Technical method for preparing high-performance perovskite solar cell
By using PbTiO3 nanoparticles as the nucleation center in perovskite films, combined with hydrothermal method and spin coating technology, the defect problems in perovskite films are solved, and the preparation of perovskite solar cell devices with high efficiency and stability is achieved. .
Patent Information
- Application Number
- CN202410714445.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-11-12
Smart Images

Figure CN118946169A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photovoltaic device preparation technology, and specifically refers to a technical method for preparing high-performance perovskite solar cells. Background Art
[0002] Perovskite materials have become a new technology that has attracted much attention in the solar industry due to their excellent photoelectric properties and relatively low manufacturing costs. To date, the photoelectric conversion efficiency of perovskite solar cells has continued to increase, exceeding 26%, demonstrating its potential in the photovoltaic field. However, compared with the theoretical limit efficiency, the efficiency of existing perovskite devices still has a lot of room for improvement. As the core material of perovskite battery devices, the film quality of the perovskite absorber layer itself is crucial to the performance of the device. High-quality perovskite films are the key factor in achieving high-performance perovskite solar cell devices. However, the inevitable defects in perovskite films prepared by the solution method, such as grain boundaries, holes, various uncoordinated bonds, etc., restrict the improvement of the photoelectric conversion efficiency of perovskite devices. Not only that, the existence of these problems will continue to cause the deterioration of device performance.
[0003] In order to solve the above problems, researchers have developed many strategies to obtain high-quality perovskite films with large grains and low defect density, such as additive engineering, interface passivation, and precursor engineering. Additive engineering is considered to be a common strategy for regulating crystal growth and passivating defects. At present, most additives can only be used to regulate perovskite crystal growth or passivate defects. Therefore, it is worth looking forward to optimizing the quality of perovskite films from the perspective of simultaneously increasing grain size and passivating film defects. Summary of the invention
[0004] The technical problem to be solved by the present invention is that the prepared perovskite film has defects such as grain boundaries, holes, various uncoordinated bonds and the like.
[0005] In order to solve the above technical problems, the technical solution provided by the present invention is: a technical method for preparing a high-performance perovskite solar cell, which comprises the following steps:
[0006] a. Spin-coat a layer of tin dioxide on the cleaned and ozone-treated indium tin oxide (ITO) conductive glass, and place the spin-coated tin dioxide on a hot plate for annealing;
[0007] b. Lead titanate (PbTiO3) nanoparticles were prepared by a hydrothermal method, and the prepared particles were ground by a ball mill to obtain spherical nanoparticles;
[0008] c. The above-mentioned PbTiO3 nanoparticles are dispersed in a solvent to obtain a PbTiO3 nanodispersion;
[0009] d. Prepare a perovskite precursor solution, take an appropriate volume of the solution in step c above and add it to the prepared perovskite precursor solution to obtain a perovskite precursor solution containing PbTiO3;
[0010] e. drop-coating the precursor solution of step d on the surface of the tin dioxide layer obtained in step a to obtain a perovskite layer;
[0011] f. Spin-coating a hole transport layer on the surface of the perovskite layer obtained in step e / tin dioxide in step a;
[0012] g. Evaporating an electrode on the surface of the perovskite / tin dioxide / hole transport layer obtained in step f.
[0013] Furthermore, the tin dioxide layer in step a is a tin dioxide precursor solution prepared by diluting tin dioxide colloid, the mass fraction of the tin dioxide precursor solution is 3%-15wt%, the ozone treatment time in step a is 30min, the spin coating process is 5000rpm, the spin coating time is 20s, the annealing temperature is 100°C, and the annealing time is 60min.
[0014] Furthermore, the particle size of the PbTiO3 nanoparticles after ball milling in step b is 10-50nm.
[0015] Furthermore, there are three types of solvents in step c, including N-methylpyrrolidone (NMP) solvent, dimethylformamide (DMF) solvent and a mixed solvent of NMP and DMF.
[0016] Furthermore, the concentration of the PbTiO3 nano-dispersion obtained in step c is 1-10 mg / mL.
[0017] Furthermore, the volume of the solution of step c used in step d is 10-100 uL.
[0018] Furthermore, the concentration of the perovskite precursor solution in step d is 1.0-1.6 mol / L, and the perovskite precursor includes methylammonium lead triiodide (MAPbI3), formamidine lead triiodide (FAPbI3) and methylammonium formamidine cesium mixed lead iodide and bromide (Csy(FA1-xMAx)yPbI3-xBrx), where 0≤x≤1, 0≤y≤0.15.
[0019] Furthermore, the preparation step of the hole transport layer solution is as follows: 72.25 mg of 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenylamino]-9,9'-spirobifluorene (Spiro-OMeTAD), 17.5 μL of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 28.75 μL of 4-tert-butylpyridine (TBP) are weighed, 1 mL of chlorobenzene (CB) is added to the mixture, and the mixture is stirred for 20 h.
[0020] Furthermore, the spin coating process in step f is 3000 rpm, the spin coating time is 35 s; and the mixture is allowed to stand in dry air for 24 hours.
[0021] Furthermore, the electrode thickness in step g is 100 nm, and the material is metal silver or gold.
[0022] The present invention has the following advantages: PbTiO3 nanoparticles are used as the nucleation center of perovskite crystals, which accelerates the nucleation rate of perovskite crystals, helps to form large-sized grains, improves the crystallization performance of the film, and reduces the internal defect density of the film. Through reasonable process control, the preparation of high-efficiency perovskite solar cell devices is achieved. The perovskite solar cell device prepared by the method has significantly improved performance and good stability compared with the comparative device, providing an effective strategy for preparing high-performance perovskite solar cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a schematic diagram of the structure of the perovskite solar cell prepared in Example 1.
[0024] Figure 2 is a scanning electron microscope image of the PbTiO3 nanoparticles prepared in Example 1.
[0025] Figure 3 It is a scanning electron microscope image of the surface of the control sample prepared in Example 1 and the perovskite film containing PbTiO3 nanoparticles.
[0026] Figure 4 It is a current density-voltage curve diagram of the control sample prepared in Example 1 and the perovskite solar cell device containing PbTiO3 nanoparticles under a light intensity of AM1.5G.
[0027] Figure 5 The detailed optoelectronic performance parameters of the current density-voltage curve of the control sample prepared in Example 1 and the perovskite solar cell device containing PbTiO3 nanoparticles under the light intensity of AM1.5G. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below in conjunction with the embodiments.
[0029] Example 1
[0030] A technical method for preparing high-performance perovskite solar cells, the specific steps are as follows:
[0031] a. Dilute commercial tin dioxide colloid into a tin dioxide precursor solution with a mass fraction of 5%, and spin-coat a layer of tin dioxide on the cleaned and ozone-treated indium tin oxide (ITO) conductive glass surface. The ozone treatment time is 30 minutes. The spin coating process is 5000 rpm and the spin coating time is 20 seconds. Then, the spin-coated tin dioxide is placed on a heating plate for annealing at a temperature of 100°C and an annealing time of 60 minutes.
[0032] b. The PbTiO3 nanoparticles prepared by a hydrothermal method were ball-milled into uniform particles with a particle size of 10-30 nm.
[0033] c. The PbTiO3 nanoparticles obtained in step b are dispersed in NMP solution to obtain a dispersion with a concentration of 5 mg / mL.
[0034] d. Mix 157 mg of methylammonium iodide (MAI) and 461 mg of lead iodide (PbI2) powder, and dissolve them in a mixed solution of 630 μL of dimethylformamide (DMF) and 70 μL of dimethyl sulfoxide (DMSO); at the same time, add 300 ul of the PbTiO3 dispersion prepared in step c above, and stir for 12 hours to obtain a perovskite precursor solution containing about 1.4 mol / L PbTiO3.
[0035] e. The tin dioxide layer obtained in step a is treated with ozone for 15 minutes; in an air environment, a perovskite layer is spin-coated on the surface of the tin dioxide, and the spin coating process adopts a single-step spin coating method, a spin coating speed of 5000 rpm, a spin coating time of 30 seconds, and an acceleration of 1000 rpm. When the spin coating time is 6 seconds, 500 μL of ethyl acetate is added as an anti-solvent to obtain a perovskite wet film; and then the perovskite wet film is placed on a heating plate for annealing at a temperature of 150° C. for 10 minutes.
[0036] f. Add 1 mL of chlorobenzene (CB) to a mixture of 72.25 mg of 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenylamino]-9,9'-spirobifluorene (Spiro-OMeTAD), 17.5 μL of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 28.75 μL of 4-tert-butylpyridine (TBP), and stir for 20 h to obtain a hole transport layer solution.
[0037] g. Spin-coat a hole transport layer on the surface of the tin dioxide / perovskite layer obtained in step e at a spin coating process of 3000 rpm for 35 s; and allow to stand in dry air for 24 h.
[0038] h. A silver electrode is evaporated on the surface of the tin dioxide / potassium dihydrogen phosphate / perovskite / hole transport layer obtained in step g, and the thickness of the silver electrode is 100 nm.
[0039] The present invention adopts PbTiO3 nanoparticles as the nucleation center of perovskite crystals, which accelerates the nucleation rate of perovskite crystals, helps to form large-sized grains, improves the crystallization performance of the film, and reduces the internal defect density of the film, thereby enabling the preparation of high-efficiency perovskite solar cell devices with significantly improved performance and good stability.
[0040] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A technical method for preparing high-performance perovskite solar cells, It is characterized in that It includes the following steps: a. Spin-coat a layer of tin dioxide on the cleaned and ozone-treated indium tin oxide (ITO) conductive glass, and place the spin-coated tin dioxide on a hot plate for annealing; b. Lead titanate (PbTiO3) nanoparticles were prepared by a hydrothermal method, and the prepared particles were ground by a ball mill to obtain spherical nanoparticles; c. The above-mentioned PbTiO3 nanoparticles are dispersed in a solvent to obtain a PbTiO3 nanodispersion; d. Prepare a perovskite precursor solution, take an appropriate volume of the solution in step c above and add it to the prepared perovskite precursor solution to obtain a perovskite precursor solution containing PbTiO3; e. drop-coating the precursor solution of step d on the surface of the tin dioxide layer obtained in step a to obtain a perovskite layer; f. Spin-coating a hole transport layer on the surface of the perovskite layer obtained in step e / tin dioxide in step a; g. Evaporating an electrode on the surface of the perovskite / tin dioxide / hole transport layer obtained in step f.
2. A technical method for preparing a high-performance perovskite solar cell according to claim 1, Features: The tin dioxide layer in step a is a tin dioxide precursor solution prepared by diluting tin dioxide colloid, the mass fraction of the tin dioxide precursor solution is 3%-15wt%, the ozone treatment time in step a is 30min, the spin coating process is 5000rpm, the spin coating time is 20s, the annealing temperature is 100°C, and the annealing time is 60min.
3. A technical method for preparing a high-performance perovskite solar cell according to claim 1, Features: The particle size of the PbTiO3 nanoparticles in the step b is 10-50nm.
4. A technical method for preparing a high-performance perovskite solar cell according to claim 1, Features: There are three types of solvents in step c, including N-methylpyrrolidone (NMP) solvent, dimethylformamide (DMF) solvent and a mixed solvent of NMP and DMF.
5. A technical method for preparing a high-performance perovskite solar cell according to claim 1, Features: The concentration of the PbTiO3 nano-dispersion obtained in step c is 1-10 mg / mL.
6. A technical method for preparing a high-performance perovskite solar cell according to claim 1, Features: The volume of the solution of step c used in step d is 10-100 uL.
7. A technical method for preparing a high-performance perovskite solar cell according to claim 1, Features: The concentration of the perovskite precursor solution in step d is 1.0-1.6 mol / L, and the perovskite precursor includes methylammonium lead triiodide (MAPbI3), formamidine lead triiodide (FAPbI3) and methylammonium formamidine cesium mixed lead iodide and bromide (Csy(FA1-xMAx)yPbI3-xBrx), where 0≤x≤1, 0≤y≤0.
15.
8. A technical method for preparing a high-performance perovskite solar cell according to claim 1, Features: The preparation steps of the hole transport layer solution are as follows: 72.25 mg of 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenylamino]-9,9'-spirobifluorene (Spiro-OMeTAD), 17.5 μL of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 28.75 μL of 4-tert-butylpyridine (TBP) are weighed, and 1 mL of chlorobenzene (CB) is added to the mixture, and stirred for 20 hours.
9. The method for preparing a high-performance perovskite solar cell according to claim 1, Features: The spin coating process in step f is 3000 rpm, the spin coating time is 35 s; and the mixture is allowed to stand in dry air for 24 h.
10. A technical method for preparing a high-performance perovskite solar cell according to claim 1, Features: The electrode thickness in step g is 100 nm and is made of metal silver or gold.