A1) and the monomer (C1). The fluorinated copolymer containing both repeating units (A), (B) and (C) can be obtained by copolymerizing the monomer (A1), the monomer (B1) and the monomer (C1).
[0167] [Monomer (A1)]
[0168] [Chemical formula 19]
[0169]
[0170] R 1 , X, Q and R shown in formula (A) 1 , X, and Q are the same.
[0171] [Monomer (B1)]
[0172] [Chemical formula 20]
[0173]
[0174] R 2 , Y and R shown in formula (B) 2 , Y are the same.
[0175] Examples of the monomer (B1) include the following monomers. 2 Particularly preferred is a hydrogen atom, a fluorine atom or a methyl group.
[0176] [Chemical formula 21]
[0177]
[0178] [Monomer (C1)]
[0179] [Chemical formula 22]
[0180]
[0181] R 3 , Z and R shown in formula (C) 3 , Z are the same.
[0182] 4-2. Synthesis method of fluorinated copolymer
[0183] In the synthesis method of the fluorinated copolymer, the above-mentioned monomers (A1), (B1), and (C1) are used as raw materials. The synthesis method can be selected from common polymerization methods. Free radical polymerization and ionic polymerization are preferred, and coordinated anionic polymerization, living anionic polymerization, and cationic polymerization can be selected according to the situation. In addition, a polymerization solvent can be used in the polymerization. The free radical polymerization is described below.
[0184] The radical polymerization can be carried out in the presence of a radical polymerization initiator or a radical polymerization initiation source by a known polymerization method such as bulk polymerization, solution polymerization, suspension polymerization or emulsion polymerization, in a batchwise, semi-continuous or continuous manner.
[0185] <Radical Polymerization Initiator>
[0186] As the free radical polymerization initiator, for example, azo compounds, peroxide compounds or redox compounds can be listed. As the azo compound, azobisisobutyronitrile can be exemplified. As the peroxide compound, tert-butyl peroxypivalate, di-tert-butyl peroxide, isobutyryl peroxide, didodecanol peroxide, peroxidated succinic acid, dicinnamyl peroxide, di-n-propyl peroxydicarbonate, allyl tert-butyl peroxycarbonate, benzoyl peroxide, hydrogen peroxide or ammonium persulfate can be exemplified. As the redox compound, a compound composed of an oxidant and a reductant can be used, such as a compound (Fenton's reagent) composed of a combination of a divalent iron ion and a hydrogen peroxide solution.
[0187] <Polymerization Solvent>
[0188] As the polymerization solvent, a solvent that does not inhibit free radical polymerization is preferred, and examples thereof include ester solvents, ketone solvents, hydrocarbon solvents, and alcohol solvents. In addition, water, ethers, cyclic ethers, freons, or aromatic solvents may also be used.
[0189] Examples of the polymerization solvent include ethyl acetate or n-butyl acetate as an ester solvent, acetone or methyl isobutyl ketone as a ketone solvent, toluene or cyclohexane as a hydrocarbon solvent, and methanol, isopropanol or ethylene glycol monomethyl ether as an alcohol solvent.
[0190] These polymerization solvents may be used alone or in combination of two or more. In addition, a molecular weight modifier such as mercaptan may be used simultaneously.
[0191] <Aggregation conditions>
[0192] The polymerization temperature may be appropriately selected according to the type of the free radical polymerization initiator or the free radical polymerization initiation source. Preferably, the type of the free radical polymerization initiator or the free radical polymerization initiation source is appropriately selected so that the polymerization temperature is, for example, 20° C. to 200° C., preferably 30° C. to 140° C. The molecular weight of the fluorinated copolymer can be controlled by selecting the free radical polymerization initiator or the free radical polymerization initiation source and adjusting the polymerization conditions.
[0193] As a method for removing the polymerization solvent such as an organic solvent or water from the solution or dispersion containing the polymerized fluorinated copolymer, a known method may be used, and examples thereof include reprecipitation, filtration, and distillation under reduced pressure.
[0194] When a fluorinated copolymer is used as a resist component, the developer solubility of the fluorinated copolymer varies depending on the molecular weight of the fluorinated copolymer, and the patterning conditions in lithography may change. If the molecular weight of the fluorinated copolymer is high, there is a tendency for the dissolution rate in the developer to decrease, and if the molecular weight is low, there is a tendency for the dissolution rate to increase. The molecular weight of the fluorinated copolymer can be controlled by adjusting the polymerization conditions.
[0195] 5. Resist pattern forming composition
[0196] By adding a photosensitizer or an acid generator, a basic compound and a solvent to the fluorinated copolymer, a composition for forming an etching resist pattern can be obtained. After the obtained composition for forming an etching resist pattern is applied to a substrate, patterning is performed by photolithography, thereby obtaining a patterned film substrate used in the method for manufacturing a patterned film substrate of the present application. Hereinafter, the composition for forming an etching resist pattern is sometimes referred to as a resist.
[0197] The above-mentioned resist can be prepared by using (a) a fluorinated copolymer as its essential component and adding (b) an alkali-soluble resin, (c) a naphthoquinone diazide group-containing compound, (d) a solvent, (e) a photoacid generator, (f) a basic compound or (g) a crosslinking agent as needed.
[0198] 5-1. (b) Alkali-soluble resin
[0199] (b) The alkali-soluble resin includes, for example, an alkali-soluble novolac resin. The alkali-soluble novolac resin can be obtained by condensing phenols and aldehydes in the presence of an acid catalyst.
[0200] <Phenols>
[0201] Examples of phenols include phenol, o-cresol, m-cresol, p-cresol, 2,3-dimethylphenol, 2,4-dimethylphenol, 2,5-dimethylphenol, 3,4-dimethylphenol, 3,5-dimethylphenol, 2,3,5-trimethylphenol, 3,4,5-trimethylphenol, resorcinol, 2-methylresorcinol, 4-ethylresorcinol, hydroquinone, methylhydroquinone, catechol, 4-methylcatechol, pyrogallol, phloroglucinol, thymol, and isothymol. These phenols may be used alone or in combination of two or more.
[0202] <Aldehydes>
[0203] Examples of the aldehydes include formaldehyde, trioxymethylene, paraformaldehyde, benzaldehyde, acetaldehyde, propionaldehyde, phenylacetaldehyde, α-phenylpropionaldehyde, β-phenylpropionaldehyde, o-hydroxybenzaldehyde, m-hydroxybenzaldehyde, p-hydroxybenzaldehyde, o-tolualdehyde, m-tolualdehyde, p-tolualdehyde, nitrobenzaldehyde, furfural, glyoxal, glutaraldehyde, terephthalaldehyde, or isophthalaldehyde.
[0204] <Acid Catalyst>
[0205] Examples of the acid catalyst include hydrochloric acid, nitric acid, sulfuric acid, phosphoric acid, phosphorous acid, formic acid, oxalic acid, acetic acid, methanesulfonic acid, diethyl sulfate, and p-toluenesulfonic acid. These acid catalysts may be used alone or in combination of two or more.
[0206] The mass average molecular weight of the (b) alkali-soluble resin component is preferably 1,000 to 50,000 from the viewpoint of developability and resolution of the positive resist composition.
[0207] 5-2. (c) Naphthoquinone diazide compounds
[0208] (c) The naphthoquinonediazide group-containing compound is not particularly limited, and compounds that can be used as a photosensitive component of an i-line resist composition can be used, for example, naphthoquinone-1,2-diazide sulfonate compounds, o-benzoquinonediazide sulfonate, o-anthraquinonediazide sulfonate, and esters of naphthoquinone-1,2-diazide sulfonyl halides and hydroxyl compounds. Examples of the naphthoquinone-1,2-diazide sulfonyl halides include naphthoquinone-1,2-diazide-5-sulfonyl chloride, naphthoquinone-1,2-diazide-4-sulfonyl chloride, and naphthoquinone-1,2-diazide-6-sulfonyl chloride.
[0209] As the naphthoquinonediazide group-containing compound (c), naphthoquinonediazide-4-sulfonate, naphthoquinonediazide-5-sulfonate or naphthoquinonediazide-6-sulfonate is preferred because of its excellent solubility. These compounds may be used alone or in combination of two or more.
[0210] The amount of the naphthoquinonediazide-containing compound (c) added is preferably 10% by mass or more and 60% by mass or less, and more preferably 20% by mass or more and 50% by mass or less, relative to the total mass of the (b) alkali-soluble resin and the (c) naphthoquinonediazide-containing compound. If the amount exceeds 60% by mass, the sensitivity as a resist cannot be obtained, and if the amount is less than 10% by mass, it is difficult to obtain a fine pattern due to the reduction of the film in the unexposed portion after photolithography.
[0211] 5-3. (d) Solvent
[0212] The (d) solvent contained in the resist may be selected from known resist solvents as long as it can dissolve the (a) fluorinated copolymer, (b) alkali-soluble resin and (c) naphthoquinonediazide-containing compound to form a uniform solution. Two or more solvents may be mixed and used.
[0213] Examples of such solvents include ketones, alcohols, polyols, esters, aromatic solvents, ethers, fluorinated solvents, and turpentine-based naphtha solvents or paraffin solvents as high-boiling-point solvents for the purpose of improving coating properties.
[0214] Examples of ketones include acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl isobutyl ketone, methyl isoamyl ketone, and 2-heptanone. Examples of alcohols include isopropanol, butanol, isobutanol, n-pentanol, isopentanol, tert-pentanol, 4-methyl-2-pentanol, 3-methyl-3-pentanol, 2,3-dimethyl-2-pentanol, n-hexanol, n-heptanol, 2-heptanol, n-octanol, n-decanol, sec-pentanol, tert-pentanol, isopentanol, 2-ethyl-1-butanol, lauryl alcohol, hexyldecanol, and oleyl alcohol. As polyols, ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, ethylene glycol monoacetate, ethylene glycol dimethyl ether (EDC), diethylene glycol monoacetate, propylene glycol monoacetate, dipropylene glycol monoacetate, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate (PGMEA) or propylene glycol monomethyl ether (PGME) and derivatives of these polyols can be illustrated. As esters, methyl lactate, ethyl lactate (EL), methyl acetate, ethyl acetate, butyl acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate or ethyl ethoxypropionate or γ-butyrolactone (GBL) can be illustrated. As aromatic solvents, toluene or xylene can be illustrated. As ethers, diethyl ether, dioxane, anisole or diisopropyl ether can be illustrated. As fluorine-based solvents, hexafluoroisopropanol can be illustrated.
[0215] Preferred are ethylene glycol dimethyl ether (EDC), propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), cyclohexanone, ethyl lactate (EL) or γ-butyrolactone (GBL).
[0216] The amount of the solvent (d) contained in the resist is preferably 1% by mass or more and 25% by mass or less, and more preferably 5% by mass or more and 15% by mass or less. The thickness of the formed resin film can be adjusted by adjusting the solid content concentration of the resist.
[0217] 5-4. (e) Photoacid generator
[0218] (e) The photoacid generator can be arbitrarily selected from compounds used as acid generators for chemically amplified resists and can be used, and examples thereof include sulfonates and sulfonate esters.
[0219] Examples of the sulfonates include iodonium sulfonate, sulfonium sulfonate, N-imide sulfonate, N-oxime sulfonate, o-nitrobenzyl sulfonate, trimesylate of pyrogallol, triphenylsulfonium trifluoromethane sulfonate, and triphenylsulfonium perfluoro-n-butane sulfonate.
[0220] These photoacid generators generate alkylsulfonic acid, aromatic sulfonic acid, or partially or fully fluorinated aromatic sulfonic acid or alkylsulfonic acid by exposure in photolithography. The photoacid generator that generates fully fluorinated alkylsulfonic acid is preferably triphenylsulfonium trifluoromethanesulfonate or triphenylsulfonium perfluorobutanesulfonate.
[0221] 5-5. (f) Basic compounds
[0222] The (f) basic compound plays a role in slowing down the diffusion rate of the acid generated by the (e) photoacid generator when diffusing in the resist film. The addition of the (f) basic compound can be expected to bring about the following effects: the shape of the resist pattern is improved by adjusting the acid diffusion distance; even if the exposure delay time after the formation of the resist film is long, the stability of forming the resist pattern with the required precision is improved.
[0223] Examples of such basic compounds include aliphatic amines, aromatic amines, heterocyclic amines, and aliphatic polycyclic amines, preferably aliphatic secondary amines, aliphatic tertiary amines, or alkanolamines. Examples of such amines include trimethylamine, triethylamine, tripropylamine, tributylamine, tripentylamine, trihexylamine, triheptylamine, trioctylamine, trinonylamine, tridecylamine, tridodecylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, dipentylamine, dihexylamine, diheptylamine, dioctylamine, dinonylamine, didecylamine, didocylamine, dicyclohexylamine, methylamine, ethylamine, propylamine, butylamine, amylamine, hexylamine, heptylamine, octylamine, nonylamine, decylamine, dodecylamine, diethanolamine, triethanolamine, diisopropanolamine, triisopropanolamine, dioctanolamine, trioctanolamine, aniline, pyridine, picoline, lutidine, bipyridine, pyrrole, piperidine, piperazine, indole, or hexamethylenetetramine. These basic compounds may be used alone or in combination of two or more.
[0224] The amount of the basic compound (f) in the resist is preferably 0.001 to 2 parts by mass, more preferably 0.01 to 1 part by mass, relative to 100 parts by mass of the fluorinated copolymer (a). If the amount of the basic compound (f) is less than 0.001 parts by mass, the effect as an additive cannot be fully obtained, and if it is greater than 2 parts by mass, there is a concern that the resolution or sensitivity may decrease.
[0225] 5-6. (g) Cross-linking agent
[0226] (g) A crosslinking agent may be added to the above-mentioned resist as needed. As the (g) crosslinking agent, a known crosslinking agent may be used. As such a crosslinking agent, for example, 2,4,6-tris[bis(methoxymethyl)amino]-1,3,5-triazine (hydroxymethyl melamine curing agent) and its derivatives, 1,3,4,6-tetrakis(methoxymethyl) glycoluril (glycoluril curing agent) and its derivatives, polyfunctional epoxides, polyfunctional oxetane compounds or polyfunctional isocyanate compounds may be cited. A variety of these crosslinking agents may be used.
[0227] 6. Pattern formation
[0228] The formation of a pattern in the method for manufacturing a patterned film substrate of the present application is described. The formation of the pattern includes: a film forming step of coating the resist on the substrate to form a film; an exposure step of irradiating an electromagnetic wave or an electron beam with a wavelength of 600 nm or less through a photomask to transfer the pattern of the photomask to the film; and a developing step of developing the film with a developer to obtain a pattern.
[0229] A pattern can be formed by using a resist containing a fluorinated copolymer and undergoing the following steps: (a) a film-forming step of coating a substrate with the resist to form a resist film; (b) an exposure step of heating the resist film and then irradiating the resist film with an electromagnetic wave or electron beam having a wavelength of less than 600 nm through a photomask on which the pattern has been processed; and (c) a development step of developing the exposed resist film with an alkaline developer or an organic solvent to obtain a resist pattern having the pattern of the photomask transferred onto the substrate.
[0230] Hereinafter, each step will be described with reference to examples.
[0231] 6-1. (a) Film-forming process
[0232] In the film forming step (a), the anti-etching agent containing the fluorinated copolymer is applied onto a silicon wafer or the like as a substrate by spin coating, and the silicon wafer is heated on a heating plate, for example, at a temperature of not less than 60° C. and not more than 200° C. for not less than 10 seconds and not more than 10 minutes, preferably at a temperature of not less than 80° C. and not more than 150° C. for not less than 30 seconds and not more than 2 minutes, to form an anti-etching film on the substrate.
[0233] As the substrate, for example, a silicon wafer, a metal substrate or a glass substrate can be used. In addition, an organic or inorganic film can be provided on the substrate. For example, an anti-reflection film or a lower layer of a multilayer resist can be provided, and a pattern can also be formed thereon.
[0234] 6-2. (b) Exposure process
[0235] In the exposure step (b), a photomask is mounted on an exposure device so that the exposure dose is, for example, 1 mJ / cm 2 Above, 200mJ / cm 2 Below, preferably 10 mJ / cm 2 Above, 100mJ / cm 2 In the following manner, after irradiating the anti-etching film with an electromagnetic wave or electron beam with a wavelength of less than 600nm through a photomask, it is heated on a heating plate, for example, at a temperature of more than 60°C and less than 150°C for more than 10 seconds and less than 5 minutes, preferably at a temperature of more than 80°C and less than 130°C for more than 30 seconds and less than 3 minutes, to transfer the pattern of the photomask to the anti-etching film.
[0236] The wavelength of the electromagnetic wave is preferably 100 to 600 nm, more preferably 300 to 500 nm. It is particularly preferred to include light of i-line (365 nm), h-line (405 nm) or g-line (436 nm). In addition, light below 330 nm may be cut off as required.
[0237] Examples of the light source include KrF excimer laser (wavelength: 248 nm), ArF excimer laser (wavelength: 193 nm), and F2 excimer laser (wavelength: 157 nm).
[0238] 6-3. (c) Development process
[0239] In the (c) development process, as a developer, a concentration of tetramethylammonium hydroxide (TMAH) is used, for example, an aqueous solution of 0.1 mass % or more and 5 mass % or less, preferably an aqueous solution of 2 mass % or more and 3 mass % or less, or an organic solvent is used to dissolve any one of the exposed part or unexposed part of the resist film in the (b) exposure process to form a pattern, and obtain a pattern film on the substrate. As an organic solvent, propylene glycol monomethyl ether acetate (PGMEA), butyl acetate, etc. can be exemplified. In the development process, a known method such as an immersion method, a puddling method, and a spray method can be used to make the developer contact the resist film for more than 10 seconds and less than 3 minutes, preferably more than 30 seconds and less than 2 minutes, thereby obtaining a patterned film substrate with a target pattern.
[0240] Example
[0241] The manufacturing method of the patterned film substrate and the fluorine-containing copolymer of the present application will be described in detail through the following examples. However, the present invention is not limited to the following examples.
[0242] 1. Synthesis of monomers
[0243] Synthesize fluorine-containing monomers for obtaining fluorine-containing copolymers.
[0244] 1-1. Synthesis of MA-CH2-OFCP
[0245] [Synthesis of 1,2,2,3,3,4,4,5-octafluorocyclopentylmethanol]
[0246] Under a nitrogen atmosphere, at room temperature (20 °C, the same below), add 31.5 ml (0.75 mol) of methanol, 1.11 g (0.0045 mol) of benzoyl peroxide (BPO), and 31.2 g (0.12 mol) of octafluorocyclopentene (manufactured by Central Glass Co., Ltd.) to a 300 ml stainless steel pressure-resistant container. Seal the container, heat it to 120 °C, and stir for 24 hours to carry out the following reaction. After cooling the container, perform atmospheric distillation on the content to obtain 28.8 g of 1,2,2,3,3,4,4,5-octafluorocyclopentylmethanol, with a yield of 80%.
[0247] [Chemical formula 23]
[0248]
[0249] The results of nuclear magnetic resonance analysis (NMR) are as follows.
[0250] [NMR analysis results]
[0251] 1 H-NMR(CDCl 3 , TMS internal standard)
[0252] δ(ppm): 4.21 - 4.05(2H, m), 5.22(1H, m)
[0253] [Synthesis of MA-CH2-OFCP]
[0254] Weigh 24.3 g (0.1 mol) of 1,2,2,3,3,4,4,5-octafluorocyclopentylmethanol obtained from the above synthesis, 15.1 g (0.15 mol) of triethylamine, and methoxyphenol (1000 ppm) as a polymerization inhibitor into a 300 ml glass flask equipped with a stirrer. While maintaining the temperature at 30 °C, add dropwise 16.9 g (0.11 mol) of methacrylic anhydride to the reaction system and stir for 2 hours. After the stirring is completed, add 40 ml of diisopropyl ether and 30 ml of pure water, and perform liquid separation. Then, add 20 ml of 1 mass% aqueous sodium hydroxide solution, stir for 1 hour, transfer to a separatory funnel, and obtain the organic layer. After washing the organic layer twice with 30 ml of pure water, perform vacuum distillation at a pressure of 1.0 kPa and a temperature of 70 - 72 °C to obtain 26.5 g of MA-CH2-OFCP shown below, with a yield of 85%.
[0255] [Chemical formula 24]
[0256]
[0257] <NMR analysis results>
[0258] 1 H-NMR (solvent: deuterated chloroform, internal standard: TMS); δ (ppm): 1.92 (3H, s), 4.21 - 4.05 (2H, m), 5.22 (1H, m), 5.65 (1H, q), 6.12 (1H, q)
[0259] 1-2. Synthesis of 1,1-bis(trifluoromethyl)butadiene (BTFBE)
[0260] Heat 400 g of concentrated sulfuric acid in a 1000 ml glass flask equipped with a stirrer to 100 °C, and slowly add dropwise 300 g of 1,1,1-trifluoro-2-trifluoromethyl-4-penten-2-ol to the concentrated sulfuric acid over 1 hour to carry out the following reaction. After adding sodium bicarbonate to the reaction system, recover the fraction at 68 - 70 °C by atmospheric distillation to obtain 1,1-bis(trifluoromethyl)butadiene (BTFBE), with a yield of 58%.
[0261] [Chemical formula 25]
[0262]
[0263] <NMR analysis results>
[0264] 1 H-NMR (solvent: deuterated chloroform, internal standard: TMS); δ (ppm): 5.95 (1H, dd), 6.05 (1H, dd), 6.85 (1H, m), 7.04 (1H, m)
[0265] 19 F-NMR (Solvent: chloroform-d, internal standard: C 6 D 6 ); δ (ppm): -58.4 (3F, m), -65.3 (3F, m)
[0266] 2. Synthesis of polymers
[0267] [Determination of molar ratio of each repeating unit] NMR
[0268] Based on the 1 H-NMR and 19 F-NMR measurement values, determine the molar ratio of each repeating unit in the polymer.
[0269] [Determination of molecular weight of polymer] GPC
[0270] Using a high-speed gel permeation chromatograph (manufactured by TOSOH CORPORATION, model HLC-8320GPC), connect an ALPHA-M column and an ALPHA-2500 column (both manufactured by TOSOH CORPORATION) in series one by one, use tetrahydrofuran (THF) as the eluent, and thus determine the number-average molecular weight Mn and weight-average molecular weight Mw of the polymer. A differential refractive index detector can be used as the detector. Calculate the molecular weight distribution Mw / Mn from the number-average molecular weight Mn and weight-average molecular weight Mw.
[0271] 2-1. Synthesis of fluorinated copolymer 1
[0272] At room temperature, in a 300 ml glass flask equipped with a stirrer, weigh 62 g of THF as a solvent into 43.2 g (0.1 mol) of 2-(perfluorohexyl)ethyl methacrylate (MA-C6F) and 19.0 g (0.1 mol) of BTFBE, add 0.8 g (0.005 mol) of α,α-azobisisobutyronitrile (AIBN) as a polymerization initiator, degas while stirring, then displace the inside of the flask with nitrogen, raise the temperature to 75 °C and react for 6 hours. Reduce the pressure of the reaction system, distill off THF, then drop the reaction system into 300 g of n-heptane to precipitate a transparent viscous substance. Decant and separate the supernatant of this viscous substance, and dry it under reduced pressure at 60 °C to obtain 22 g of fluorinated copolymer 1 as a transparent viscous substance, with a yield of 37%.
[0273] <NMR measurement results>
[0274] In terms of molar ratio, the content ratio of each repeating unit in the fluorine-containing copolymer 1 is: repeating unit from MA-C6F: repeating unit from BTFBE = 28:72.
[0275] [Chemical formula 26]
[0276]
[0277] <GPC measurement result>
[0278] Mw = 7,300, Mw / Mn = 1.4
[0279] 2-2. Synthesis of fluorine-containing copolymer 2
[0280] At room temperature, in a 300 ml glass flask equipped with a stirrer, 90 g of THF was added to 43.2 g (0.1 mol) of MA-C6F, 27.0 g (0.1 mol) of 1,1,1,3,3,3-hexafluoro-2-(4-vinylphenyl)propan-2-ol (4-HFA-St), and 19.0 g (0.1 mol) of BTFBE. Further, 0.8 g (0.005 mol) of AIBN was added, and after degassing with stirring, the inside of the flask was purged with nitrogen. After raising the temperature to 75 °C, the reaction was carried out for 6 hours. After the reaction was completed, the solution was concentrated under reduced pressure to remove THF, and then 350 g of n-heptane was added dropwise to precipitate a transparent viscous substance. The supernatant of this viscous substance was separated by decantation and dried under reduced pressure at 60 °C to obtain 48 g of fluorine-containing copolymer 2 as a transparent viscous substance, with a yield of 52%.
[0281] <NMR measurement result>
[0282] In terms of molar ratio, the content ratio of each repeating unit in the fluorine-containing copolymer 2 is: repeating unit from MA-C6F: repeating unit from 4-HFA-St: repeating unit from BTFBE = 17:37:46.
[0283] [Chemical formula 27]
[0284]
[0285] <GPC measurement result>
[0286] Mw = 13,300, Mw / Mn = 1.3
[0287] 2-3. Synthesis of fluorine-containing copolymer 3
[0288] At room temperature, 43.2 g (0.1 mol) of MA-C6F, 16.2 g (0.1 mol) of p-acetoxystyrene (AcO-St), 19.0 g (0.1 mol) of BTFBE, 80 g of THF were weighed into a 300 ml glass flask equipped with a stirrer, and 0.8 g (0.005 mol) of AIBN was added. After degassing with stirring, the inside of the flask was purged with nitrogen, the temperature was raised to 75 °C and the reaction was carried out for 6 hours. The reaction system was depressurized, THF was distilled off, and 350 g of n-heptane was added dropwise to the reaction system to precipitate a transparent viscous substance. The supernatant of the viscous substance was separated by decantation, and after dissolving in 100 g of methanol, 10.1 g (0.1 mol) of triethylamine (TEA) was added. To decompose the acetoxy group solvent, the temperature was raised to 50 °C and stirred for 8 hours. After confirming the removal of the acetoxy group, it was concentrated and then dried under reduced pressure at 60 °C to obtain 35 g of a fluorine-containing copolymer 3 as a white solid, with a yield of 55%.
[0289] <NMR measurement results>
[0290] In terms of molar ratio, the content ratio of each repeating unit in the fluorine-containing copolymer 3 is: repeating unit from MA-C6F: repeating unit from p-hydroxystyrene (p-HO-St): repeating unit from BTFBE = 12:38:50.
[0291] [Chemical formula 28]
[0292]
[0293] <GPC measurement results>
[0294] Mw = 17,500, Mw / Mn = 1.4
[0295] 2-4. Synthesis of fluorine-containing copolymer 4
[0296] Except for using hexafluoroisopropyl methacrylate (HFIP-M) instead of MA-C6F used in the synthesis of the above fluorine-containing copolymer 3, a fluorine-containing copolymer 4 containing the following repeating units was synthesized by the same procedure as the synthesis of the fluorine-containing copolymer 3, and the fluorine-containing copolymer 4 was obtained with a yield of 51%.
[0297] <NMR measurement results>
[0298] In terms of molar ratio, the content ratio of each repeating unit in the fluorine-containing copolymer 4 is: repeating unit from HFIP-M: repeating unit from p-HO-St: repeating unit from BTFBE = 15:39:46.
[0299] [Chemical formula 29]
[0300]
[0301] <GPC measurement results>
[0302] Mw = 15,200, Mw / Mn = 1.4
[0303] 2-5. Synthesis of fluorinated copolymer 5
[0304] Except for using MA-CH2-OFCP instead of MA-C6F used in the synthesis of the above-mentioned fluorinated copolymer 3, fluorinated copolymer 5 containing the following repeating units was synthesized in the same steps as the synthesis of fluorinated copolymer 3, and fluorinated copolymer 5 was obtained in a yield of 54%.
[0305] <NMR measurement results>
[0306] In terms of molar ratio, the content ratio of each repeating unit in fluorinated copolymer 5 is: repeating unit from MA-CH2-OFCP: repeating unit from p-HO-St: repeating unit from BTFBE = 13:38:49.
[0307] [Chemical formula 30]
[0308]
[0309] <GPC measurement results>
[0310] Mw = 16,100, Mw / Mn = 1.5
[0311] 2-6. Synthesis of fluorinated copolymer 6
[0312] Except for using 2-(perfluorohexyl)ethyl vinyl ether (V-C6F) instead of MA-C6F used in the synthesis of the above-mentioned fluorinated copolymer 3, fluorinated copolymer 6 containing the following repeating units was synthesized in the same steps as the synthesis of fluorinated copolymer 3, and fluorinated copolymer 6 was obtained in a yield of 41%.
[0313] <NMR measurement results>
[0314] In terms of molar ratio, the content ratio of each repeating unit in fluorinated copolymer 6 is: repeating unit from V-C6F: repeating unit from p-HO-St: repeating unit from BTFBE = 10:38:52.
[0315] [Chemical formula 31]
[0316]
[0317] <GPC measurement results>
[0318] Mw = 11,900, Mw / Mn = 1.4
[0319] 2-7. Synthesis of Fluorine-containing Copolymer 7
[0320] At room temperature, 74.1 g (0.31 mol) of HFIP-M, 16.5 g (0.12 mol) of 2-hydroxyethyl methacrylate (HEMA), 9.5 g (0.11 mol) of vinyl acetate (VAc), and 50 g of butyl acetate were weighed into a 1000 ml glass flask equipped with a stirrer. 1.6 g (0.01 mol) of AIBN was added, and the mixture was degassed while stirring. Then, the flask was purged with nitrogen, heated to 80 °C, and reacted for 6 hours. The reaction system was depressurized, and butyl acetate was distilled off. The resulting mixture was dropped into 500 g of n-heptane, and a white solid was precipitated. After filtration, the solid was dried under reduced pressure at 60 °C to obtain 85.7 g of fluorine-containing copolymer 7 as a white solid, with a yield of 78%.
[0321] <NMR Measurement Results>
[0322] In terms of molar ratio, the content ratio of each repeating unit in fluorine-containing copolymer 7 is: repeating unit from HFIP-M: repeating unit from HEMA: repeating unit from VAc = 68:25:7.
[0323] [Chemical Formula 32]
[0324]
[0325] <GPC Measurement Results>
[0326] Mw = 55,500, Mw / Mn = 2.1
[0327] 2-8. Synthesis of Fluorine-containing Copolymer 8
[0328] At room temperature, 84.6 g (0.2 mol) of MA-C6F, 31.7 g (0.2 mol) of p-acetoxystyrene (AcO-St), 11.2 g (0.06 mol) of BTFBE, 127 g of THF were weighed into a 300 ml glass flask equipped with a stirrer, and 2.2 g (0.0135 mol) of AIBN was added. After degassing with stirring, the inside of the flask was purged with nitrogen, the temperature was raised to 70 °C and the reaction was carried out for 6 hours. The reaction system was depressurized, THF was removed by distillation, 850 g of n-heptane was added dropwise to the reaction system, and a transparent viscous substance was precipitated. The supernatant of the viscous substance was separated by decantation, dissolved in 100 g of methanol, and 10.1 g (0.1 mol) of triethylamine (TEA) was added. To decompose the acetoxy group solvent, the temperature was raised to 50 °C and stirred for 8 hours. After confirming the removal of the acetoxy group, it was concentrated and then dried under reduced pressure at 60 °C to obtain 95 g of fluorine-containing copolymer 8 as a white solid, with a yield of 86%.
[0329] <NMR measurement results>
[0330] In terms of molar ratio, the content ratio of each repeating unit in fluorine-containing copolymer 8 is: repeating unit from MA-C6F: repeating unit from p-HO-St: repeating unit from BTFBE = 30:50:20.
[0331] [Chemical formula 33]
[0332]
[0333] <GPC measurement results>
[0334] Mw = 7,500, Mw / Mn = 1.4
[0335] 2-9. Synthesis of fluorine-containing copolymer 9
[0336] At room temperature, 110.5 g (0.26 mol) of MA-C6F, 45.9 g (0.31 mol) of p-vinylbenzoic acid (VBA), 16.0 g (0.09 mol) of BTFBE, 340 g of methyl ethyl ketone (MEK) were weighed into a 300 ml glass flask equipped with a stirrer, 10.8 g (0.065 mol) of AIBN was added. After degassing with stirring, the inside of the flask was purged with nitrogen, the temperature was raised to 75 °C and the reaction was carried out for 6 hours. The reaction system was depressurized, MEK was removed by distillation, 1350 g of n-heptane was added dropwise to the reaction system, and a white precipitate was obtained. After filtration, it was dried under reduced pressure at 60 °C to obtain 146.2 g of fluorine-containing copolymer 9 as a thick white solid, with a yield of 85%.
[0337] <NMR measurement results>
[0338] In terms of molar ratio, the content ratio of each repeating unit in the fluorine-containing copolymer 9 is: repeating unit from MA-C6F: repeating unit from VBA: repeating unit from BTFBE = 30:50:20.
[0339] [Chemical formula 34]
[0340]
[0341] <GPC measurement results>
[0342] Mw = 8,000, Mw / Mn = 1.4
[0343] 3. Synthesis of comparative polymers
[0344] 3-1. Synthesis of comparative polymer 1
[0345] At room temperature, 236.2 g (1 mol) of HFIP-M and 450 g of butyl acetate were weighed into a 300 ml glass flask equipped with a stirrer. 8 g (0.05 mol) of AIBN was added, and degassing was carried out while stirring. Then, the inside of the flask was replaced with nitrogen, and the temperature was raised to 80 °C and reacted for 6 hours. The reaction system was dropped into 500 g of n-heptane to obtain a white precipitate. After filtration, it was dried under reduced pressure at 60 °C to obtain 165 g of comparative polymer 1 as a white solid containing only repeating units from HFIP-M, with a yield of 70%.
[0346] [Chemical formula 35]
[0347]
[0348] <GPC measurement results>
[0349] Mw = 11,200, Mw / Mn = 1.4
[0350] 3-2. Synthesis of comparative polymer 2
[0351] At room temperature, 43.2 g (0.1 mol) of MA-C6F and 85 g of butyl acetate were weighed into a 300 ml glass flask equipped with a stirrer. 0.8 g (0.005 mol) of AIBN was added, and degassing was carried out while stirring. Then, the inside of the flask was replaced with nitrogen, and the temperature was raised to 80 °C and reacted for 6 hours. The content was dropped into 500 g of n-heptane to obtain a white precipitate. The precipitate was filtered out and dried under reduced pressure at 60 °C to obtain 32 g of comparative polymer 2 as a white solid containing repeating units from MA-C6F, with a yield of 74%.
[0352] [Chemical Formula 36]
[0353]
[0354] <GPC Measurement Results>
[0355] Mw = 13,800, Mw / Mn = 1.6
[0356] 3-3. Synthesis of Comparative Polymer 3
[0357] At room temperature, 23.6 g (0.1 mol) of HFIP-M, 43.2 g (0.1 mol) of MA-C6F, and 130 g of butyl acetate were weighed into a 300 ml glass flask equipped with a stirrer. 0.8 g (0.005 mol) of AIBN was added, and the mixture was degassed while stirring. Then, the inside of the flask was purged with nitrogen, and the temperature was raised to 80 °C and reacted for 6 hours. The reaction product was dropped into 500 g of n-heptane to obtain a white precipitate. The precipitate was filtered out and dried under reduced pressure at 60 °C to obtain 53 g of Comparative Polymer 3 as a white solid, with a yield of 80%.
[0358] <NMR Measurement Results>
[0359] In terms of molar ratio, the content ratio of each repeating unit in Comparative Polymer 3 is: repeating unit from HFIP-M: repeating unit from MA-C6F = 51:49.
[0360] [Chemical Formula 37]
[0361]
[0362] <GPC Measurement Results>
[0363] Mw = 14,700, Mw / Mn = 1.7
[0364] 3-4. Synthesis of Comparative Polymer 4
[0365] The following synthesis was carried out according to Synthesis Example 6 of Patent Document 4.
[0366] At room temperature, 2.50 g of the condensate of 4-hydroxyphenyl methacrylate and 1,2-naphthoquinone-2-diazide-5-sulfonyl chloride (HPMA-QD), 0.70 g of methacrylic acid (MAA), 5.26 g of MA-C6F, 2.58 g of methacryloxypropyl tris(trimethylsiloxy)silane (MA-P-TTMS), 1.46 g of N-cyclohexylmaleimide (N-CyM), and 51.3 g of cyclohexanone were weighed into a 300 ml glass flask equipped with a stirrer. 0.33 g of AIBN was added, and the mixture was stirred at 110 °C for 20 hours to obtain Comparative Polymer 4 having a solid content concentration of 20% by mass and containing the following repeating units.
[0367] [Compound 38]
[0368]
[0369] <GPC measurement results>
[0370] Mw = 11,000, Mw / Mn = 1.5
[0371] 3-5. Synthesis of Comparative Polymer 5
[0372] At room temperature, 7.2 g (0.083 mol) of methacrylic acid (MAA), 9.6 g (0.022 mol) of MA-C6F, 7.2 g (0.055 mol) of 2-hydroxyethyl methacrylate (HEMA), and 55 g of methyl ethyl ketone were weighed into a 300 ml glass flask equipped with a stirrer. 0.6 g (0.004 mol) of AIBN was added, and the mixture was stirred at 75 °C for 6 hours. The reaction mixture after completion of the reaction was added dropwise to 500 g of n-heptane to obtain a white precipitate. The precipitate was filtered out and dried under reduced pressure at 60 °C to obtain 19 g of Comparative Polymer 5 as a white solid, with a yield of 80%.
[0373] <NMR measurement results>
[0374] In terms of molar ratio, the content ratio of each repeating unit in Comparative Polymer 5 is: repeating unit from MA-C6F: repeating unit from MAA: repeating unit from HEMA = 14:52:34.
[0375] [Chemical formula 39]
[0376]
[0377] <GPC measurement results>
[0378] Mw = 5,000, Mw / Mn = 1.4
[0379] 3-6. Mole ratio and molecular weight of repeating units of fluorinated copolymers 1 to 9 and comparative polymers 1 to 5
[0380] Table 1 shows the repeating units contained in the obtained fluorinated copolymers 1 to 9 and comparative polymers 1 to 5, their molar ratios, weight average molecular weight (Mw), molecular weight distribution (Mw / Mn) and yields.
[0381] [Table 1]
[0382]
[0383] 4. Liquid repellency of each polymer film before and after UV ozone cleaning or oxygen plasma cleaning and after heating
[0384] After forming a film on a silicon wafer using fluorinated copolymers 1 to 9 and comparative polymers 1 to 5, the contact angles of water, anisole, propylene glycol monomethyl ether acetate (PGMEA) or xylene were measured before and after UV ozone cleaning or oxygen plasma cleaning and after heating. Water, anisole, PGMEA and xylene were used as ink solvents.
[0385] [Manufacturing of film-coated silicon wafers]
[0386] In addition, fluorinated copolymers 1 to 6, 8, 9 and comparative copolymers 1 to 5 were dissolved in propylene glycol monomethyl ether acetate (PGMEA) to form a predetermined film thickness, and applied on a silicon wafer using a spin coater to form a coating film. Then, the coating film was heated on a hot plate at 230° C. for 60 minutes to obtain a silicon wafer with a film.
[0387] Fluorinated copolymer 7 contains a large number of OH groups, and exhibits liquid repellency due to crosslinking of OH groups. Therefore, after preparing the following coating solution, it was applied on a silicon wafer using a spin coater to form a coating film. Then, after pre-baking at 100°C for 150 seconds on a hot plate, the entire film surface was exposed and heated at 230°C for 60 minutes. In addition, the exposure device used was a mask aligner MA6 manufactured by SUSS MICROTEC Co., Ltd.
[0388] [Preparation of coating solution containing fluorinated copolymer 7]
[0389] 0.2 g of 2,4,6-tris[bis(methoxymethyl)amino]-1,3,5-triazine as a crosslinking agent and 0.01 g of a photoacid generator (2-[2-(4-methylphenylsulfonyloxyimino)thiophene-3(2H)-ylidene]-2-(2-methylphenyl)acetonitrile) were dissolved in 4 g of PGMEA with respect to 1 g of the fluorinated copolymer 7, and the mixture was stirred at room temperature for 3 hours to prepare a coating liquid containing the fluorinated copolymer 7. The photoacid generator was decomposed by exposure after the coating film was formed to generate an acid, and the OH group was reduced by crosslinking caused by the acid, thereby obtaining liquid repellency.
[0390] [Washing process and heating process]
[0391] Each silicon wafer with a film was subjected to UV ozone cleaning or oxygen plasma cleaning for 10 minutes using a UV ozone cleaning device, model PL17-110 manufactured by SEN LIGHTS CORPORATION, and a plasma cleaning device, model PDC210 manufactured by Yamato Scientific Co., Ltd. Then, the wafer was heated at 200° C. for 60 seconds.
[0392] [Measurement of contact angle]
[0393] The contact angle of the surface of the film on the silicon wafer before and after UV ozone cleaning or oxygen plasma cleaning and after subsequent heating to water, anisole, PGMEA or xylene was measured using a contact angle meter (DMs-601 manufactured by Kyowa Interface Science Co., Ltd.).
[0394] [Measurement of film thickness]
[0395] The film thickness of the film on the silicon wafer was measured before and after UV ozone cleaning or oxygen plasma cleaning and after subsequent heating using a contact-type film thickness meter.
[0396] [Determination of molecular weight]
[0397] The film on the silicon wafer before and after UV ozone cleaning or oxygen plasma cleaning and after subsequent heating was dissolved in THF and measured using the above-mentioned GPC.
[0398] Table 2 shows the results of measuring the contact angle to water or anisole and the film thickness before and after UV ozone cleaning and after subsequent heating.
[0399] [Table 2]
[0400]
[0401] As shown in Table 2, the contact angles of the films containing fluorinated copolymers 1 to 9 on silicon wafers to water and anisole decreased after UV ozone cleaning, but after heating, the contact angles recovered to almost the same values as before UV ozone cleaning. In contrast, the contact angles of comparative polymers 1 to 5 recovered only slightly by heating.
[0402] Table 3 shows the measurement results of the contact angle to water or anisole and the film thickness before and after oxygen plasma cleaning and after subsequent heating.
[0403] [Table 3]
[0404]
[0405] As shown in Table 3, the contact angles of the films containing fluorinated copolymers 1 to 9 on the silicon wafer to water and anisole decreased after oxygen plasma cleaning, but after heating, the contact angles recovered to almost the same values as before oxygen plasma cleaning. In contrast, the contact angles of comparative polymers 1 to 5 recovered only slightly by heating.
[0406] Table 4 shows the measurement results of the contact angle and film thickness to PGMEA or xylene before and after UV ozone cleaning and after subsequent heating.
[0407] [Table 4]
[0408]
[0409] As shown in Table 4, the contact angles of the films containing fluorinated copolymers 1 to 9 on silicon wafers to PGMEA and xylene decreased after UV ozone cleaning, but after heating, the contact angles recovered to almost the same values before UV ozone cleaning. In contrast, the contact angles of comparative polymers 1 to 5 recovered only slightly by heating.
[0410] Table 5 shows the measurement results of the contact angle and film thickness to PGMEA or xylene before and after oxygen plasma cleaning and after subsequent heating.
[0411] [Table 5]
[0412]
[0413] As shown in Table 5, the contact angles of the films containing fluorinated copolymers 1 to 9 on the silicon wafer to PGMEA and xylene decreased after oxygen plasma cleaning, but after heating, the contact angles recovered to almost the same values as before oxygen plasma cleaning. In contrast, the contact angles of comparative polymers 1 to 5 recovered only slightly by heating.
[0414] Table 6 shows the results of dissolving the film on the silicon wafer before and after UV ozone cleaning, before and after oxygen plasma cleaning and after subsequent heating in THF and measuring using the above-mentioned GPC.
[0415] [Table 6]
[0416]
[0417] As shown in Table 6, the molecular weights of the films containing the nitrogen-containing copolymers 1 to 9 on the silicon wafer were dissolved in THF and measured. After UV ozone cleaning and oxygen plasma cleaning, no significant change in the molecular weight was observed, indicating that the decomposition of the polymers was suppressed. In contrast, it was confirmed that the molecular weights of the comparative polymers 1 to 5 were greatly reduced.
[0418] 5. Evaluation of resist
[0419] Resists 2, 3, 7 and comparative resist 4 were prepared using fluorinated copolymers 2, 3, 7 and comparative polymer 4, and the resist performance of each resist was evaluated and compared.
[0420] 5-1. Preparation of resist
[0421] [Resist 2]
[0422] To 1.6 g of the fluorinated copolymer 2, 20 g of BMR C-1000 (solid content: 40 mass %) manufactured by TOKYO OHKA KOGYO CO., LTD. as a negative resist and 0.2 g of TPA-100 manufactured by Asahi Kasei Corporation as an isocyanate crosslinking agent were added to prepare the above-mentioned solution.
[0423] [Resist 3]
[0424] To 1.6 g of the fluorinated copolymer 3, 20 g of BMR C-1000 (solid content 40% by mass) manufactured by TOKYO OHKA KOGYO CO., LTD. as a negative resist, 0.2 g of 2,4,6-tris[bis(methoxymethyl)amino]-1,3,5-triazine as a crosslinking agent, and 0.01 g of (2-[2-(4-methylphenylsulfonyloxyimino)thiophene-3(2H)-ylidene]-2-(2-methylphenyl)acetonitrile as a photoacid generator were added to prepare a negative resist.
[0425] [Resist 7]
[0426] Relative to 1 g of the fluorinated copolymer 7, 0.2 g of 2,4,6-tris[bis(methoxymethyl)amino]-1,3,5-triazine as a cross-linking agent and 0.01 g of (2-[2-(4-methylphenylsulfonyloxyimino)thiophene-3(2H)-ylidene]-2-(2-methylphenyl)acetonitrile as a photoacid generator were dissolved in 4 g of PGMEA, and the mixture was stirred at room temperature for 3 hours to prepare an anti-etching agent 7 containing the fluorinated copolymer 7.
[0427] [Comparative resist 4]
[0428] Comparative Polymer 4 was used to prepare a positive photosensitive resin composition disclosed in Patent Document 4, and Comparative Resist 4 was obtained.
[0429] 5-2. Formation of resist film
[0430] Ultrapure water and then acetone were sprayed onto a silicon wafer having a diameter of 4 inches, and after cleaning by spin coating, UV ozone cleaning was performed for 5 minutes using the above-mentioned UV ozone cleaning device. Next, the above-mentioned resists 2, 3, 7 and comparative resist 4 were filtered using a 0.2 μm membrane filter, and then the filtered resists were applied to the silicon wafer using a spinner at a rotation speed of 1,000 rpm, and heated and dried on a hot plate at 100°C for 150 seconds to form a resist film with a film thickness of 2 μm on the silicon wafer.
[0431] 5-3. Evaluation of resist solubility in developer and resolution of resist pattern
[0432] The resist films formed on the silicon wafers were evaluated for solubility in a developer and resolution of the resist pattern, and the contact angles were measured. The measurement method is described below.
[0433] The resist film formed on the silicon wafer was exposed to i-line (wavelength 365 nm) through a mask with a line width / space of 5 μm using the above-mentioned mask aligner, and then "post-exposure baking" was performed at 120° C. for 60 seconds.
[0434] [Solubility in developer solution]
[0435] At room temperature, the silicon wafer with resist film before and after exposure is immersed in alkaline developer or PGMEA for 60 seconds, and the solubility relative to developer or organic solvent is evaluated. As alkaline developer, 2.38% by mass of tetramethylammonium hydroxide aqueous solution (hereinafter, sometimes referred to as TMAH) is used. The film thickness of the resist film after immersion is measured using an optical interference film thickness meter, thus evaluating the solubility of the resist film. The situation that the resist film is completely dissolved is recorded as "soluble", and the situation that the resist film is not dissolved and has residue is recorded as "insoluble".
[0436] [Sensitivity]
[0437] The optimal exposure Eop (mj / cm2) for forming the pattern of the line width / line spacing is calculated. 2 ), which is used as an indicator of sensitivity.
[0438] [Resolution]
[0439] The resist pattern on the patterned silicon wafer was observed under a microscope. The case where no line edge roughness was observed was rated as "excellent", the case where some line edge roughness was observed was rated as "good", and the case where the line edge roughness was significant was rated as "failed".
[0440] Table 7 shows the evaluation results of the developer solubility of each resist and the sensitivity and resolution of the resist pattern.
[0441] [Table 7]
[0442]
[0443] <Evaluation of developer solubility>
[0444] As shown in Table 7, the unexposed parts of resists 2 and 3 are soluble in alkaline developer or PGMEA, and the exposed parts are insoluble. The unexposed parts of resist 7 are soluble in PGMEA, and the exposed parts are insoluble, and can be used as negative resists. The exposed parts of comparative resist 4 are soluble in alkaline developer, and can be used as positive resists.
[0445] <Sensitivity>
[0446] Resist 3 and comparative resist 4 showed the same degree of sensitivity. Compared with these resists, resist 7 was highly sensitive.
[0447] <Resolution>
[0448] The resist patterns using Resists 2, 3, 7 and Comparative Resist 4 all transferred the line width / line spacing of 5 μm of the mask with good resolution. In particular, Resist 7 had no line edge roughness observed, and the resolution was "excellent".
[0449] 5-4. Evaluation of liquid repellency of resist pattern before and after UV ozone cleaning and after heating
[0450] The contact angle of p-anisole was measured for the resist film on the silicon wafer using resists 2, 3, 7 and comparative resist 4 before and after UV ozone cleaning and after subsequent heating. The silicon wafer with the resist film was UV ozone cleaned for 10 minutes using the above-mentioned UV ozone cleaning device, and then heated at 200°C for 60 seconds. The contact angle measuring instrument used was a contact angle measuring instrument manufactured by Kyowa InterfaceScience Co., Ltd.
[0451] [Table 8]
[0452]
[0453] [Contact angle measurement results]
[0454] As shown in Table 8, for Resists 2, 3, and 7, the contact angle of anisole at the exposed portion constituting the bank during patterning decreased due to UV ozone cleaning, but increased due to heating, and the liquid repellency was restored.
[0455] 5-5. Evaluation of the liquid repellency of the resist pattern before and after oxygen plasma cleaning and after heating
[0456] The contact angle of p-anisole was measured for the resist film on the silicon wafer using resists 2, 3, 7 and comparative resist 4 before and after oxygen plasma cleaning and after subsequent heating. The resist-filmed silicon wafer was oxygen plasma cleaned for 10 minutes using the above-mentioned oxygen plasma cleaning apparatus, and then heated at 200° C. for 60 seconds. The contact angle measuring instrument used was a contact angle measuring instrument manufactured by Kyowa Interface Science Co., Ltd.
[0457] [Table 9]
[0458]
[0459] [Contact angle measurement results]
[0460] As shown in Table 9, for Resists 2, 3, and 7, the contact angle of anisole at the exposed portion constituting the bank during patterning decreased due to oxygen plasma cleaning, but increased due to heating, thereby restoring the liquid repellency.
[0461] Industrial Applicability
[0462] The method for manufacturing a patterned film substrate of the present application can maintain the lyophilicity of the concave portion of the patterned film while making the dam sufficiently lyophobic. Therefore, the method for manufacturing a patterned film substrate of the present application can be applied not only to the manufacture of display elements using an inkjet method, but also to the manufacture of thin films such as organic semiconductor films or colored resin films, or to the manufacture of devices such as display wiring and thin film transistors.
Claims
1. A method for manufacturing a patterned film substrate, comprising: The patterned film substrate is cleaned by UV ozone cleaning or oxygen plasma cleaning to obtain a first patterned film substrate cleaning process, wherein: The patterned film substrate is a patterned film substrate having a patterned film formed on a substrate, wherein the patterned film contains a fluorine-containing copolymer, and the fluorine-containing copolymer contains both a repeating unit represented by formula (A) and a repeating unit represented by formula (C); and a heating step of heating the first patterned film substrate to obtain a second patterned film substrate, [Chemical formula 1] In the formula, R 1 , R 3 Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group are optionally substituted by fluorine atoms; Q is a fluoroalkyl group having 1 to 20 carbon atoms, which optionally has a hydrogen atom, an oxygen atom or a nitrogen atom; X is a single bond or a divalent group; Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups are optionally substituted by fluorine atoms, oxygen atoms or nitrogen atoms; O is an oxygen atom.
2. The manufacturing method according to claim 1, wherein: The fluorinated copolymer contains a repeating unit represented by formula (A), a repeating unit represented by formula (B), and a repeating unit represented by formula (C). [Chemical formula 2] In the formula, R 1 , R 2 , R 3 Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group are optionally substituted by fluorine atoms; Q is a fluoroalkyl group having 1 to 20 carbon atoms, which optionally has a hydrogen atom, an oxygen atom or a nitrogen atom; X and Y are each independently a single bond or a divalent group; Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups are optionally substituted by fluorine atoms, oxygen atoms or nitrogen atoms; O is an oxygen atom, and H is a hydrogen atom.
3. The manufacturing method according to claim 1 or 2, wherein: In the heating step, the first patterned film substrate is heated at a temperature of 50° C. to 350° C. for 10 seconds or more.
4. The manufacturing method according to claim 1 or 2, wherein: The second patterned film substrate is a substrate for forming a display element by an inkjet method.
5. The manufacturing method according to claim 1 or 2, wherein: In the repeating unit represented by the formula (A), Q is a fluoroalkyl group having 3 to 10 carbon atoms, and X is a carbonyl group.
6. The manufacturing method according to claim 5, wherein: In the repeating unit represented by the formula (A), Q is a perfluorohexylethyl group, and X is a carbonyl group.
7. The manufacturing method according to claim 5, wherein: In the repeating unit represented by the formula (A), Q is a hexafluoroisopropyl group, and X is a carbonyl group.
8. The manufacturing method according to claim 1 or 2, wherein: The repeating unit represented by the formula (A) is a repeating unit represented by the formula (A-1), [Chemical formula 3] In formula (A-1), R 4 , R 5 Each independently represents a hydrogen atom, a fluorine atom or an alkyl group having 1 to 3 carbon atoms, wherein a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group are optionally substituted with fluorine atoms; O represents an oxygen atom, H represents a hydrogen atom, and F represents a fluorine atom.
9. The manufacturing method according to claim 2, wherein: In the repeating unit represented by the formula (A), Q is a hexafluoroisopropyl group and X is a carbonyl group; and in the repeating unit represented by the formula (B), Y is a p-phenylene group or a carboxyethylene group.
10. The manufacturing method according to claim 2, wherein: The repeating unit represented by the formula (A) has Q that is hexafluoroisopropyl and X that is carbonyl; the repeating unit represented by the formula (B) has Y that is p-phenylene or carboxyethylene; and the repeating unit represented by the formula (C) has Z that is alkoxy, carboxyl, acetoxy or bistrifluoromethylvinyl.
11. The manufacturing method according to claim 2, wherein: In the repeating unit represented by the formula (C), Z is a bistrifluoromethylvinyl group.
12. The manufacturing method according to claim 2, wherein: In the repeating unit represented by the formula (A), Q is a fluoroalkyl group having 3 to 10 carbon atoms, and X is a carbonyl group; in the repeating unit represented by the formula (B), Y is a p-phenylene group, a p-phenylenecarbonyl group, or a p-phenylenehexafluoroisopropylidene group; and in the repeating unit represented by the formula (C), Z is a bistrifluoromethylvinyl group.
13. A fluorinated copolymer comprising a repeating unit represented by the following formula (A) and a repeating unit represented by the following formula (C), [Chemical formula 4] In the formula, R 1 , R 3 Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group are optionally substituted by fluorine atoms; Q is a fluoroalkyl group having 1 to 20 carbon atoms, which optionally has a hydrogen atom, an oxygen atom or a nitrogen atom; X is a single bond or a divalent group; Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups are optionally substituted by fluorine atoms, oxygen atoms or nitrogen atoms; O is an oxygen atom.
14. The fluorinated copolymer according to claim 13, wherein In the repeating unit represented by the formula (A), Q is a fluoroalkyl group having 3 to 10 carbon atoms, and X is a carbonyl group; and in the repeating unit represented by the formula (C), Z is a bistrifluoromethylvinyl group.
15. A fluorinated copolymer comprising a repeating unit represented by the following formula (A), a repeating unit represented by the following formula (B), and a repeating unit represented by the following formula (C), [Chemical formula 5] In the formula, R 1 , R 2 , R 3 Each is independently a hydrogen atom, a fluorine atom or an alkyl group having 1 to 20 carbon atoms, and a part or all of the hydrogen atoms bonded to the carbon atoms in the alkyl group are optionally substituted by fluorine atoms; Q is a fluoroalkyl group having 1 to 20 carbon atoms, which optionally has a hydrogen atom, an oxygen atom or a nitrogen atom; X and Y are each independently a single bond or a divalent group; Z is an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, a phenyl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an alkylcarbonyloxy group having 1 to 20 carbon atoms or a carboxyl group, and the hydrogen atoms possessed by these groups are optionally substituted by fluorine atoms, oxygen atoms or nitrogen atoms; O is an oxygen atom, and H is a hydrogen atom.
16. The fluorinated copolymer according to claim 15, wherein The repeating unit represented by the formula (A) has Q that is hexafluoroisopropyl and X that is carbonyl; the repeating unit represented by the formula (B) has Y that is carboxyethylene; the repeating unit represented by the formula (C) has R that is 3 is a hydrogen atom or a methyl group, and Z is an alkylcarbonyloxy group having 1 to 4 carbon atoms.
17. The fluorinated copolymer according to claim 15, wherein The repeating unit represented by formula (A) has Q which is a fluoroalkyl group having 3 to 10 carbon atoms and X which is a carbonyl group; the repeating unit represented by formula (B) has Y which is p-phenylene, p-phenylenecarbonyl or p-phenylenehexafluoroisopropylidene; the repeating unit represented by formula (C) has R 3 is a hydrogen atom or a methyl group, and Z is a bistrifluoromethylvinyl group.