Semi-flexible board formed by laminating prepregs and manufacturing method of semi-flexible board

By adding semi-cured sheets between the copper foil layers of the semi-flexible plate and laminating them multiple times, and capping the protective layer, the problem that the prior art cannot protect the semi-flexible region is solved, and high-quality semi-flexible plate products are realized , reduces production costs.

CN118946042APending Publication Date: 2024-11-12SHANGHAI FAST PCB CIRCUIT TECH CORP LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410926048.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art cannot effectively protect the semi-flexible area of ​​the semi-flexible plate, resulting in the product quality not meeting the standards.

Method used

Using the semi-cured sheet pressing process, by adding semi-cured sheets between the copper foil layers, laminating multiple times and covering the protective layer on the surface of the semi-flexible area, combining flow and non-flow semi-cured sheets to ensure protection and performance of the semi-flexible area. .

Benefits of technology

It realizes effective protection of the semi-flexible area, maintains bending performance, simplifies the difficulty of removing protective layers of finished products, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946042A_ABST
    Figure CN118946042A_ABST
Patent Text Reader

Abstract

The invention relates to a semi-flexible board formed by laminating prepregs and a manufacturing method of the semi-flexible board. The manufacturing method comprises the following steps: adding prepregs between copper foil layers, and laminating to obtain a semi-flexible plate; making a pattern on the semi-flexible plate, covering the semi-flexible plate with a prepreg to carry out pattern protection, and then carrying out secondary lamination; after secondary lamination, covering a non-flowing prepreg on the semi-flexible plate, windowing on the non-flowing prepreg, and covering a protective layer on the inner surface layer of the corresponding semi-flexible area after windowing; sequentially covering a plurality of layers of hard board base materials on the semi-flexible board, adding flowing prepregs between the adjacent layers of hard board base materials, and then laminating for the third time. And performing outer layer treatment after lamination, and removing the protective layer after treatment to obtain the semi-flexible board. Compared with the prior art, the bendable semi-flexible plate with the protected semi-flexible area pattern is finally manufactured through three times of lamination and covering of the protective layer on the inner surface layer of the windowed semi-flexible area.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of circuit board manufacturing, and in particular relates to a semi-flexible board formed by laminating prepreg sheets and a manufacturing method thereof. Background Art

[0002] Semi-flexible boards are electronic interconnect materials, usually used to connect printed circuit boards or other electronic components. Semi-flexible boards are PCB boards obtained by milling thin the middle part that needs to be bent during conventional hard board processing or by using rigid-flex board processing technology. They have complete electrical properties and a certain degree of flexibility. Semi-flexible boards are generally made by board manufacturers and processed and used by customers. Semi-flexible boards have their own design characteristics. The semi-flexible area of ​​the semi-flexible board connects the hard board parts at both ends together to achieve static bending or semi-dynamic bending in the middle to meet usage requirements.

[0003] Usually, in some applications, continuous dynamic bending is not required, but limited bending is required during installation, maintenance, etc. The use of conventional rigid-flexible boards is obviously "overkill" and too costly. In this case, semi-flexible boards are the better choice.

[0004] Conventional methods for making semi-flexible printed circuit boards include controlled depth milling, windowing, and milling and covering. Among them, the milling and covering method is suitable for semi-flexible boards with conductor patterns on both sides of the flexible area, and the boards after processing have a high bending resistance. However, the current milling and covering method cannot protect the semi-flexible area, which easily causes the quality of the final product to be substandard.

[0005] Therefore, it is urgent to develop a new manufacturing process for a semi-flexible board to protect the semi-flexible area of ​​the semi-flexible board. Summary of the invention

[0006] The purpose of the present invention is to provide a semi-flexible board formed by laminating prepreg sheets and a manufacturing method thereof in order to overcome the defect that the prior art cannot protect the semi-flexible area of ​​the semi-flexible board.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] The present invention provides a method for manufacturing a semi-flexible board formed by laminating prepregs, comprising the following steps:

[0009] S1: Add prepreg between copper foil layers and laminate to obtain semi-flexible sheet;

[0010] S2: Patterns are made on semi-flexible sheets, covered with prepreg for pattern protection, followed by secondary lamination;

[0011] S3: After secondary lamination, a non-flowing prepreg is placed on the semi-flexible sheet, and a window is opened on the non-flowing prepreg. After the window is opened, a protective layer is placed on the surface of the corresponding semi-flexible area;

[0012] S4: sequentially covering the semi-flexible sheet with multiple layers of hard board substrates, adding a flowable prepreg between adjacent layers of hard board substrates, and then laminating three times;

[0013] S5: After three laminations, the outer layer is treated and the protective layer is removed to obtain a semi-flexible board.

[0014] Furthermore, in step S1, the prepreg includes resin and glass fiber cloth. The prepreg acts as an insulating medium for the inner and outer layers in the multilayer board to ensure electrical isolation of the circuit. The non-flowing prepreg has less glue content than the flowing prepreg and has a higher glass transition temperature, which can prevent glue overflow during lamination under high pressure and high temperature. The glass fiber cloth is selected from models such as 1080, 2116, 7628, etc., which are flat and have a large fineness.

[0015] Furthermore, in step S1, the heating rate of the lamination is 3-5°C / min, preferably 4°C / min.

[0016] Furthermore, in step S1, the temperature of the lamination after heating is 160-200°C, preferably 180°C.

[0017] Furthermore, in step S1, the heat preservation time after the lamination is heated is 80-100 minutes, preferably 90 minutes.

[0018] Furthermore, in step S1, the lamination pressure is 400-500 psi.

[0019] Furthermore, in step S3, the single-side size of the window is 0.2-1 mm larger than the single-side size of the semi-flexible area.

[0020] Furthermore, in step S3, the protective layer includes one or more of polyimide (PI) tape or polytetrafluoroethylene (PTFE) gasket to ensure that the surface layer in the semi-flexible area will not be affected by the glue flow of the prepreg during subsequent lamination.

[0021] Furthermore, in step S4, the hard board substrate includes a PCB substrate, and copper foil is provided on both the upper and lower surfaces of the PCB substrate.

[0022] Furthermore, in step S5, the outer layer processing includes drilling, copper electroplating, outer layer pattern production, solder mask production, surface treatment and electrical testing.

[0023] The present invention also provides a semi-flexible board obtained by the above-mentioned manufacturing method, wherein the semi-flexible board comprises a group of main hard board areas and semi-flexible areas connected between the main hard board areas;

[0024] The main hard board area is a hard board substrate that has been processed with outer layer graphics, and the semi-flexible area is a semi-flexible board after three layers of lamination.

[0025] Furthermore, the semi-flexible area is an elastic strip structure.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The present invention performs three-time lamination and covers the surface of the semi-flexible area after the window is opened with a protective layer, thereby finally producing a bendable semi-flexible board product with a protected pattern in the semi-flexible area.

[0028] (2) The present invention affixes a protective layer to the inner surface of the semi-flexible area, thereby ensuring that the inner surface of the semi-flexible area is not affected by the flow of glue from the semi-cured sheet during subsequent lamination and remains intact. At the same time, it simplifies the difficulty of removing the protective layer on the semi-flexible area in the finished product, thereby preventing the semi-flexible area from being damaged and affecting the bending performance.

[0029] (3) The present invention can combine the advantages of the flowable prepreg and the non-flowable prepreg by flexibly selecting the flowable prepreg and the non-flowable prepreg, and obtain a semi-flexible board with better performance through lamination.

[0030] (4) The semi-flexible board of the present invention is made by laminating copper foil and prepreg, and then connected to the hard board area at both ends to form a semi-flexible board. Compared with conventional rigid boards, it can be bent and installed to reduce space; compared with traditional soft-hard boards, it greatly saves production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a flow chart of the method for manufacturing a semi-flexible board according to Example 1 of the present invention.

[0032] Figure 2 This is a structural relationship diagram of the semi-flexible plate material of Example 2 of the present invention.

[0033] Figure 3 Schematic diagram of the structural relationship between the semi-flexible plate and the second prepreg sheet of Example 2 of the present invention.

[0034] Figure 4 Schematic diagram of the window area of ​​the semi-flexible plate of Example 2 of the present invention.

[0035] Figure 5 This is a schematic diagram of the structure of the semi-flexible board prepared in Example 3 of the present invention before the protective layer is removed.

[0036] Figure 6This is a schematic diagram of the final product of the semi-flexible board made in Example 3 of the present invention.

[0037] Figure 7 This is a final product picture of the semi-flexible board made in Example 3 of the present invention.

[0038] Description of the markings in the figure:

[0039] 1-copper foil layer, 2-first semi-cured sheet, 3-second semi-cured sheet, 4-third semi-cured sheet, 5-protective layer, 6-rigid board substrate, 7-opening window, 8-fourth semi-cured sheet, 9-main rigid board area, 10-semi-flexible area. DETAILED DESCRIPTION

[0040] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0041] Unless otherwise specified, the reagents, methods, instruments and equipment used in the present invention are conventional reagents, methods, instruments and equipment in the art. Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0042] Embodiment 1:

[0043] A method for manufacturing a semi-flexible board formed by laminating prepreg sheets, such as Figure 1 As shown, the following steps are included:

[0044] S1: Add prepreg between copper foil layers and laminate to obtain semi-flexible sheet;

[0045] S2: Patterns are made on semi-flexible sheets, covered with prepreg for pattern protection, followed by secondary lamination;

[0046] S3: After secondary lamination, a non-flowing prepreg is placed on the semi-flexible sheet, and a window is opened on the non-flowing prepreg. After the window is opened, a protective layer is placed on the surface of the corresponding semi-flexible area;

[0047] S4: sequentially covering the semi-flexible sheet with multiple layers of hard board substrates, adding a flowable prepreg between adjacent layers of hard board substrates, and then laminating three times;

[0048] S5: After three laminations, the outer layer is treated and the protective layer is removed to obtain a semi-flexible board.

[0049] In this embodiment, a protective layer is added to the inner surface of the semi-flexible area after the window is opened to ensure that the inner surface of the semi-flexible area is not affected by the glue flow of the semi-cured sheet during subsequent pressing and remains intact, and a bendable semi-flexible board is finally produced through three laminations.

[0050] Embodiment 2:

[0051] A method for manufacturing a semi-flexible board formed by laminating prepreg sheets, such as Figure 2-5 As shown, the specific steps include:

[0052] S1: adding a first prepreg 2 between two copper foil layers 1, and laminating to obtain a semi-flexible sheet;

[0053] S2: making a pattern on the semi-flexible sheet, covering it with a second prepreg 3 to protect the pattern, and then performing secondary lamination;

[0054] S3: After the secondary lamination, a third prepreg 4 is covered on the semi-flexible sheet, and a window 7 is opened on the third prepreg 4. After the window is opened, a protective layer 5 is covered on the inner surface of the corresponding semi-flexible area 10;

[0055] S4: sequentially covering the semi-flexible sheet with multiple layers of hard board substrates 6, adding a fourth prepreg 8 between adjacent layers of hard board substrates 6, and then laminating three times;

[0056] S5: After the three-layer lamination, the outer layer is treated, and the protective layer 5 is removed after the treatment, so that a semi-flexible board is obtained.

[0057] In step S1, the first prepreg 2 includes resin and glass fiber cloth. The prepreg acts as an insulating medium for the inner and outer layers in the multilayer board to ensure the electrical isolation of the circuit. The prepreg can be divided into a non-flowing prepreg and a flowing prepreg according to the fluidity of the resin. The non-flowing prepreg has less glue content than the flowing prepreg and has a higher glass transition temperature, which can prevent glue overflow during the lamination process under high pressure and high temperature. The glass fiber cloth of this embodiment is selected from models such as 2116 and 7628, which are flat and have a larger fineness.

[0058] In step S1, the heating rate of lamination is 3-5°C / min, the temperature after heating is 160-200°C, the holding time after heating is 80-100min, and the lamination pressure is 400-500psi. The parameters of the secondary lamination and the tertiary lamination are all referenced to the primary lamination.

[0059] In step S3, the single-side size of the window 7 is 0.2-1 mm larger than the single-side size of the semi-flexible area 10. The suspended rigid layer is peeled off by controlled depth milling to expose the semi-flexible area 10. The protective layer 5 includes one or more of polyimide tape or polytetrafluoroethylene gasket to ensure that the inner surface of the semi-flexible area 10 is not affected by the flow of prepreg during subsequent lamination.

[0060] In step S4, the hard board substrate 6 includes a PCB substrate (hard board core), and copper foils are provided on both the upper and lower surfaces of the PCB substrate to meet specific electrical requirements.

[0061] In step S5, the outer layer processing includes drilling, copper plating, outer layer pattern production, solder mask production, surface treatment and electrical testing. Drill holes where necessary and plate copper or other metals to achieve electrical connection. Surface treatment can be processed by green oil, silk screen printing, etc. as needed. Electrical testing can be performed on the completed semi-flexible board for reliability testing, such as thermal stress testing, hot and cold shock testing, salt spray testing, etc., to ensure its performance and reliability. Finally, the electronic components are installed on the semi-flexible board, and final assembly and installation are performed.

[0062] In this embodiment, the first prepreg 2, the second prepreg 3 and the fourth prepreg 8 are all flowable prepregs, and the third prepreg 4 is a non-flowable prepreg.

[0063] The semi-flexible board prepared in this embodiment includes a group of main hard board areas 9 and semi-flexible areas 10 connected between the main hard board areas 9. The main hard board areas 9 are the hard board substrate 6 after the outer layer pattern is made and processed, and the semi-flexible area 10 is the semi-flexible board after three layers of lamination. The semi-flexible area 10 is an elastic strip structure, which can realize static bending or semi-dynamic bending in the middle of the semi-flexible board.

[0064] Embodiment 3:

[0065] This embodiment provides a semi-flexible board formed by laminating prepreg sheets and a method for making the same. Figure 6-7 As shown, in the lamination production of the semi-flexible sheet, it is also necessary to carry out graphic protection of the semi-flexible area to simplify the difficulty of removing the protective layer on the semi-flexible area in the finished product and avoid damage to the semi-flexible area and affect the bending performance. Specifically, the following steps are included:

[0066] S101, production of semi-flexible sheet, copper foil is bonded with semi-cured sheet made of flat glass fiber cloth with large fiber density, and the first lamination is implemented. The lamination process parameters are: heating rate at 3-5℃ / min, material temperature at 180℃, insulation time for 90min, and pressure controlled at 400-500psi.

[0067] S102, patterning the laminated semi-flexible sheet material.

[0068] S103, protecting the pattern of the semi-flexible sheet with a prepreg and performing a second lamination.

[0069] After the semi-flexible sheet is made, the third lamination with the remaining layers is carried out, including the following steps:

[0070] S201, stacking hard board substrates on the semi-flexible board in sequence to complete the production of the remaining parts of the semi-flexible board.

[0071] S202, laminating between one side of the semi-flexible area and the hard board substrate through a non-flowing prepreg, and laminating between the remaining layers with a flowing prepreg.

[0072] S203, protecting the semi-flexible area, and affixing a layer of PI tape or PTFE gasket to the inner surface of the semi-flexible area for protection.

[0073] S204, drilling, copper plating, outer layer pattern production, solder mask production, surface treatment, electrical testing, and appearance.

[0074] S205, removing the protective layer on the surface of the semi-flexible board to expose the semi-flexible area to obtain the semi-flexible board.

[0075] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for manufacturing a semi-flexible board formed by laminating prepreg sheets, It is characterized in that The following steps are involved: S1: Add prepreg between copper foil layers and laminate to obtain semi-flexible sheet; S2: Patterns are made on semi-flexible sheets, covered with prepreg for pattern protection, followed by secondary lamination; S3: After secondary lamination, a non-flowing prepreg is placed on the semi-flexible sheet, and a window is opened on the non-flowing prepreg. After the window is opened, a protective layer is placed on the surface of the corresponding semi-flexible area; S4: sequentially covering the semi-flexible sheet with multiple layers of hard board substrates, adding a flowable prepreg between adjacent layers of hard board substrates, and then laminating three times; S5: After three laminations, the outer layer is treated and the protective layer is removed to obtain a semi-flexible board.

2. A method for manufacturing a semi-flexible board formed by laminating prepreg sheets according to claim 1, It is characterized in that In step S1, the prepreg comprises resin and glass fiber cloth.

3. A method for manufacturing a semi-flexible board formed by laminating prepreg sheets according to claim 1, It is characterized in that In step S1, the heating rate of the lamination is 3-5°C / min, the temperature after heating is 160-200°C, and the insulation time after heating is 80-100min.

4. A method for manufacturing a semi-flexible board formed by laminating prepreg sheets according to claim 1, It is characterized in that In step S1, the lamination pressure is 400-500 psi.

5. A method for manufacturing a semi-flexible board formed by laminating prepreg sheets according to claim 1, It is characterized in that In step S3, the single-side size of the window is 0.2-1 mm larger than the single-side size of the semi-flexible area.

6. A method for manufacturing a semi-flexible board formed by laminating prepreg sheets according to claim 1, It is characterized in that In step S3, the protective layer includes one or more of polyimide tape or polytetrafluoroethylene gasket.

7. A method for manufacturing a semi-flexible board formed by laminating prepreg sheets according to claim 1, It is characterized in that In step S4, the hard board substrate includes a PCB substrate, and copper foil is provided on both the upper and lower surfaces of the PCB substrate.

8. A method for manufacturing a semi-flexible board formed by laminating prepreg sheets according to claim 1, It is characterized in that In step S5, the outer layer processing includes drilling, copper electroplating, outer layer pattern production, solder mask production, surface treatment and electrical testing.

9. A semi-flexible board obtained by the manufacturing method according to any one of claims 1 to 8, It is characterized in that The semi-flexible plate includes a group of main hard plate areas and semi-flexible areas connected between the main hard plate areas; The main hard board area is a hard board substrate that has been processed with outer layer graphics, and the semi-flexible area is a semi-flexible board after three layers of lamination.

10. A semi-flexible board according to claim 9, It is characterized in that The semi-flexible area is a strip structure with elasticity.

Citation Information

Cited By

  • Semi-flexible combined plate and manufacturing method thereof

    CN120980772A