Method for producing alpha-alumina powder
By using organosilane compounds to treat and control the calcination conditions of alumina raw material powder, the problem of calcium and sodium impurities in alumina powder was solved, resulting in a reduction in calcium concentration and suppression of BET specific surface area, thus improving filling performance and thermal conductivity.
Patent Information
- Application Number
- CN202380031238.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-12
AI Technical Summary
In existing alumina powder manufacturing methods, the presence of impurities such as calcium and sodium leads to deterioration of insulation, and existing technologies are difficult to remove them effectively, resulting in deterioration of filling and formability, and an increase in BET specific surface area.
The alumina raw material powder is immersed in an aqueous solution of an organosilane compound containing hydrolyzable groups. After the treatment process, the calcium and sodium concentrations are reduced, and the particle size and BET specific surface area are controlled. Halogen mineralizers and appropriate calcination temperatures and pulverization methods are used.
It effectively reduces the concentration of calcium and sodium in alumina powder, inhibits the increase of BET specific surface area, improves filling and formability, and enhances thermal conductivity and insulation.
Smart Images

Figure BDA0005063957270000091 
Figure BDA0005063957270000151 
Figure BDA0005063957270000201
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing alpha-alumina powder. Background Art
[0002] α-alumina (Al2O3) is chemically stable, and has excellent heat resistance, corrosion resistance, wear resistance, and insulation, as well as high strength and hardness. Taking advantage of these characteristics, α-alumina powder is widely used in various applications such as structural parts, tools, abrasives, fillers (filling materials), spark plugs, insulators, electronic substrates, and refractories.
[0003] In particular, α-alumina powder is currently used as a heat dissipation filler due to its high chemical stability, electrical insulation and thermal conductivity. Specifically, alumina powder is filled into resin or rubber to make a resin composition, and the resin composition itself or a molded body of the resin composition is applied to products such as heat sinks, optical pickup parts, heat dissipation paste, potting agents for circuit boards, belts or parts with heat dissipation properties, various injection molded products, sealing materials for motors or ICs, or copper-clad laminated boards.
[0004] However, aluminum oxide used in industry is mainly produced by the Bayer process. In the Bayer process, aluminum ore, i.e., bauxite, is subjected to high-temperature treatment with a sodium hydroxide solution to extract the aluminum oxide component. Then, after the extraction residue is separated, seed crystals are added to the obtained sodium aluminate solution to crystallize aluminum hydroxide (Al(OH)3). After the aluminum hydroxide is separated and washed, it is calcined at a temperature above 1000°C to obtain aluminum oxide. The Bayer process has the advantage of being able to produce aluminum oxide powder at a low cost.
[0005] However, the alumina powder produced by the Bayer process generally contains impurities from the raw materials and the production process. For example, since sodium hydroxide is used in the production, sodium (sodium; Na) components remain in the alumina powder. In addition, the raw material bauxite also contains calcium (Ca) as an impurity. Moreover, in the production of the Bayer process, calcium compounds such as slaked lime are often added to decompose the sodium carbonate accumulated in the sodium aluminate solution. Therefore, the obtained alumina powder contains calcium (Ca) components or sodium (Na) components as impurities.
[0006] Such impurities often become a problem when alumina powder is applied to products. In particular, when used as a heat dissipation filler filled in resin or rubber, the electrical properties of the product, such as insulation, may be degraded. For example, as an insulating material for electric plugs, vinyl chloride resin containing fillers is mostly used. If the filler contains a large amount of calcium (Ca), the chlorine generated by the thermal degradation of the vinyl chloride resin sometimes reacts with the calcium in the filler and bonds. If this reaction occurs, the insulation of the material will deteriorate, and sometimes a fire may occur depending on the situation. In addition, in the case of using epoxy resin containing fillers to form a printed circuit board or a semiconductor device, if the filler contains a large amount of impurities such as calcium or sodium, the insulation reliability of the material will deteriorate. In addition, for alumina used in secondary batteries, there are reports that impurities such as calcium increase the resistivity.
[0007] Therefore, technologies for reducing impurities in alumina powder have been proposed. For example, Patent Document 1 proposes a method for producing α-alumina, wherein aluminum hydroxide or transition alumina obtained by the Bayer process is pulverized and then calcined at a temperature of 600 to 1400° C. in an atmosphere containing hydrogen chloride gas (claim 1 of Patent Document 1). In addition, Patent Document 1 also describes that high-purity α-alumina having a sodium content of less than 40 ppm and an iron content of less than 20 ppm can be obtained, and that α-alumina having a reduced calcium content can be obtained by washing the calcined α-alumina (
[0017] and
[0037] of Patent Document 1).
[0008] Patent document 2 discloses a method for producing α-alumina, wherein aluminum hydroxide obtained by the Bayer process is calcined using a calcination container containing Al2O3 and SiO2 in a specified amount, and the obtained α-alumina is washed (claims of patent document 2). In addition, patent document 2 also records that high-purity α-alumina in which impurity metals such as Si, Fe, Ca, and Na are removed as much as possible can be simply and inexpensively produced by adding α-alumina to repulping water to slurry it and stirring and washing it, and then washing it while passing pure water and filtering it with suction (
[0021] and
[0021] in patent document 2). Prior art literature Patent Literature
[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 8-290914 Patent Document 2: Japanese Patent Application Publication No. 2008-150238 Summary of the invention Technical problem to be solved by the invention
[0010] As described above, methods for producing α-alumina powder with less impurities have been proposed so far, but there is still room for improvement in the existing methods. For example, in the method of Patent Document 1, the crushed aluminum hydroxide or transition alumina is fired in an atmosphere containing hydrogen chloride. Therefore, equipment such as a firing furnace must be made of a material that is not corroded by hydrogen chloride gas. In addition, in order to prevent the leakage of toxic hydrogen chloride gas, the firing furnace must also be made airtight, which leads to an increase in manufacturing costs.
[0011] The method proposed in Patent Document 2 can relatively easily obtain alumina powder with reduced sodium (Na) content, which is effective to a certain extent. However, the inventors have found that although the method of Patent Document 2 reduces the sodium (Na) content by washing, the reduction of calcium (Ca) content has not been confirmed. In order to obtain alumina powder with less calcium, it is necessary to reduce the calcium content of aluminum hydroxide, which is its raw material. For this purpose, it is necessary to use a sodium aluminate solution and seed crystals with higher purity, or design a manufacturing device such as a container used for crystallization, which has the problem of increasing costs.
[0012] Moreover, if the alumina powder obtained by the method of patent document 2 is filled into a resin or rubber as a heat dissipation filler to prepare a resin composition, the filling property of the alumina powder may deteriorate, and the viscosity of the resin composition may become too high. If the filling property deteriorates, the uniform dispersion of the alumina powder in the resin composition may be hindered, and the thermal conductivity of the product made of the resin composition may be reduced. If the viscosity of the resin composition is too high, it may be difficult to shape the composition. In addition, in order to find out the cause of the deterioration of the filling property, the inventors have found that in the method proposed in patent document 2, the BET specific surface area of the alumina powder increases during the water washing treatment. Therefore, it is believed that the increase in the BET specific surface area leads to the deterioration of the filling property and the formability. Among them, as the cause of the increase in the BET specific surface area, it is believed that it is due to the hydration of the alumina powder by the water washing treatment.
[0013] Under such circumstances, the inventors conducted further research and found that the calcium (Ca) concentration in the α-alumina powder can be reduced by a simple method of treating the α-alumina powder in an aqueous solution containing an organic silane compound having a hydrolyzable group. It was also found that such treatment can inhibit the hydration of the α-alumina powder and the resulting increase in the BET specific surface area.
[0014] The present invention has been accomplished based on such findings, and the technical problem to be solved is to provide a method for producing an alumina powder having a reduced calcium (Ca) concentration by a simple method while suppressing an increase in the BET specific surface area caused by hydration. Solutions to technical problems
[0015] The present invention includes the following embodiments (1) to (17). In addition, in this specification, the expression "to" includes both numerical values. That is, "X to Y" is synonymous with "X or more and Y or less".
[0016] (1) A method for producing α-alumina powder, comprising: a treatment step in which the α-alumina raw material powder is placed in and immersed in a treatment aqueous solution containing an organic silane compound having a hydrolyzable group, thereby obtaining an α-alumina powder having a reduced calcium (Ca) concentration; and An evaluation step of measuring and comparing the concentration of calcium contained in the α-alumina raw material powder and the concentration of calcium contained in the α-alumina powder.
[0017] (2) The method according to (1) above, wherein the treatment aqueous solution contains the organosilane compound in a ratio of 0.10 mass % or more relative to the mass of the α-alumina raw material powder.
[0018] (3) The method according to (1) or (2) above, wherein the organosilane compound is at least one selected from the group consisting of alkoxysilane, vinyl-containing silane coupling agent, and epoxy-containing silane coupling agent.
[0019] (4) A method as described in any one of (1) to (3) above, wherein in the evaluation step, the CaO-converted concentration of the soluble calcium component contained in the α-alumina raw material powder (c1[f-CaO]) and the CaO-converted concentration of the soluble calcium component contained in the α-alumina powder (c2[f-CaO]) are measured, and the soluble calcium concentration ratio (c2[f-CaO] / c1[f-CaO]) is further calculated.
[0020] (5) The method according to (4) above, wherein the soluble calcium concentration ratio (c2[f-CaO] / c1[f-CaO]) is less than 0.90.
[0021] (6) A method as described in any one of (1) to (5) above, wherein the CaO conversion concentration (c2[T-CaO]) of all calcium components contained in the above-mentioned α-alumina powder is less than 0.030 mass%, and the CaO conversion concentration (c2[f-CaO]) of soluble calcium components is less than 0.010 mass%.
[0022] (7) A method as described in any one of (1) to (8) above, wherein the Na2O conversion concentration (c2[T-Na2O]) of all sodium components contained in the above-mentioned α-alumina powder is less than 0.10 mass%, and the Na2O conversion concentration (c2[f-Na2O]) of the soluble sodium component is greater than 0.001 mass% and less than 0.015 mass%.
[0023] (8) A method as described in any one of (1) to (7) above, wherein the SiO2 conversion concentration (c2[SiO2]) of the silicon component contained in the above-mentioned α-alumina powder is greater than 0.030 mass% and less than 0.500 mass%.
[0024] (9) A method as described in any one of (1) to (8) above, wherein the difference (|c2[SiO2] - c1[SiO2]|) between the SiO2 conversion concentration (c1[SiO2]) of the silicon component contained in the above-mentioned α-alumina raw material powder and the SiO2 conversion concentration (c2[SiO2]) of the silicon component contained in the above-mentioned α-alumina powder is greater than 0.001 mass%.
[0025] (10) A method as described in any one of (1) to (9) above, wherein the 45 μm unsieved amount of the above-mentioned α-alumina raw material powder is less than 100 ppm.
[0026] (11) The method according to any one of (1) to (10) above, wherein the average particle size (Dp50) of the α-alumina powder is not less than 2.0 μm and not more than 5.0 μm.
[0027] (12) A method as described in any one of (1) to (11) above, wherein the BET specific surface area of the α-alumina powder is 1.0 m 2 / g or more and 3.5m 2 / g or less.
[0028] (13) A method as described in any one of (1) to (12) above, wherein the span value ((Dp90-Dp10) / Dp50) represented by the cumulative 10% diameter (Dp10), the cumulative 50% diameter (Dp50) and the cumulative 90% diameter (Dp90) in the particle size distribution of the α-alumina powder based on mass is less than 2.0.
[0029] (14) The method according to any one of (1) to (13) above, further comprising: A preparation step in which a halogen-based mineralizer is added and mixed to aluminum hydroxide obtained by the Bayer process to prepare a mixture, and then the mixture is fired at a temperature of 1100° C. to 1600° C. to prepare a fired product, and the fired product is further pulverized to prepare the α-alumina raw material powder.
[0030] (15) A method as described in (14) above, wherein the Na2O conversion concentration (c0[T-Na2O]) of all sodium components contained in the above-mentioned aluminum hydroxide is less than 0.3 mass%.
[0031] (16) The method of (14) or (15) above, wherein, when the mixture is fired, the mixture is filled into a firing container made of alumina ceramic containing silicon dioxide and fired to produce a molding density of 2.05 g / cm at a molding pressure of 98.07 MPa. 3 Above and BET specific surface area is 0.9m 2 / g or less of the fired product.
[0032] (17) The method according to any one of (14) to (16) above, wherein when the calcined product is pulverized to produce the α-alumina raw material powder, the average particle size (Dav) of the α-alumina raw material powder is 0.0447 W / m / s relative to the BET equivalent particle size (Dav) of the calcined product. BET ) ratio (Dav / D BET ) falls within the range of 1.0 to 2.0, the fired product is crushed. Effects of the Invention
[0033] According to the present invention, there is provided a method for producing an alumina powder having a reduced calcium (Ca) concentration by a simple method while suppressing an increase in the BET specific surface area due to hydration. DETAILED DESCRIPTION
[0034] Hereinafter, a specific embodiment of the present invention (hereinafter referred to as "this embodiment") will be described. In addition, the present invention is not limited to the following embodiment, and various changes can be made within the scope of not changing the gist of the present invention.
[0035] <Method for producing α-alumina powder> The method for producing α-alumina powder of the present embodiment comprises: a treatment step, in which α-alumina raw material powder is put into and immersed in a treatment aqueous solution containing an organic silane compound having a hydrolyzable group, thereby obtaining α-alumina powder with a reduced calcium (Ca) concentration; and an evaluation step, in which the concentration of calcium contained in the α-alumina raw material powder and the concentration of calcium contained in the α-alumina powder are measured and compared. In addition, as required, the production method of the present embodiment may further comprise: a preparation step, in which a halogen-based mineralizer is added and mixed to aluminum hydroxide obtained by the Bayer process to produce a mixture, and then the obtained mixture is fired at a temperature of 1100° C. or more and 1600° C. or less to produce a fired product, and the obtained fired product is further pulverized to produce α-alumina raw material powder. The details of each step are described below.
[0036] <Preparation process> In the preparation process, first prepare α-alumina raw material powder. α-alumina raw material powder is a raw material for processing to produce α-alumina powder as a final product. α-alumina raw material powder contains α-alumina (Al2O3) as a main component. α-alumina has a corundum-type crystal structure of a trigonal system. In addition, it has the characteristics of chemical stability, excellent heat resistance, corrosion resistance, wear resistance, insulation, thermal conductivity, and high strength and hardness. As long as the α-alumina raw material powder contains α-alumina as the main component, its preparation method is not particularly limited. For example, it can be manufactured by the Bayer process. Alternatively, it can be manufactured by directly thermally decomposing aluminum salts such as aluminum sulfate, or by reacting oxygen or water vapor with aluminum chloride vapor, or by neutralizing aluminum salts.
[0037] It is preferred to use an α-alumina raw material powder produced by the Bayer process. The Bayer process is the main method for producing α-alumina powder, and has the advantage of being able to produce α-alumina powder at a low price. It is particularly preferred to add and mix a halogen mineralizer to aluminum hydroxide (Al(OH)3) obtained by the Bayer process to produce a mixture, then sinter the resulting mixture at a temperature of 1100°C to 1600°C to produce a sintered product, and further pulverize the resulting sintered product to produce an α-alumina raw material powder. In this way, it is possible to easily obtain an alumina powder with less impurities, a desired average particle size, and a sharp particle size distribution.
[0038] Aluminum hydroxide is the aluminum source of α-alumina powder. The Na2O conversion concentration (c0[T-Na2O]) of all sodium contained in aluminum hydroxide is preferably below 0.3 mass%. In addition, the average secondary particle size of aluminum hydroxide is preferably above 10 μm and below 200 μm, more preferably above 30 μm and below 150 μm. Here, the average secondary particle size is a value measured by a laser scattering particle size distribution analyzer. By using such aluminum hydroxide, it is possible to more reliably obtain α-alumina powder having a desired average particle size and a sharp particle size distribution.
[0039] Halogen mineralizers have the effect of promoting the crystallization of α-alumina. As halogen mineralizers, there can be cited: fluoride mineralizers such as aluminum fluoride, sodium fluoride, cryolite, magnesium fluoride, calcium fluoride, etc.; chloride mineralizers such as hydrogen chloride, ammonium chloride, aluminum chloride; iodide mineralizers such as ammonium iodide. The optimal addition amount of the halogen mineralizer varies depending on the type of mineralizer used. Therefore, it is difficult to clearly determine the optimal addition amount. For example, in the case of a fluoride mineralizer, the addition amount of the mineralizer in the mixture is preferably 0.05 mass% or more and 1.0 mass% or less in terms of fluorine conversion, and more preferably 0.1 mass% or more and 0.5 mass% or less.
[0040] The mixture is fired at a temperature of 1100°C to 1600°C. If the firing temperature is lower than 1100°C, the primary particles will not grow to the desired size, and if it exceeds 1600°C, the particles will fuse, and the operability of the obtained alumina powder may be deteriorated. The firing time is usually 1 minute to 24 hours, preferably 1 hour to 20 hours. The firing can be performed using a known firing furnace such as a continuous furnace such as a tunnel kiln or a batch electric furnace.
[0041] The mixture is preferably filled into a silicon dioxide-containing alumina ceramic sintering container and sintered to produce a molded product with a density of 2.05 g / cm at a molding pressure of 98.07 MPa. 3 Above and BET specific surface area is 0.9m 2 / g or less. If the molding density is less than 2.05g / cm 3 , the shape of the particles in the obtained alumina powder is likely to be plate-shaped. Therefore, when the alumina powder is filled into a resin or rubber to prepare a resin composition, the viscosity of the resin composition may become too high. The molding density is more preferably 2.1 g / cm 3 Above and 2.5g / cm 3 In addition, the BET specific surface area exceeds 0.9 m 2 / g of the calcined product, the particle growth caused by calcination is insufficient. Therefore, it may be difficult to obtain an alumina powder having a desired average particle size and a sharp particle size distribution. In addition, the molding density and BET specific surface area of the calcined product can be adjusted by controlling the manufacturing conditions of the α-alumina raw material powder, such as the particle size of aluminum hydroxide, the amount of halogen-based mineralizer added and / or the calcination temperature and calcination time.
[0042] The pulverization of the calcined product can be carried out by a known method. For example, a vibration mill; a container-driven medium mill such as a vibration ball mill, a rotary ball mill or a planetary mill; a medium stirring mill such as an attritor; an air flow mill such as a jet mill, a reverse jet mill, and a jet miser can be used. By pulverizing, an α-alumina raw material powder can be obtained.
[0043] It is preferred that the average particle size (Dav) of the α-alumina raw material powder obtained by pulverization is equal to the BET equivalent particle size (D BET ) ratio (Dav / D BET The fired product is crushed under the condition that the ratio (Dav / D BET) exceeds 2.0, the pulverization is insufficient. Therefore, the final α-alumina powder will contain a large number of prickly chestnut-shaped or pumice-shaped agglomerated particles. Moreover, the agglomerated particles will absorb the resin or rubber. Therefore, when the α-alumina powder (sintered product) is filled into the resin or rubber to prepare a resin composition, there is a problem of increased viscosity of the resin composition. BET ) is less than 1.0, the pulverization is excessive. A large number of debris particles (fine particles) are generated, and coarse particles formed by the aggregation of the debris particles are generated. As a result, it may be difficult to uniformly disperse the final α-alumina powder in the resin or rubber.
[0044] Here, the average particle size (Dav) is equivalent to the 50% cumulative diameter (Dp50) in the particle size distribution of the α-alumina raw material powder based on mass (volume). The particle size distribution can be measured by a laser scattering particle size distribution analyzer. In addition, the BET equivalent diameter (D BET ) was measured by measuring the BET specific surface area (S BET ), and the BET specific surface area obtained was calculated using the following formula (1). In the following formula (1), ρ is the true specific gravity of α-alumina (3.98 g / cm 3 ).
[0045]
Number 1
[0046] <Processing process> In the treatment process, the prepared α-alumina raw material powder is put into and immersed in a treatment aqueous solution containing an organic silane compound having a hydrolyzable group. As a result, calcium (Ca) is dissolved in the treatment aqueous solution, and as a result, an α-alumina powder with a reduced calcium concentration can be obtained. Moreover, since the sodium (Na) component is also dissolved in the treatment aqueous solution, an α-alumina powder with not only reduced calcium but also reduced sodium content can be obtained. The detailed reason is not clear, but it is speculated that the impurities (Ca, Na) in the α-alumina raw material powder form a water-soluble complex with the organic silane compound, resulting in the impurities being easily dissolved in the aqueous solution.
[0047] In particular, according to the treatment of this embodiment, the concentration of impurities (Ca, Na) attached to the surface of the alumina powder can be effectively reduced. That is, the impurities include impurities attached to the surface of the powder and impurities present inside the powder. The impurities attached to the surface of the powder are soluble components that are easily dissolved in the treatment aqueous solution. Therefore, by immersing in the treatment aqueous solution, the impurities attached to the surface of the alumina powder can be easily removed.
[0048] Moreover, according to the method of this embodiment using an aqueous solution containing an organic silane compound, the hydration of the α-alumina powder can be suppressed to prevent an excessive increase in the BET specific surface area. Therefore, when the obtained α-alumina powder is filled into a resin or rubber to prepare a resin composition, the problem of deterioration of filling and formability due to an increase in the BET specific surface area can be prevented. In contrast, in the existing method of removing the sodium (Na) component by washing the α-alumina powder with water, the α-alumina powder will hydrate and the BET specific surface area will increase excessively. Moreover, water washing cannot fully remove the calcium (Ca) component.
[0049] The detailed reason why the hydration of the α-alumina powder is suppressed by the method of this embodiment is not clear, but it is presumed that the organic silane compound in the aqueous solution is adsorbed on the surface of the α-alumina powder and inhibits hydration by some mechanism.
[0050] Furthermore, according to the method of this embodiment, since the surface of the obtained α-alumina powder is modified by silane, when the α-alumina powder is used as a heat dissipation filler filled in resin or rubber, the compatibility or adhesion with the resin or rubber can be improved.
[0051] In addition, in the method of this embodiment, the α-alumina raw material powder is put into the treatment aqueous solution in the state of dry powder. That is, if the α-alumina raw material powder is dispersed in water in advance to make it slurry, the powder will be hydrated in this stage. Therefore, it is important to put the α-alumina raw material powder into the treatment aqueous solution in the state of dry powder rather than in the state of slurry.
[0052] As long as the organosilane compound has a hydrolyzable group, its type is not limited. For example, silane or silane coupling agent can be cited. As silane, alkoxysilane, silazane and siloxane can be cited. As silane coupling agent, silane coupling agent containing vinyl, epoxy, styryl, methacryl, acryl and / or amino can be cited. The organosilane compound is preferably selected from at least one of methylsilane, vinyl-containing silane coupling agent and epoxy-containing silane coupling agent, and is particularly preferably selected from at least one of methyltrimethoxysilane, vinyltrimethoxysilane, 3-glycidyloxypropyltrimethoxysilane and 3-glycidyloxypropylmethyldimethoxysilane.
[0053] The content of the organosilane compound in the treated aqueous solution is not limited. However, the more the content of the organosilane compound, the more effectively the impurities (Ca, Na) can be removed. The treated aqueous solution preferably contains the organosilane compound in a ratio of 0.10% by mass or more relative to the mass of the α-alumina powder, more preferably contains the organosilane compound in a ratio of 0.25% by mass or more, further preferably contains the organosilane compound in a ratio of 0.50% by mass or more, and particularly preferably contains the organosilane compound in a ratio of 1.00% by mass or more. If expressed in molar amount, the treated aqueous solution preferably contains the organosilane compound in a ratio of 0.0007mol / kg or more per 1kg of the mass of the α-alumina powder, more preferably contains the organosilane compound in a ratio of 0.0010mol / kg or more, further preferably contains the organosilane compound in a ratio of 0.0050mol / kg or more, and particularly preferably contains the organosilane compound in a ratio of 0.0110mol / kg or more.
[0054] On the other hand, even if the content of the organosilane compound is too much, the effect of removing impurities (Ca, Na) will not be higher. Moreover, silicon (Si) from the organosilane compound may be excessively mixed into the α-alumina powder in large quantities. The organosilane compound also plays the role of a binder for the alumina particles. Therefore, if there are a large amount of organosilane compounds, the particles in the alumina powder will sometimes agglomerate. If particle aggregation occurs, it is necessary to perform strong crushing in the subsequent steps to resolve the agglomeration, which will lead to the problem of increased BET specific surface area of the alumina powder. The treatment aqueous solution may contain the organosilane compound in a ratio of 20.00 mass % or less relative to the mass of the α-alumina powder, may contain it in a ratio of 10.00 mass % or less, may contain it in a ratio of 5.00 mass % or less, and may contain it in a ratio of 3.00 mass % or less. If expressed in molar amount, the treated aqueous solution may contain the organosilane compound in a ratio of 1.35 mol / kg or less per 1 kg of the mass of the α-alumina powder, may contain it in a ratio of 1.00 mol / kg or less, may contain it in a ratio of 0.68 mol / kg or less, or may contain it in a ratio of 0.45 mol / kg or less.
[0055] There is no limit to the impregnation time of the α-alumina raw material powder. However, the longer the impregnation time, the more effectively the impurities (Ca, Na) are removed. The impregnation time can be more than 0.5 hours, more than 1 hour, or more than 10 hours. On the other hand, even if the impregnation time is too long, the impurity removal effect will not be higher. Moreover, silicon (Si) from the organosilane compound may be excessively mixed in large quantities into the α-alumina powder. The impregnation time can be less than 100 hours, less than 50 hours, or less than 30 hours.
[0056] As long as the α-alumina raw material powder is immersed in the treatment aqueous solution, the treatment method is not limited. The treatment aqueous solution into which the α-alumina raw material powder is added can be left to stand, or it can be stirred. However, it is preferred to treat the treatment aqueous solution while stirring. This is because stirring promotes the dissolution of impurities (Ca, Na) in the treatment aqueous solution.
[0057] By such treatment, an α-alumina powder with reduced calcium (Ca) and sodium (Na) concentrations can be obtained. The obtained α-alumina powder can be recovered from the treated aqueous solution and further dried before the subsequent evaluation process. The recovery can be carried out by solid-liquid separation methods such as filtration or centrifugal separation. And the drying can be carried out at a temperature at which the α-alumina powder does not undergo particle growth, for example, a temperature above 80°C and below 600°C. Furthermore, the dried α-alumina powder can be crushed.
[0058] <Evaluation process> In the evaluation step, the concentration of calcium (Ca) contained in the α-alumina raw material powder and the concentration of calcium (Ca) contained in the α-alumina powder are measured and compared. By providing this step, the degree of reduction in calcium concentration in the treatment step can be accurately estimated.
[0059] As long as the calcium concentration can be measured, the measurement method is not limited. For example, a fluorescent X-ray analyzer, an atomic absorption spectrophotometer and / or an ICP emission spectrophotometer can be used. In addition, the comparison method is not particularly limited. For example, the difference between the calcium concentration contained in the α-alumina raw material powder and the calcium concentration contained in the α-alumina powder can be calculated, and an evaluation can be performed based on the size of the difference. Alternatively, the ratio of the calcium concentration contained in the α-alumina raw material powder to the calcium concentration contained in the α-alumina powder can be calculated, and an evaluation can be performed based on the size of the ratio. The comparison can be performed automatically or manually. For example, a method in which the measured value is sent from the analyzer to a computer and automatically analyzed can be cited.
[0060] It is preferred to measure the CaO-converted concentration of the soluble calcium component contained in the α-alumina raw material powder (c1[f-CaO]) and the CaO-converted concentration of the soluble calcium component contained in the α-alumina powder (c2[f-CaO]), and further calculate the soluble calcium concentration ratio (c2[f-CaO] / c1[f-CaO]). In addition, it is preferred to measure the CaO-converted concentration of all calcium components contained in the α-alumina raw material powder (c1[T-CaO]) and the CaO-converted concentration of all calcium components contained in the α-alumina powder (c2[T-CaO]). The soluble calcium concentration ratio (c2[f-CaO] / c1[f-CaO]) is preferably below 0.90, more preferably below 0.80, and further preferably below 0.65. The total calcium concentration ratio (c2[T-CaO] / c1[T-CaO]) is preferably 0.97 or less, more preferably 0.95 or less, and further preferably 0.90 or less.
[0061] As mentioned above, the impurities (Ca, Na) contained in the alumina powder include soluble impurities attached to the surface of the powder and impurities present inside the powder. The concentration of soluble calcium components (c[f-CaO]) is the concentration of calcium components attached to the surface of the powder. The concentration of total calcium components (c[T-CaO]) is the combined concentration of calcium components attached to the surface of the powder and calcium components present inside the powder. By using the soluble calcium concentration ratio (c2[f-CaO] / c1[f-CaO]) or the total calcium concentration ratio (c2[T-CaO] / c1[T-CaO]) as an indicator, the degree of reduction of the soluble calcium components attached to the surface of the powder and the total calcium components can be accurately estimated.
[0062] In addition, the soluble calcium concentration (c1[f-CaO], c2[f-CaO]) can be obtained by adding alumina powder to water and then heating it to dissolve calcium in the water, and analyzing the calcium concentration in the water after dissolution by ICP emission spectrometry. In addition, the total calcium concentration (c1[T-CaO]) of the α-alumina raw material powder can be obtained by fluorescent X-ray analysis. In addition, the total calcium concentration (c2[T-CaO]) of the α-alumina powder can be calculated according to the following formula (2).
[0063]
Number 2
[0064] <Judgment process> If necessary, a determination step may be provided after the evaluation step. In the determination step, qualified products and unqualified products are determined based on the calcium concentration or reduction amount of the obtained α-alumina powder. For example, α-alumina powders having a soluble calcium concentration (c2[f-CaO]) or a total calcium concentration (c2[f-CaO]) below a specified value are determined as qualified products, and powders other than these are determined as unqualified products.
[0065] According to the method of this embodiment, an α-alumina powder with a reduced concentration of impurities (Ca, Na) can be obtained. The CaO conversion concentration (c2[T-CaO]) of all calcium components contained in the α-alumina powder is preferably less than 0.030 mass%, and more preferably less than 0.020 mass%. In addition, the CaO conversion concentration (c2[f-CaO]) of the soluble calcium component is preferably less than 0.010 mass%, and more preferably less than 0.006 mass%. In addition, the Na2O conversion concentration (c2[T-Na2O]) of all sodium components contained in the α-alumina powder is preferably less than 0.10 mass%, and more preferably less than 0.08 mass%. The Na2O conversion concentration (c2[f-Na2O]) of soluble sodium is preferably greater than 0.001 mass% and less than 0.015 mass%, and more preferably greater than 0.001 mass% and less than 0.012 mass%. The concentration of soluble sodium can be determined by atomic absorption analysis, while the concentration of all sodium components can be determined by fluorescent X-ray analysis.
[0066] The SiO2 conversion concentration (c2[SiO2]) of the silicon component contained in the α-alumina powder is preferably above 0.030 mass % and below 0.500 mass %, and more preferably above 0.040 mass % and below 0.400 mass %. Generally speaking, the α-alumina powder contains a silicon (Si) component from a raw material or a sintering process as an impurity in an amount of about 0.01 to 0.03 mass %. In the manufacturing method of this embodiment, the concentration of the silicon component increases after a treatment step using an organosilane compound. By using the concentration of the silicon component in the α-alumina powder as an indicator, the effect produced by the treatment with the organosilane compound can be fully ensured. In addition, the concentration of the silicon component can be obtained by using a molybdenum blue absorptiometry method using a double-beam spectrophotometer.
[0067] The difference (|c2[SiO2]-c1[SiO2]|) between the SiO2 conversion concentration of the silicon component contained in the α-alumina raw material powder (c1[SiO2]) and the SiO2 conversion concentration of the silicon component contained in the above-mentioned α-alumina powder (c2[SiO2]) is preferably 0.001 mass% or more, more preferably 0.002 mass% or more, and further preferably 0.003 mass% or more. By using the increase in the concentration of the silicon component in the α-alumina powder as an indicator, the effect of the treatment with the organosilane compound can be fully ensured. However, since the organosilane compound has been used for cleaning, it is not necessary to fix it in the treated alumina.
[0068] The 45μm unscreened amount of the α-alumina raw powder is preferably less than 100ppm, and more preferably less than 50ppm. The 45μm unscreened amount is a benchmark for the amount of coarse particles in the α-alumina raw powder. If the α-alumina raw powder contains a large amount of coarse particles, the amount of coarse particles in the final α-alumina powder will increase. Therefore, when the α-alumina powder is filled into a resin or rubber to make a resin composition and the resin composition is formed into a molded product, there is a risk that the coarse particles will become protrusions protruding from the surface of the product. If such protrusions are generated, it will be difficult to make the product close to other components such as heat sources, which may cause problems such as poor heat dissipation. Therefore, the less 45μm unscreened amount, the better.
[0069] In addition, the 45 μm unscreened amount can be obtained by screening the α-alumina powder using a JIS Z8801-1 test sieve (aperture 45 μm). Among them, the span value can be obtained based on the particle size distribution measured using a laser scattering particle size distribution analyzer. Specifically, the cumulative 10% diameter (Dp10), cumulative 50% diameter (Dp50) and cumulative 90% diameter (Dp90) in the particle size distribution based on mass standard (volume standard) are used to obtain it according to the following formula (3).
[0070]
Number 3
[0071] The average particle size (Dp50) of the α-alumina powder finally obtained is preferably greater than 2.0 μm and less than 5.0 μm, and more preferably greater than 2.5 μm and less than 4.0 μm. If the particle size of the α-alumina powder is too small, the viscosity of the resin composition prepared by filling the α-alumina powder into a resin or rubber will be too high, and there is a risk of difficulty in forming. Moreover, even if it can be formed, the filling property of the α-alumina powder in the composition will deteriorate, and the thermal conductivity of the product made from the resin composition may be reduced. Therefore, from the viewpoint of formability, filling property and thermal conductivity, the particle size of the α-alumina powder is appropriately larger. On the other hand, the particle size of the α-alumina powder produced by the Bayer process has an upper limit due to the production process.
[0072] The BET specific surface area of α-alumina powder is preferably 1.0 m 2 / g or more and 3.5m 2 / g or less, more preferably 1.2m 2 / g or more and 2.7m 2 / g or less. The larger the BETE specific surface area, the smaller the particle size of the powder. From the viewpoints of formability, filling properties and thermal conductivity, the BET specific surface area of α-alumina powder is preferably appropriately smaller.
[0073] The span value (Dp90-Dp10) / Dp50) of α-alumina powder is preferably less than 2.0, and more preferably less than 1.6. If the span value is too large, the particle size distribution is too wide. When α-alumina powder is used as a heat dissipation filler, the thermal conductivity deteriorates and the filler is difficult to disperse evenly. Furthermore, when α-alumina powder is used for applications requiring a specific particle size distribution, the particle size distribution design becomes difficult. Therefore, the smaller the span value, the better.
[0074] According to the manufacturing method of this embodiment, an α-alumina powder with a reduced calcium (Ca) concentration can be obtained by a simple method while suppressing the increase in BET specific surface area caused by hydration. Such α-alumina powder can be used for well-known applications such as structural parts, tools, abrasives, fillers (filling materials), spark plugs, insulators, electronic substrates, and refractory materials. In particular, when used as a heat dissipation filler filled in resin or rubber, there will be no problem of deterioration in filling and forming properties, and a product with excellent thermal conductivity can be obtained. Example
[0075] The present invention is described in more detail by using the following examples. However, the present invention is not limited to the following examples.
[0076] <<Experimental Examples A and B>> In Experimental Example A, an epoxy-containing silane coupling agent, i.e., 3-glycidoxypropylmethyldimethoxysilane or 3-glycidoxypropyltrimethoxysilane, was used as an organosilane compound for treatment, and its influence was studied. In addition, the influence of adding acetic acid together with the organosilane compound was also studied. And, in Experimental Example B, a vinyl-containing silane coupling agent, i.e., vinyltrimethoxysilane, was used as an organosilane compound for treatment, and its influence was studied.
[0077] (1) Preparation of α-alumina powder [Comparative Example A1] <Preparation of α-alumina raw material powder> First, aluminum hydroxide (Nippon Light Metal Co., Ltd., B52) obtained by the Bayer process was prepared. The average secondary particle size of the aluminum hydroxide was 55 μm, and the Na2O conversion concentration (c0[T-Na2O]) of the total sodium component was 0.2% by mass. Then, aluminum fluoride as a halogen mineralizer was added to the prepared aluminum hydroxide at a ratio of 0.4% by mass in terms of aluminum oxide, and then mixed to obtain a mixture. The obtained mixture was filled into a silicon dioxide-containing alumina ceramic firing container and fired at 1500°C ± 10°C for about 15 hours using a tunnel kiln.
[0078] Next, the obtained calcined product was pulverized to produce a pulverized product, i.e., α-alumina raw material powder. During the pulverization, a ball mill was filled with an amount of 44% by volume of the inner volume of the ball mill. Alumina balls were used in a rotating ball mill (manufactured by Chuko Seiki Co., Ltd.). The amount of the calcined product filled was 0.18 kg per liter of the ball mill's internal volume. The calcined product was ground to an average particle size (Dav) of 3.0 μm after grinding and a BET equivalent particle size (Dav) before grinding of 0.18 kg. BET ) particle size ratio (Dav / D BET ) is 1.10 or more and 1.45 or less. Then, the obtained α-alumina raw material powder was evaluated without being treated with an organosilane compound.
[0079] [Example A1] In Example A1, the α-alumina raw material powder obtained in Comparative Example A1 was treated with an organic silane compound to produce α-alumina powder. 3-glycidyloxypropylmethyldimethoxysilane ((CH3O)2CH3SiC6H 11 O2) as an organic silane compound. The specific steps are as follows.
[0080] <Processing process> 3-glycidyloxypropylmethyldimethoxysilane (Shin-Etsu Chemical Co., Ltd., KBM-402, molecular weight 220.3) was placed in a polypropylene container filled with pure water, and stirred for 1 hour using a Teflon (registered trademark) stirring blade to prepare a treatment aqueous solution. At this time, the amount of 3-glycidyloxypropylmethyldimethoxysilane added to the aqueous solution was adjusted to 0.25% by mass relative to the mass of the added α-alumina raw material powder (0.011 mol / kg per 1 kg of the mass of the α-alumina raw material powder).
[0081] Next, 100 g of the α-alumina raw material powder was added to the prepared treatment aqueous solution in the form of dry powder, and then stirred at room temperature for 20 hours. Then, the aqueous solution was subjected to solid-liquid separation using a Buchner funnel, and the obtained solid component was dried at 110° C. for a day and night, and then pulverized in a mortar to obtain α-alumina powder.
[0082] [Example A2] In Example A2, 3-glycidoxypropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd., KBM-403, molecular weight 236.3) was used instead of 3-glycidoxypropylmethyldimethoxysilane. In addition, the addition amount of 3-glycidoxypropyltrimethoxysilane was adjusted to 0.25 mass% relative to the mass of the α-alumina raw material powder (0.011 mol / kg relative to the mass of 1 kg of the α-alumina raw material powder). In addition, α-alumina powder was prepared in the same manner as in Example A1.
[0083] [Example A3] In Example A3, when preparing the treatment aqueous solution, an organic silane compound (3-glycidoxypropyltrimethoxysilane) was added to pure water, acetic acid was added to adjust the pH of the aqueous solution to 4, and the solution was stirred for 1 hour. α-Alumina powder was prepared in the same manner as in Example A2 except for this.
[0084] [Comparative Example B1] An α-alumina raw material powder was prepared by the same procedure as in Comparative Example A1. Then, the obtained α-alumina raw material powder was evaluated as it is without being treated with an organosilane compound.
[0085] [Example B1] In Example B1, the α-alumina raw material powder prepared in Comparative Example B1 was treated with an organic silane compound. Among them, vinyl trimethoxysilane (Shin-Etsu Chemical Co., Ltd., KBM-1003, molecular weight 148.2) was used as the organic silane compound. The amount of vinyl trimethoxysilane added was adjusted to 0.25 mass % relative to the mass of the α-alumina raw material powder (0.017 mol / kg relative to the mass of 1 kg of the α-alumina raw material powder). In addition, α-alumina powder was prepared in the same manner as in Example A1.
[0086] (2) Evaluation Aluminum hydroxide, a calcined product, a pulverized product (α-alumina raw material powder), and α-alumina powder were evaluated for various properties in the following procedures.
[0087] <Ingredient Analysis> The concentration of all calcium components and the concentration of all sodium components contained in the α-alumina raw material powder and the α-alumina powder were determined by fluorescent X-ray analysis. Specifically, the fluorescent X-ray intensity of the sample was measured using a fluorescent X-ray analyzer (Rigaku Co., Ltd., ZSX100e), and the total calcium component concentration (c[T-CaO]) and the total sodium component concentration (c[T-Na2O]) in the sample were determined using the obtained data and the calibration curve. In addition, the total calcium content concentration (c0[T-CaO]) in the raw aluminum hydroxide was also determined by the same method.
[0088] In addition, the concentration of soluble calcium components and soluble sodium components contained in the α-alumina raw material powder and α-alumina powder were obtained by atomic absorption spectroscopy. Specifically, water was added to the sample so that the mass ratio of the sample to water was 1:60, and the sample was boiled in boiling water for 30 minutes to dissolve the soluble calcium components and soluble sodium components in the sample in the water. Then, the soluble calcium component concentration (c[f-CaO]) was measured using an ICP emission spectrophotometer (Hitachi High-Technologies Corporation, PS3520UVDD). The soluble sodium component concentration (c[f-Na2O]) was also measured using an atomic absorption spectrophotometer (Hitachi High-Technologies Corporation, Z-2000). At this time, the measurement was performed under the conditions of measurement mode: atomic absorption, measurement wavelength range: 589.0nm.
[0089] In addition, the concentration of silicon components (c[SiO2]) contained in the α-alumina raw material powder and the α-alumina powder was determined by quantitative analysis using a double-beam spectrophotometer (Hitachi, Ltd., U-3010) by molybdenum blue absorptiometry.
[0090] <Molding density> The forming density of the sintered product was determined according to the following steps. First, the sintered product was press-formed at a pressure of 98.07 MPa using a hydraulic 20-ton compression tester (Maekawa Testing Machine Manufacturing Co., Ltd.) to produce a part. The size of the resulting sheet was 40 mm × 20 mm × 10 mm. Next, the mass of the sheet was measured, and the forming density was calculated based on the volume and mass of the sheet.
[0091] <BET specific surface area> The BET specific surface areas of the calcined product, the α-alumina raw material powder (crushed product) and the α-alumina powder were measured by a N2 gas adsorption method using an automatic specific surface area measuring device (Micromeritics, FlowSorb II 2300 model).
[0092] <45μm unsieved amount> The α-alumina raw material powder (crushed material) was sieved using a JIS Z8801-1 test sieve (aperture: 45 μm). The mass of the residue remaining on the sieve was measured, and the mass of the residue obtained was divided by the total mass to calculate the 45 μm non-sieved amount.
[0093] <Particle size distribution> The particle size distribution of the α-alumina raw material powder was measured using a laser scattering particle size analyzer (Nikkiso Co., Ltd., Microtrac 9320HRA (×100)). Subsequently, the 10% cumulative diameter (Dp10), 50% cumulative diameter (Dp50) and 90% cumulative diameter (Dp90) in the particle size distribution based on mass (volume) were calculated. Then, the span value was calculated using Dp10, Dp50 and Dp90 according to the following formula (3).
[0094]
Number 4
[0095] (3) Evaluation results The properties of the α-alumina raw material powders obtained in Comparative Examples A1 and B1 are shown together with the properties of the raw aluminum hydroxide and the calcined product in Table 1. It was confirmed that the obtained α-alumina raw material powders had the desired properties (BET specific surface area, 45 μm unsieved amount, and span value).
[0096] In addition, the properties of the α-alumina powder are shown in Table 2. As can be seen, the samples treated with the organosilane compound (Examples A1 to A3 and Example B1) have lower calcium and sodium component concentrations than the samples not treated with the organosilane compound (Comparative Examples A1 and B1). In addition, the increase in the BET specific surface area is suppressed, and the progress of hydration is suppressed.
[0097] Table 1 Characteristics of aluminum hydroxide, calcined product and pulverized product
[0098] Table 2 Effects of the type of organosilane compound
[0099] <<Experimental Example C>> In Experimental Example C, vinyl-containing silane, i.e., vinyltrimethoxysilane, was used as an organosilane compound for treatment, and the influence of its concentration was studied (Examples C1 to C4). In addition, for comparison, a sample not treated with an organosilane compound (Comparative Example C1) and a sample treated only with water without using an organosilane compound (Comparative Example C2) were prepared and evaluated.
[0100] (1) Preparation of α-alumina powder [Comparative Example C1] <Preparation of α-alumina raw material powder> An α-alumina raw material powder was prepared by the same procedure as in Comparative Example A1. The obtained α-alumina raw material powder was evaluated without being treated with an organosilane compound.
[0101] [Comparative Example C2, Examples C1 to C4] In Comparative Example C2 and Examples C1 to C4, the α-alumina raw material powder obtained in Comparative Example C1 was treated with an organosilane compound to produce α-alumina powder. Vinyltrimethoxysilane ((CH3O)3SiCH3=CH2) was used as the organosilane compound; vinyl-containing silane). The specific steps are as follows.
[0102] <Processing process> Vinyl trimethoxysilane (Shin-Etsu Chemical Co., Ltd., KBM-1003, molecular weight 148.2) was placed in a polypropylene container filled with pure water, and stirred for 1 hour using a Teflon (registered trademark) stirring blade to prepare a treated aqueous solution. At this time, the amount of vinyl trimethoxysilane added to the aqueous solution was adjusted to a value shown in Table 3 relative to the mass of the added α-alumina raw material powder.
[0103] Next, 100 g of the α-alumina raw material powder was added to the prepared treatment aqueous solution in the form of dry powder, and then stirred at room temperature for 20 hours. Then, the treated aqueous solution was subjected to solid-liquid separation using a Buchner funnel, and the obtained solid component was dried at 110° C. for a day and night, and then pulverized in a mortar to obtain α-alumina powder. In addition, in Comparative Example C1, the treatment of the α-alumina raw material powder was performed in pure water without vinyltrimethoxysilane.
[0104] (2) Evaluation The aluminum hydroxide, the calcined product, the α-alumina raw material powder (crushed product), and the α-alumina powder were evaluated for various properties by the same methods as in Experimental Example A.
[0105] (3) Evaluation results The properties of the α-alumina raw material powder obtained in Comparative Example C1 are shown together with the properties of the raw aluminum hydroxide and the fired product in Table 1. It was confirmed that the obtained α-alumina raw material powder had the desired properties (BET specific surface area, 45 μm unsieved amount, and span value).
[0106] The properties of the α-alumina powder are shown in Table 3. The samples treated with the organosilane compound (Examples C1 to C4) showed a decrease in the concentration of calcium and sodium components compared to the samples not treated with the organosilane compound (Comparative Example C1), and the effect was particularly significant in the region where the amount of organosilane compound added was 0.5% by mass or more. Moreover, in Examples C1 to C4, the increase in the BET specific surface area was suppressed. In contrast, the sample treated only with pure water (Comparative Example C2) showed a decrease in the concentration of sodium components, but no decrease in the calcium concentration was confirmed. Moreover, the BET specific surface area increased significantly.
[0107] Table 3 Effects of the type of organosilane compound
[0108] <<Experimental Example D>> In Experimental Example D, 3-glycidoxypropyltrimethoxysilane, an epoxy-containing silane, was used as an organosilane compound for treatment, and the effect of its concentration was studied (Examples D1 to D4). In addition, for comparison, a sample not treated with an organosilane compound (Comparative Example D1) and a sample treated only with water without using an organosilane compound (Comparative Example D2) were prepared and evaluated.
[0109] (1) Preparation of α-alumina powder [Comparative Example D1] <Preparation of α-alumina raw material powder> First, aluminum hydroxide (Nippon Light Metal Co., Ltd., B52) obtained by the Bayer process was prepared. The average secondary particle size of the aluminum hydroxide was 55 μm, and the Na2O conversion concentration of all sodium (c0[T-Na2O]) was 0.2% by mass. Then, aluminum fluoride as a halogen mineralizer was added to the prepared aluminum hydroxide at a ratio of 0.4% by mass in terms of alumina conversion and mixed to obtain a mixture. The obtained mixture was filled into a silicon dioxide-containing alumina ceramic firing container and fired at 1500°C ± 10°C for about 15 hours using a tunnel kiln.
[0110] Next, the fired product was pulverized to produce a pulverized product, i.e., α-alumina raw material powder. During the pulverization, a ball mill was filled with an amount of 44% by volume of the inner volume of the ball mill. Alumina balls were used in a rotating ball mill (manufactured by Chuko Seiki Co., Ltd.). The amount of the calcined product filled was 0.18 kg per liter of the ball mill's internal volume. The calcined product was ground to an average particle size (Dav) of 3.0 μm after grinding and a BET equivalent particle size (Dav) before grinding of 0.18 kg. BET ) particle size ratio (Dav / D BET ) is 1.10 or more and 1.45 or less. Then, the obtained α-alumina raw material powder is evaluated without being treated with an organic silane compound.
[0111] [Comparative Example D2, Examples D1 to D4] In Comparative Example D2 and Examples D1 to D4, the α-alumina raw material powder obtained in Comparative Example D1 was treated with an organic silane compound to produce α-alumina powder. The organic silane compound was 3-glycidyloxypropyltrimethoxysilane (CH3O)3SiC6H 11 O2); epoxy-containing silane coupling agent). The specific steps are as follows.
[0112] <Processing process> 3-Glycidoxypropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd., KBM-403, molecular weight 236.3) was placed in a polypropylene container filled with pure water, and stirred for 1 hour using a Teflon (registered trademark) stirring blade to prepare a treated aqueous solution. At this time, the amount of 3-glycidoxypropyltrimethoxysilane added to the aqueous solution was adjusted to a value shown in Table 4 relative to the mass of the added α-alumina raw material powder.
[0113] Next, 100 g of the α-alumina raw material powder was added to the prepared treatment aqueous solution in the form of dry powder, and then stirred at room temperature for 20 hours. Then, the treated aqueous solution was subjected to solid-liquid separation using a Buchner funnel, and the obtained solid component was dried at 110° C. for a day and night, and then pulverized in a mortar to obtain α-alumina powder. In Comparative Example D2, the α-alumina raw material powder was treated in pure water that did not contain 3-glycidyloxypropyltrimethoxysilane.
[0114] (2) Evaluation The aluminum hydroxide, the calcined product, the pulverized product (α-alumina raw material powder), and the α-alumina powder were evaluated for various properties by the same methods as in Experimental Example A.
[0115] (3) Evaluation results The properties of the α-alumina raw material powder obtained in Comparative Example D1 are shown together with the properties of the raw aluminum hydroxide and the fired product in Table 1. It was confirmed that the obtained α-alumina raw material powder had the desired properties (BET specific surface area, 45 μm unsieved amount, and span value).
[0116] The properties of the α-alumina powder are shown in Table 4. The samples treated with the organosilane compound (Examples D1 to D4) have reduced calcium and sodium concentrations compared to the samples not treated with the organosilane compound (Comparative Example D1), and the effect is particularly significant in the region where the amount of organosilane compound added is 1.0 mass % or more. In addition, regardless of the amount of organosilane compound added, the increase in BET specific surface area is suppressed. In contrast, the sample treated only with pure water (Comparative Example D2) has a reduced sodium concentration, but only a slightly reduced calcium concentration. Moreover, the BET specific surface area is significantly increased.
[0117] Table 4 Effect of the type of organosilane compound
[0118] <<Experimental Example E>> In Experimental Example E, sugar was used instead of the organosilane compound to study its effect. It is well known that calcium oxide (CaO) is highly soluble in aqueous solutions of sugars such as glucose or xylose. Therefore, by using sugar for treatment, it is expected that alumina powder with reduced calcium concentration can be obtained.
[0119] (1) Preparation of α-alumina powder [Comparative Example E1] An α-alumina raw material powder was prepared by the same procedure as in Comparative Example A1. Then, the obtained α-alumina raw material powder was evaluated without being treated.
[0120] [Comparative Example E2] In Comparative Example E2, the α-alumina raw material powder obtained in Comparative Example E1 was treated with an aqueous solution of sugar to produce α-alumina powder. D-(+)-glucose anhydride was used as sugar. The specific steps are as follows.
[0121] <Processing process> D-(+)-glucose anhydride (Alfa Aesar, Cat No. A16828, molecular weight 180.16) was placed in a polypropylene container filled with pure water and stirred for 1 hour using a Teflon (registered trademark) stirring blade to prepare a treatment aqueous solution. At this time, the amount of D-(+)-glucose anhydride added to the aqueous solution was adjusted to 1.0 mass % relative to the mass of the added α-alumina raw material powder (0.566 mol / kg per 1 kg of the mass of the α-alumina raw material powder).
[0122] Next, 100 g of the α-alumina raw material powder was added to the prepared treatment aqueous solution in the form of dry powder, and then stirred at room temperature for 20 hours. Then, the aqueous solution was subjected to solid-liquid separation using a Buchner funnel, washed with 100 g of pure water, and the obtained solid component was dried at 110° C. for a day and night, and then pulverized in a mortar to obtain α-alumina powder.
[0123] (2) Evaluation The aluminum hydroxide, the calcined product, the pulverized product (α-alumina raw material powder), and the α-alumina powder were evaluated for various properties by the same methods as in Experimental Example A.
[0124] (3) Evaluation results The properties of the α-alumina raw material powder obtained in Comparative Example E1 are shown together with the properties of the raw aluminum hydroxide and the fired product in Table 1. It was confirmed that the obtained α-alumina raw material powder had the desired properties (BET specific surface area, 45 μm unsieved amount, and span value).
[0125] The properties of the α-alumina powder are shown in Table 5. The sample treated with sugar (D-(+)-glucose) (Comparative Example E2) showed a decrease in sodium content compared to the untreated sample (Comparative Example E1), but almost no decrease in calcium content was observed. In addition, the BET specific surface area increased.
[0126] Table 5 Effects of added sugar
[0127] This shows that when the sugar aqueous solution is used, the effect of reducing calcium in aluminum oxide cannot be obtained, and this effect is a unique effect of the present embodiment using the organosilane compound having a hydrolyzable group.
[0128] From the above results, it is understood that according to the production method of the present embodiment, an alumina powder having a reduced calcium (Ca) concentration can be obtained by a simple method while suppressing an increase in the BET specific surface area due to hydration.
Claims
1. A method for producing α-alumina powder, comprising: a treatment step in which the α-alumina raw material powder is placed in and immersed in a treatment aqueous solution containing an organic silane compound having a hydrolyzable group, thereby obtaining an α-alumina powder having a reduced calcium (Ca) concentration; and An evaluation step of measuring and comparing the concentration of calcium contained in the α-alumina raw material powder and the concentration of calcium contained in the α-alumina powder.
2. The method of claim 1, wherein: The treatment aqueous solution contains the organosilane compound in a ratio of 0.10 mass % or more relative to the mass of the α-alumina raw material powder.
3. The method according to claim 1 or 2, wherein: The organic silane compound is at least one selected from alkoxysilane, a vinyl-containing silane coupling agent, and an epoxy-containing silane coupling agent.
4. The method according to any one of claims 1 to 3, wherein: In the evaluation process, the CaO conversion concentration of the soluble calcium component contained in the α-alumina raw material powder (c1[f-CaO]) and the CaO conversion concentration of the soluble calcium component contained in the α-alumina powder (c2[f-CaO]) are measured, and the soluble calcium concentration ratio (c2[f-CaO] / c1[f-CaO]) is further calculated.
5. The method of claim 4, wherein: The soluble calcium concentration ratio (c2[f-CaO] / c1[f-CaO]) is below 0.
90.
6. The method according to any one of claims 1 to 5, wherein: The CaO-converted concentration of all calcium components contained in the α-alumina powder (c2[T-CaO]) is less than 0.030 mass%, and the CaO-converted concentration of soluble calcium components (c2[f-CaO]) is less than 0.010 mass%.
7. The method according to any one of claims 1 to 6, wherein: The Na2O conversion concentration (c2[T-Na2O]) of all sodium components contained in the α-alumina powder is less than 0.10 mass%, and the Na2O conversion concentration (c2[f-Na2O]) of soluble sodium components is greater than 0.001 mass% and less than 0.015 mass%.
8. The method according to any one of claims 1 to 7, wherein The SiO2 conversion concentration (c2[SiO2]) of the silicon component contained in the α-alumina powder is greater than or equal to 0.030 mass % and less than or equal to 0.500 mass %.
9. The method according to any one of claims 1 to 8, wherein: The difference (|c2[SiO2]-c1[SiO2]|) between the SiO2 conversion concentration (c1[SiO2]) of the silicon component contained in the α-alumina raw material powder and the SiO2 conversion concentration (c2[SiO2]) of the silicon component contained in the α-alumina powder is greater than 0.001 mass%.
10. The method according to any one of claims 1 to 9, wherein: The 45 μm unscreened amount of the α-alumina raw material powder is less than 100 ppm.
11. The method according to any one of claims 1 to 9, wherein: The average particle size (Dp50) of the α-alumina powder is greater than or equal to 2.0 μm and less than or equal to 5.0 μm.
12. The method according to any one of claims 1 to 11, wherein: The BET specific surface area of the α-alumina powder is 1.0 m 2 / g or more and 3.5m 2 / g or less.
13. The method according to any one of claims 1 to 12, wherein: The span value ((Dp90-Dp10) / Dp50) represented by the cumulative 10% diameter (Dp10), the cumulative 50% diameter (Dp50) and the cumulative 90% diameter (Dp90) in the particle size distribution of the α-alumina powder based on mass is less than 2.
0.
14. The method according to any one of claims 1 to 13, wherein: It further has: A preparation step in which a halogen-based mineralizer is added and mixed to aluminum hydroxide obtained by the Bayer process to prepare a mixture, and then the mixture is fired at a temperature of 1100° C. to 1600° C. to prepare a fired product, and the fired product is further pulverized to prepare the α-alumina raw material powder.
15. The method of claim 14, wherein: The Na2O conversion concentration (c0[T-Na2O]) of all sodium components contained in the aluminum hydroxide is less than 0.3 mass%.
16. The method according to claim 14 or 15, wherein: When the mixture is fired, the mixture is filled into a firing container made of alumina ceramic containing silicon dioxide and fired to produce a molded product having a molding density of 2.05 g / cm at a molding pressure of 98.07 MPa. 3 Above and BET specific surface area is 0.9m 2 / g or less of the fired product.
17. The method according to any one of claims 14 to 16, wherein: When the calcined product is pulverized to prepare the α-alumina raw material powder, the average particle size (Dav) of the α-alumina raw material powder is proportional to the BET equivalent diameter (Dav) of the calcined product. BET ) ratio (Dav / D BET ) falls within the range of 1.0 to 2.0, the fired product is crushed.