Ammonia-free latex composition
By using a processing method that does not use ammonia, and by stabilizing and preserving natural rubber with components such as surfactants and halogenated acids, the environmental pollution and health hazards of traditional methods are solved, and an ammonia-free rubber composition with high mechanical properties, low allergenicity and long shelf life is produced.
Patent Information
- Application Number
- CN202380030512.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-26
- Filing Date
- 2023-01-24
- Publication Date
- 2024-11-12
AI Technical Summary
Existing natural rubber processing methods use ammonia and biocides, leading to environmental pollution, health hazards, allergies, and odor problems. Furthermore, the waste residues generated by traditional methods require expensive treatment.
Using an ammonia-free method, surfactants such as alkylbenzene sulfonates, fatty acid alcohols, and ethoxylated fatty acid alcohols are used as stabilizers, combined with haloacids as preservatives, and through refrigeration, pH adjustment, and coagulation steps, ammonia-free, stable liquid and solid rubber compositions are formed.
The production of ammonia-free rubber compositions reduces environmental hazards, lowers health risks, improves mechanical properties, reduces allergies, lessens odor, and extends shelf life, making them suitable for applications such as athletic shoes.
Smart Images

Figure BDA0005060283300000141 
Figure BDA0005060283300000151 
Figure BDA0005060283300000171
Abstract
Description
background
[0001] Ammonia is a key ingredient in the conventional method of processing natural rubber latex.
[0002] When processing latex extracted from trees, a small amount of ammonia is often added to inhibit coagulation of the latex when it is transported to the processing facility. In addition to ammonia, biocides are often used to preserve the latex to inhibit bacterial action and decomposition. Typically, a large amount of ammonia (~4% by weight) and a small amount of biocide (~1%), or a small amount of ammonia (~1%) and a large amount of biocide (~4%) is required.
[0003] After processing the latex, waste residues representing approximately 65% of the extracted material are usually discarded. In conventional processing, the discarded residues are contaminated with ammonia and biocides and are therefore not environmentally friendly; the ammonia acts as a fertilizer, causing undesirable growth of plants and algae, and the biocides kill desirable microorganisms and microfauna. Some countries require expensive treatments of the residues to reduce the amount of ammonia discarded into the environment. These treatments consume large amounts of water.
[0004] Furthermore, the added ammonia breaks down the proteins contained in latex. This makes the resulting products, such as rubber gloves and condoms, allergenic to approximately 2% of the global population. Furthermore, ammonia generates carcinogenic nitrosamines in the material.
[0005] Furthermore, ammonia vapors affect the health of people throughout the substance production and manufacturing chain, from farmers to workers in processing plants.
[0006] Finally, due to the ammonia, the resulting rubber material has a strong odor, making it unattractive for applications such as sports shoes despite its excellent mechanical properties. For these applications, the current alternative is to use natural rubber without ammonia, which also results in rubber with an unpleasant odor due to decomposition. In addition, the material requires large amounts of water to process.
[0007] Furthermore, biocides used to supplement traditional preservation treatments generate high levels of environmental contamination.
[0008] Therefore, it is desirable to develop new methods for processing natural rubber latex that do not contain environmentally polluting ammonia and / or biocides, or that do not require expensive treatment to remove ammonia and biocides before the residue is discarded into the environment. Preferably, such methods would produce rubber having equivalent or superior physical, chemical, and mechanical properties, as well as rubber and latex containing less allergenic proteins, compared to conventional ammonia treated rubber. summary
[0009] In one aspect, provided herein is a method for processing natural latex without the use of ammonia, the method comprising a stabilization step, wherein the liquid latex composition is contacted with a stabilizer comprising a surfactant selected from the group consisting of alkylbenzene sulfonates, fatty acid alcohols, and ethoxylated fatty acid alcohols.
[0010] In another aspect, the present invention provides a method comprising one or more of the following steps: (a) a collection step, in which liquid latex is collected from a factory and preferably filtered to remove impurities from the environment; (b) a stabilization step, in which the liquid latex composition is refrigerated and / or the liquid latex composition is contacted with a stabilizer; (c) a preservation step, in which the liquid latex composition is contacted with a preserving agent; (d) a pH adjustment step, in which the liquid latex composition is contacted with a pH adjuster; (e) a storage step, in which the liquid latex composition is stored for a period of time; and (f) a coagulation step, in which the liquid latex composition is contacted with a coagulant to form a solid latex composition.
[0011] Also provided herein is an ammonia-free latex composition. In some embodiments, the composition is produced by the methods provided herein.
[0012] Other objects and features of the invention will be in part apparent and in part pointed out hereinafter. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 is a graphic depiction of the NETZSCH DMA apparatus used for the double shear test experiment described in Example 10.
[0014] Figure 2 yes Figure 1 Graphic depiction of a cross section of the device and illustrating the double shear cycle test described in Example 10.
[0015] Figure 3 Depicted are the stress behavior observed during dynamic testing at 1 Hz and 21° C. with 30% double shear strain, as described in Example 10.
[0016] Figure 4 Depicted are the normalized stress behavior observed during dynamic testing at 1 Hz and 21° C. with 30% double shear strain, as described in Example 10.
[0017] Figure 5 Depicted are the stress behavior observed during dynamic testing at 50% double shear strain at 1 Hz, as described in Example 10.
[0018] Figure 6Depicted are the normalized stress behavior observed during dynamic testing at 1 Hz and 21° C. with 50% double shear strain, as described in Example 10.
[0019] Figure 7 The NETZSCH Graphical depiction of the 500N DMA device.
[0020] Figure 8 Depicted are the stress behavior observed during relaxation testing at 30% strain and 21°C, as described in Example 11.
[0021] Fig. 9 Depicted are the normalized stress behavior observed during relaxation testing at 30% strain and 21°C, as described in Example 11.
[0022] Fig.10 Depicted are the stress responses observed during relaxation at 30% tensile strain and two different temperatures, 21°C and 50°C, as described in Example 11.
[0023] Fig.11 Depicted are the normalized stress responses observed during relaxation at 30% tensile strain and two different temperatures, 21°C and 50°C, as described in Example 11.
[0024] Fig.12 Depicted are the stress behavior observed during relaxation testing at 30% strain and 3 different temperatures (21°C, 50°C and 80°C), as described in Example 11.
[0025] Fig.13 Depicted are the normalized stress behavior observed during relaxation testing at 30% strain and 3 different temperatures (21°C, 50°C and 80°C), as described in Example 11.
[0026] Fig.14 Depicted are the stress behavior observed during relaxation testing at 50% strain and 21°C, as described in Example 11.
[0027] Fig.15 Depicted are the normalized stress behavior observed during relaxation testing at 50% strain and 21°C, as described in Example 11.
[0028] Fig.16 As an illustration of the 180° peel strength test described in Example 12, the test was conducted according to ASTM Standard F2256.
[0029] Fig.17 Depicted are the peel strength test results of glue composition A and a commercial polyvinyl acetate-based glue.
[0030] Fig.18 The peel strength test results of glue composition B and three commercial leather glues are depicted. Glue 1 is an ammoniated natural rubber adhesive, glue 2 is a solvent-based leather adhesive with a composition of ethyl acetate, heptane, and cyclohexane, and glue 3 is a solvent-based leather adhesive with a composition of ethyl acetate, acetone, solvent naphtha, and zinc oxide.
[0031] Fig.19 This is an illustration of the shear strength test method for flooring and carpet adhesives described in Example 13, which was conducted in accordance with ASTM Standard D6004.
[0032] Fig. 20 Depicted are the shear strength test results of Glue Composition B and a commercial carpet solvent based adhesive having a composition of n-hexane, toluene, and naphthalene.
[0033] Fig.21 The geometries of the stacking gel and the resolving gel are depicted, with the stacking gel housing the sample wells.
[0034] Fig. 22 Depicted is the electrophoresis process, in which an electric current forces molecules to move from the cathode to the anode side.
[0035] Fig.23 Depicted are graphs of electrophoretic tests performed on liquid latex samples having a dry rubber content of approximately 35% (ie, ammoniated latex, field latex without additives, Alfapreno, and Betapreno).
[0036] Fig.24 Depicted are images and graphs of electrophoretic testing of centrifuged liquid latex samples having approximately 60% dry rubber content (ie, Alfapreno, Betapreno, and two ammoniated latex samples). Detailed Description
[0037] Provided herein are methods for processing natural rubber (also known as latex) without the use of ammonia.
[0038] Compared to traditional latex processing methods, the ammonia-free method described herein has multiple advantages. For example, the method described herein does not require workers to be exposed to ammonia liquid or ammonia vapor, and therefore the health hazards to the personnel involved in natural rubber production, processing and management are much smaller. In addition, the waste product of this process is ammonia-free, and therefore the harm to the environment is significantly less than the traditional by-product based on ammonia processing, and does not contain pesticides, biocides or microbicides.
[0039] In preferred embodiments, the methods described herein can produce liquid latex having a shelf life of one year or longer (e.g., at least two years, at least three years, or even longer), which is much longer than conventional ammonia-treated liquid latex. As used herein, the term "shelf life" refers to the period of time over which a product can be stored under ambient conditions (i.e., without refrigeration or freezing) without exhibiting significant deterioration or changes in its physical or chemical properties.
[0040] Likewise, the ammonia-free rubber compositions described herein exhibit a variety of advantages over conventional ammonia-treated rubbers. For example, the methods described herein produce non-allergic liquid latex compositions (due to the absence of added ammonia). The latex produced according to the methods described herein does not exhibit the strong odor characteristic of added ammonia, making it more attractive for consumer-oriented applications such as sports shoes. In addition, the ammonia-free rubber produced according to the methods described herein is purer than conventional ammonia-treated rubbers, and the color is clearer, and therefore more suitable for medical applications. In addition, the ammonia-free rubber of the present invention has more excellent physical and chemical properties than conventional ammonia-treated rubbers.
[0041] As described in further detail below, the methods provided herein may include one or more of the following steps: (a) a collection step, in which the liquid latex is collected from a factory and preferably filtered to remove impurities from the environment; (b) a stabilization step, in which the liquid latex composition is refrigerated and / or the liquid latex composition is contacted with a stabilizer; (c) a preservation step, in which the liquid latex composition is contacted with a preservative; (d) a storage step, in which the liquid latex composition is stored for a period of time; and (e) a coagulation step, in which the liquid latex composition is contacted with a coagulant to form a solid latex composition. Components
[0042] The methods provided herein can utilize one or more of the following: (1) a stabilizer; (2) a preservative; (3) a pH adjuster; and (4) a coagulant. These components are described in further detail below.
[0043] Stabilizer
[0044] The methods provided herein can use stabilizers. The function of the stabilizer is to stabilize and preserve the latex in liquid form (ie, to prevent coagulation). Advantageously, the stabilizer does not contain ammonia.
[0045] The stabilizer may include a surfactant. The surfactant may be, for example, an anionic or nonionic surfactant. For example, the stabilizer may include one or more surfactants selected from the group consisting of alkylbenzene sulfonates, fatty acid alcohols, and ethoxylated fatty acid alcohols.
[0046] Non-limiting examples of suitable stabilizers include methanesulfonic acid, p-toluenesulfonic acid, 2-sulfoacetic acid, 2-naphthalenesulfonic acid, 2-anthracenesulfonic acid, p-toluenesulfonic acid, 4-amino-2,3-dichlorobenzenesulfonic acid, benzenesulfonic acid, 1-phenanthrenesulfonic acid, phenolsulfonic acid, ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, pentanesulfonic acid, hexanesulfonic acid, heptanesulfonic acid, octanesulfonic acid, nonanesulfonic acid, decanesulfonic acid, isopropylsulfonic acid, tert-butylsulfonic acid, benzenesulfonic acid, o-toluenesulfonic acid, dodecylsulfonic acid, Benzenesulfonic acid, toluenesulfonic acid, tert-butylsulfonic acid, propylbenzenesulfonic acid, toluenesulfonic acid, ethylbenzenesulfonic acid, butylbenzenesulfonic acid, pentylbenzenesulfonic acid, hexylbenzenesulfonic acid, heptylbenzenesulfonic acid, octylbenzenesulfonic acid, nonylbenzenesulfonic acid, decabenzenesulfonic acid, undecenesulfonic acid, trifluoromethanesulfonic acid, 10-camphorsulfonic acid, metasulfonic acid, xylenesulfonic acid, lauryl alcohol, ethoxylated lauryl alcohol, ethoxylated long-chain alcohols with 7 to 15 carbons and mixtures or combinations thereof. Typically, the surfactant can be aqueous or anhydrous. For example, the stabilizer can include ethoxylated lauryl alcohol. As a further example, the stabilizer can include dodecylbenzenesulfonic acid.
[0047] Preservative
[0048] The methods provided herein can use a preservative. The role of the preservative is to protect the latex and prevent it from being degraded by bacteria or other microorganisms or microfauna. Advantageously, the preservative does not contain ammonia.
[0049] The preservative may include an acid. For example, the preservative may include a halogenated acid. Non-limiting examples of suitable preservatives include hydrochloric acid, hydrofluoric acid, iodic acid, and hydrobromic acid. Typically, the acid may be aqueous or anhydrous. For example, the preservative may include hydrofluoric acid.
[0050] Without being bound by a particular theory, it is believed that the addition of the halogenated acid serves to replace the hydrogen sulfide present in the cysteine of the peptides and / or proteins in the natural latex juice and that this process serves to preserve the natural latex in its liquid form and prevent microbial degradation.
[0051] pH Adjusters
[0052] The methods provided herein can utilize pH adjusters. If desired, a pH adjuster can be used to raise the pH of the liquid latex composition to a range of about 6 to about 10, which is optimal for storage stability of the composition.
[0053] Non-limiting examples of suitable pH adjusting agents include sodium hydroxide, potassium hydroxide, amines, and mixtures or combinations thereof.
[0054] Coagulant
[0055] The methods provided herein can utilize a coagulant. The function of a coagulant (which may also be referred to herein as a synthesizing agent) is to coagulate a liquid latex, thereby producing a solid latex composition.
[0056] The coagulant may include an alcohol. For example, the coagulant may include a C1 to C8 alcohol, more preferably a C1 to C6 alcohol. Non-limiting examples of suitable coagulants include methanol, ethanol, n-propanol, benzyl alcohol, isopropanol, isobutanol, tert-butyl alcohol, amyl alcohol, hexanol, heptanol, octanol, and mixtures or combinations thereof. Typically, the alcohol may be aqueous or anhydrous. For example, the coagulant may include ethanol. Method for preparing latex composition
[0057] The methods provided herein may include one or more of the following steps: (a) a collection step, in which the liquid latex is collected from a factory and filtered to remove all impurities from the environment; (b) a stabilization step, in which the liquid latex composition is refrigerated and / or the liquid latex composition is contacted with a stabilizer; (c) a storage step, in which the liquid latex composition is contacted with a preservative; (d) a pH adjustment step, in which the liquid latex composition is contacted with a pH adjuster; (e) a storage step, in which the liquid latex composition is stored for a period of time; and (f) a coagulation step, in which the liquid latex composition is contacted with a coagulant to form a solid latex composition. These steps are described in further detail below.
[0058] Collection steps
[0059] The methods provided herein can optionally include a collecting step, wherein the natural liquid latex is collected from the plant.
[0060] The collecting step may include filtering the natural liquid latex to remove foreign matter and contaminants. For example, the natural liquid latex may be filtered using a sieve or mesh having a pore size of about 5 mm or less, about 4 mm or less, about 3 mm or less, about 2 mm or less, or about 1 mm or less.
[0061] Optionally, the natural liquid latex may be stored for a period of time prior to the stabilization step. For example, the natural liquid latex may be stored for a period of time of 0 hours to about 10 hours prior to the stabilization step.
[0062] Stabilization Steps
[0063] The methods provided herein can include a stabilization step, wherein the liquid latex composition is contacted with a stabilizer, thereby providing a stable liquid latex composition.The liquid latex composition can include natural liquid latex collected, for example, from a plant, and optionally filtered as described above.
[0064] The stabilization step may include adding a stabilizer in an amount of about 0.1% to about 30% by volume, and more typically about 0.5% to about 5% by volume, relative to the initial volume of the liquid latex composition. For example, a stabilizer may be added in an amount of at least about 0.1% by volume, at least about 0.2% by volume, at least about 0.5% by volume, at least about 1.0% by volume, at least about 1.5% by volume, or at least about 2.0% by volume, relative to the initial volume of the liquid latex composition. In a preferred embodiment, a stabilizer is added in an amount of about 0.5% to about 3% by volume, such as about 0.5% to about 2.5% by volume, or about 1% to about 2% by volume, relative to the initial volume of the liquid latex composition.
[0065] Alternatively, in some embodiments, the stabilizing step can include refrigerating the liquid latex composition. For example, the stabilizing step can include refrigerating the latex composition at a temperature no greater than about 5°C for a period of at least about 12 hours.
[0066] The stabilizing step may include refrigerating the liquid latex composition at a temperature no greater than about 4° C. or no greater than about 3° C. The stabilizing step may include refrigerating the liquid latex composition for a period of at least about 16 hours, at least about 20 hours, at least about 24 hours, at least about 30 hours, at least about 36 hours, or at least about 48 hours.
[0067] When the liquid latex composition comprises natural latex collected from a plant, and the stabilization step comprises refrigerating the liquid latex composition, the method preferably comprises initiating the stabilization step before about 72 hours after the natural latex is collected from the plant. For example, the stabilization step is preferably initiated before about 48 hours, before about 36 hours, before about 30 hours, before about 24 hours, before about 16 hours, before about 12 hours, or even before about 8 hours after the natural latex is collected from the plant.
[0068] Optionally, the stabilizing step can include refrigerating the liquid latex composition and contacting the liquid latex composition with a stabilizer, as described above.
[0069] Save Steps
[0070] The methods provided herein can optionally include a preservation step, wherein the liquid latex composition is contacted with a preservative, thereby providing a preserved liquid latex composition. Liquid latex compositions that have been stabilized and preserved are referred to herein as "stable preservation" liquid latex compositions.
[0071] The stabilization step and the preservation step may be performed in either order, or simultaneously. In some cases, the stabilizer also acts as a preservative, and thus no additional preservative needs to be added. For example, when the stabilizer is an alkylbenzene sulfonate (e.g., dodecylbenzene sulfonic acid), and / or when the stabilizer is present in an amount greater than about 1% by volume of the liquid latex composition, a separate preservation step may not be required. In this case, the stabilizer also acts as a preservative as described herein.
[0072] The preserving step may include adding a preservative in an amount of about 0.05% to about 30% by volume, more typically about 0.1% by volume to about 5% by volume, relative to the initial volume of the liquid latex composition. For example, a preservative in an amount of at least about 0.05% by volume, at least about 0.1% by volume, at least about 0.2% by volume, at least about 0.5% by volume, at least about 1.0% by volume, at least about 1.5% by volume, or at least about 2.0% by volume may be added relative to the initial volume of the liquid latex composition. In a preferred embodiment, a preservative in an amount of about 0.05% to about 2% by volume, such as about 0.05% to about 1%, or about 0.1% to about 0.5% by volume, relative to the initial volume of the liquid latex composition is added.
[0073] pH Adjustment Procedure
[0074] The methods provided herein can optionally include a pH adjustment step, wherein the liquid latex composition is contacted with a pH adjusting agent.
[0075] The liquid latex composition generally has a pH between about 6 and about 10, which is optimal for its shelf life. However, after the storage step, the pH of the liquid latex composition may be below the desired range (e.g., about 3 to about 5). In this case, it is desirable to perform a pH adjustment step, wherein the liquid latex composition is contacted with a pH adjuster in an amount sufficient to bring the pH of the liquid latex composition to the desired range (i.e., about 6 to about 10).
[0076] Storage steps
[0077] The methods provided herein may optionally include a storage step, wherein the shelf-stable liquid latex composition is stored for a period of time prior to coagulation.
[0078] The composition can be stored for a period of at least about 1 day, at least about 1 week, at least about 2 weeks, at least about 3 weeks, at least about 4 weeks, at least about 1 month, at least about 2 months, at least about 3 months, at least about 6 months, at least about 1 year, at least about 2 years, or even at least about 3 years or longer.
[0079] Condensation step
[0080] The methods provided herein may optionally include a coagulation step, wherein the liquid latex composition is contacted with a coagulant, thereby forming a solid latex composition.
[0081] The coagulation step may include adding a coagulant in an amount of about 0.5% to about 50% by volume relative to the initial volume of the liquid latex composition. For example, the coagulant may be added in an amount of at least about 1% by volume, at least about 5% by volume, at least about 10% by volume, at least about 15% by volume, at least about 20% by volume, at least about 25% by volume, or at least about 30% by volume relative to the initial volume of the liquid latex composition. In a preferred embodiment, the coagulant is added in an amount of about 10% to about 50% by volume, such as about 15% to about 40% by volume, or about 20% to about 40% by volume relative to the initial volume of the liquid latex composition. Storage-stable liquid latex composition
[0082] Also provided herein is an ammonia-free storage-stable liquid latex composition. In some embodiments, the composition is prepared by the method described above.
[0083] For example, a shelf-stable liquid latex composition may include (a) latex; (b) a stabilizer, which may be selected as described above; and (c) optionally, a preservative, which may be selected as described above.
[0084] The shelf-stable liquid latex composition preferably comprises natural latex. Typically, the composition comprises latex in an amount of about 80% by volume to about 99% by volume. For example, the shelf-stable liquid latex composition may comprise latex in an amount of at least about 80% by volume, at least about 85% by volume, at least about 90% by volume, at least about 95% by volume, at least about 96% by volume, at least about 97% by volume, at least about 98% by volume, or at least about 99% by volume.
[0085] Typically, a shelf-stable liquid latex composition comprises a stabilizer in an amount of about 0.1% to about 30% by volume, and more typically in an amount of about 0.5% by volume to about 5% by volume. For example, the composition may comprise a stabilizer in an amount of at least about 0.1% by volume, at least about 0.2% by volume, at least about 0.5% by volume, at least about 1.0% by volume, at least about 1.5% by volume, or at least about 2.0% by volume.
[0086] Typically, a shelf-stable liquid latex composition comprises a preservative in an amount of about 0.1% to about 30% by volume, and more typically in an amount of about 0.5% by volume to about 5% by volume. For example, the composition may comprise a preservative in an amount of at least about 0.05% by volume, at least about 0.1% by volume, at least about 0.2% by volume, at least about 0.5% by volume, at least about 1.0% by volume, at least about 1.5% by volume, or at least about 2.0% by volume.
[0087] The stable ammonia-free liquid latex composition provided herein is more stable than its ammonia-based counterpart. When stored at room temperature, the rheological properties of the composition provided herein remain constant over time (e.g., at least two years, at least three years or even longer). On the other hand, the rheological properties of the latex based on ammonia change significantly over time, affecting processability and handling. Depending on the ammonia content, the viscosity of the liquid latex based on ammonia can be doubled (0.35% by weight of ammonia) or even increased by 6 times (0.8% by weight of ammonia) within 45 days. The shelf life of the liquid latex based on ammonia is at most 4 months, at which point it begins to decompose.
[0088] In addition, the ammonia-free solid rubber produced using the method provided herein shows a significant improvement in mechanical properties. These improvements in mechanical properties can lead to a reduction in materials in the manufacturing process, which not only reduces costs, but also leads to lighter products. This is particularly advantageous in applications such as sports shoe manufacturing, where strong and lightweight materials are very much needed. Solid rubber composition
[0089] The present invention also provides an ammonia-free solid rubber composition. Preferably, the composition is produced by the method as described above. For example, the solid rubber composition can be prepared by contacting the storage-stable liquid latex composition as described above with a coagulant.
[0090] Figure 3 and 5 Dynamic mechanical measurements presented in show that ammonia-free solid rubber produced using the methods described herein exhibit significant improvements in mechanical properties. Relaxation tests (where 30% shear strain is applied to thin rubber samples) exhibit stresses that are at least twice that observed using ammonia-based natural rubbers. The formulation described as "Betapreno" in the examples below has a stress 2.3 times higher than the ammonia-based system. The formulations called Alfapreno and Gammapreno presented below are on average 1.8 times harder than the ammonia-based formulations.
[0091] It is also worth noting that the solid rubber compositions prepared as described herein have higher mechanical properties when dynamically tested using a sinusoidal 30% strain input. When compared to ammonia-based natural rubber, Alfapreno exhibited 1.6 times higher stress during dynamic testing, Gammapreno 1.5 times higher, and Betapreno 1.3 times higher ( Figure 3 ). The overall damping effect and hysteresis effect of the new rubber ammonia-free formula are the same as those of all rubber formulas, such as Figure 4 Therefore, influences during the use of the product (such as heating of the car tire during use) are not affected. Example
[0092] The following non-limiting examples are provided to further illustrate the present disclosure.
[0093] Example 1: Synthesis of Alfapreno
[0094] A shelf-stable liquid latex composition was prepared by mixing: 98.6 volume % of filtered stock latex; 1.0 volume % of ethoxylated lauryl alcohol (7 moles); and (c) 0.4 volume % of a mixture of 50% hydrofluoric acid and 50% water.
[0095] The shelf-stable latex was stored for two months and no degradation was observed. A solid rubber composition was then prepared by adding 300 mL of ethanol to 1 L of the shelf-stable liquid latex.
[0096] Example 2: Synthesis of Deltapreno
[0097] A storage-stable liquid latex composition was prepared by mixing: 98.6 volume percent of filtered raw latex; 1.0 volume percent of a mixture of 50% ethoxylated lauryl alcohol (3 moles) and 50% ethoxylated lauryl alcohol (7 moles) (the molar average being 5 moles); and 0.4 volume percent of a mixture of 50% hydrofluoric acid and 50% water.
[0098] The shelf-stable latex was stored for two months and no degradation was observed. A solid rubber composition was then prepared by adding 300 mL of ethanol to 1 L of the shelf-stable liquid latex.
[0099] Example 3: Synthesis of Gammapreno
[0100] A shelf-stable liquid latex composition was prepared by mixing: 98.6% by volume of filtered stock latex; 1% by volume of ethoxylated lauryl alcohol (9 moles); and 0.4% by volume of a mixture of 50% hydrofluoric acid and 50% water.
[0101] The shelf-stable latex was stored for two months and no degradation was observed. A solid rubber composition was then prepared by adding 300 mL of ethanol to 1 L of the shelf-stable liquid latex.
[0102] Example 4: Synthesis of Omegapreno
[0103] A shelf-stable liquid latex composition was prepared by mixing: 98.6% by volume of filtered stock latex; 1% by volume of ethoxylated lauryl alcohol (10 moles); and 0.4% by volume of a mixture of 50% hydrofluoric acid and 50% water.
[0104] The shelf-stable latex was stored for two months and no degradation was observed. A solid rubber composition was then prepared by adding 300 mL of ethanol to 1 L of the shelf-stable liquid latex.
[0105] Example 5: Synthesis of Epsilonpreno
[0106] A shelf-stable liquid latex composition was prepared by mixing: 98.6% by volume of filtered stock latex; 1% by volume of ethoxylated lauryl alcohol (12 moles); and 0.4% by volume of a mixture of 50% hydrofluoric acid and 50% water.
[0107] The shelf-stable latex was stored for two months and no degradation was observed. A solid rubber composition was then prepared by adding 300 mL of ethanol to 1 L of the shelf-stable liquid latex.
[0108] Example 6: Synthesis of Thetapreno
[0109] A shelf-stable liquid latex composition was prepared by mixing: 98.6% by volume of filtered stock latex; 1% by volume of ethoxylated lauryl alcohol (18 moles); and 0.4% by volume of a mixture of 50% hydrofluoric acid and 50% water.
[0110] The shelf-stable latex was stored for two months and no degradation was observed. A solid rubber composition was then prepared by adding 300 mL of ethanol to 1 L of the shelf-stable liquid latex.
[0111] Example 7: Synthesis of Betapreno
[0112] A storage-stable liquid latex composition was prepared by mixing: 98.0% by volume of the filtered raw latex; and 2.0% by volume of linear dodecylbenzenesulfonic acid.
[0113] The shelf-stable latex was stored for two months and no degradation was observed. A solid rubber composition was then prepared by adding 300 mL of ethanol to 1 L of the shelf-stable liquid latex.
[0114] Example 8: Synthesis of Fipreno
[0115] A storage-stable liquid latex composition was prepared by storing 100.0 volume % of the filtered raw latex at 3° C. for twenty-four (24) to forty-eight (48) hours, and then a solid rubber composition was prepared by adding 300 mL of ethanol to 1 L of the storage-stable liquid latex.
[0116] Example 9: Materials and sample preparation
[0117] The following materials and preparation procedures were used to prepare samples for the test methods described further below.
[0118] Samples of ammonia-free natural rubber (NR) materials (Alfapreno, Betapreno, Gammapreno, Fipreno) produced in Victoria, Colombia, were used for mechanical characterization. The corrugated sheet of natural rubber was pressed between two aluminum plates, pre-cleaned with acetone, and placed in a YAMATO convection oven at 70°C for 4 hours to ensure complete relaxation between the plates and suitable flat samples. After the flat unprocessed natural rubber sheet was pressed, a 7.50mm wide rectangular die was used to cut the relaxation test sample from the sheet to ensure that all samples had the same cross-sectional area. Similarly, a cylindrical die with a diameter of 10mm was used to cut the double shear test sample from the sheet to ensure that all samples had the same cross-sectional area.
[0119] Example 10: Dynamic Measurements in Double Shear
[0120] Test Method
[0121] Using NETZSCH A 500N Dynamic Mechanical Analyzer (DMA) was used to characterize the Lissajous plots and tan(δ) for each specific sample. The NETZSCH DMA is a dynamic analyzer capable of high forces (up to 500 Newtons, compared to up to 20 Newtons for conventional DMA units) and can perform transient and dynamic testing in the frequency range of 0.01 Hz and 100 Hz. The instrument is also capable of testing in the temperature range of 20°C and 500°C. It is important to note that a single shear test produces a moment load on the sample and does not represent pure shear. For this reason, we used the NETZSCH DMA unit to eliminate the moment and rely entirely on shear-driven loading. Figure 1 A graphical depiction of selected portions of the NETZCH DMA (illustrated as device 100) is included, as used in the following examples.
[0122] Figure 1The arrows in show the overall process by which a sample is loaded into the apparatus 100 for testing. The apparatus 100 includes a sample loading tool 105 ("tool 105") that is removably connected to a double shear fixture 110. The tool 105 includes a cylindrical container 115 having a surface 120 to which a sample 125 may be adhered, fixed, or otherwise connected. Once the sample 125 is connected to the surface 120 and the various cylindrical containers 115 of the tool 105 are engaged or connected together, the tool 105 may be inserted or received in the double shear fixture 110. More specifically, the tool 105 may be positioned through the hole 130 of the double shear fixture 110. As shown in FIG. Figure 2 As illustrated, after the tool 105 is received into the dual shear apparatus 110, the device 100 may apply a pure shear load on the sample 125 via an oscillatory motion (eg, by forcing the sample 125 to repeatedly move a predetermined distance in an upward direction and a downward direction).
[0123] In order to achieve the best possible shear loading, the sample thickness in the shear gap was kept between 1 mm–2 mm. For each example, the samples were adhered between cylindrical containers using a cyanoacrylate adhesive to achieve the highest possible bonding stability to the contact surface. After attaching the two cylindrical samples (diameter = 10 mm, and thickness = 1.5 mm) to the metal container, pressure was applied to ensure proper bonding and eliminate air bubbles trapped between the sample and the metal surface. The samples were left at room temperature for 24 hours to ensure that the adhesive achieved complete curing.
[0124] Once fully cured, the cylindrical specimens were inserted into a dual shear fixture where an oscillating motion applies a pure shear load on the two rubber samples. This study focused on testing the material at 30% and 50% shear strains at 1 Hz.
[0125] Observation of material behavior
[0126] Evaluation of the Lissajous curves extracted from cyclic tests allows one to determine how much damping a material exhibits during deformation and how nonlinear the material's viscoelastic behavior is. A sign that a material behaves in a linear viscoelastic manner is that the Lissajous curve remains elliptical. The damping of a material is characterized by a property called tan(δ). The wider the ellipse, the larger the tan(δ). A very narrow ellipse approaching a line means there is almost no damping, where tan(δ) is zero. A wide ellipse approaching a circle is a material with only damping and no elasticity, where tan(δ) approaches infinity. The equation below defines tan(δ) as the ratio between the loss modulus (damping) and the storage modulus (elastic component), which provides insight into how much energy is lost and dissipated during dynamic loading.
[0127] Once the 30% strain Lissajous curve is analyzed, Figure 3 As can be seen in the graph, the ammonia-free rubber material is much stiffer than the material processed with ammonia, as Fipreno reaches a maximum stress of 258 kPa and the rubber processed with ammonia reaches 124 kPa for a 30% double shear test at 1 Hz.
[0128] Will Figure 3 The curve in is normalized to get Figure 4 , where a shape analysis of the curves is possible. From this figure it can be seen that the width of the curves for each material is very similar, indicating that all materials have similar tan(δ). Similar trends were obtained for the 50% test, with the non-ammonia rubber materials showing higher stresses and the tan(δ) values they produced being similar to the rubber processed with ammonia (see Figure 5 and 6 ). This means that although the non-ammonia sample is stiffer than the ammonia-containing rubber, the basic viscoelastic behavior of the ammonia rubber material and the non-ammonia rubber material is the same.
[0129] Example 11: Relaxation Measurement in Tension
[0130] Test Method
[0131] Similar to the dynamic test, the NETZSCH 500NDMA characterizes relaxation behavior. Temperature-dependent behavior is captured by testing at 21°C, 50°C, and 80°C. In addition, the cross-sectional area of each sample is 22.65 mm 2 , and the clamping distance or sample length for the 10%, 30% and 50% tests were 20mm, 20mm and 15mm respectively. The clamping distance for the 50% test was slightly smaller due to the limitation of the DMA stroke length. The following equation defines the tensile strain, while Figure 7 Depicted is the relaxation test setup.
[0132] More specifically, Figure 7 Explains NETZSCH used in relaxation testing 500N DMA (here shown as device 200) is a graphical representation of selected portions. Device 200 includes a first clamp 205 and a second clamp 210. During testing, clamps 205, 210 can be moved closer to and farther from each other. In addition, sample 215 can be inserted into device 200 between clamps 205, 210 and adhered, fixed or otherwise connected to clamps 205, 210. During testing, as Figure 7As shown, the clamps 205 , 210 may first be separated by a distance L1 ; then the clamps 205 , 210 may be moved apart such that the clamps 205 , 210 are separated by a distance L2 .
[0133] Observation of material behavior
[0134] When a static strain is applied to a sample, the stress experienced by the material increases to its maximum point and then begins to decay. Relaxation is defined as the time required for the material to experience 1% of the maximum stress experienced at the beginning of the test. Ammonia-free rubber samples outperform conventional natural rubber processed with ammonia in terms of relaxation. Figure 8 As can be seen in the graph, the rubber processed with ammonia produces a material that is less rigid than the ammonia-free natural rubber, and it is understandable how Fipreno achieves four times the stress during relaxation compared to the rubber processed with ammonia. This is a good indicator of performance, as the formulation will need less reinforcement to produce a stronger material, or the neat material can be foamed to reduce weight and still maintain the same mechanical properties. All four ammonia-free natural rubber materials outperform the conventional natural rubber processed with ammonia in terms of rigidity.
[0135] Fig. 9 express Figure 8 Normalization of the curves allows analyzing the relaxation decay behavior, and it can be seen that Alfapreno, Betapreno and Gammapreno have faster relaxation capabilities, while Fipreno behaves in a more elastic way, minimizing the relaxation decay behavior.
[0136] The increase in the test environment temperature increases the free volume between molecules, thereby accelerating relaxation and reducing the rigidity of the material. Testing at 21°C, 50°C and 80°C allows analysis of these curves at different temperatures, and studying the temperature-dependent behavior of the ammonia-free rubber material leads to the determination that the relaxation behavior of the ammonia-free rubber material is less sensitive to temperature changes. Fig.10 shows a comparison of Betapreno and rubber processed with ammonia, where it can be seen that increasing temperature actually reduces the stiffness of both materials, but it is important to note that Betapreno is still stiffer than conventional natural rubber and the relaxation decay behavior is not changed, as Fig.11 shown.
[0137] In addition, the same conclusion can be drawn for the test at 80°C. Fig.12 As can be seen from the figure, increasing the temperature from 50°C to 80°C causes a slight change in the relaxation decay behavior of Betapreno, but Fig.13 As can be seen, it is still the stiffest material in the comparison.
[0138] Polymers exhibit time and temperature dependent behavior, and when tested at large strain levels, the material behaves in a nonlinear manner. The nonlinear regime is crucial to understanding what happens in real applications, as strain levels primarily fall within this region. Fig.14 The 50% relaxation test of the ammonia-free material is shown. It can be understood that the above Fig.13 The decay behavior of the 30% and 50% tests is evaluated, as shown in Figure 2. Fig.15 As shown, it can be appreciated that the increase in strain does not change the relaxation decay behavior. This minimal effect on the decay behavior indicates that the decay is independent of strain application up to 50% strain.
[0139] Example 12: Ammonia-free natural rubber glue
[0140] A glue composition comprising ammonia-free natural rubber was prepared as follows.
[0141] Glue composition A (paper glue) : A glue composition is prepared by mixing an Alfapreno natural rubber composition (99.2% by weight) with hydroxyethyl cellulose (0.8% by weight). The dry rubber content (DRC) of the natural rubber composition is about 35%. The resulting composition can be used as, for example, paper glue or leather glue.
[0142] Glue Composition B (Wood Glue and Leather Glue) : A glue composition is prepared by mixing a centrifuged Alfapreno natural rubber composition (99.0% by weight) with hydroxyethylcellulose (0.5% by weight) and collagen (0.5% by weight). The centrifuged natural rubber composition has a dry rubber content (DRC) of about 60%. The resulting composition can be used as, for example, wood glue and leather glue.
[0143] Glue compositions A and B were each tested using a 180° peel test, which was performed according to ASTM standard F2256. Fig.16 An exemplary illustration of a peel test is provided. As further described below, a first sheet 300 and a second sheet 305 (each having a width W) are separated during a peel test by applying a force F to the sheets 300, 305. The force F is applied along Fig.16 The direction indicated by the middle arrow is applied to the sheets 300, 305.
[0144] According to ASTM F2256, the interfacial toughness of the glue is reported as follows Where F is the force in Newtons and W is the width in centimeters. The specimens were cut from natural grain cowhide leather sheets with a width W of 2.54 cm (1”). The peel strength of glue composition A was compared with that of a commercial polyvinyl acetate glue, such as Fig.17 As shown. Table 1 presents the results. It can be seen that the peel strength of glue composition A is 23.64N / cm, which is significantly higher than the commercial adhesive (which exhibits a peel strength of 6.29N / cm). Each test was repeated 6 times, and the two materials performed in a repeatable manner, with standard deviations of 1.91 and 0.68N / cm for glue composition A and PVA-based commercial glue, respectively. Table 1. Comparison of leather peeling test results of glue composition A (paper glue) and commercially available PVA-based glue
[0145] The peel strength of Glue Composition B was compared with that of a commercial ammoniated natural rubber glue (Glue 1) and two commercial ethyl acetate solvent-based leather adhesives (Glues 2 and 3). Fig.18 As shown. Table 2 presents the results. It can be seen that the peel strength of glue composition B is 44.53N / cm, which is significantly higher than the commercial leather adhesive counterpart. The peel strength of ammoniated natural rubber adhesive (glue 1) is 15.72N / cm, and the peel strength of solvent-based ethyl acetate is 17.94 (glue 2) and 36.63N / cm (glue 3), respectively. All tests were repeated 6 times and were reproducible, as reflected by the standard deviation shown in Table 2. Table 2. Comparison of leather peel test results for Glue Composition B (wood and leather glue) with various commercial adhesives used in the footwear industry.
[0146] The shear strength of Glue Composition B was compared to commercial solvent-based flooring and carpet adhesives using a test performed according to ASTM Standard D6004. Fig.19 An exemplary illustration of a shear strength test is provided, wherein a first material 350 (here provided as a carpet backing) and a second material 355 (here provided as plywood) are bonded to each other. Fig.19 A force F is applied to materials 350, 355 in the direction indicated by the arrow. According to ASTM D6004, the interfacial shear strength of the adhesive is reported as follows: Where F is the force in Newtons; W is the width of the sample in meters; and L is the length of the sample bonded to the plywood substrate in meters. Carpet backing test specimens were cut into 2.54 cm (1") widths and bonded to plywood. In the tests, W and L were 2.54 cm (1") and 7.62 cm (3"), respectively. Fig. 20The shear strength of Glue Composition B and solvent-based floor and carpet adhesives were compared. Table 3 shows the results. It can be seen that the shear strength of Glue Composition B is 203.15 kPa, which is higher than the commercial solvent-based carpet adhesive, which exhibits a shear strength of 185.23 kPa. The test was repeated 8 times, and the results are consistent with the standard deviation of Glue Composition B and the commercial carpet adhesive (47.08 and 54.82 kPa, respectively). Table 3. Comparison of carpet shear test results for Glue Composition B (wood and leather glue) with commercial adhesives used in the flooring and carpet industry.
[0147] Example 13: Allergy Test
[0148] Sample preparation
[0149] Natural rubber is known to contain allergenic proteins from the Hevea brasiliensis (Hev b). Of the 14 officially recognized protein allergens found in natural rubber latex, four are known to be the most potent allergens: Hev b 1, Hev b 3, Hev b 5, and Hev b 6.02. To test the amount of these allergens in the new ammonia-free natural rubber, Alfapreno from Example 1 and Betapreno from Example 7 were compared to ammoniated natural rubber and fresh latex without additives. For the control test, 11 liters of liquid natural rubber latex were collected from a plantation in the Caldas de Victoria region of Colombia on the same day and prepared into 7 different samples that were tested for protein content using electrophoresis and ELISA tests. Table 4 lists the liquid latex samples prepared for the tests. Table 4. Seven liquid latex samples used for allergy testing
[0150] Electrophoresis test
[0151] In order to separate and qualitatively assess the Hev b 1, Hev b 3, Hev b 5 and Hev b 6.02 protein content in the seven liquid latex samples described in Table 4, an electrophoresis test was performed on each sample. Two separate tests were performed, one for four uncentrifuged samples and one for three centrifuged samples. For each test, a vertically stacked double-layer gel system, a concentrating gel and a separating gel, with a thickness of approximately 0.75 mm, was used, which was fixed between two glass plates. Fig.21A vertical gel system 400 (hereinafter referred to as "system 400") designed to perform the electrophoresis test described herein is schematically illustrated. In system 400, a first glass plate 405 and a second glass plate 410 may be placed to hold a separation gel 415 and a concentration gel 420 between plates 405, 410. Standards 425 and samples 430 may be placed in sample wells 435, which are located at the upper portion of system 400.
[0152] The composition of the separating gel and the concentrating gel included three different solutions as described in Tables 5-7 below. The composition of each gel is listed in Tables 8 and 9. Table 5. Solution 1 composition Table 6. Solution 2 composition Table 7. Solution 3 composition Table 8. Separation gel composition (15% gel) Table 9. Concentrated gel composition (4% gel)
[0153] Conductive buffer compositions were prepared to surround the gel system during electrophoresis testing (as shown in Table 10). In addition, dye buffer compositions shown in Table 11 were added to the liquid latex samples as shown in Tables 12 and 13. Once prepared, the sample crucibles were heated to 100°C for 5 minutes to allow sodium dodecyl sulfate to denature the proteins, resulting in strict separation of the proteins based on their molecular weight. Table 10. Surrounding Buffer Composition Table 11. Dry buffer composition (for 10 mL) Table 12. Sample preparation composition for fresh latex samples (approximately 35% dry rubber content) Table 13. Sample preparation composition for centrifuged latex samples (approximately 60% dry rubber content)
[0154] In the next step, 5 μL of sample was placed into the wells, as Fig.21A standard sample (Spectra Multicolor LowRange Protein Ladder 26628 provided by Thermo Fisher) was placed in the left well. This standard produces a standard ladder or scale in the gel to characterize bands corresponding to proteins with molecular weights of 40 kDa, 25 kDa, 15 kDa, 10 kDa, 4.6 kDa, and 1.7 kDa.
[0155] Once the liquid latex sample is deposited within the well, the system is placed in a surrounding buffer composition. Fig. 22 A schematic diagram of a system including a buffer composition is depicted in FIG. As shown, a buffer composition 450 is located in an upper buffer 455 and a lower buffer 460 of the system 400. In addition, a power source (not shown) can be connected to the system 400 so that the upper buffer 455 can be used as a cathode and the lower buffer 460 can be used as an anode. Therefore, when a voltage is applied to the system 400, proteins in the standard 425 and the sample 430 can pass through the gels 415, 420. The standard 425 is calibrated so that it provides reference points at 1.7 kDa, 4.6 kDa, 10 kDa, 15 kDa, 25 kDa and 40 kDa mass units, which can be used to interpret the data generated by the electrophoresis test.
[0156] A Bio-America Equipment DYY-6CBA power battery (set to 80V) was connected to the upper (cathode) and lower (anode) surrounding buffers of the Bio-RadMini-PROTEAN Tetra System to force the protein to move toward the anode (positive electrode) to the point where the concentrated gel ends. At this point, the power battery was set to 100V to force the protein to pass through the separation gel. The charge was maintained for up to 3.5 hours to ensure that the protein moved the appropriate distance indicated by the molecular weight standard (ladder) until the stained protein approached the bottom of the separation gel in the lower buffer.
[0157] The next step in the denaturing polyacrylamide gel electrophoresis procedure is to remove the gel from the glass plate and fix the standard ladder in a 5% glutaraldehyde solution. Once the ladder is fixed, the gel is immersed in a container containing a stain, the composition of which is shown in Table 14. The container containing the immersed gel system is agitated very slowly to allow the dye to stain the proteins, ultimately making the proteins visible throughout the gel lane. To ensure proper resolution, a destaining solution is used to wash away excess pigment. The destaining solution composition is presented in Table 15 below.
[0158] Fig.23 Gels tested on samples with 35% dry rubber content are presented. They are (from left to right) ammoniated latex, fresh latex without additives, Alfapreno and Betapreno. The wells of some samples are empty, however, they show bands due to migration from adjacent columns. The grayscale intensity of the captured gel images was analyzed using a MATLAB program (pixel intensity 255 reflects perfect white pixels, and pixel intensity 0 reflects perfect black pixels). These qualitative images and graphs clearly show the large amount of protein present in ammoniated latex. The lowest protein content can be seen in the Alfapreno sample. Fig.24 Gels tested on centrifuged 60% dry rubber content samples are presented, from left to right Alfapreno, Betapreno and two ammoniated latex samples. The qualitative images and graphs also show that the protein content is higher in the ammoniated liquid latex samples and significantly lower in the Alfapreno and Betapreno samples.
[0159] ELISA test
[0160] The ELISA test was performed according to ASTM 7427: Standard Test Method for Immunological Measurement of Four Major Allergenic Proteins (Hev b 1, 3, 5, and 6.02) in Hevea Natural Rubber and Products Derived from Latex. The test was performed using the Latex 4-in-1 ELISA (Hev b1, b3, b5, b6.02) test kit produced by ICOSAGEN AS in Estonia. ELISA kit 4 for latex allergen was performed.
[0161] Table 14 presents the ELISA test results for the seven liquid latex samples presented in Table 4. The results clearly show the lower amount of allergenic proteins in the new ammonia-free latex. Centrifuged Alfapreno liquid latex had the lowest amount of allergenic proteins, consistent with the electrophoresis test results. Table 14. Allergenic protein content according to ELISA test *Uncertain, beyond the scope of testing §Below the test limit
[0162] When introducing elements of the present disclosure or the preferred embodiments thereof, the articles "a", "an", "the" and "said" are intended to mean that there are one or more of the elements. The terms "comprising", "including" and "having" are intended to be inclusive and mean that there may be additional elements besides the listed elements.
[0163] In view of the above, it will be seen that the several objects of the disclosure are achieved and other advantageous results attained.
[0164] As various changes could be made in the above products and methods without departing from the scope of the disclosure, it is intended that all matter contained in the above description shall be interpreted as illustrative and not in a limiting sense.
Claims
1. A method for processing natural latex without using ammonia, the method comprising: A stabilization step wherein the liquid latex composition is contacted with a stabilizer selected from the group consisting of alkylbenzene sulfonates, fatty acid alcohols, and ethoxylated fatty acid alcohols.
2. The method according to claim 1, wherein the stabilizer comprises a surfactant selected from the group consisting of methanesulfonic acid, p-toluenesulfonic acid, 2-sulfoacetic acid, 2-naphthalenesulfonic acid, 2-anthracenesulfonic acid, p-toluenesulfonic acid, 4-amino-2,3-dichlorobenzenesulfonic acid, benzenesulfonic acid, 1-phenanthrenesulfonic acid, phenolsulfonic acid, ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, pentanesulfonic acid, hexanesulfonic acid, heptanesulfonic acid, octanesulfonic acid, nonanesulfonic acid, decanesulfonic acid, isopropylsulfonic acid, tert-butylsulfonic acid, benzenesulfonic acid Acid, o-toluenesulfonic acid, dodecylbenzenesulfonic acid, toluenesulfonic acid, tert-butylsulfonic acid, propylbenzenesulfonic acid, methylbenzenesulfonic acid, ethylbenzenesulfonic acid, butylbenzenesulfonic acid, pentylbenzenesulfonic acid, hexylbenzenesulfonic acid, heptylbenzenesulfonic acid, octylbenzenesulfonic acid, nonylbenzenesulfonic acid, decabenzenesulfonic acid, undecylbenzenesulfonic acid, trifluoromethanesulfonic acid, 10-camphorsulfonic acid, m-sulfonic acid, xylenesulfonic acid, lauryl alcohol, ethoxylated lauryl alcohol, ethoxylated long chain alcohols having 7 to 15 carbons, and mixtures or combinations thereof.
3. The method of claim 2, wherein the stabilizer comprises ethoxylated lauryl alcohol.
4. The method of claim 2, wherein the stabilizer comprises dodecylbenzenesulfonic acid.
5. The method according to any one of claims 1 to 4, wherein the stabilizing step comprises adding a stabilizer in an amount of about 0.1% to about 30% by volume, or about 0.5% by volume to about 5% by volume, relative to the initial volume of the liquid latex composition.
6. The method of any one of claims 1 to 5, wherein the stabilizing step comprises adding a stabilizer in an amount of at least about 0.1% by volume, at least about 0.2% by volume, at least about 0.5% by volume, at least about 1.0% by volume, at least about 1.5% by volume, or at least about 2.0% by volume relative to the initial volume of the liquid latex composition.
7. The method according to any one of claims 1 to 6, wherein the stabilizing step comprises adding a stabilizer in an amount of about 0.5% to about 3% by volume, for example about 0.5% to about 2.5% or about 1% to about 2% by volume, relative to the initial volume of the liquid latex composition.
8. A method for processing natural latex without using ammonia, the method comprising: A stabilization step wherein the liquid latex composition is refrigerated at a temperature no greater than about 5°C for at least about 12 hours.
9. The method of claim 8, wherein the liquid latex composition is refrigerated at a temperature no higher than about 4°C or no higher than about 3°C.
10. The method of claim 8 or 9, wherein the liquid latex composition is refrigerated for a period of at least about 16 hours, at least about 20 hours, at least about 24 hours, at least about 30 hours, at least about 36 hours, or at least about 48 hours.
11. The method according to any one of claims 1 to 10, further comprising a preservation step, wherein the liquid latex composition is contacted with a preservative, And the preservative does not include ammonia.
12. The method of claim 11, wherein the preservative comprises an acid.
13. The method of claim 12, wherein the preservative comprises a halogenated acid.
14. The method of claim 13, wherein the preservative comprises a halogenated acid selected from the group consisting of hydrochloric acid, hydrofluoric acid, iodic acid, and hydrobromic acid.
15. The method of claim 14, wherein the preservative comprises hydrofluoric acid.
16. The method according to any one of claims 11 to 15, wherein the stabilization step is performed before the preservation step.
17. The method according to any one of claims 11 to 15, wherein the stabilizing step and the preserving step are performed simultaneously.
18. The method of any one of claims 11 to 17, wherein the preserving step comprises adding a stabilizer in an amount of about 0.05% to about 30% by volume, or in an amount of about 0.1% by volume to about 5% by volume, relative to the initial volume of the liquid latex composition.
19. The method of any one of claims 11 to 18, wherein the preserving step comprises adding a preservative in an amount of at least about 0.05% by volume, at least about 0.1% by volume, at least about 0.2% by volume, at least about 0.5% by volume, at least about 1.0% by volume, at least about 1.5% by volume, or at least about 2.0% by volume relative to the initial volume of the liquid latex composition.
20. The method of any one of claims 11 to 19, wherein the preserving step comprises adding a preservative in an amount of about 0.05% to about 2% by volume, about 0.05% to about 1% by volume, or about 0.1% to about 0.5% by volume relative to the initial volume of the liquid latex composition.
21. The method of any one of claims 1 to 20, further comprising a pH adjustment step, wherein the liquid latex composition is contacted with a pH adjuster.
22. The method of claim 21, wherein the pH of the liquid latex composition prior to the pH adjustment step is less than about 6.
23. The method of claim 21 or 22, wherein the pH of the liquid latex composition after the pH adjustment step is from about 6 to about 10.
24. The method according to any one of claims 21 to 23, wherein the pH adjusting agent is selected from the group consisting of sodium hydroxide, potassium hydroxide, amines, and mixtures or combinations thereof.
25. The method of any one of claims 1 to 24, further comprising a coagulation step, wherein the liquid latex composition is contacted with a coagulant to form a solid latex composition.
26. The method of claim 25, wherein the coagulant comprises an alcohol.
27. The method of claim 26, wherein the coagulant comprises a C1 to C8 alcohol.
28. The method of claim 27, wherein the coagulant comprises a C1 to C6 alcohol.
29. The method of claim 28, wherein the coagulant comprises an alcohol selected from the group consisting of methanol, ethanol, n-propanol, benzyl alcohol, isopropanol, isobutanol, tert-butanol, pentanol, hexanol, heptanol, octanol, and mixtures or combinations thereof.
30. The method of claim 29, wherein the coagulant comprises ethanol.
31. The method of any one of claims 25 to 30, wherein the coagulating step comprises adding a coagulant in an amount of about 0.5% to about 50% by volume relative to the initial volume of the liquid latex composition.
32. The method of any one of claims 25 to 30, wherein the coagulating step comprises adding a coagulant in an amount of about 10% to about 50% by volume, about 15% to about 40% by volume, or about 20% to about 40% by volume relative to the initial volume of the liquid latex composition.
33. The method of any one of claims 25 to 32, wherein the coagulating step comprises adding a coagulant in an amount of at least about 1% by volume, at least about 5% by volume, at least about 10% by volume, at least about 15% by volume, at least about 20% by volume, at least about 25% by volume, or at least about 30% by volume relative to the initial volume of the liquid latex composition.
34. The method of any one of claims 25 to 33, further comprising a storage step, wherein the liquid latex composition is stored for a period of at least about 1 day after the stabilization step and before the coagulation step.
35. The method of claim 34, wherein the liquid latex composition is stored for a period of at least about 1 week, at least about 2 weeks, at least about 3 weeks, at least about 4 weeks, at least about 1 month, at least about 2 months, at least about 3 months, at least about 6 months, at least about 1 year, at least about 2 years, or at least about 3 years.
36. A storage-stable liquid latex composition prepared according to the method of any one of claims 1 to 24.
37. A storage-stable liquid latex composition comprising: (a) latex; and (b) A stabilizer comprising a surfactant selected from the group consisting of alkylbenzene sulfonates, fatty acid alcohols and ethoxylated fatty acid alcohols.
38. The composition of claim 37 comprising about 80% by volume to about 99% by volume latex.
39. The composition of claim 38, comprising latex in an amount of at least about 80% by volume, at least about 85% by volume, at least about 90% by volume, at least about 95% by volume, at least about 96% by volume, at least about 97% by volume, at least about 98% by volume, or at least about 99% by volume.
40. The composition of claim 39, comprising a stabilizer in an amount from about 0.1% to about 30% by volume, or from about 0.5% by volume to about 5% by volume.
41. The composition of claim 40, comprising a stabilizer in an amount of at least about 0.1% by volume, at least about 0.2% by volume, at least about 0.5% by volume, at least about 1.0% by volume, at least about 1.5% by volume, or at least about 2.0% by volume.
42. The composition of any one of claims 37 to 41, wherein the stabilizer comprises a surfactant selected from the group consisting of methanesulfonic acid, p-toluenesulfonic acid, 2-sulfoacetic acid, 2-naphthalenesulfonic acid, 2-anthracenesulfonic acid, p-toluenesulfonic acid, 4-amino-2,3-dichlorobenzenesulfonic acid, benzenesulfonic acid, 1-phenanthrenesulfonic acid, phenolsulfonic acid, ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, pentanesulfonic acid, hexanesulfonic acid, heptanesulfonic acid, octanesulfonic acid, nonanesulfonic acid, decanesulfonic acid, isopropylsulfonic acid, tert-butylsulfonic acid, Sulfonic acid, benzenesulfonic acid, o-toluenesulfonic acid, dodecylbenzenesulfonic acid, methylbenzenesulfonic acid, tert-butylsulfonic acid, propylbenzenesulfonic acid, methylbenzenesulfonic acid, ethylbenzenesulfonic acid, butylbenzenesulfonic acid, pentylbenzenesulfonic acid, hexylbenzenesulfonic acid, heptylbenzenesulfonic acid, octylbenzenesulfonic acid, nonylbenzenesulfonic acid, decabenzenesulfonic acid, undecylbenzenesulfonic acid, trifluoromethanesulfonic acid, 10-camphorsulfonic acid, m-sulfonic acid, xylenesulfonic acid, lauryl alcohol, ethoxylated lauryl alcohol, ethoxylated long chain alcohols having 7 to 15 carbons, and mixtures or combinations thereof.
43. The composition of claim 42, wherein the stabilizer comprises ethoxylated lauryl alcohol.
44. The composition of claim 43, wherein the stabilizer comprises dodecylbenzenesulfonic acid.
45. The composition according to any one of claims 37 to 44, further comprising: (c) A preservative comprising an acid.
46. The composition of claim 45, wherein the preservative comprises a halogenated acid.
47. The composition of claim 46, wherein the preservative comprises a halogenated acid selected from the group consisting of hydrochloric acid, hydrofluoric acid, iodic acid, and hydrobromic acid.
48. The composition of claim 47, wherein the preservative comprises hydrofluoric acid.
49. The composition of any one of claims 45 to 48, comprising a preservative in an amount of about 0.1% to about 30% by volume, or about 0.5% by volume to about 5% by volume.
50. The composition of any one of claims 45 to 49, comprising a preservative in an amount of at least about 0.05% by volume, at least about 0.1% by volume, at least about 0.2% by volume, at least about 0.5% by volume, at least about 1.0% by volume, at least about 1.5% by volume, or at least about 2.0% by volume.
51. A method of preparing an ammonia-free solid rubber composition, the method comprising contacting the storage-stable liquid latex composition of any one of claims 36 to 50 with a coagulant.
52. The method of claim 51, wherein the coagulant comprises an alcohol.
53. An ammonia-free solid rubber composition prepared according to the method of claim 51 or 52.