Electromagnetic shielding film and circuit board
By opening holes and setting up projections on the shielding layer of the electromagnetic shielding film, the short circuit problem of circuit board is solved, the breathability and shielding efficiency are improved, and the electromagnetic shielding function is realized.
Patent Information
- Application Number
- CN202411166391.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing electromagnetic shielding film may easily lead to short circuits on the circuit board after being pressed onto the circuit board substrate, affecting the quality of use.
An electromagnetic shielding film is designed, with several holes on the shielding layer and a raised portion is provided on one side surface. The density of the raised portion is 100 to 600/mm2, and the residual rate is 40% to 80%. The maximum width and density are within a specific range, ensuring effective connection and conductivity of the shielding layer to the circuit board substrate.
By increasing breathability and optimizing the density of the projection, the moisture accumulation on the surface of the circuit board is reduced, the probability of short circuit is reduced, and the shielding efficiency is ensured, so as to achieve normal derivation of interfering charges and electromagnetic shielding functions.
Smart Images

Figure CN118946128A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electronic materials, and in particular to an electromagnetic shielding film and a circuit board. Background Art
[0002] With the rapid development of the electronics industry, electronic products are further developing towards miniaturization, lightness, and high-density assembly, which has greatly promoted the development of flexible circuit boards, thereby realizing the integration of component devices and wire connections. Flexible circuit boards can be widely used in industries such as mobile phones, liquid crystal displays, communications, and aerospace. Driven by the international market, functional flexible circuit boards dominate the flexible circuit board market, and an important indicator for evaluating the performance of functional flexible circuit boards is electromagnetic interference shielding (EMI Shielding). With the integration of functions of mobile phones and other communication equipment, their internal components are rapidly becoming high-frequency and high-speed. For example, in addition to the original audio transmission function, the camera function of mobile phones has become a necessary function, and WLAN (Wireless Local Area Networks), GPS (Global Positioning System) and Internet access functions have become popular. Coupled with the integration of future sensing components, the trend of rapid high-frequency and high-speed components is even more inevitable. Driven by the high-frequency and high-speed trends, the problems of electromagnetic interference inside and outside the components, signal attenuation during transmission, insertion loss and jitter are becoming increasingly serious.
[0003] The electromagnetic shielding film commonly used in existing circuit boards includes a shielding layer and an adhesive film layer. The shielding layer is connected to the ground layer of the circuit board through the adhesive film layer, and then the interference charge is introduced into the ground layer of the circuit board, thereby achieving shielding. However, after the current electromagnetic shielding film is pressed on the circuit board substrate, it is easy to cause the circuit board to short-circuit, affecting the quality of the circuit board. Summary of the invention
[0004] The present invention provides an electromagnetic shielding film and a circuit board to solve the technical problem that a circuit board short circuit easily occurs after the existing electromagnetic shielding film is pressed onto a circuit board substrate, and can effectively improve the use quality of the circuit board.
[0005] In order to solve the above technical problems, the first aspect of the embodiment of the present invention provides an electromagnetic shielding film, including a shielding layer, a plurality of holes are opened on the shielding layer, and a plurality of protrusions are provided on one side surface of the shielding layer, and the density of the protrusions is 100 to 600 per mm 2 The residual rate of the shielding layer is 40% to 80%; wherein the residual rate is the weight ratio of the shielding layer after the opening to the shielding layer before the opening.
[0006] As a preferred solution, the maximum width of the hole is 20 μm to 80 μm; wherein the maximum width is the straight-line distance between two points on the edge of the hole that are farthest apart.
[0007] As a preferred solution, the maximum width of the hole is 40 μm to 60 μm.
[0008] As a preferred embodiment, the ratio of the number of holes with a maximum width of 20 μm to 40 μm to the total number of holes is 20% to 30%, the ratio of the number of holes with a maximum width of 40 μm to 60 μm to the total number of holes is 40% to 60%, and the ratio of the number of holes with a maximum width of 60 μm to 80 μm to the total number of holes is 20% to 30%.
[0009] As a preferred solution, within each square millimeter, the number N of the protrusions and the number N1 of the holes satisfy the following relationship: 2≤N / N1≤4; wherein N and N1 are both positive integers.
[0010] As a preferred solution, the distance between any two adjacent holes is 20 μm to 50 μm; wherein the distance is the shortest straight-line distance between the edges of any two adjacent holes.
[0011] As a preferred solution, the density of the protrusions is 200 to 400 per mm. 2 The residual rate of the shielding layer is 45% to 65%.
[0012] As a preferred solution, the density of the holes is 50 to 150 per mm. 2 .
[0013] As a preferred solution, the density of the holes is 70 to 120 per mm. 2 .
[0014] As a preferred solution, at least three holes are staggered per square millimeter.
[0015] As a preferred solution, the holes include regular shapes and / or irregular shapes.
[0016] As a preferred solution, the shape of the hole includes at least one of a circle, an ellipse, a rectangle, a rhombus, a triangle, and a regular polygon.
[0017] As a preferred solution, it further comprises a film layer, wherein the film layer and the shielding layer are stacked, the protrusion is arranged on one side of the shielding layer close to the film layer, and the film layer comprises an adhesive layer without conductive particles.
[0018] As a preferred solution, it also includes an insulating layer, which is arranged on a surface of the shielding layer on a side away from the adhesive film layer.
[0019] A second aspect of an embodiment of the present invention provides a circuit board, comprising a circuit board substrate and an electromagnetic shielding film as described in any one of the first aspects; the electromagnetic shielding film is pressed together with the circuit board substrate.
[0020] Compared with the prior art, the embodiments of the present invention have the following advantages:
[0021] (1) By opening a plurality of holes on the shielding layer, the air permeability of the circuit board can be increased after the electromagnetic shielding film is pressed onto the circuit board substrate, so that the water vapor on the surface of the circuit board can be discharged through the holes on the shielding layer, thereby reducing the moisture accumulated on the surface of the circuit board and significantly reducing the probability of short circuit on the circuit board.
[0022] (2) By limiting the residual rate of the shielding layer, the exhaust efficiency of the circuit board surface can be guaranteed, while at the same time ensuring that the volume occupied by the hole opening is not too large, thereby ensuring the shielding effectiveness of the shielding layer.
[0023] (3) By limiting the density of the protrusions on the surface of one side of the shielding layer, it is ensured that there are a sufficient number of protrusions per unit area so that when the electromagnetic shielding film is pressed onto the circuit board substrate, it can effectively pierce the adhesive film layer, so that the shielding layer is connected to the ground layer of the circuit board substrate, ensuring the conductive performance, allowing the interference charge of the shielding layer to be normally discharged, and realizing the electromagnetic shielding function. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is a schematic structural diagram of a first electromagnetic shielding film provided by an embodiment of the present invention;
[0025] Figure 2 is an electron microscope image of an electromagnetic shielding film with a protrusion pressed onto a circuit board substrate in an embodiment of the present invention;
[0026] Figure 3 is a schematic diagram of staggered arrangement of holes on the shielding layer in an embodiment of the present invention;
[0027] Figure 4 is an electron microscope image of the holes on the shielding layer in an embodiment of the present invention being arranged in a staggered manner;
[0028] Figure 5 is a schematic diagram of openings on the surface of the shielding layer in an embodiment of the present invention;
[0029] Figure 6 is a schematic structural diagram of a second electromagnetic shielding film provided by an embodiment of the present invention;
[0030] Figure 7 is a schematic structural diagram of a third electromagnetic shielding film provided by an embodiment of the present invention;
[0031] Among them, 100, electromagnetic shielding film; 101, shielding layer; 102, film layer; 103, insulating layer; 104, protrusion; 105, hole. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] In the description of this application, the terms "first", "second", "third", etc. are used for descriptive purposes only and are not to be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first", "second", "third", etc. may explicitly or implicitly include one or more of the feature. In the description of this application, unless otherwise specified, "plurality" means two or more.
[0034] In the description of the present application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be a connection between the two elements. The terms "vertical", "horizontal", "left", "right", "upper", "lower" and similar expressions used herein are only for illustrative purposes, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items. For those of ordinary skill in the art, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0035] In the description of this application, it should be noted that, unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. For those of ordinary skill in the art, the specific meanings of the above terms in this application can be understood by specific circumstances.
[0036] See also Figure 1In a first aspect, an embodiment of the present invention provides an electromagnetic shielding film 100, comprising a shielding layer 101, wherein the shielding layer 101 is provided with a plurality of holes 105, and a plurality of protrusions 104 are provided on a surface of one side of the shielding layer 101, wherein the density of the protrusions 104 is 100 to 600 per mm 2 , the residual rate of the shielding layer 101 is 40% to 80%; wherein the residual rate is the weight ratio of the shielding layer 101 after the opening to the shielding layer 101 before the opening.
[0037] In this embodiment, a plurality of holes 105 are provided on the shielding layer 101, so that after the electromagnetic shielding film 100 is pressed onto the circuit board, water vapor on the surface of the circuit board can be discharged through the holes 105 on the shielding layer 101, thereby reducing the moisture accumulated on the surface of the circuit board and the relative humidity of the surface of the circuit board, thereby effectively avoiding short circuits between copper circuits.
[0038] Further, in order to ensure a good water vapor removal effect, the present embodiment limits the residual rate of the shielding layer 101 to 40% to 80%. For example, the residual rate can be 40%, 42%, 48%, 51%, 53%, 57%, 63%, 65%, 69%, 70%, 72%, 75%, 77%, 80%, etc., which is not specifically limited in the present embodiment. Since the shapes of the holes 105 opened on the shielding layer 101 include regular shapes and irregular shapes, and their areas are difficult to measure accurately, the present embodiment uses the ratio between the weight of the shielding layer 101 after the holes are opened and the weight of the shielding layer 101 before the holes are opened, that is, the residual rate, to characterize the volume occupied by the opening of the holes 105. Within this residual rate range, it can be ensured that the volume occupied by the opening of the holes 105 will not be too small, that is, the residual rate is less than or equal to 80%, so as to ensure that the holes 105 on the shielding layer 101 account for a large proportion and ensure the exhaust efficiency of the circuit board surface. At the same time, it can be ensured that the volume occupied by the opening of the hole 105 is not too large, that is, the residual rate is greater than or equal to 40%, so as to ensure the shielding effectiveness of the shielding layer 101.
[0039] In order to further ensure the shielding effectiveness of the shielding layer 101, the density of the protrusions 104 is set to 100 to 600 per mm. 2 For example, the density of the protrusions 104 may be 100 / mm 2 , 112 pieces / mm 2 , 136 pieces / mm 2 , 147 pieces / mm 2 , 171 pieces / mm 2 , 215 pieces / mm 2 , 264 pieces / mm 2 、297pcs / mm 2 、301pcs / mm 2、324pcs / mm 2 、368pcs / mm 2 、391pcs / mm 2 , 400 pieces / mm 2 , 406 pieces / mm 2 , 423 pieces / mm 2 , 447 pieces / mm 2 , 475 pieces / mm 2 , 490 pieces / mm 2 , 512 pieces / mm 2 , 536 pieces / mm 2 、559pcs / mm 2 、571pcs / mm 2 、592pcs / mm 2 , 600 pieces / mm 2 After the shielding layer 101 is opened, by limiting the density of the protrusions 104 within this density range, it is possible to ensure a certain air permeability within a unit area and ensure that there are a sufficient number of protrusions 104, so that when the electromagnetic shielding film 100 is pressed on the circuit board substrate, it can effectively pierce the adhesive film layer 102, so that the shielding layer 101 is connected to the ground layer of the circuit board substrate, ensuring the conductive performance, allowing the interference charge of the shielding layer to be normally discharged, and realizing the electromagnetic shielding function.
[0040] As one of the optional embodiments, in order to ensure that the shielding layer 101 can smoothly pierce the adhesive film layer 102 when the electromagnetic shielding film 100 is pressed onto the circuit board substrate, the protrusion 104 has a structure with a pointed lower end and a flat upper end, wherein the lower end is the end away from the shielding layer 101, and the upper end is the end close to the shielding layer 101.
[0041] It is worth noting that the protrusion 104 in this embodiment is formed by sputtering or electroplating when the shielding layer 101 has no holes. After the protrusion 104 is formed, holes are opened on the shielding layer 101. The opening position is preferably at a position where the protrusion 104 is less, such as Figure 2 As shown, it is ensured as much as possible that after the hole is opened, the puncture grounding performance of the metal shielding film and the circuit board substrate is not affected when pressed together, thereby avoiding affecting the shielding effectiveness.
[0042] As a preferred solution, the maximum width of the hole 105 is 20 μm to 80 μm; wherein the maximum width is the straight-line distance between two points on the edge of the hole 105 that are farthest apart.
[0043] Specifically, in order to further enhance the air permeability, the maximum width of the hole 105 on the shielding layer 101 is limited in this embodiment. Specifically, the maximum width of the hole 105 on the shielding layer 101 is 30μm to 80μm. For example, the maximum width of the hole 105 can be 20μm, 22μm, 25μm, 27μm, 29μm, 30μm, 35μm, 42μm, 46μm, 53μm, 57μm, 61μm, 69μm, 73μm, 78μm, 80μm, etc. This embodiment does not make any specific limitations here. By limiting the maximum width of the hole 105 on the shielding layer 101 within the above range, it is possible to avoid affecting the water vapor removal effect due to the hole 105 being too small, effectively avoiding the short circuit between the copper lines, and at the same time avoiding affecting the shielding effectiveness of the electromagnetic shielding film 100 due to the hole 105 being too large.
[0044] As a preferred solution, the maximum width of the hole 105 is 40 μm to 60 μm.
[0045] Specifically, the maximum width range of the hole 105 on the shielding layer 101 is further limited in this embodiment, that is, the maximum width of the hole 105 is further 40μm to 60μm, for example, the maximum width of the hole 105 can be 40μm, 42μm, 46μm, 48μm, 51μm, 53μm, 55μm, 57μm, 60μm, etc., which is not specifically limited in this embodiment. Within this range, it is possible to better avoid the water vapor effect caused by the hole 105 being too small, effectively avoid the short circuit between the copper lines, and better avoid the shielding effectiveness of the electromagnetic shielding film 100 caused by the hole 105 being too large.
[0046] As a preferred solution, the ratio of the number of holes 105 with a maximum width of 20μm to 40μm to the total number of holes is 20% to 30%, the ratio of the number of holes 105 with a maximum width of 40μm to 60μm to the total number of holes is 40% to 60%, and the ratio of the number of holes 105 with a maximum width of 60μm to 80μm to the total number of holes is 20% to 30%.
[0047] It is worth noting that the present embodiment limits the proportion of the holes 105 with maximum widths in different ranges. Specifically, the ratio of the number of holes 105 with maximum widths of 20 μm to 40 μm to the total number of holes is 20% to 30%. For example, the ratio may be 20%, 22%, 24%, 25%, 27%, 29%, 30%, etc., which is not specifically limited in the present embodiment. The ratio of the number of holes 105 with maximum widths of 40 μm to 60 μm to the total number of holes is 40% to 60%. 60%, for example, the ratio may be 40%, 42%, 44%, 46%, 47%, 49%, 51%, 53%, 55%, 57%, 59%, 60% and the like, which is not specifically limited in this embodiment; the ratio of the number of holes 105 with a maximum width of 60 μm to 80 μm to the total number of holes is 20% to 30%, for example, the ratio may be 20%, 21%, 23%, 25%, 27%, 29%, 30% and the like, which is not specifically limited in this embodiment. By setting the distribution ratio of holes 105 in different width ranges, it can be ensured that the number of holes 105 with a maximum width of 40μm to 60μm accounts for a larger proportion, which can avoid that there are too many holes 105 with a maximum width of 20μm to 40μm, which may affect the water vapor discharge effect, and better avoid short circuits between copper lines. At the same time, it can avoid that there are too many holes 105 with a maximum width of 60μm to 80μm, which may affect the shielding effectiveness of the electromagnetic shielding film 100.
[0048] As a preferred solution, within each square millimeter, the number N of the protrusions 104 and the number N1 of the holes 105 satisfy the following relationship: 2≤N / N1≤4; wherein N and N1 are both positive integers.
[0049] Specifically, in this embodiment, the number N of protrusions 104 and the number N1 of holes 105 per square millimeter are limited to satisfy the relationship: 2≤N / N1≤4. For example, the ratio of the number N of protrusions 104 to the number N1 of holes 105 per square millimeter can be 2, 2.3, 2.6, 2.9, 3.1, 3.3, 3.5, 3.7, 4, etc., and this embodiment does not make any specific limitation here, so as to ensure that the number N of protrusions 104 is at least twice the number N1 of holes 105, and that a sufficient number of protrusions 104 are present while ensuring a certain air permeability per unit area, so that when the electromagnetic shielding film 100 is pressed onto the circuit board substrate, it can effectively pierce the adhesive film layer 102, so that the shielding layer 101 is connected to the ground layer of the circuit board substrate, thereby ensuring the conductive performance and allowing the interference charge of the shielding layer to be normally discharged, thereby realizing the electromagnetic shielding function. In addition, in order to ensure the puncture performance of the protrusion 104, the present embodiment limits the ratio of the number N of the protrusions 104 to the number N1 of the holes 105 to no more than 4, which can ensure that the number of holes 105 on the shielding layer 101 is not too small, thereby affecting the water vapor dissipation effect and effectively avoiding short circuits between copper lines.
[0050] It is worth noting that in this embodiment, the number N of the protrusions 104 and the number N1 of the holes 105 can be determined by SEM electron microscope observation. Specifically, the surface of one side of the shielding layer 101 is observed by SEM electron microscope, and the number N of the protrusions 104 and the number N1 of the holes 105 per square millimeter on the surface are obtained in the SEM electron microscope image.
[0051] As a preferred solution, the distance between any two adjacent holes 105 is 20 μm to 50 μm; wherein the distance is the shortest straight-line distance between the edges of any two adjacent holes 105 .
[0052] Specifically, the present embodiment limits the spacing between any two adjacent holes 105, that is, the spacing between any two adjacent holes 105 is 20μm to 50μm, for example, the spacing can be 20μm, 22μm, 24μm, 26μm, 28μm, 30μm, 32μm, 34μm, 37μm, 41μm, 43μm, 45μm, 47μm, 50μm, etc., which is not specifically limited in the present embodiment. It is worth noting that if the spacing between any two adjacent holes 105 on the shielding layer 101 is too small, the holes 105 on the shielding layer 101 will be too densely distributed, affecting the shielding effectiveness of the electromagnetic shielding film 100; if the spacing between any two adjacent holes 105 on the shielding layer 101 is too large, the holes 105 on the shielding layer 101 will be too dispersed, affecting the water vapor removal effect, and failing to ensure that each copper circuit etched on the surface of the circuit board substrate has a corresponding hole 105. Therefore, this embodiment can avoid any two adjacent holes 105 being too far apart by limiting the distance between any two adjacent holes 105 within the above-mentioned range, thereby ensuring the water vapor dissipation effect. After the electromagnetic shielding film 100 is pressed onto the circuit board substrate, it can ensure as much as possible that each copper circuit etched on the surface of the circuit board substrate has a corresponding hole 105. At the same time, it can avoid any two adjacent holes 105 being too close to each other, which will affect the shielding effectiveness of the electromagnetic shielding film 100.
[0053] As a preferred solution, the distance between any two adjacent holes 105 is 25 μm to 35 μm.
[0054] Specifically, in order to further improve the water vapor dissipation effect, the present embodiment further limits the spacing between any two adjacent holes 105 to 25μm to 35μm. For example, the spacing may be 25μm, 26μm, 28μm, 30μm, 32μm, 34μm, 35μm, etc. The present embodiment does not make any specific limitation here, so as to better avoid any two adjacent holes 105 being too far apart, further improve the water vapor dissipation effect, better ensure that each copper circuit etched on the surface of the circuit board substrate has a corresponding hole 105, and at the same time better avoid any two adjacent holes 105 being too close to each other, affecting the shielding effectiveness of the electromagnetic shielding film 100.
[0055] As a preferred solution, the density of the protrusions 104 is 200 to 400 per mm. 2 , the residual rate of the shielding layer 101 is 45% to 65%.
[0056] Specifically, in order to further ensure the shielding effectiveness of the shielding layer 101, the density of the protrusions 104 is further limited to 200 to 400 per mm2 in this embodiment. 2 For example, the density of the protrusions 104 may be 200 / mm 2 , 203 pieces / mm 2 , 205 pieces / mm 2 , 208 pieces / mm 2 , 215 pieces / mm 2 , 224 pieces / mm 2 , 229 pieces / mm 2 , 235 pieces / mm 2 , 247 pieces / mm 2 , 250 pieces / mm 2 , 264 pieces / mm 2 , 279 pieces / mm 2 、291pcs / mm 2 、302pcs / mm 2 、315pcs / mm 2 、326pcs / mm 2 、338pcs / mm 2 、351pcs / mm 2 、364pcs / mm 2 、377pcs / mm 2 、383pcs / mm 2 、390pcs / mm 2 , 400 pieces / mm 2Etc., this embodiment is not specifically limited here, so that under the condition of ensuring a certain air permeability within a unit area, it can better ensure that the number of protrusions 104 is sufficient, so that when the electromagnetic shielding film 100 is pressed onto the circuit board substrate, it can more effectively pierce the adhesive film layer 102 to ensure the shielding effectiveness of the shielding layer 101.
[0057] In addition, the present embodiment further limits the residual rate of the shielding layer 101 to 45% to 65%. For example, the residual rate may be 45%, 46%, 48%, 51%, 53%, 57%, 60%, 63%, 65%, etc., and the present embodiment does not make any specific limitations here, so as to better ensure that the volume occupied by the opening of the hole 105 is not too small, that is, the residual rate is less than or equal to 65%, so as to better ensure that the proportion of the hole 105 on the shielding layer 101 is relatively large, and the exhaust efficiency of the circuit board surface is more effectively ensured. At the same time, it can better ensure that the volume occupied by the opening of the hole 105 is not too large, that is, the residual rate is greater than or equal to 45%, so as to more effectively ensure the shielding effectiveness of the shielding layer 101.
[0058] As a preferred solution, the density of the holes 105 is 50 to 150 per mm. 2 .
[0059] Specifically, in order to ensure a good water vapor drainage effect, the present embodiment also limits the density of the holes 105 on the shielding layer 101, that is, the number of holes 105 per unit area. Specifically, the density of the holes 105 on the shielding layer 101 is 50 to 150 per mm. 2 For example, the density of holes 105 may be 50 / mm 2 , 55 pieces / mm 2 、62pcs / mm 2 , 76 pieces / mm 2 、89 pieces / mm 2 , 93 pieces / mm 2 , 105 pieces / mm 2 , 110 pieces / mm 2 , 117 pieces / mm 2 , 120 pieces / mm 2 , 126 pieces / mm 2 , 131 pieces / mm 2 , 137 pieces / mm 2 , 143 pieces / mm 2 , 148 pieces / mm 2 , 150 pieces / mm 2Etc., which are not specifically limited in this embodiment. Since the shielding layer 101 is used to introduce interference charges into the ground layer of the circuit board when in use, by limiting the density of the holes 105 on the shielding layer 101 within the above range, the uniformity of the distribution of the holes 105 on the shielding layer 101 can be ensured, so that after the electromagnetic shielding film 100 is pressed onto the circuit board substrate, it is ensured as much as possible that each copper circuit etched on the surface of the circuit board substrate has a corresponding hole 105, thereby enhancing the air permeability and improving the water vapor dissipation effect. At the same time, it can avoid that the number of holes 105 per unit area is too large to affect the shielding effectiveness of the electromagnetic shielding film 100.
[0060] As a preferred solution, the density of the holes 105 is 70 to 120 per mm. 2 .
[0061] Specifically, this embodiment further limits the density range of the holes 105 on the shielding layer 101, that is, the density of the holes 105 is further 70 to 120 per mm. 2 For example, the density of holes 105 may be 70 / mm 2 , 71 pieces / mm 2 , 76 pieces / mm 2 , 79 pieces / mm 2 , 85 pieces / mm 2 , 90 pieces / mm 2 , 93 pieces / mm 2 , 96 pieces / mm 2 , 100 pieces / mm 2 , 102 pieces / mm 2 , 106 pieces / mm 2 , 109 pieces / mm 2 , 113 pieces / mm 2 , 115 pieces / mm 2 , 117 pieces / mm 2 , 120 pieces / mm 2 Within this range, it is possible to better avoid the water vapor removal effect caused by too few holes 105 per unit area on the shielding layer 101, enhance the air permeability, and at the same time, it is possible to better avoid the shielding effectiveness of the electromagnetic shielding film 100 caused by too many holes 105 per unit area on the shielding layer 101.
[0062] As a preferred solution, at least three holes 105 are staggered in each square millimeter.
[0063] Specifically, Figure 3 and Figure 4As shown, the present embodiment limits the staggered arrangement of at least 3 holes 105 per square millimeter on the shielding layer 101, so as to ensure that the distribution of the holes 105 per square millimeter is relatively dispersed, and the shielding effectiveness of the electromagnetic shielding film 100 will not be affected by the overly dense distribution. At the same time, the relatively dispersed distribution of the holes 105 per square millimeter can ensure the uniformity of the distribution of the holes 105. After the electromagnetic shielding film 100 is pressed on the circuit board substrate, it can ensure as much as possible that each copper circuit etched on the surface of the circuit board substrate has a corresponding hole 105, thereby enhancing the air permeability and improving the water vapor removal effect. It is worth noting that in the present embodiment, at least 3 holes 105 per square millimeter are staggered, that is, there can be 3 holes 105 per square millimeter, or there can be more than 3 holes 105, such as 6, 8, 10, 14, 25, 36, etc., and all holes 105 per square millimeter can also be staggered, which is not specifically limited in the present embodiment.
[0064] In one of the optional embodiments, the holes 105 on the shielding layer 101 include blind holes and / or through holes, that is, the holes 105 on the shielding layer 101 may all be blind holes, may all be through holes, or may include both blind holes and through holes. Preferably, the holes 105 on the shielding layer 101 are all set as through holes. If the holes 105 on the shielding layer 101 include blind holes, the bottom surface of the blind holes is made of a material with low density, such as copper, which can be achieved by sputtering a thin layer of copper on the blind holes. Since the bottom surface of the blind holes has a certain degree of sparseness, the water vapor accumulated on the surface of the circuit board can be discharged through the bottom surface of the blind holes. Preferably, the sealing surface of the blind holes is arranged on the side away from the circuit board substrate, and the opening end thereof is arranged on the side close to the circuit board substrate, so as to effectively enhance the water vapor discharge effect.
[0065] As a preferred solution, the hole 105 includes a regular shape and / or an irregular shape.
[0066] It is worth noting that the present embodiment does not specifically limit the shape of the hole 105 on the shielding layer 101, and the shape of the hole 105 may include different regular shapes, different irregular shapes, or different regular shapes and irregular shapes at the same time. Further, the shape of the hole 105 on the shielding layer 101 is preferably a regular shape, so as to facilitate the production of the electromagnetic shielding film 100, and the regular geometric shape facilitates the measurement of the maximum width of the hole 105 and the hole spacing.
[0067] As a preferred solution, the shape of the hole 105 includes at least one of a circle, an ellipse, a rectangle, a rhombus, a triangle, and a regular polygon.
[0068] Specifically, the present embodiment limits the shape of the hole 105 to a regular geometric figure, thereby facilitating the production of the electromagnetic shielding film 100, and the regular geometric figure facilitates the measurement of the maximum width and the hole spacing of the hole 105. It is worth noting that the shape of the hole 105 in the present embodiment can be one of a circle, an ellipse, a rectangle, a rhombus, a triangle, and a regular polygon, such as Figure 5 As shown, the shapes of the holes 105 on the shielding layer 101 are all circular, and may also include two or more of these geometric shapes. For example, the shapes of the holes 105 on the shielding layer 101 may all be circular, elliptical, rectangular, rhombus, triangular or regular polygonal, or may include circular and elliptical, or include rectangular, rhombus and circular, or include circular, triangle and regular polygon, or include circular, elliptical, rectangular, rhombus, triangle and regular polygon at the same time. This embodiment will not be repeated here.
[0069] See also Figure 6 As a preferred embodiment, it further includes a film layer 102, wherein the film layer 102 and the shielding layer 101 are stacked, the protrusion 104 is arranged on one side of the shielding layer 101 close to the film layer 102, and the film layer 102 includes an adhesive layer that does not contain conductive particles.
[0070] Specifically, the adhesive film layer 102 in this embodiment is arranged between the shielding layer 101 and the circuit board substrate. The material of the adhesive film layer 102 is generally a polymer matrix, including polyethylene terephthalate, polyethylene, polyvinyl alcohol, cycloolefin copolymer, etc. These materials have good flexibility, transparency and processing performance, and are ideal substrates for preparing flexible transparent electromagnetic shielding film 100.
[0071] In order to ensure that the electromagnetic shielding film 100 can be tightly bonded to the circuit board substrate after being pressed together, the film layer 102 further includes an adhesive layer that does not contain conductive particles. The protrusion 104 is arranged on the side surface of the shielding layer 101 close to the film layer 102. When the electromagnetic shielding film 100 is pressed together with the circuit board substrate, the protrusion 104 on the shielding layer 101 can pierce the film layer 102 so that the shielding layer 101 can be connected to the ground layer of the circuit board substrate, thereby ensuring that the interference charge is normally discharged and realizing the electromagnetic shielding function.
[0072] As one of the optional embodiments, the protrusion 104 can extend into the adhesive film layer 102, so that the protrusion 104 can more easily pierce the adhesive film layer 102 during the process of laminating the electromagnetic shielding film 100 with the circuit board substrate. Alternatively, the protrusion 104 can also pierce the adhesive film layer 102, so that during the process of laminating the electromagnetic shielding film 100 with the circuit board substrate, the protrusion 104 can directly insert into the ground layer of the circuit board substrate. Of course, the protrusion 104 can also not extend into the adhesive film layer 102 but be covered by the adhesive film layer 102.
[0073] It is worth noting that the adhesive layer included in the film layer 102 in this embodiment is achieved by adding an adhesive to the film layer 102. Commonly used adhesives include silicone, silicone fluoride, EPDM (Ethylene Propylene Diene Monomer), fluorocarbon-silicon fluoride, etc. These adhesives have good adhesion and stability.
[0074] See also Figure 7 As a preferred solution, it further includes an insulating layer 103 , and the insulating layer 103 is disposed on a surface of the shielding layer 101 away from the adhesive film layer 102 .
[0075] It is worth mentioning that, since the insulating layer 103 has an isolation effect, arranging the insulating layer 103 on one side surface of the shielding layer 101 is helpful to ensure the shielding effectiveness of the shielding layer 101; in addition, the insulating layer 103 also has a protective effect to ensure that the shielding layer 101 is not scratched or damaged during use, thereby helping to maintain the high shielding effectiveness of the shielding layer 101.
[0076] The insulating layer 103 in this embodiment includes a PPS film layer, a PEN film layer, a polyester film layer, a polyimide film layer, a film layer formed after epoxy resin ink is cured, a film layer formed after polyurethane ink is cured, a film layer formed after modified acrylic resin is cured, or a film layer formed after polyimide resin is cured, etc. This embodiment is not specifically limited here.
[0077] A second aspect of the embodiments of the present invention provides a circuit board, comprising a circuit board substrate and the electromagnetic shielding film 100 as described in any embodiment of the first aspect; the electromagnetic shielding film 100 is pressed together with the circuit board substrate.
[0078] It is worth noting that the electromagnetic shielding film 100 in this embodiment is pressed against the circuit board substrate, and the ground layer of the circuit board substrate is connected to the shielding layer 101 in the electromagnetic shielding film 100, thereby ensuring that the interference charges are normally extracted.
[0079] The electromagnetic shielding film 100 and the circuit board provided by the embodiment of the present invention have the beneficial effects of at least one of the following:
[0080] (1) By opening a plurality of holes 105 on the shielding layer 101, the air permeability of the circuit board can be increased after the electromagnetic shielding film 100 is pressed onto the circuit board substrate, so that water vapor on the surface of the circuit board can be discharged through the holes 105 on the shielding layer 101, thereby reducing the moisture accumulated on the surface of the circuit board and significantly reducing the probability of a short circuit on the circuit board.
[0081] (2) By limiting the residual rate of the shielding layer 101 , the exhaust efficiency of the circuit board surface can be guaranteed, while at the same time ensuring that the volume occupied by the opening of the hole 105 is not too large, thereby ensuring the shielding effectiveness of the shielding layer 101 .
[0082] (3) By limiting the density of the protrusions 104 on one side surface of the shielding layer 101, it is ensured that there are a sufficient number of protrusions 104 per unit area, so that when the electromagnetic shielding film 100 is pressed onto the circuit board substrate, it can effectively pierce the adhesive film layer 102, so that the shielding layer 101 is connected to the ground layer of the circuit board substrate, ensuring the conductive performance, allowing the interference charge of the shielding layer to be normally discharged, and realizing the electromagnetic shielding function.
[0083] In order to demonstrate the beneficial effects of the electromagnetic shielding film and circuit board provided by the embodiments of the present invention, several embodiments and comparative examples are described below.
[0084] Example 1
[0085] An electromagnetic shielding film comprises a shielding layer, a plurality of holes are opened on the shielding layer, and a plurality of protrusions are arranged on one side surface of the shielding layer, and the density of the protrusions is 230 to 320 per mm 2 , the residual rate of the shielding layer is 77%. The maximum width of the holes on the shielding layer is 32μm to 66μm, among which the ratio of the number of holes with a maximum width of 30μm to 40μm to the total number of holes is 22%, the ratio of the number of holes with a maximum width of 40μm to 60μm to the total number of holes is 51%, and the ratio of the number of holes with a maximum width of 60μm to 80μm to the total number of holes is 27%. In each square millimeter, the ratio of the number of protrusions N to the number of holes N1 is 2.15 to 3.76, satisfying the relationship: 2≤N / N1≤4, and the density of holes is 85 to 107 / mm 2 , the thickness of the shielding layer is 2μm.
[0086] Example 2
[0087] An electromagnetic shielding film comprises a shielding layer, a plurality of holes are opened on the shielding layer, and a plurality of protrusions are arranged on one side surface of the shielding layer, and the density of the protrusions is 160 to 272 per mm 2 , the residual rate of the shielding layer is 60%. The maximum width of the holes on the shielding layer is 53μm to 65μm. In each square millimeter, the ratio of the number of protrusions N to the number of holes N1 is about 2.1 to 4, satisfying the relationship: 2≤N / N1≤4, and the density of the holes is 68 to 78 / mm 2 , the thickness of the shielding layer is 1.5μm.
[0088] Example 3
[0089] An electromagnetic shielding film comprises a shielding layer, a plurality of holes are formed on the shielding layer, and a plurality of protrusions are formed on one side of the shielding layer, wherein the density of the protrusions is 240 to 350 per mm 2 , the residual rate of the shielding layer is 70%. The maximum width of the holes on the shielding layer is 36μm to 68μm, among which the ratio of the number of holes with a maximum width of 30μm to 40μm to the total number of holes is 26%, the ratio of the number of holes with a maximum width of 40μm to 60μm to the total number of holes is 53%, and the ratio of the number of holes with a maximum width of 60μm to 80μm to the total number of holes is 21%. In each square millimeter, the ratio of the number of protrusions N to the number of holes N1 is 2 to 3.5, satisfying the relationship: 2≤N / N1≤4, and the density of holes is 100 to 120 / mm 2 , the thickness of the shielding layer is 2.5μm.
[0090] Example 4
[0091] An electromagnetic shielding film comprises a shielding layer, a plurality of holes are opened on the shielding layer, and a plurality of protrusions are arranged on one side surface of the shielding layer, and the density of the protrusions is 350 to 480 per mm 2 , the residual rate of the shielding layer is 53%. The maximum width of the holes on the shielding layer is 66μm to 75μm. In each square millimeter, the ratio of the number of protrusions N to the number of holes N1 is 2.5 to 4, satisfying the relationship: 2≤N / N1≤4, and the density of the holes is 120 to 140 / mm 2 The thickness of the shielding layer is 2.5 μm. The distance between any two adjacent holes is 21 μm to 32 μm, and at least three holes are staggered in each square millimeter.
[0092] Example 5
[0093] An electromagnetic shielding film includes a shielding layer, a film layer and an insulating layer. The shielding layer is provided with a plurality of holes, and a plurality of protrusions are provided on one side of the shielding layer. The film layer and the shielding layer are stacked, and the protrusions are provided on one side of the shielding layer close to the film layer. The film layer includes an adhesive layer that does not contain conductive particles, and the insulating layer is provided on one side of the shielding layer away from the film layer. The density of the protrusions is 280 to 363 per mm 2 , the residual rate of the shielding layer is 47%. The maximum width of the holes on the shielding layer is 56μm to 78μm. In each square millimeter, the ratio of the number of protrusions N to the number of holes N1 is 2.09 to 3, satisfying the relationship: 2≤N / N1≤4, and the density of the holes is 121 to 135 / mm 2 The thickness of the shielding layer is 2 μm. The distance between any two adjacent holes is 37 μm to 42 μm, and at least three holes are staggered in each square millimeter.
[0094] Comparative Example 1
[0095] An electromagnetic shielding film comprises a shielding layer, the thickness of the shielding layer is 2 μm, and no holes are opened on the shielding layer.
[0096] Comparative Example 2
[0097] An electromagnetic shielding film comprises a shielding layer, the thickness of the shielding layer is 3 μm, a plurality of holes are opened on the shielding layer, and a plurality of protrusions are arranged on one side surface of the shielding layer, and the density of the protrusions is 643 to 721 per mm 2 , the residual rate of the shielding layer is 94%. The maximum width of the holes on the shielding layer is 12μm to 23μm. In each square millimeter, the ratio of the number of protrusions N to the number of holes N1 is 16.01 to 28.84, which does not satisfy the relationship: 2≤N / N1≤4, and the density of the holes is 25 to 40 / mm 2 The distance between any two adjacent holes is 83 μm to 107 μm.
[0098] Comparative Example 3
[0099] An electromagnetic shielding film comprises a shielding layer, the thickness of the shielding layer is 3 μm, a plurality of holes are opened on the shielding layer, and a plurality of protrusions are arranged on one side of the surface of the shielding layer, and the density of the protrusions is 46 to 83 per mm 2 , the residual rate of the shielding layer is 32%. The maximum width of the holes on the shielding layer is 82μm to 87μm. In each square millimeter, the ratio of the number of protrusions N to the number of holes N1 is 0.28 to 0.53, which does not satisfy the relationship: 2≤N / N1≤4, and the density of the holes is 156 to 167 / mm 2 The distance between any two adjacent holes is 7 μm to 16 μm.
[0100] The above-mentioned embodiment and comparative example are used to measure the shielding effectiveness and detect whether a short circuit occurs during the use of the circuit board according to the GB / T-30142-2013 test standard. The pressing method for covering the electromagnetic shielding film on the circuit board substrate is: at 185°C, 120kg / cm 2 The electromagnetic shielding film was pressed onto the circuit board substrate with a pressure of 3 minutes. The test environment of the circuit board after pressing was as follows: the test temperature was 75°C, the humidity was 90% RH, the SIR test voltage was 50V, the test time was 24 hours, and the judgment standard for circuit board short circuit was: insulation resistance <100MΩ was considered to be a short circuit. The test results are shown in Table 1 below.
[0101] Table 1 Shielding effectiveness of electromagnetic shielding film and short circuit situation of circuit board
[0102]
[0103] As can be seen from Table 1 above, since the shielding layer in Examples 1 to 5 is provided with a plurality of holes, and a plurality of protrusions are provided on one side of the surface of the shielding layer, the density of the protrusions, the residual rate of the shielding layer, the density of the holes, the maximum width, and the spacing between any two adjacent holes are limited within the ranges described in the embodiments of the present invention, and within each square millimeter, the number of protrusions N and the number of holes N1 both satisfy the relationship: 2≤N / N1≤4, so that the air permeability of the circuit board can be increased after the electromagnetic shielding film is pressed onto the circuit board substrate, so that the water vapor on the surface of the circuit board can be discharged through the holes on the shielding layer, thereby reducing the moisture accumulated on the surface of the circuit board, significantly reducing the probability of short circuits on the circuit board, and ensuring the shielding effectiveness of the electromagnetic shielding film (generally, shielding effectiveness is considered good when it is around 60dB).
[0104] In Comparative Example 1, since no holes are formed on the shielding layer, water vapor gradually accumulates on the surface of the circuit board during use, causing a short circuit in the etched copper circuits on the circuit board.
[0105] In Comparative Example 2, a number of holes are provided on the shielding layer, but the density and maximum width of the holes are too small, and the distance between any two adjacent holes is too large. In addition, the residual rate of the shielding layer and the density of the protrusions are too large. In each square millimeter, the ratio of the number of protrusions N to the number of holes N1 is too large, and does not satisfy the relationship: 2≤N / N1≤4. Therefore, the water vapor separation effect is poor. Although the shielding performance is good, short circuits still occur in the circuit board during use.
[0106] In Comparative Example 3, a number of holes are opened on the shielding layer, but the density and maximum width of the holes are too large, and the distance between any two adjacent holes is too small. In addition, the residual rate of the shielding layer and the density of the protrusions are too small. In each square millimeter, the ratio of the number of protrusions N to the number of holes N1 is too small, and does not satisfy the relationship: 2≤N / N1≤4. Although the circuit board did not have a short circuit during use, the residual rate was too low and the number of protrusions per unit area was insufficient, which resulted in the inability to effectively pierce the adhesive film layer during lamination, greatly affecting the shielding effectiveness of the electromagnetic shielding film.
[0107] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.
Claims
1. An electromagnetic shielding film, characterized in that: The invention comprises a shielding layer, wherein a plurality of holes are formed on the shielding layer, and a plurality of protrusions are formed on one side of the surface of the shielding layer, and the density of the protrusions is 100 to 600 per mm 2 The residual rate of the shielding layer is 40% to 80%; wherein the residual rate is the weight ratio of the shielding layer after the opening to the shielding layer before the opening.
2. The electromagnetic shielding film according to claim 1, wherein The maximum width of the hole is 20 μm to 80 μm, wherein the maximum width is a straight-line distance between two points on the edge of the hole that are farthest apart.
3. The electromagnetic shielding film according to claim 2, wherein: The maximum width of the pores is 40 μm to 60 μm.
4. The electromagnetic shielding film according to claim 2, wherein: The ratio of the number of holes with a maximum width of 20 μm to 40 μm to the total number of holes is 20% to 30%, the ratio of the number of holes with a maximum width of 40 μm to 60 μm to the total number of holes is 40% to 60%, and the ratio of the number of holes with a maximum width of 60 μm to 80 μm to the total number of holes is 20% to 30%.
5. The electromagnetic shielding film according to claim 1, wherein In each square millimeter, the number N of the protrusions and the number N1 of the holes satisfy the following relationship: 2≤N / N1≤4; wherein N and N1 are both positive integers.
6. The electromagnetic shielding film according to claim 1, wherein The distance between any two adjacent holes is 20 μm to 50 μm; wherein the distance is the shortest straight-line distance between the edges of any two adjacent holes.
7. The electromagnetic shielding film according to claim 1, wherein The density of the protrusions is 200 to 400 per mm 2 The residual rate of the shielding layer is 45% to 65%.
8. The electromagnetic shielding film according to any one of claims 1 to 7, characterized in that: The density of the holes is 50 to 150 per mm 2 .
9. The electromagnetic shielding film according to claim 8, wherein The density of the holes is 70 to 120 per mm 2 .
10. The electromagnetic shielding film according to any one of claims 9, characterized in that At least three holes are staggered in each square millimeter.
11. The electromagnetic shielding film according to any one of claims 1 to 7, characterized in that: The holes include regular shapes and / or irregular shapes.
12. The electromagnetic shielding film according to any one of claims 11, characterized in that: The shape of the hole includes at least one of a circle, an ellipse, a rectangle, a rhombus, a triangle, and a regular polygon.
13. The electromagnetic shielding film according to any one of claims 1 to 7, characterized in that: It also includes a film layer, which is stacked with the shielding layer. The protrusion is arranged on a side surface of the shielding layer close to the film layer, and the film layer includes an adhesive layer without conductive particles.
14. The electromagnetic shielding film according to claim 13, wherein It also includes an insulating layer, which is arranged on a surface of the shielding layer on one side away from the adhesive film layer.
15. A circuit board, characterized in that: It comprises a circuit board substrate and the electromagnetic shielding film as claimed in any one of claims 1 to 14; the electromagnetic shielding film is pressed together with the circuit board substrate.
Citation Information
Cited By
Composite metal foil, metal-clad laminated board and circuit board
CN119724780A