OTS gating material, OTS gating unit, preparation method of OTS gating material and preparation method of OTS gating unit, and phase change memory
By incorporating Sb elements into the OTS gate material and forming nano grains through annealing, the problem of high threshold voltage during the initial ignition of the OTS gate material is solved, the risk of Vth drift is reduced, and the device safety and reading window are improved. stability.
Patent Information
- Application Number
- CN202410999175.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
The threshold voltage of the OTS gate material during the initial ignition is higher than the threshold voltage during subsequent operation, resulting in Vth drift, affecting the stability of the memory read window and increasing the risk of device damage.
A certain proportion of Sb elements are incorporated into the OTS gate material to reduce the threshold voltage of the first ignition, making it equal to the threshold voltage during subsequent operation, and nano-grains are formed by annealing to reduce the opening voltage and disappear after annealing , stabilizes the device state.
It effectively reduces the risk of Vth drift phenomenon, improves the safety and reliability of the OTS gate unit, reduces the impact of excessively high initial ignition threshold voltage on the device, and improves the stability of the memory read window.
Smart Images

Figure CN118946250A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of microelectronic technology, and in particular relates to an OTS gating material, an OTS gating unit and a preparation method thereof, and a phase change memory. Background Art
[0002] Binary threshold transition (OTS) materials based on sulfide compounds can be used as a gating switch in phase change memory. The principle of OTS gating switch is as follows: the switch of the gating device is controlled by an electrical signal. When the voltage applied to the gating device is higher than its threshold voltage (Vth), the OTS material will change from a high resistance state to a low resistance state, and the device is in the on state; when the electrical signal is removed, the OTS material will return to a high resistance state, and the device is in the off state. Usually, when the OTS that has not been operated undergoes the initial threshold transition, an initial ignition operation (First fire) is required, which is manifested as the threshold voltage of the initial opening being significantly higher than the threshold voltage of the subsequent opening. After the voltage is removed, as time passes, the Vth of the device will gradually recover and increase toward the state before the First fire. This phenomenon is called Vth drift. This phenomenon will affect the stability of the memory read window and even cause the device to fail. In addition, an excessively high threshold voltage of the initial ignition will impact the OTS device and increase the risk of damage.
[0003] Therefore, how to reduce the Vth drift phenomenon and reduce the impact of the excessively high initial ignition threshold voltage on the OTS device, and improve the safety and reliability of the OTS device, is a technical problem that needs to be solved urgently. Summary of the invention
[0004] In view of the deficiencies of the prior art, the object of the present invention is to provide an OTS gating material, an OTS gating unit and a preparation method thereof and a phase change memory. The present invention, by doping a certain proportion of Sb elements into the OTS gating material, can effectively reduce the threshold voltage of the first ignition of the OTS gating material, and make the threshold voltage of the first ignition equal to the threshold voltage during subsequent operation, which not only reduces the risk of Vth drift, but also reduces the impact of the excessively high threshold voltage of the first ignition on the OTS gating unit, thereby improving the safety and reliability of the OTS gating unit.
[0005] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides an OTS gating material, wherein the chemical formula of the OTS gating material is As x Se y Sb m , where 0.15≤x≤0.25, 0.65≤y<0.75, and 0<m≤0.15.
[0007] The present invention adds a certain proportion of Sb element into the OTS gating material, which can effectively reduce the threshold voltage of the first ignition of the OTS gating material, and make the threshold voltage of the first ignition equal to the threshold voltage during subsequent operation, which not only reduces the impact of the excessively high threshold voltage of the first ignition on the OTS gating unit, improves the safety and reliability of the OTS gating unit, but also reduces the risk of Vth drift phenomenon.
[0008] In the present invention, 0.15≤x≤0.25, for example, it can be 0.15, 0.175, 0.2, 0.225 or 0.25, 0.65≤y<0.75, for example, it can be 0.65, 0.675, 0.7, 0.725 or 0.75, 0<m≤0.15, for example, it can be 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14 or 0.15, etc.
[0009] In the present invention, if the value of m is too large, that is, the doping amount of the Sb element is too much, the leakage of the OTS will increase. If the value of m is too small, that is, the doping amount of the Sb element is too small, the purpose of lowering the initial turn-on threshold voltage cannot be achieved.
[0010] Preferably, the value range of m is 0.02-0.1.
[0011] In the present invention, within this preferred range, the leakage of OTS is within the specified index of 10 nA, and at the same time, the threshold voltage of the initial turn-on can be reduced to close to the operating threshold voltage.
[0012] In a second aspect, the present invention provides an OTS gating unit, comprising an upper electrode layer, a lower electrode layer and an OTS gating material layer arranged between the upper electrode layer and the lower electrode layer, wherein the OTS gating material layer comprises the OTS gating material as described in the first aspect.
[0013] Preferably, the threshold voltage of the OTS gating material layer during the first ignition is equal to the threshold voltage during operation.
[0014] In the present invention, by doping a certain proportion of Sb elements, the threshold voltage of the OTS gating material layer during operation is equal to the threshold voltage of the first ignition, which is beneficial to improving the stability of the memory read window and ensuring the quality of the device.
[0015] It should be noted that the “equal” means that the values of the two are equal within a certain precision range, for example, they are equal when the value of the threshold voltage is accurate to one decimal place.
[0016] Preferably, the thickness of the OTS gating material layer is 10-30 nm, for example, 10 nm, 15 nm, 20 nm, 25 nm or 30 nm.
[0017] Preferably, the materials of the upper electrode layer and the lower electrode layer independently include metal elements or metal nitrides.
[0018] Preferably, the metal element includes any one of W, Pt, Au, Ti, Al, Ag, Cu or Ni, or a combination of at least two of them.
[0019] Preferably, the metal nitride comprises TiN.
[0020] Preferably, the thickness of the upper electrode layer and the lower electrode layer is independently 20-60 nm, for example, 20 nm, 30 nm, 40 nm, 50 nm or 60 nm.
[0021] In a third aspect, the present invention provides a method for preparing the OTS gating unit according to the second aspect, the preparation method comprising the following steps:
[0022] (1) Preparing a lower electrode layer: depositing a lower electrode layer material on a substrate to form a lower electrode layer;
[0023] (2) preparing an OTS gating material layer: depositing an OTS gating material layer on the surface of the lower electrode layer;
[0024] (3) Preparing an upper electrode layer: depositing an upper electrode layer material on a surface of the OTS gating material layer away from the lower electrode layer to form an upper electrode layer, and then annealing to obtain the OTS gating unit.
[0025] In the preparation method provided by the present invention, annealing can form nano-crystals inside the OTS gating material. The nano-crystals have lower resistance than the amorphous region and can assist in generating a conductive path when the OTS gating unit is turned on, thereby reducing the turn-on voltage during the first ignition. After the first ignition, the nano-crystals disappear, and the entire OTS gating material is in a stable state after the first ignition.
[0026] Preferably, the deposition method of the OTS gating material layer in step (2) includes any one of magnetron sputtering, evaporation or atomic layer deposition.
[0027] Preferably, during the magnetron sputtering method, co-sputtering is performed by target AsSe and target SbSe, and the sputtering power of the target AsSe is 10-20W, for example, 10W, 12W, 14W, 16W, 18W or 20W, etc., and the sputtering power of the target SbSe is 5-15W, for example, 5W, 7W, 10W, 12W or 15W, etc.
[0028] Preferably, the preparation method of the lower electrode layer and the upper electrode layer comprises any one of sputtering, evaporation, chemical vapor deposition, molecular beam epitaxy or atomic layer deposition.
[0029] Preferably, the annealing temperature in step (3) is 220-280°C, for example, it can be 220°C, 230°C, 240°C, 250°C, 260°C, 270°C or 280°C.
[0030] In the present invention, the annealing temperature is 220-280°C, which can ensure that the threshold voltage of the first ignition is reduced to the same level as the threshold voltage of the subsequent operation. If the annealing temperature is too low, nanocrystals cannot be formed, that is, the threshold voltage of the first ignition cannot be reduced; if the annealing temperature is too high, the device will be damaged.
[0031] Preferably, the annealing time in step (2) is 10-20 min, for example, it can be 10 min, 12 min, 14 min, 16 min, 18 min or 20 min.
[0032] In the present invention, the annealing time is 10-20 minutes, which can ensure that the threshold voltage of the first ignition will be reduced to the same level as the threshold voltage of the subsequent operation. If the annealing time is too short, the size and number of the formed nanocrystals are insufficient, and the threshold voltage of the first ignition cannot be reduced to the threshold voltage of the subsequent operation; if the annealing time is too long, the size and number of the formed nanocrystals are too large, and the threshold voltage of the first ignition is reduced too much.
[0033] In a fourth aspect, the present invention provides a phase change memory, wherein the phase change memory comprises the OTS gating material as described in the first aspect.
[0034] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) The present invention adds a certain proportion of Sb element into the OTS gating material, which can effectively reduce the threshold voltage of the first ignition of the OTS gating material, and make the threshold voltage of the first ignition equal to the threshold voltage during subsequent operation, which not only reduces the impact of the excessively high threshold voltage of the first ignition on the OTS gating unit, improves the safety and reliability of the OTS gating unit, but also reduces the risk of Vth drift.
[0037] (2) In the preparation method provided by the present invention, annealing can form nano-crystals inside the OTS gating material. The nano-crystals have lower resistance than the amorphous region and can assist in generating a conductive path when the OTS gating unit is turned on, thereby reducing the turn-on voltage during the first ignition. After the first ignition, the nano-crystals disappear, and the entire OTS gating material is in a stable state after the first ignition. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a schematic diagram of the structure of the OTS gating unit prepared in Example 1 of the present invention.
[0039] Figure 2 The diagram shows the working mechanism of the OTS gating material layer provided in Example 1 of the present invention.
[0040] Figure 3 TEM comparison diagram of the OTS gating unit provided in Example 1 of the present invention before and after the first ignition.
[0041] Figure 4 This is a graph showing the value changes of the first ten turn-on voltages of the OTS gating unit provided in Example 1 of the present invention.
[0042] Figure 5 This is a comparison curve of the threshold voltage of the OTS gating unit provided in Embodiments 8 and 10 of the present invention.
[0043] Figure 6 This is a graph showing the value changes of the first ten turn-on voltages of the OTS gating unit provided in Example 9 of the present invention.
[0044] Figure 7 The threshold voltage variation curve of the OTS gating unit provided in Embodiment 1 and Embodiments 4-9 of the present invention as the annealing time varies.
[0045] Figure 8 The threshold voltage comparison curves of the OTS gating unit provided in Comparative Examples 2 and 3 of the present invention are shown.
[0046] Fig. 9 TEM image of the OTS gating unit provided in Comparative Example 2 of the present invention before the first ignition.
[0047] Among them, 1-lower electrode layer; 2-OTS gating material layer; 3-upper electrode layer. DETAILED DESCRIPTION
[0048] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0049] Example 1
[0050] This embodiment provides an OTS gating material, the chemical formula of which is As x Se y Sb m , where x=0.22, y=0.71, and m=0.07.
[0051] This embodiment also provides an OTS gating unit, and its structural diagram is as follows: Figure 1 As shown, the OTS gating unit includes an upper electrode layer 3, a lower electrode layer 1, and an OTS gating material layer 2 disposed between the upper electrode layer 3 and the lower electrode layer 1, and the OTS gating material layer 2 includes the above-mentioned OTS gating material;
[0052] The upper electrode layer 3 and the lower electrode layer 1 are both made of TiN, and have a thickness of 40 nm;
[0053] The thickness of the OTS gating material layer 2 is 20 nm.
[0054] This embodiment also provides a method for preparing the above-mentioned OTS gating unit, and the preparation method comprises the following steps:
[0055] (1) The Si substrate was placed in acetone and alcohol solutions respectively, cleaned for 3 min each under ultrasonic action, and then baked at 120°C for 20 min to complete the pretreatment;
[0056] (2) preparing the lower electrode layer 1: depositing the lower electrode layer material on the pretreated Si substrate by magnetron sputtering to form the lower electrode layer 1;
[0057] (3) preparing the OTS gating material layer 2: using the target material AsSe and the target material SbSe to co-sputter and deposit the OTS gating material layer 2 on the surface of the lower electrode layer 1;
[0058] Among them, the sputtering power of the target material AsSe is 15W, and the sputtering power of the target material SbSe is 10W;
[0059] Figure 2 The working mechanism diagram of the above-mentioned OTS gating material layer is shown;
[0060] (4) preparing the upper electrode layer 3: using a magnetron sputtering method, depositing an upper electrode layer material on the surface of the annealed OTS gating material layer 2 away from the lower electrode layer 1 to form an upper electrode layer 3, and then annealing, to finally obtain the OTS gating unit;
[0061] The annealing temperature is 250° C. and the annealing time is 15 min.
[0062] Figure 3 The cross-sectional TEM comparison images of the OTS gating unit provided in this embodiment before and after the first ignition are shown, wherein the left image is before the first ignition, and the right image is after the first ignition. It can be seen from the images that there is crystallization in part of the OTS gating material layer before ignition (i.e., the circle in the left image), but there is no crystallization after ignition, which indicates that the crystals are melted after the first ignition and return to the amorphous state.
[0063] Example 2
[0064] This embodiment provides an OTS gating material, the chemical formula of which is As x Se y Sb m , where x=0.25, y=0.72, and m=0.03.
[0065] This embodiment further provides an OTS gating unit, the OTS gating unit comprising an upper electrode layer, a lower electrode layer and an OTS gating material layer disposed between the upper electrode layer and the lower electrode layer, the OTS gating material layer comprising the above-mentioned OTS gating material;
[0066] The upper electrode layer and the lower electrode layer are both made of TiN and have a thickness of 40 nm;
[0067] The thickness of the OTS gating material layer is 10 nm.
[0068] This embodiment also provides a method for preparing the above-mentioned OTS gating unit, and the preparation method comprises the following steps:
[0069] (1) The Si substrate was placed in acetone and alcohol solutions respectively, cleaned for 3 min each under ultrasonic action, and then baked at 120°C for 20 min to complete the pretreatment;
[0070] (2) preparing a lower electrode layer: depositing a lower electrode layer material on a pretreated Si substrate by a magnetron sputtering method to form a lower electrode layer;
[0071] (3) preparing an OTS gating material layer: using a target material AsSe and a target material SbSe for co-sputtering to deposit an OTS gating material layer on the surface of the lower electrode layer;
[0072] Among them, the sputtering power of the target material AsSe is 20W, and the sputtering power of the target material SbSe is 5W;
[0073] (4) preparing an upper electrode layer: using a magnetron sputtering method, depositing an upper electrode layer material on the surface of the annealed OTS gating material layer away from the lower electrode layer to form an upper electrode layer, and then annealing, to finally obtain the OTS gating unit;
[0074] The annealing temperature is 250° C. and the annealing time is 15 min.
[0075] Example 3
[0076] This embodiment provides an OTS gating material, the chemical formula of which is As x Se y Sb m , where x=0.19, y=0.71, and m=0.1.
[0077] This embodiment further provides an OTS gating unit, the OTS gating unit comprising an upper electrode layer, a lower electrode layer and an OTS gating material layer disposed between the upper electrode layer and the lower electrode layer, the OTS gating material layer comprising the above-mentioned OTS gating material;
[0078] The upper electrode layer and the lower electrode layer are both made of TiN and have a thickness of 40 nm;
[0079] The thickness of the OTS gating material layer is 30 nm.
[0080] This embodiment also provides a method for preparing the above-mentioned OTS gating unit, and the preparation method comprises the following steps:
[0081] (1) The Si substrate was placed in acetone and alcohol solutions respectively, cleaned for 3 min each under ultrasonic action, and then baked at 120°C for 20 min to complete the pretreatment;
[0082] (2) preparing a lower electrode layer: depositing a lower electrode layer material on a pretreated Si substrate by a magnetron sputtering method to form a lower electrode layer;
[0083] (3) preparing an OTS gating material layer: using a target material AsSe and a target material SbSe for co-sputtering to deposit an OTS gating material layer on the surface of the lower electrode layer;
[0084] Among them, the sputtering power of the target material AsSe is 20W, and the sputtering power of the target material SbSe is 20W;
[0085] (4) preparing an upper electrode layer: using a magnetron sputtering method, depositing an upper electrode layer material on the surface of the annealed OTS gating material layer away from the lower electrode layer to form an upper electrode layer, and then annealing, to finally obtain the OTS gating unit;
[0086] The annealing temperature is 280° C. and the annealing time is 10 min.
[0087] Example 4
[0088] The difference between this embodiment and embodiment 1 is that the annealing time in step (4) is 10 minutes.
[0089] The rest of the preparation methods and parameters were the same as those in Example 1.
[0090] Example 5
[0091] The difference between this embodiment and embodiment 1 is that the annealing time in step (4) is 13 minutes.
[0092] The rest of the preparation methods and parameters were the same as those in Example 1.
[0093] Example 6
[0094] The difference between this embodiment and embodiment 1 is that the annealing time in step (4) is 17 minutes.
[0095] The rest of the preparation methods and parameters were the same as those in Example 1.
[0096] Example 7
[0097] The difference between this embodiment and embodiment 1 is that the annealing time in step (4) is 20 minutes.
[0098] The rest of the preparation methods and parameters were the same as those in Example 1.
[0099] Example 8
[0100] The difference between this embodiment and embodiment 1 is that the annealing time in step (4) is 30 minutes.
[0101] The rest of the preparation methods and parameters were the same as those in Example 1.
[0102] Example 9
[0103] The difference between this embodiment and embodiment 1 is that no annealing is performed in step (4).
[0104] The rest of the preparation methods and parameters were the same as those in Example 1.
[0105] Figure 4 and Figure 6The numerical change diagrams of the first ten turn-on voltages of the OTS gating units provided in Example 1 and Example 9 are respectively shown. From the comparison of the figures, it can be seen that the threshold voltage of the first ignition of the OTS gating unit prepared in Example 1 is greatly reduced and reduced to the average level of the subsequent threshold voltages.
[0106] Figure 7 The threshold voltage variation curves of the OTS gating units provided in Example 1 and Examples 4-9 as the annealing time changes are shown. It can be seen from the figure that as the annealing time increases, the threshold voltage of the first ignition decreases, and the overall decrease rate is faster than the decrease rate of the threshold voltage during subsequent operation. Moreover, when the annealing time is 15 minutes, the threshold voltage of the first ignition is equal to the threshold voltage during subsequent operation.
[0107] Example 10
[0108] The difference between this embodiment and embodiment 8 is that no annealing is performed in step (4).
[0109] The rest of the preparation methods and parameters were the same as those in Example 8.
[0110] Embodiment 11
[0111] The difference between this embodiment and embodiment 1 is that the annealing temperature in step (4) is 150°C.
[0112] The rest of the preparation methods and parameters were the same as those in Example 1.
[0113] Example 12
[0114] The difference between this embodiment and embodiment 1 is that the annealing temperature in step (4) is 350°C.
[0115] The rest of the preparation methods and parameters were the same as those in Example 1.
[0116] Example 13
[0117] The difference between this embodiment and embodiment 1 is that the value of m is 0.15, and the values of x and y are adjusted to 0.15 and 0.7.
[0118] The rest of the preparation methods and parameters were the same as those in Example 1.
[0119] Comparative Example 1
[0120] The difference between this comparative example and Example 1 is that the value of m is 0.25, and the values of x and y are adjusted to 0.1 and 0.65.
[0121] The rest of the preparation methods and parameters were the same as those in Example 1.
[0122] Comparative Example 2
[0123] The difference between this comparative example and Example 8 is that Sb is not doped.
[0124] The rest of the preparation methods and parameters were the same as those in Example 8.
[0125] Figure 5 The threshold voltage comparison curves of the OTS gating unit provided in Example 8 and Example 10 are shown, Figure 8 The threshold voltage comparison curves of the OTS gating units provided in Comparative Examples 2 and 3 are shown. It can be seen from the figure that even if the OTS gating unit without Sb doping includes an annealing process, no nano-crystals are generated, so that the threshold voltage of the first ignition does not change substantially during the annealing process. However, for the OTS gating unit doped with Sb and obtained after adding an annealing process, the threshold voltage of the first ignition drops sharply during the annealing process.
[0126] Fig. 9 The TEM image of the OTS gating unit provided in this comparative example before the first ignition is shown. It can be seen from the image that no nano-crystals are generated in the OTS gating material layer.
[0127] Comparative Example 3
[0128] The difference between this comparative example and comparative example 2 is that no annealing is performed.
[0129] The rest of the preparation methods and parameters were the same as those in Comparative Example 2.
[0130] Performance Testing
[0131] 1. Test the threshold voltage of the OTS gating unit provided in the above embodiments and comparative examples.
[0132] The threshold voltage test process is as follows: use a triangular pulse with a peak value slightly higher than the OTS threshold voltage to act on both ends of the OTS. At a certain point on the rising edge of the pulse, the threshold voltage of the OTS will be reached and it will be turned on. The corresponding pulse voltage value when it is turned on is recorded, which is the threshold voltage of the OTS.
[0133] The test results are shown in Table 1.
[0134] Table 1
[0135]
[0136]
[0137] It can be seen from Example 1 and Examples 4-9 in the above table that when the annealing temperature is 250° C. and the annealing time is 15 min, the threshold voltage of the first ignition of the Sb-doped OTS gating unit is almost equal to the threshold voltage during operation.
[0138] It can be seen from Example 8, Example 10 and Comparative Examples 2-3 in the above table that the threshold voltage of the OTS gating unit provided by Example 8 and Example 10 for the first ignition is reduced to be lower than the threshold voltage during the operation process, while the difference between the threshold voltage of the OTS gating unit provided by Comparative Examples 2 and Comparative Examples 3 for the first ignition and the threshold voltage during the operation process is basically unchanged, which indirectly proves the role of the Sb element in the formation of "nano-grains", which also shows that the reason for the generation of nano-grains and the reduction of the threshold voltage of the first ignition is the doping of Sb.
[0139] It can be seen from Example 1 and Examples 11-12 that if the annealing temperature is too low, the threshold voltage of the first ignition cannot be reduced; if the annealing temperature is too high, the OTS device will be damaged.
[0140] It can be seen from Example 1, Example 13 and Comparative Example 1 that as the value of m increases, the threshold voltage of the OTS gating unit will be reduced, and the leakage will increase. If the value of m is too large, that is, the Sb doping amount is too large, the device will be directly turned on, and the OTS will lose its function as a gating switch.
[0141] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. An OTS gating material, characterized in that: The chemical formula of the OTS gating material is As x Se y Sb m , where 0.15≤x≤0.25, 0.65≤y<0.75, and 0<m≤0.
15.
2. The OTS gating material according to claim 1, characterized in that: The value range of m is 0.02-0.
1.
3. An OTS gating unit, characterized in that: The OTS gating unit comprises an upper electrode layer, a lower electrode layer and an OTS gating material layer disposed between the upper electrode layer and the lower electrode layer, wherein the OTS gating material layer comprises the OTS gating material according to claim 1 or 2.
4. The OTS gating unit according to claim 3, characterized in that: The threshold voltage of the OTS gating material layer when it is first ignited is equal to the threshold voltage when it is working.
5. The OTS gating unit according to claim 3 or 4, characterized in that: The thickness of the OTS gating material layer is 10-30 nm.
6. The OTS gating unit according to any one of claims 3 to 5, characterized in that: The materials of the upper electrode layer and the lower electrode layer independently include metal elements or metal nitrides; Preferably, the metal element includes any one or a combination of at least two of W, Pt, Au, Ti, Al, Ag, Cu or Ni; Preferably, the metal nitride comprises TiN; Preferably, the thickness of the upper electrode layer and the lower electrode layer are independently 20-60 nm.
7. A method for preparing an OTS gating unit according to any one of claims 3 to 6, characterized in that: The preparation method comprises the following steps: (1) Preparing a lower electrode layer: depositing a lower electrode layer material on a substrate to form a lower electrode layer; (2) preparing an OTS gating material layer: depositing an OTS gating material layer on the surface of the lower electrode layer; (3) Preparing an upper electrode layer: depositing an upper electrode layer material on a surface of the OTS gating material layer away from the lower electrode layer to form an upper electrode layer, and then annealing to obtain the OTS gating unit.
8. The preparation method according to claim 7, characterized in that: The deposition method of the OTS gating material layer in step (2) includes any one of magnetron sputtering, evaporation or atomic layer deposition; Preferably, during the magnetron sputtering method, co-sputtering is performed by using the target material AsSe and the target material SbSe, the sputtering power of the target material AsSe is 10-20W, and the sputtering power of the target material SbSe is 5-15W; Preferably, the preparation method of the lower electrode layer and the upper electrode layer comprises any one of sputtering, evaporation, chemical vapor deposition, molecular beam epitaxy or atomic layer deposition.
9. The preparation method according to claim 7 or 8, characterized in that: The annealing temperature in step (3) is 230-280° C. Preferably, the annealing time in step (2) is 10-20 min.
10. A phase change memory, characterized in that: The phase change memory comprises the OTS gating material as claimed in claim 1 or 2.