Production method and ceramic product obtained through method

Through rotary mold extrusion and heat treatment technology, the problem that existing ceramic product manufacturing methods are difficult to produce new products is solved, and efficient and low-cost ceramic product manufacturing is realized. The production of ceramic products with complex shapes and patterns is improved, and the product Strongness and surface quality.

CN118946442AInactive Publication Date: 2024-11-12RELIEFED AB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030179.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-31
Filing Date
2023-01-31
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing ceramic product manufacturing methods are difficult to produce ceramic products with new designs, resulting in expensive and time-consuming post-processing and process adjustments, and due to the capacity of production equipment, it cannot meet the needs of a variety of ceramic products.

Method used

Using the method of forming ceramic material by extrusion or stretching, a rotary mold is used to create a variety of structures and patterns, and combining heat treatment to form ceramic products, including adjusting the material flow and rotary mold position during the molding process, using multiple rotary molds to form complex shapes and Structural surface pattern and molded materials are reduced in heat treatment to achieve a combination of multiple individual products.

Benefits of technology

A more general method of ceramic product production is realized, reducing production costs and time, and being able to manufacture ceramic products with complex shapes and patterns, improving product robustness and surface quality, reducing liquid content and solvent use, and reducing final product cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946442A_ABST
    Figure CN118946442A_ABST
Patent Text Reader

Abstract

The invention provides a production method. The production method comprises a channel (10) by extruding or pulling the ceramic material through an extrusion die, the channel being at least partially defined by a side surface area (4) of at least one rotating die (3); and thermally treating the molding material to form a ceramic product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a production method for manufacturing a variety of ceramic products, and a variety of ceramic products produced by the method. Background Art

[0002] Ceramic products are used in a wide variety of applications. One common application for ceramic products is structural elements such as bricks, pipes and wall and floor tiles for interior and exterior decoration. The production of such tiles involves several steps. The raw materials, including clay minerals, are prepared by mixing and grinding and optional drying. A shaping step is then performed. One available shaping method is based on dry pressing, in which the powdered material is arranged and compressed in a shaping mold. Another option requires more moist raw materials and allows the ceramic product to be shaped by extrusion and subsequent stamping.

[0003] Once the object has been formed into the desired shape, it typically undergoes a post-forming process including drying, glazing and firing.

[0004] Existing methods of manufacturing ceramic products require the raw materials to have certain properties, while the design of the final product is limited by the capabilities of existing production equipment. Often, if new ceramic products with new designs are required, there is a significant risk that these products cannot be manufactured with existing manufacturing processes, requiring expensive and time-consuming post-processing and process adjustments.

[0005] Therefore, there is a need for improved manufacturing processes that not only provide a more versatile method of producing ceramic products, but also reduce the cost and time of producing ceramic products. Summary of the invention

[0006] The object of the present invention is to at least partially overcome one or more of the above limitations of the prior art. In particular, the object of the present invention is to provide a manufacturing method in which the raw material is continuously shaped and the shaping allows the creation of advanced patterns and multiple structures for the final ceramic product.

[0007] To address these objectives, a production method is provided, comprising the steps of: i) forming a material by extruding or pulling a ceramic material through a channel of an extrusion die, the channel being at least partially defined by a side surface area of ​​at least one rotating die; and ii) heat treating the formed material to form a ceramic product.

[0008] Preferably, the method is performed by extruding or pulling the ceramic material through a plurality of bearing surfaces defining the channel. The channel is preferably formed by an extrusion die, wherein the plurality of bearing surfaces includes at least one rotating bearing surface, the at least one rotating bearing surface being a surface of a rotating die defining a cross-section of the molding material, such that the channel is at least partially defined by at least one rotating die.

[0009] The rotating mold can apply a pattern to the molding material. Preferably, the applied pattern is a repeating pattern.

[0010] The method may further include a step of shrinking the molding material so that the pattern size of the rotational mold is different from the pattern size of the ceramic product. Preferably, the shrinking is performed during the heat treatment.

[0011] The method may further comprise a step of regulating the flow rate of the ceramic material upstream of the channel. This enables the ceramic material to control a correct flow distribution and a uniform velocity when entering the channel.

[0012] The method may further include a step of driving the rotating mold. Such driving may be performed continuously during the manufacturing method.

[0013] Driving the rotating mold may further include synchronizing the rotation of the rotating mold with the speed of a downstream conveyor belt of the ceramic products.

[0014] The method may further comprise the step of determining at least one dimension of the ceramic product and adjusting the speed of the rotating mould and / or the downstream conveyor belt according to the determined dimension.

[0015] The step of heat treatment can be carried out by firing the molding material. Optionally, the heat treatment can be a multi-step process, which also includes an initial drying step. Typically, this drying step is carried out at a temperature significantly lower than the firing temperature.

[0016] The method may further comprise separating a separate product from the formed material before, during or after the heat treatment.It should be noted that the steps of separation and heat treatment may be performed in any order.

[0017] In one embodiment, the method further comprises installing a plurality of individual products together before the step of heat treating. By arranging a plurality of individual products together and contacting each other during the heat treating process, the products will be mechanically bonded and form a uniform product.

[0018] Separation of an individual product can be carried out by the cutting action of the rotating die. This achieves effective separation without the need for additional multiple components and multiple cutting or punching stations.

[0019] The circumference of the rotating mold may be equal to the length of the individual product, or may be different from the length of the individual product. Therefore, the pattern of the rotating mold can be determined to match the periodicity of the plurality of final individual products in a very flexible manner.

[0020] The channel can have a longitudinal extension in a production direction, and the axis of rotation of the rotary mold can be arranged at a certain angle relative to the production direction, preferably the rotary mold is arranged at an angle of 90°±25° relative to the production direction. Thus, not only can the rotary mold be completely transverse to the production direction, but the rotary mold can also be "screwed" on the material to be formed.

[0021] The channel may be defined by a bottom region, an upper region and two opposite side regions, together forming a closed space, wherein at least a portion of one of the plurality of regions may be formed by a side surface region of the at least one rotating mold.

[0022] In some embodiments, at least a portion of the at least one further region is defined by a side surface region of another rotational mold.

[0023] At least one of the bottom region, the upper region and the two opposing side regions may be defined by a bearing surface.

[0024] Thus, the manufacturing method allows the use of one or more (two, three, four, five, etc.) rotating molds to provide a repeating pattern for the material to be formed.

[0025] The method may further include pressing or pulling the ceramic material through a preload channel disposed upstream of the rotating die.

[0026] The preload channel may be disposed immediately upstream of the rotating mold, or the preload channel may be disposed upstream of the rotating mold but away from the rotating mold.

[0027] The preload channel may be configured to deform the ceramic material into a primary profile, and the channel may be configured to further deform the material into a final profile having a final shape.

[0028] The dimensions of the pre-loaded channel may be static.

[0029] The side surface area of ​​the rotating mold may be provided with a topographic pattern. The topographic pattern may include at least one protrusion configured to form a separation recess in the ceramic product and / or to significantly reduce the thickness of the ceramic product locally.

[0030] The significant reduction in thickness of the ceramic product may define a removable portion of the ceramic product. Due to the reduced thickness, only very little force is required to remove these removable portions.

[0031] At least one protrusion may extend across the entire width of the rotating mold, or may extend across a portion of the width of the rotating mold. The protrusion may extend across the width of the rotating mold in a linear or curvilinear manner.

[0032] The method may further comprise adding an additional material to the ceramic material. Adding the additional material may be performed before, during or after the ceramic material passes through the rotating die.

[0033] The further material may be embedded in the ceramic material to form a reinforcement of the ceramic product.

[0034] The further material may be a fibrous material or a web material.

[0035] The further material may be added as at least one layer to the ceramic material.

[0036] The further material may be a liquid material or a solid material in the form of a powder or granules.

[0037] The additional material may include a variety of different ceramic and / or non-ceramic materials.

[0038] The ceramic material and the at least one further material may be supplied through the passage.

[0039] The method may further include adjusting a position of the rotating mold to adjust a size of the channel.

[0040] The method may further comprise providing the channel with at least one core, the core forming a hollow portion of the ceramic product.

[0041] The ceramic product may be a brick or a plate-like product, such as a ceramic tile.

[0042] The channel may provide a first structured surface pattern defined by a side surface region of at least one rotating mold to one side of the molding material, and a second structured surface pattern defined by a side surface region of another rotating mold to an opposite side of the molding material.

[0043] The first structured surface pattern and the second structured surface pattern may provide a matching fit when a plurality of ceramic products are stacked together.

[0044] According to a second aspect, there is provided a ceramic product formed by extruding or pulling a ceramic material through a channel at least partially defined by at least one extrusion die to form the ceramic material, followed by heat treatment to form the ceramic product.

[0045] Preferably, the ceramic product is formed by pressing or pulling the ceramic material through a plurality of bearing surfaces defining the channel. The channel is preferably formed by a rotating die, wherein the plurality of bearing surfaces includes at least one rotating bearing surface, the at least one rotating bearing surface being a surface of a rotating die defining a cross-section of the molding material, such that the channel is at least partially defined by the at least one rotating die.

[0046] The ceramic product may be a brick or a plate-like product, such as a tile or a coating.

[0047] The ceramic product may include a plurality of sides, wherein each side is provided with a contour that matches a corresponding contour of a side of another ceramic product.

[0048] The ceramic product may include a structured surface pattern corresponding to the pattern of the rotational mold.

[0049] The structured surface pattern may be arranged on an upper side of the ceramic product during its intended use.

[0050] The ceramic product may also include a structured surface pattern on its bottom side during the intended use of the ceramic product.

[0051] The structured surface pattern on the bottom side of the ceramic product may form a plurality of mounting structures for the ceramic product.

[0052] The plurality of corresponding structured surface patterns may provide a fit when a plurality of ceramic products are stacked on top of each other.

[0053] The ceramic product may comprise at least one further material.

[0054] According to a third aspect, there is provided a device comprising at least one ceramic product according to the second aspect.

[0055] The device may be a thermal device and the ceramic product may form part of a heat exchanger, a cooling profile and / or a heating element.

[0056] The device may be a chemical reactor and the ceramic product may form part of a catalyst or a condenser.

[0057] The device may be an anti-slip device, and the ceramic product may form a surface of the anti-slip device.

[0058] Other objects, features, aspects and advantages of the present invention will become apparent from the following detailed description and the accompanying drawings.

[0059] Some specific terms are used in this specification and are defined as follows.

[0060] Extrusion: The process of forcing a material under pressure through a profile-forming tool (also called a die) with holes that define the cross-section and appearance of the output material.

[0061] Pultrusion: The process of pulling a material under pressure through a profile-forming tool (also called a die) with holes that define the cross-section and appearance of the output material.

[0062] Dynamic Extrusion: The process of extruding a material under pressure through a tool having multiple rotating molding members (multiple dies) that can impart a variety of cross-sections and / or appearances to the material, such as in the form of multiple patterns on one or more surfaces and dimensional variations in cross-sectional area and / or material thickness.

[0063] Dynamic pultrusion: A process in which a material is pulled under pressure through a tool having multiple rotating forming members (multiple dies) which can impart a variety of cross-sections and / or appearances to the material, such as in the form of multiple patterns on one or more surfaces and dimensional variations in cross-sectional area and / or material thickness.

[0064] Mold: Generally, it is the name given by professionals to various profile forming tools.

[0065] Rotary Die: The rotating profile forming part of the tool used for dynamic extrusion / pultrusion.

[0066] Bearing Surface: The surface of the smallest cross-sectional area of ​​an extrusion die through which the extruded material is forced under pressure, thereby forming the surface that ultimately defines the cross-section and appearance of the molded material.

[0067] Static bearing surface: A solid bearing surface that the extruded material is forced to pass at a speed relative to the output material speed. Because it is static, there is a speed difference between the static bearing surface and the extruded material, which generates friction and heat. By adjusting the length of the multiple bearing surfaces, the total amount of friction can be adjusted, thereby adjusting the pressure, balance and speed of the output material.

[0068] Rotating bearing surface: A rotating bearing surface is the surface of the rotating mold that defines the cross-section of the molded material, allowing pattern generation and material thickness variations. A rotating bearing surface generally provides much less resistance and friction to the flowing material than a static bearing surface, which previously caused significant problems with imbalance between multiple different parts of the molded material cross-section, and the static bearing surface was defined by all the bearing surfaces of the entire mold. This often caused process interruptions at startup.

[0069] Preload (surface): The surface area through which the extruded material passes before (preferably immediately before) entering the rotating die area and its rotating bearing surface. The preload reduces the material cross-section to such an extent that the subsequent rotating die does not have to bear unnecessary large forces from the molding material. Preload, in conjunction with upstream material shaping, plays a central role in controlling and / or regulating the flow of material through the die.

[0070] Dynamic extrusion and dynamic pultrusion: A process for molding (ceramic) materials using multiple rotating dies integrally molded in multiple extrusion dies. The extrusion die has one or more rotating dies. The cross-sectional profile of the molded material can optionally be defined by the outer periphery of the rotating die, i.e. the side surface area, defining a rotating bearing surface upstream of the material to be molded, i.e. the side surface area, which ultimately defines the appearance and cross-section of the molded material together with other rotating and / or static bearing surfaces in the die.

[0071] Ceramic material: In the context of this specification, the term should be interpreted broadly to cover any material suitable for forming a ceramic product. Ceramic materials include any formable inorganic, non-metallic oxide, nitride or carbide material that, after heat treatment, preferably causes vitrification to at least some extent to form a hard, brittle, heat-resistant and corrosion-resistant ceramic product. Although no specific compounds or minerals are listed herein, general characteristics of ceramic products include high melting point, high hardness, poor electrical conductivity, high elastic modulus, high chemical resistance and low ductility. Various examples of ceramic materials include clay minerals such as kaolinite, alumina and silicon carbide.

[0072] Pattern: Any configuration of structures that can be transferred from a mold to a ceramic material. A pattern can be macroscopic, i.e., visible to the human eye, or microscopic. A pattern can also extend through the entire molded material, or only through a small portion thereof. Typically, although not necessarily, a pattern is a configuration of topography. Examples of patterns included in the context of this specification include variations in thickness of the molded material, multiple reinforcing ribs, multiple channels, and multiple macroscopic and microscopic structures. Even a completely smooth surface is considered to define a pattern. BRIEF DESCRIPTION OF THE DRAWINGS

[0073] Several embodiments of the present invention will now be described by way of example with reference to the accompanying drawings, in which:

[0074] Figure 1 is a schematic diagram of an apparatus for producing a plurality of ceramic products according to an embodiment;

[0075] Figure 2schematically showing a cross-sectional perspective side view of an apparatus configured to perform at least a portion of a method according to the present invention, wherein ceramic material is being processed;

[0076] Figure 3 Schematically showing an example Figure 2 A cross-sectional side view of the device;

[0077] Figure 4 schematically showing an isometric view of components of an apparatus configured to perform at least a portion of a method according to the invention;

[0078] Figures 5 to 10 Schematically showing an example Figure 2 A cross-sectional side view of the device;

[0079] Fig.11 and Fig.12 showing examples of ceramic products according to various embodiments; and

[0080] Fig.13 is a schematic flow chart of a manufacturing method according to various embodiments. DETAILED DESCRIPTION

[0081] Extrusion of ceramic materials is not an easy task. Many ceramic materials are difficult to extrude due to the high friction between the material being extruded and the bearing surface. This high friction results in slow production speeds, and a common approach to addressing this problem is to add various solid or fluid lubricants to the ceramic material. During extrusion, such lubricants include polyethylene or polypropylene, such as silicon nitride, and / or various liquid lubricants, such as water, oil, or other evaporable or flammable lubricants.

[0082] The present invention is based on the principle of extruding a ceramic material using at least one rotating die, thereby forming a rotating bearing surface. The inventors unexpectedly realized that using this technology, the friction that causes internal shear in the molded material (i.e., the friction between the extruded material and the plurality of bearing surfaces) is largely eliminated. Since friction is significantly reduced, many advantages are obtained.

[0083] First, the present invention allows for faster extrusion of ceramic materials. Second, the present invention allows for a reduced amount of liquid (i.e., water, solvent, and / or lubricant) in the ceramic material while still achieving the desired production speed. This also reduces the cost and time required to dry the ceramic material after forming, thereby increasing the yield of the production process.

[0084] Since the liquid content can be reduced, this brings additional advantages; the molding material will be harder and stronger, making it possible to extrude geometries that are not achievable with existing technical methods. In addition, due to the lower liquid content, the cost of solvents and / or lubricants will also be reduced, and the shrinkage of the final ceramic product will also be reduced, which makes the design of the final ceramic product easier.

[0085] The invention has also been shown to significantly improve the surface quality of the extruded ceramic material. This in turn enables the extrusion of thinner materials and the extrusion of ceramic materials that were previously unsuitable for extrusion, such as ceramic materials containing a plurality of large solid particles, or ceramic materials that result in a particularly high friction.

[0086] Now from Figure 1 Initially, the figure schematically shows an apparatus 100 for implementing the method of the present invention. The apparatus 100 requires a supply 102 of ceramic raw material. During operation of the apparatus, the ceramic material is supplied to an extrusion device 1, which processes the ceramic material and forms it into a desired shape. After the ceramic material is formed, it is transported to a heat treatment station 104, which typically includes a dryer, a kiln, etc., for producing a plurality of ceramic products from the formed ceramic material. Typically, the heat treatment includes exposing the formed material to a temperature of 800°C or higher. The specific heat exposure (i.e., temperature, time and gradient) depends on the specific material and the size of the final ceramic product.

[0087] It should be noted that Figure 1 The apparatus 100 schematically shown in FIG. 1 may also be equipped with a conveyor, a feeder, etc. (not shown).

[0088] The following will refer to Figures 2 to 10 The extrusion device 1 for forming the ceramic material will be described in detail.

[0089] from Figure 2 Initially, the device 1 is configured to process (ie form) a ceramic material along a production direction PD. The ceramic material is a plastically deformable material and / or a viscoelastic material and / or a plastically deformable material with elasticity and / or a viscoplastic material with elasticity.

[0090] The device 1 includes a rotating mold 3 extending in a radial direction R and a width direction X, having two opposite first side walls 5 and second side walls 6, and a peripheral (side) surface area 4 extending between the first side walls 5 and the second side walls 6 along the width direction X. The rotating mold 3 includes a first side portion 23 connected to the first side wall 5 and a second side portion 25 connected to the second side wall 6, and a middle portion 22 extending between the first side portion 23 and the second side portion 25.

[0091] The device 1 further comprises a material definition area 7 having a longitudinal direction Y coinciding with the production direction PD, a height direction Z and a width direction X perpendicular to the height direction Z. The material definition area 7 comprises a channel 10. Figure 1 In the device 1 shown, a channel 9 is provided in front of the channel 10 (in the production direction PD).

[0092] The channel 9 is circumferentially bounded by one or more walls 11 to form a closed circumference of the ceramic material. The channel 10 is arranged just downstream of the channel 9 and is at least partially defined by the side surface area 4 of the rotating mold 3. In the example shown, the channel 10 is also defined by a counter-bearing 14 arranged opposite to the rotating mold 3 and opposite first and second channel part side walls extending between the rotating mold 3 and the counter-bearing 14.

[0093] The rotary mould 3 is rotatable about an axis transverse to the production direction PD and is arranged to allow the lateral surface area 4 to exert a pressure on the surface of the ceramic material when the ceramic material is fed through the material definition area 7 while the rotary mould 3 is rotating.

[0094] according to Figure 2 In the embodiment shown, the channel 9 is configured to deform the ceramic material into a main profile 36 having a maximum height H1 at a predetermined feed rate depending on the ceramic material and having a minimum cross-sectional area with a first maximum height D1 when leaving the channel 9 .

[0095] The passage 10 is configured to further deform the ceramic material into a final shape 37 having a minimum height H2 by means of the rotary mold 3, which is configured to exert an increasing pressure on the main contour 36, which bears against the counter-bearing 14. To this end, the rotary mold 3 is configured at a minimum distance D2 from the counter-bearing 14, depending on the maximum permissible pressure exerted by the rotary mold 3 at the location of the minimum distance D2. The maximum permissible pressure corresponds to the maximum height difference between the main contour 36 and the final contour 37 and depends on a specific pattern on the lateral surface area 4 of the rotary mold 3. Due to the elasticity of the material, the maximum permissible pressure also depends on the viscoelasticity and viscoplasticity of the ceramic material and therefore on the difference between the final height H3 of the molded material and the height H2 after the passage 10.

[0096] According to one example, the channel 9 is formed between at least two side walls 11, a top pre-bearing and an opposite bottom pre-bearing, wherein the top pre-bearing is arranged above the opposite bottom pre-bearing in the height direction Z. The top pre-bearing and / or the bottom pre-bearing may comprise a wake element.

[0097] Typically, the wake element protrudes from the side wall in the direction of the channel 9. According to one example, the wake element protrudes from the side wall into the channel in the height direction. The wake element can be designed according to the elasticity of the ceramic material so as to provide the correct height of the main profile when entering the channel 10. Here, elasticity means that the material expands after being pressed into shape in the channel 9. When passing through the wake element, the wake element generates a waveform in the ceramic material.

[0098] An advantage of the device 1 is that the maximum load is controlled in both the channel 9 and the channel 10, which makes it possible to design the extrusion device 1 according to the ceramic material to be processed and the desired processing speed. Controlling the maximum load according to the ceramic material to be processed allows a high-quality output productivity and reduces the risk of cracking due to excessive pressure on the ceramic material.

[0099] according to Figure 2 In the example shown, the extrusion device 1 receives ceramic material; this ceramic material is formed in the channel 9 into the shape of a main contour 36 , and subsequently the ceramic material is formed directly in the channel 10 into the shape of the final contour 37 . Figure 2 It is also shown that, due to the further pressure on the main profile 36 in the channel 10 , the height H1 of the final profile 37 is smaller than the height H2 of the main profile 36 . Figure 2 It is also shown that if molding is performed at a high temperature, the height H3 of the molded material 2 may be smaller than the height H1 of the final contour 36 due to shrinkage when cooling from the final contour 37 to the product contour 2.

[0100] Figure 3 Schematically a cross-sectional side view of an extrusion device 1 according to an embodiment is shown. Here, the rotary die 3 is shown in a rotated position in which the portion of the rotary die 3 pressing the ceramic material against the counter-bearing 14 does not contain any local pattern or indentation 38 .

[0101] Figure 3An initial area A is schematically shown, in which the ceramic material is pressed into the channel 9 by a device (not shown), and the pressing method is to apply an external pressure in the production direction PD by a device (not shown), i.e. extrusion, and / or to drag the material in the production direction PD by a device (not shown), i.e. pultrusion, to drag the ceramic material through the channel 9.

[0102] Zone A of the device 1 comprises a funnel-shaped opening 43, in which the ceramic material changes from an initial form having a larger cross section than the channel 9. However, the shape of the opening may vary depending on the type of ceramic material, the temperature and the means by which the material is pressed.

[0103] A region B is arranged directly after region A, wherein region B corresponds to the longitudinal extension of the channel 9 and the formation of the main profile 36 occurs in this region, which is the result of the side wall 11 of the channel 9 exerting pressure on the ceramic material when the ceramic material moves through the channel 9, causing the ceramic material to change shape.

[0104] A region C is arranged directly after region B, wherein region C corresponds to the longitudinal extension of the channel 10 and the formation of the final profile 36 occurs in this region as a result of the ceramic material changing shape due to the pressure exerted on the ceramic material by at least the relative counter-bearing 14 of the rotating mold 3 and the channel 10.

[0105] A zone D is provided directly after zone C, wherein zone D corresponds to a section of the production line after the channel 10, and the ceramic material optionally begins to cool (if the extrusion process is carried out using high temperatures). In this case, the final profile 36 begins to shrink and change shape due to the temperature drop. It should be noted that shrinkage may also occur due to drying of the molding material. In zone D, the final profile 37 can be subjected to various production measures to achieve the desired properties of the molding material, such as cooling, heating, stretching, compression, etc., in order to change the final profile 37 to a desired shape with desired material properties.

[0106] The length of region D generally depends on various material properties and the operating environment around the ceramic material in region D. The various material properties include heat dissipation and the mass of the ceramic material to be cooled. For example, a thinner material cools faster than a thicker material. The operating environment refers to, for example, ambient temperature and humidity. For example, a warmer environment slows down the cooling process compared to a colder environment.

[0107] A zone E is provided directly after zone D, wherein zone E corresponds to a section of the production line in which the ceramic material has dried or cooled to a predetermined temperature, which represents the temperature of the final form of the molding material, and in which the form does not change or continues to change only slightly. In zone E, the height H3 of the molding material is optionally less than the height H2 of the final contour 37. Likewise, due to drying / evaporative cooling, the pattern 39 of the final contour 37 may be reduced to the pattern 40 in zone E.

[0108] For example, the method may be used to reduce the ceramic material in the range of 0-50%, such as between 0 and 20%. The reduction process may take place during any step of cooling, drying or heat treatment (such as firing and / or glazing).

[0109] It should be noted that for some ceramic materials, the extrusion device 1 can be operated at room temperature, so little or no cooling is required, and most of the shrinkage usually occurs due to drying and heat treatment. If necessary, regions D and E will be very short in such embodiments.

[0110] exist Figure 3 In the embodiment of the present invention, the extrusion device 1 comprises a pulling and stretching device 54, which is arranged downstream of the channel 10 and is configured to pull the ceramic material along the production direction PD when leaving the channel 10. One advantage is that the pulling and stretching device 54 can dynamically stretch the ceramic material during the forming of the ceramic material, for example, in order to obtain an equidistant pattern in the production direction PD of the formed material. The pulling and stretching device 54 can also be used to guide the formed material in the width and / or height direction.

[0111] According to one example, the distance between the indentations 38 in the pattern 38 on the rotating mold 3 is smaller than the distance between the protrusions 40 in the corresponding pattern 38 in the production direction PD on the molding material 2, wherein the pulling and stretching device 54 is configured to stretch the molding material, so that high precision of the distance between multiple features on the molding material can be achieved by adjusting the stretching.

[0112] The pulling and stretching device 54 can be any type of device, which includes a device for grabbing the molding material and a device for pulling. According to one example, the pulling and stretching device 54 includes a control device 55 for controlling the tension applied to the molding material. The control device 55 may include a sensor and / or may be connected to a sensor 56 for monitoring the state of the molding material. The sensor includes a device for sending analog and / or digital information to the control device. The information is related to the state of the molding material, and the control device 55 is configured to process the information for controlling the pulling and stretching device.

[0113] In one embodiment, the rotary mold 3 and / or the counter-bearing 14 include a cooling device 57, which cools the ceramic material during molding. The advantage of this is that a predetermined temperature of the ceramic material is achieved to achieve the best material properties of the molded material. For some ceramic materials, the material temperature during extrusion and / or pultrusion is crucial to the quality of the final ceramic product. The temperature is also important due to the friction characteristics between the ceramic material and the rotary mold 3 and / or the counter-bearing 14. The cooling device 57 can, for example, be arranged in the form of a cooling circuit, in which a gas or liquid fluid conductor is arranged inside the rotary mold 3 and / or the counter-bearing 14; and / or an external device that cools the rotary mold 3 and / or the counter-bearing 14; and / or a liquid or gaseous fluid added to the rotary mold 3 and / or the counter-bearing 14, or a combination of these devices or any other suitable cooling device. It should be noted that the rotary mold 3 can be configured to operate without the cooling device 57.

[0114] According to an example, the rotating mold 3 is configured to be cooled on the surface so that the temperature of the side surface area of ​​the rotating mold 3 is lower than a predetermined allowable temperature of the ceramic material.

[0115] Figure 3The rotary mold 3 is schematically shown to include a pattern 38, which includes at least one indentation 38 in the side surface area 4. The number of indentations is here only an illustrative example, and depending on the desired characteristics of the molding material, there may be more or fewer indentations or protrusions in the pattern, which are distributed on the rotary mold 3 in a predetermined design. The plurality of indentations or protrusions may have any suitable shape, such as an ellipse, a circle, a polygon, or a mixture of these or other shapes. The indentation 38 has a bottom 44 at the maximum depth of the indentation, and the indentations may have different or similar depths. Between the indentations 38, the rotary mold 3 includes a plurality of portions having a default distance D2 between the rotary mold 3 and the counter-bearing 14 when facing the counter-bearing 14. It should be noted that the height of any protrusion should not be greater than the default distance D2.

[0116] According to an example, a minimum distance D2 between the lateral surface area 4 and the counter-bearing 14 in the height direction Z is smaller than a maximum distance D1 , ie, the height of the channel 9 .

[0117] exist Figure 2 and Figure 3 In the embodiment, the channel 10 is formed between the side surface area 4 of the rotating mold 3 and the counter bearing 14 arranged opposite to the rotating mold 3. These two parts form the upper area and the bottom area of ​​the channel 10. In order to define the channel from the side, the channel 10 also has a side area, thereby closing the boundary of the channel 10.

[0118] like Figure 4 As shown, one or more static areas of the channel 10, namely the counter-bearing 14 and the side areas, can be replaced by one or more additional rotating dies.

[0119] Figure 4 The rotary mold assembly including four rotary molds is schematically shown. The channel 10 is defined by the first rotary mold 3, a second rotary mold 33 arranged opposite to the first rotary mold 3 and replacing the counter bearing 14, a third rotary mold 34 replacing one of the side areas, and a fourth rotary mold 35 arranged opposite to the third rotary mold 34.

[0120] Figure 4Just one example. The channel 10 may be defined by one or more rotating molds 3, 33, 34, 35. For example, the channel 10 may be defined by two rotating molds 3, 33, 34, 35, while the remaining areas defining the channel 10 are static. As another example, the channel 10 need not have a rectangular cross-section; the channel 10 may be defined by three areas forming a triangular cross-section, or by six areas forming a hexagonal cross-section, etc. One or more (possibly all) areas of the channel 10 may be defined by a specific rotating mold 3, 33, 34, 35. Each of the rotating molds 3, 33, 34, 35 may have a specific pattern on its side surface area for printing such a pattern on one side of the molding material.

[0121] The second, third and / or fourth rotary molds 33, 34, 35 may be arranged in a similar manner to the first rotary mold 3 to form the same or different patterns on both sides of the molding material. The second, third and / or fourth rotary molds 33, 34, 35 may include an annular recess and / or a flange portion, which may be arranged to cooperate with the annular recess and / or flange portion of the first rotary mold 3.

[0122] One or more rotating dies 3, 33, 34, 35 may be driven. According to one example, two or more rotating dies 3, 33, 34, 35 are synchronized. This has the advantage that the ceramic material is fed through the channel 10 at the same speed. However, non-synchronous rotating dies 3, 33, 34, 35 may also be used in order to generate friction and / or a special pattern and / or to compensate for material differences.

[0123] The extrusion device 1 may be arranged with a combination of textured and non-textured rotary dies 3 , 33 , 34 , 35 .

[0124] Figures 5 to 10 A co-extrusion device 1 and / or a single extrusion device 1 is schematically shown. Such an extrusion device comprises an extrusion and / or pultrusion device 1 according to any of the above examples, wherein the device 1 comprises at least two inlet channels 45, 46, 47, which are directly or indirectly connected to the channel 10. Each of the at least two inlet channels 45, 46, 47 is configured to supply one or more materials, at least one of which is a ceramic material, at a predetermined distance upstream of the channel 10 or at a junction of at least two inlet channels 45, 46, 47, the junction being connected to the location where the channel 9 transitions into the channel 10.

[0125] Here, coextrusion means processing at least two material flows together and forming the main profile and then forming the final profile, or processing the at least two material flows together and forming the final profile.

[0126] Here, single extrusion means that the at least two material flows are placed in a layered manner, processed together and formed into the main profile, and then the final profile is formed, or the at least two material flows are converged into the main profile at the joining point, and then processed together in the channel 10 and the connected at least two material flows are formed into the final profile.

[0127] Figure 5 Schematically shown is a cross-sectional side view of an extrusion device 1. The contour defining zone 7 comprises a first inlet channel 45 in the form of the channel 9 and a second inlet channel 46 in the form of a second channel, which is connected to the contour defining zone 7 upstream of the channel 10. The second channel supplies additional material from the channel 9 to the channel 10 to form a layered contour product 2 with ceramic material.

[0128] According to an example, the second channel 46 is an extrusion or pultrusion channel similar to the channel 9, arranged for processing material. According to an example, the second channel 46 is a channel configured as a conveyor unit for conveying a material to the contour definition area 7.

[0129] The device 1 further comprises an additional channel 46b arranged to guide another material to the ceramic material. Such channel 46b can be arranged to guide the another material to the side surface area 4 of the upstream rotating mold 3, wherein the side surface area 4 defines the channel 10. When the rotating mold 3 rotates, the side surface area 4 will carry the another material to the channel 10, wherein the another material is added to the ceramic material extrusion process. As an example, the another material can be a glazing material distributed on the surface of the molding material.

[0130] Figure 6 and Figure 7 The same device 1 is shown schematically, however the additional channel 46b is omitted in these figures. As previously mentioned, the device 1 comprises a rotating device 3 as described above and two material flows brought together via the channels 9, 46.

[0131] Figure 8 A cross-sectional side view of a device 1 comprising two opposing rotating moulds 3, 33 is schematically shown. Figure 8 The device 1 is also shown to include the channel 9 and a second channel 46 connected to the contour definition zone 7 upstream of the channel 10 for supplying additional material to the channel 10 , thereby forming a layered contour product 2 using material from the channel 9 . Figure 8It is also shown that the device 1 comprises a third channel 47 for supplying a third material to the contour defining area 7 .

[0132] According to one example, the third channel 47 is an extrusion or pultrusion channel similar to the channel 9 , arranged for processing material. According to one example, the channel 47 is a channel configured as a conveyor unit for conveying a material to the contour definition area 7 .

[0133] Fig. 9 Schematically shows a cross-sectional side view of a device 1, which comprises a rotating mold 3 and three channels 9, 45, 46 for combining Figure 8 The content in question supplies three different materials to the contour definition area 7 .

[0134] Fig. 9 An example is also shown in which the channel 45 conveys a solid material 50, such as a wire, a mesh, etc., to the channel 9, and the channels 46, 47 introduce one or more materials to be extruded or pultruded into the channel 9 and the channel 10. The one or more materials may be layered onto the solid material 50 or may surround the solid material 50.

[0135] Fig.10 The channel 45 is schematically shown as an example of conveying a continuous solid material 50 in the form of a wire, mesh or the like and a ceramic material to be extruded or pultruded in the channels 9 and 10. Fig.10 In the embodiment, the channels 45, 46 are arranged such that material from the channel 46 surrounds the solid material 50 and is embedded in the solid material 50. Fig.10 In the embodiment, the channel 46 comprises a pressurized chamber 51 upstream of the channel 9, the pressurized chamber 51 being used to form the ceramic material around the solid material 50. The pressurized chamber 51 comprises a rear wall 52 delimiting the pressurized chamber 51.

[0136] The channel 46 includes a feed channel 53 leading to the pressurized chamber 51 for supplying the material to the chamber 51. The rear wall 52 includes the channel 45, which conveys the solid material 50 and acts as a barrier to leakage of the ceramic material in the chamber through the channel 45. Here, "pressurized" means that the ceramic material in the channel 46 is subjected to pressure because the ceramic material is forced into the channel 46 and deforms in a manner similar to that described above with respect to the channel 9.

[0137] exist Fig.10In the embodiment, the passages 9 and the channels 10 plastically deform the material in a similar manner as described above. Plastic deformation may also occur in the pressurized chamber 51, but is not limited to such deformation. Therefore, the material in the pressurized chamber 51 can be formed to surround the solid material 50 without plastic deformation.

[0138] Here, "solid material" refers to a material that does not undergo any deformation in the contour definition area 7. Non-exhaustive examples of solid materials include: bendable wires, rigid rod-like elements, meshes of metal and / or fabric and / or composite materials and / or other suitable materials, combinations of these solid materials, etc.

[0139] refer to Figures 5 to 10 , the different materials are brought together before the channel 10 and then processed in the channel 10 as described above. The invention is not limited to three channels 9, 45, 46, 47, but there can be more channels, thereby producing ceramic products with the same or different materials between different layers.

[0140] According to any of the foregoing examples, the ceramic material fed into the device 1 to form the final ceramic product is a homogeneous material or a mixture of two or more mixed or layered materials. These materials can be mixed in different proportions and can be mixed into a homogeneous mixture or a mixture with a gradient inside the material. One material can be solid and the other material can be moldable, such as stone and clay, wherein the clay forms the ceramic material. The material can also be a layered material, including two or more layers of the same or different materials. The material can include one or more solid material lines throughout the entire extrusion or pultrusion process, such as a metal wire or another reinforcing material surrounded by the deformable material. Fibers can also be used as reinforcing materials.

[0141] According to one example, the maximum permissible pressure exerted by the rotating mold 3 at the position of the minimum distance D2 depends on the friction between the ceramic material and the counter-bearing 14 in the channel 10 .

[0142] According to one example, the device 1 is configured to supply a friction material between the counter-bearing 14 and the molding material and / or is configured to supply a friction material between the rotating mold 3 and the molding material.

[0143] According to one example, the friction material is delivered through any one of the channels 45 , 46 , 47 to control the friction associated with the rotating mold 3 and / or the counter-bearing 14 , at least during the activation of the device 1 .

[0144] According to one example, the friction material is delivered through any one of the channels 45 , 46 , 47 to control the friction associated with the rotating mold 3 and / or the counter-bearing 14 during a portion of the production process or during the entire production process.

[0145] According to one example, the friction material is directly supplied to the rotating mold 3 so that the friction material rotates with the rotating mold 3 from a position upstream of the channel 10. A friction material supply device may be any one of the channels 45, 46, 47. In addition, the friction material may be a solid material, a liquid or a gas or a combination thereof.

[0146] Now turn to Fig.11 and Fig.12 , some examples of ceramic products manufactured by a method according to an embodiment will be described.

[0147] In general, the present invention allows for the continuous shaping of a ceramic material which, after appropriate heat treatment, forms a ceramic product. Most preferably, the method described herein is used to produce a continuous profile of a shaped material which, after a separation operation, such as cutting, forms a series of identical or at least similar products. For example, the method can produce a profile cut at a specific location to produce a product of that specific length, while another part of the profile is cut at another location to produce a product of a different length. Thus, these products are not identical, but are similar because they are cut from the same profile.

[0148] Fig.11 and Fig.12 The ceramic product shown has been subjected to a heat treatment. Therefore, these figures also represent the shape of the shaped material, at least after separation from the continuous profile extruded in the extrusion device 1.

[0149] Fig.11 A plate-shaped ceramic product 60 is shown which is produced by forming a ceramic material using at least one rotary mold 3 and then heat treating it. The ceramic product 60 has an upper side 61, a lower side 62 and two opposite sides 63, 64. Each side 61, 62, 63, 64 is provided with a repeating pattern 61x, 62x, 63x, 64x formed by the associated rotary mold 3, 33, 34, 35. Therefore, in order to produce the ceramic product 60, four rotary molds 3, 33, 34, 35 must be used, with Figure 4 The example shown in .

[0150] The pattern 61x of the upper side 61 includes parallel transverse wavy protrusions formed by corresponding depressions of the rotating mold 3. The pattern 62x of the lower side 62 includes parallel longitudinal grooves formed by corresponding protrusions of the rotating mold 33. The first side 63 includes a pattern 63x of equally spaced protrusions, while the opposite side 63 includes a pattern 64x of equally spaced depressions. The patterns 63x, 64x on the opposite sides are matched so that the protrusions of the pattern 63x match the depressions of the pattern 64x.

[0151] Therefore, the ceramic product 60 can be used in an assembly requiring multiple ceramic products 60, because the cooperation of the sides 63, 64 makes it very easy to mate multiple products 60 with each other. For example, the ceramic product 60 can be a floor tile, wherein the pattern 61x of the upper side 61 provides a non-slip surface.

[0152] Fig.12 There is shown another example of a ceramic product 70. Here, the ceramic product 70 is in the shape of a brick rather than a plate, but is produced in a similar manner by forming a ceramic material using at least one rotating mold 3 and then performing a heat treatment.

[0153] The ceramic product 70 has an upper side 71, a lower side 72 and two opposite sides 73, 74. Each side 71, 72, 73, 74 may be provided with a repeating pattern 71x, 72x, 73x, 74x formed by the associated rotary mould 3, 33, 34, 35. Thus, in order to produce the ceramic product 70, four rotary moulds 3, 33, 34, 35 must be used, with Figure 4 The example shown in .

[0154] The pattern 71x of the upper side 71 comprises repeated protrusions arranged in rows and columns and formed by corresponding recesses of the rotating mold 3. The pattern 72x of the bottom side 72 may be completely planar or may comprise recesses matching the protrusions of the upper side 71.

[0155] The first side 73 comprises a pattern 73x of parallel wavy protrusions, while the opposite side 73 may be completely planar or comprise any type of protrusion or depression pattern 74x.

[0156] The ceramic product 70 can be used in assemblies that require multiple ceramic products 70, because the cooperation of the sides 71, 72 makes it very easy to mate multiple products 70 with each other. For example, the ceramic product 70 can be a brick, wherein the pattern 73x of the side 71 provides a better aesthetics for the final structure.

[0157] The ceramic product 70 is partially hollow in that a plurality of channels 75 extend longitudinally through the entire ceramic product 70 .

[0158] According to the above description, the ceramic products 60, 70 are formed by pressing or pulling a ceramic material through a channel at least partially defined by at least one rotating die, and subsequent heat treatment.

[0159] Examples of ceramic products are a brick or a plate-like product, such as a tile or a coating.

[0160] To improve the usability of the ceramic products, each or either side of the ceramic product may be provided with a profile that matches a corresponding profile on a side of another ceramic product. This means that two or more ceramic products 60, 70 may be connected together in a jigsaw-like manner, thereby providing new and improved methods for aligning and mating ceramic products to each other and to adjacent structures.

[0161] Due to the versatility of the rotational mold 3, the ceramic product can include a structured surface pattern corresponding to the pattern of the rotational mold.

[0162] Typically, the structured surface pattern is disposed on an upper side of the ceramic product 60 , 70 during its intended use and / or on a bottom side of the ceramic product 60 , 70 during its intended use.

[0163] As described above, the structural surface pattern on the bottom side of the ceramic product 60, 70 can form a mounting structure for the ceramic product. For example, the ceramic product can be an exterior wall tile or cladding, wherein during the extrusion process, the use of a rotating mold 33 acting on the bottom surface of the molding material, the suspension piece is integrally formed on the bottom side of the ceramic product.

[0164] The ceramic products 60, 70 may be included in different types of devices. For example, the ceramic products 60, 70 may form part of a thermal device, such as a heat exchanger, cooling profile and / or heating element. For example, the ceramic products 60, 70 may form part of a chemical reactor, such as a catalyst or a condenser. For example, the ceramic products 60, 70 may form an anti-slip device, such as forming part of the surface of the anti-slip device.

[0165] Now turn to Fig.13 , the method 200 for manufacturing the ceramic products 60, 70 will be further explained. Generally speaking, the method 200 includes two main steps 210, 250, and a plurality of optional steps ( Fig.13 marked with a dotted line).

[0166] Most commonly, the method 200 includes step 210 of forming a ceramic material by pressing or pulling the ceramic material through a channel 10 of an extrusion device 1, wherein the channel 10 is at least partially defined by a side surface area 4 of at least one rotating mold 1. In a subsequent step 250, the formed material is heat treated to form a ceramic product.

[0167] As mentioned above, the rotating mold 3 preferably imparts a repeating pattern to the molding material.

[0168] Depending on the type of ceramic material used in the method, the method 200 may further include step 252 of shrinking the molding material so that the pattern size of the rotational mold 3 is different from the pattern size of the ceramic products 60, 70. Preferably, the shrinking is caused after the step of forming the material, preferably during the heat treatment of the molding material.

[0169] During operation of the extrusion device 1, the method may perform step 208, i.e. regulating the flow of the ceramic material upstream of the channel 10, and / or step 212, i.e. driving the rotating mold 3. Step 212 is preferably performed in a manner that synchronizes the rotation of the rotating mold 3 with the speed of the downstream conveyor belt of the ceramic product.

[0170] A further optional step 214 may be performed, during which at least one dimension of the ceramic product is determined and the speed of the rotating mould 3 and / or the downstream conveyor belt is adjusted based on the determined dimension.

[0171] The step 250 of heat treatment can be performed in one or more sub-steps. For example, the step can include firing the ceramic material, but can also include an initial drying step. Typically, the drying step can be performed at room temperature or a relatively moderate temperature, while firing is performed using a higher temperature (e.g., 800 to 1500° C.). It is readily understood that the exact design of the step 250 of heat treatment must be selected based on the ceramic material used and the desired properties of the final ceramic product.

[0172] Another optional step 240 is separating an individual product from the molding material, which step may be performed before, during or after the heat treating step 250. Optionally, step 248 may be performed before the heat treating step 250, in which a plurality of individual products are mounted to each other.

[0173] Step 240 may be performed by a cutting action of the rotating mold 3, or by using a separate cutting station.

[0174] The method 200 may further include step 216 of adding another material to the ceramic material. Step 216 may be performed before, during or after the ceramic material passes through the rotating mold 3.

[0175] The additional material is, for example, embedded in the ceramic material to form a reinforcement of the ceramic product. The additional material may be a fiber material or a web material. The additional material may be added to the ceramic material as at least one layer. The additional material may be a liquid material or a solid material in powder or granular form. The additional material may include a variety of different ceramic and / or non-ceramic materials.

[0176] Step 216 may be performed by feeding the ceramic material and at least one additional material through the passageway.

[0177] The method 200 may further include step 218, i.e., adjusting the position of the rotating mold 3, thereby adjusting the size of the channel 10, and thereby adjusting the size of the ceramic product. The step 218 may be performed by changing the position of the rotating mold 3 relative to other regions of the channel 10, which may be defined by a plurality of static bearing surfaces or other rotating molds. Optionally, step 218 may be performed by arranging the rotation axis of the rotating mold 3 at an angle relative to the production direction, preferably, the rotating mold is arranged at an angle of 90°±25° relative to the production direction.

[0178] An optional step 220 may also be performed, which consists in providing the channel 10 with at least one core, the core forming a hollow portion 75 of the ceramic product 60 , 70 .

[0179] Step 222 may also be performed, wherein the channel 10 provides a first structural surface pattern defined by a side surface area of ​​at least one rotating mold 3 for one side of the molding material, and provides a second structural surface pattern defined by a side area of ​​another rotating mold 33, 34, 35 for the opposite side of the molding material. When a plurality of ceramic products are stacked on top of each other, the first and second structural surface patterns will provide a matching fit.

[0180] It should be noted that although the method 200 is described as a series of steps, these steps can be performed in any suitable order, and can even be performed simultaneously. In particular, the extrusion portion of the method 200 is preferably performed continuously, which means that many of the above steps are performed simultaneously and repeatedly.

[0181] In summary, the present disclosure proposes an improved method for processing a ceramic material to form a ceramic product. The ceramic material is fed through a channel 9, in which a main profile 36 is formed, and the ceramic material is further fed to a channel at least partially defined by at least one rotating mold 3, in which the main profile 36 is transformed into a final profile 37. The final profile 37 is transformed into a ceramic product 60, 70 by heat treatment.

[0182] From the above it emerges that, although various embodiments of the invention have been described and shown, the invention is not restricted thereto but may also be embodied in other ways within the scope of the subject-matter defined in the following claims.

Claims

1. A production method, characterized in that: The production method comprises the following steps: forming the material by extruding or pulling the ceramic material through a plurality of bearing surfaces defining an extrusion die channel, the plurality of bearing surfaces including at least one rotating bearing surface, the at least one rotating bearing surface being a surface of a rotating die defining a cross-section of the formed material, such that the channel is at least partially defined by a side surface area of ​​at least one rotating die; and The molded material is heat treated to form a ceramic product.

2. The production method according to claim 1, characterized in that: The rotational mold imparts a pattern to the molding material.

3. The production method according to claim 2, characterized in that: The rotational mold imparts a repeating pattern to the molding material.

4. The production method according to claim 2 or 3, characterized in that: The production method further includes shrinking the molding material so that a pattern size of the rotational mold is different from a pattern size of the ceramic product.

5. The production method according to claim 4, characterized in that: The shrinkage is caused after the step of forming the material, preferably during heat treatment of the shaped material.

6. The production method according to any one of the preceding claims, characterized in that: The production method also includes regulating the flow rate of the ceramic material upstream of the channel.

7. The production method according to any one of the preceding claims, characterized in that: The production method further includes driving the rotating mold.

8. The production method according to claim 7, characterized in that: Driving the rotating mold further includes synchronizing the rotation of the rotating mold with the speed of the ceramic product downstream conveyor.

9. The production method according to claim 7 or 8, characterized in that: The production method further comprises determining at least one dimension of the ceramic product and adjusting the speed of the rotating mold and / or the downstream conveyor belt according to the determined dimension.

10. The production method according to any one of the preceding claims, characterized in that: The heat treatment is performed by firing the molded material.

11. The production method according to any one of the preceding claims, characterized in that: The production method also includes separating a separate product from the molded material before, during or after the heat treatment.

12. The production method according to claim 11, characterized in that: The production method further comprises installing a plurality of individual products to one another prior to the step of heat treating.

13. The production method according to claim 11 or 12, characterized in that: Separation of an individual product is performed by the cutting action of the rotating die.

14. The production method according to any one of claims 11 to 13, characterized in that: The circumference of the rotating mold is equal to the length of the individual products.

15. The production method according to any one of claims 11 to 13, characterized in that: The circumference of the rotating mold is different from the length of the individual products.

16. The production method according to any one of the preceding claims, characterized in that: The channel has a longitudinal extension in a production direction, and wherein the rotation axis of the rotary mould is arranged at a certain angle relative to the production direction, preferably the rotary mould is arranged at an angle of 90°±25° relative to the production direction.

17. The production method according to any one of the preceding claims, characterized in that: The channel is defined by a bottom region, an upper region and two opposite side regions, which together form a closed space, wherein at least a portion of one of the regions is formed by a side surface region of the at least one rotating mold.

18. The production method according to claim 17, characterized in that: At least a portion of the at least one further region is defined by a side surface region of another rotational mold.

19. The production method according to claim 17 or 18, characterized in that: At least one of the bottom region, the upper region and the two opposing side regions is defined by a bearing surface.

20. The production method according to any one of the preceding claims, characterized in that: The production method also includes pressing or pulling the ceramic material through a preload channel disposed upstream of the rotating die.

21. The production method according to claim 20, characterized in that: The preload channel is disposed immediately upstream of the rotating die.

22. The production method according to claim 20, characterized in that: The preload channel is disposed upstream of the rotating mold but away from the rotating mold.

23. The production method according to any one of claims 20 to 22, characterized in that: The pre-load channel is configured to deform the ceramic material into a primary profile, and the channel is configured to further deform the ceramic material into a final profile.

24. The production method according to any one of claims 20 to 23, characterized in that: The dimensions of the preload channel are static.

25. The production method according to any one of the preceding claims, characterized in that: The side surface area of ​​the rotating mold is provided with a topographic pattern.

26. The production method according to claim 25, characterized in that: The topographic pattern includes at least one protrusion configured to form a separation recess in the ceramic product and / or to significantly reduce the thickness of the ceramic product locally.

27. The production method according to claim 26, characterized in that: The substantial reduction in thickness of the ceramic product defines a removable portion of the ceramic product.

28. The production method according to claim 26 or 27, characterized in that: The at least one protrusion extends across the entire width of the rotating mold, or extends across a portion of the width of the rotating mold.

29. The production method according to any one of claims 26 to 28, characterized in that: The protrusions extend across the width of the rotating mold in a linear or curvilinear manner.

30. The production method according to any one of the preceding claims, characterized in that: The production method also includes adding a further material to the ceramic material.

31. The production method according to claim 30, characterized in that: The addition of the additional material is performed before, during or after the ceramic material passes through the rotating mold.

32. The production method according to claim 30 or 31, characterized in that: The further material is embedded in the ceramic material to form a reinforcement of the ceramic product.

33. The production method according to claim 32, characterized in that: The additional material is a fibrous material or a web material.

34. The production method according to claim 30 or 31, characterized in that: The further material is added as at least one layer to the ceramic material.

35. The production method according to claim 34, characterized in that: The further material is a liquid material or a solid material in powder or granular form.

36. The production method according to any one of claims 30 to 35, characterized in that: The additional materials include a variety of different ceramic and / or non-ceramic materials.

37. The production method according to claim 27, characterized in that: The ceramic material and the at least one further material are supplied through the passage.

38. The production method according to any one of the preceding claims, characterized in that: The production method further includes adjusting the position of the rotating mold to adjust the size of the channel.

39. The production method according to any one of the preceding claims, characterized in that: The production method further comprises providing at least one mould core for the channel, the mould core forming a hollow part of the ceramic product.

40. The production method according to any one of the preceding claims, characterized in that: The ceramic product is a brick or a plate-shaped product, such as a tile.

41. The production method according to any one of the preceding claims, characterized in that: The channel provides a first structured surface pattern defined by a side surface area of ​​at least one rotating mold to one side of the molding material, and a second structured surface pattern defined by a side surface area of ​​another rotating mold to an opposite side of the molding material.

42. The production method according to claim 41, characterized in that: When a plurality of ceramic products are stacked together, the first structured surface pattern and the second structured surface pattern will provide a matching fit.

43. A ceramic product formed by extruding or pulling the ceramic material through a plurality of bearing surfaces defining an extrusion die channel to form the ceramic material, characterized in that: The plurality of bearing surfaces include at least one rotating bearing surface, which is a surface of a rotating mold that defines a cross-section of the molding material, such that the channel is at least partially defined by at least one rotating mold, and is subsequently heat treated to form the ceramic product.

44. The ceramic product according to claim 43, characterized in that: The ceramic product is a brick or a plate-like product, such as a tile or a coating.

45. A ceramic product according to claim 43 or 44, characterized in that: The ceramic product comprises a plurality of side surfaces, wherein each side surface is provided with a contour matching a corresponding contour of a side surface of another ceramic product.

46. ​​A ceramic product according to any one of claims 43 to 45, characterized in that: The ceramic product includes a structured surface pattern corresponding to the pattern of the rotational mold.

47. The ceramic product according to claim 46, characterized in that: The structured surface pattern is disposed on an upper side of the ceramic product during intended use of the ceramic product.

48. The ceramic product according to claim 47, characterized in that: The ceramic product further comprises a structured surface pattern on its bottom side during the intended use of the ceramic product.

49. The ceramic product according to claim 48, characterized in that: The structured surface pattern on the bottom side of the ceramic product forms a plurality of mounting structures for the ceramic product.

50. The ceramic product of claim 48, wherein: The plurality of corresponding structured surface patterns provide a fit when a plurality of ceramic products are stacked on top of each other.

51. A ceramic product according to any one of claims 43 to 50, characterized in that: The ceramic product comprises at least one further material.

52. An apparatus comprising at least one ceramic product according to any one of claims 43 to 51.

53. The device according to claim 52, characterized in that: The device is a thermal device and wherein the ceramic product forms part of a heat exchanger, a cooling profile and / or a heating element.

54. The device of claim 52, wherein: The device is a chemical reactor and wherein the ceramic product forms part of a catalyst or a condenser.

55. The device of claim 52, wherein: The device is an anti-slip device, and wherein the ceramic product forms a surface of the anti-slip device.