Silane-modified copolymer, method for producing same, and composition comprising same

By introducing epoxy, hydrolyzable silane and polybutadiene frameworks into the silane coupling agent, and manufacturing silane modified copolymers through specific processes, the volatile nature of epoxy silane coupling agents in the prior art is solved by the introduction of epoxy silane coupling agents. The problem of high is achieved, and the coexistence effect of high adhesion and low volatility is achieved.

CN118946596APending Publication Date: 2024-11-12SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031401.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-11
Filing Date
2023-03-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The conventional silane coupling agent with epoxy groups has high volatility and safety problems, and it is difficult to achieve both high adhesion and low volatility.

Method used

A silane modified copolymer with an epoxy group, a hydrolyzable silyl group and a polybutadiene backbone was developed and the copolymer was produced by hydrosilylation reaction in the presence of a platinum-containing compound catalyst, combining with an organosilicon compound compound. The composition is formed to improve its adhesiveness and reduce volatile properties.

Benefits of technology

The high adhesion and low volatility are achieved, and the silane modified copolymer exhibits excellent adhesion properties in the composition, and reduces contamination on peripheral equipment by reducing volatility and improving productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946596A_ABST
    Figure CN118946596A_ABST
Patent Text Reader

Abstract

Provided is a silane-modified copolymer containing structural units represented by formula (1) and formula (2) and structural units containing an epoxy group. # imgabs0 # (In the formula, R1 each independently represents an alkyl group having 1-10 carbon atoms or an aryl group having 6-20 carbon atoms, R2 each independently represents an alkyl group having 1-10 carbon atoms or an aryl group having 6-20 carbon atoms, m represents an integer of 1-3, and star * represents a bond to an adjacent structural unit. Wherein the order of each structural unit is arbitrary).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a silane-modified copolymer, a method for producing the same, and a composition containing the same. More specifically, the present invention relates to a copolymer having an epoxy group and a hydrolyzable silyl group and having a polybutadiene skeleton, a method for producing the same, and a composition containing the copolymer. Background Art

[0002] Organosilicon compounds having both functional groups reactive with organic materials, such as epoxy, amino, acryloyl, methacryloyl, mercapto, isocyanate, and anhydride residues, and functional groups reactive with inorganic materials, such as hydrolyzable silyl groups, are generally referred to as silane coupling agents, and generally function as a medium for combining organic and inorganic materials that are difficult to combine.

[0003] Taking advantage of such characteristics, silane coupling agents are widely used as modifiers for organic and inorganic materials, adhesive aids used for bonding two materials, various additives, and the like.

[0004] Among them, 3-glycidyloxypropyltrimethoxysilane is generally used as a silane coupling agent having an epoxy functional group. Its effect has been proven in a wide range of applications. However, since it is a monomer, it has high volatility and concerns about safety. Therefore, a material with low volatility is required.

[0005] Furthermore, the following technical documents can be cited as prior art documents related to the present invention.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2009-191155 Summary of the invention

[0009] Problems to be solved by the invention

[0010] The present invention has been made in view of the above-mentioned actual situation, and an object of the present invention is to provide a silane-modified copolymer having an epoxy group and having high adhesion to a substrate and low volatility.

[0011] Means for solving problems

[0012] The present inventors have conducted intensive studies to solve the above problems and have found that a predetermined copolymer having an epoxy group and a hydrolyzable silyl group and a polybutadiene skeleton has low volatility and high adhesion to a substrate, thereby completing the present invention.

[0013] That is, the present invention provides:

[0014] 1. A silane-modified copolymer comprising structural units represented by the following formulae (1) and (2) and a structural unit containing an epoxy group,

[0015] [Chemistry 1]

[0016]

[0017] (In the formula, the asterisk * indicates the bond with the adjacent structural unit. In formula (2), R 1 each independently represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 20 carbon atoms, and R 2 Each of the structural units independently represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 20 carbon atoms, and m represents an integer of 1 to 3. The order of each structural unit is arbitrary.

[0018] 2. The silane-modified copolymer according to 1, wherein the epoxy group-containing structural unit is one or more structural units selected from the group consisting of the structural units represented by the following formula (3) and formula (4);

[0019] [Chemistry 2]

[0020]

[0021] (In the formula, the asterisk * has the same meaning as above.)

[0022] 3. The method for producing a silane-modified copolymer according to item 1, comprising the steps of: subjecting a copolymer comprising structural units represented by the following formulae (1) and (5) and structural units containing epoxy groups (wherein the order of the structural units is arbitrary) to a hydrosilylation reaction with an organosilicon compound represented by the following formula (6) in the presence of a catalyst containing a platinum compound;

[0023] [Chemistry 3]

[0024]

[0025] (In the formula, the asterisk * has the same meaning as above.)

[0026] [Chemistry 4]

[0027]

[0028] (Where R 1 , R 2 and m have the same meanings as above.)

[0029] 4. The method for producing a silane-modified copolymer according to 3, wherein the epoxy group-containing structural unit is one or more structural units selected from the group consisting of the structural units represented by the following formula (3) and formula (4);

[0030] [Chemistry 5]

[0031]

[0032] (In the formula, the asterisk * has the same meaning as above.)

[0033] 5. A composition comprising the silane-modified copolymer according to 1 or 2;

[0034] 6. The composition according to 5, comprising an organopolysiloxane.

[0035] Effects of the Invention

[0036] The silane-modified copolymer of the present invention has an epoxy group, a hydrolyzable silyl group and a polybutadiene skeleton, has low volatility, and can exhibit high adhesiveness when mixed in a composition. DETAILED DESCRIPTION

[0037] The present invention will be described in detail below.

[0038] [1] Silane-modified copolymer

[0039] The silane-modified copolymer of the present invention comprises a polybutadiene-constituting unit represented by the following formula (1), a hydrolyzable silyl group-containing structural unit represented by the formula (2), and an epoxy group-containing structural unit. The order of the structural units is arbitrary.

[0040] [Chemistry 6]

[0041]

[0042] (In the formula, the asterisk * indicates a bond to an adjacent structural unit.)

[0043] In the above formula (2), R 1 each independently represents an alkyl group having 1 to 10 carbon atoms, preferably 1 to 8 carbon atoms, more preferably 1 to 6 carbon atoms, or an aryl group having 6 to 20 carbon atoms, preferably 6 to 15 carbon atoms, more preferably 6 to 10 carbon atoms, and R 2 Each of them independently represents an alkyl group having 1 to 10 carbon atoms, preferably 1 to 8 carbon atoms, more preferably 1 to 6 carbon atoms, or an aryl group having 6 to 20 carbon atoms, preferably 6 to 15 carbon atoms, more preferably 6 to 10 carbon atoms; and m represents an integer of 1 to 3.

[0044] As R 1 and R 2The alkyl group may be a linear, branched or cyclic group having 1 to 10 carbon atoms. Specific examples thereof include methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl and cyclooctyl groups.

[0045] As R 1 and R 2 Specific examples of the aryl group having 6 to 20 carbon atoms include phenyl, α-naphthyl, β-naphthyl and the like.

[0046] Among these, R 1 , preferably a straight-chain alkyl group, more preferably a methyl group or an ethyl group.

[0047] In addition, as R 2 , preferably a straight-chain alkyl group, more preferably a methyl group or an ethyl group.

[0048] m is an integer of 1 to 3, preferably 2 or 3, and more preferably 3.

[0049] In the silane-modified copolymer of the present invention, the structure of the epoxy-containing structural unit is not particularly limited as long as it contains an epoxy group and can constitute a copolymer together with the structural units represented by the above-mentioned formula (1) and formula (2). It is preferably selected from one or more of the structural units represented by the following formula (3) and formula (4), and more preferably both of them.

[0050] [Chemistry 7]

[0051]

[0052] (In the formula, the asterisk * has the same meaning as above.)

[0053] In the silane-modified copolymer of the present invention, the total number of the structural units represented by the above formula (1) and formula (2) in the total number of structural units constituting the silane-modified copolymer is preferably 30 mol% or more, more preferably 40 mol% or more. There is no particular upper limit, but it is preferably 90 mol% or less.

[0054] In particular, in order to further enhance the effect of the silane-modified copolymer of the present invention as an adhesive aid, the proportion of the structural unit having a hydrolyzable silyl group represented by the above formula (2) in the total number of structural units constituting the silane-modified copolymer is preferably 2 mol% or more, more preferably 4 mol% or more, and there is no particular upper limit, but it is preferably 25 mol% or less.

[0055] The total ratio of the structural units containing epoxy groups represented by the above formula (3) and formula (4) is preferably 0.5 mol% or more, more preferably 1 mol% or more. There is no particular limitation on the upper limit, but it is preferably 30 mol% or less. It should be noted that the total of the structural units constituting the silane-modified copolymer is 100 mol%.

[0056] In the silane-modified copolymer of the present invention, in addition to the structural units represented by the above-mentioned formulas (1) to (4), other structural units may be included. As specific examples of other structural units, structural units represented by the following formula (5), structural units represented by the following formula (7), etc. may be listed. In the case of including other structural units, their total proportion is preferably less than 50 mol%, more preferably less than 45 mol% in the total number of structural units constituting the silane-modified copolymer. It should be noted that in the case of including other structural units, the order of each structural unit is also arbitrary. In addition, in this case, the total of each structural unit constituting the silane-modified copolymer is also 100 mol%.

[0057] [Chemistry 8]

[0058]

[0059] (In the formula, the asterisk * has the same meaning as above.)

[0060] The number average molecular weight of the silane-modified copolymer of the present invention is not particularly limited, but is preferably 500 or more, more preferably 1000 or more. The upper limit of the number average molecular weight is preferably 10000 or less, more preferably 5000 or less.

[0061] In addition, the number average molecular weight is a polystyrene conversion value using gel permeation chromatography (GPC).

[0062] [2] Manufacturing method

[0063] The silane-modified copolymer of the present invention can be obtained, for example, by subjecting a raw material copolymer containing structural units represented by the following formulas (1) and (5) and a structural unit containing an epoxy group and an organic silicon compound represented by the following formula (6) to a hydrosilylation reaction in the presence of a catalyst containing a platinum compound. However, the order of the structural units is arbitrary.

[0064] [Chemistry 9]

[0065]

[0066] (In the formula, asterisks *, R 1 , R 2 and m have the same meanings as above.)

[0067] In the raw material copolymer, as long as the structural unit containing an epoxy group contains an epoxy group, it can constitute a copolymer together with the structural units represented by the above formula (1) and formula (5), and there is no particular limitation on its structure. It is preferably selected from one or more of the structural units represented by the following formula (3) and formula (4), and more preferably both of them.

[0068] [Chemistry 10]

[0069]

[0070] (In the formula, the asterisk * has the same meaning as above.)

[0071] Copolymers containing structural units represented by the above formula (1) and formula (5) and structural units containing epoxy groups can be obtained as commercial products, for example, Ricon 657 (manufactured by Cray Valley Co., Ltd.), JP-100, JP-200 (all manufactured by Nippon Soda Co., Ltd.), EPOLEAD PB4700 (manufactured by Daicel Corporation), ADEKA SIZER BF-1000 (manufactured by ADEKA Corporation), etc. are already on the market.

[0072] Alternatively, a copolymer obtained by epoxidizing a part of the unsaturated bonds of a copolymer having structural units represented by the above formulae (1) and (5), such as Ricon 130 (manufactured by Cray Valley Co., Ltd.), may be used.

[0073] On the other hand, examples of the organic silicon compound represented by the above formula (6) include trimethoxysilane, triethoxysilane, dimethoxymethylsilane, diethoxymethylsilane and the like.

[0074] The reaction ratio of the raw copolymer and the organosilicon compound represented by the above formula (6) is preferably 0.01 to 3 mol, more preferably 0.05 to 1 mol, per 1 mol of the structural unit represented by the formula (5) in the raw copolymer.

[0075] The catalyst containing a platinum compound used in the above-mentioned hydrosilylation reaction is not particularly limited. Specific examples thereof include chloroplatinic acid, an alcohol solution of chloroplatinic acid, a toluene or xylene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex, tetrakis(triphenylphosphine)platinum, dichlorobis(triphenylphosphine)platinum, dichlorobisacetonitrile platinum, dichlorobisbenzonitrile platinum, dichlorocyclooctadiene platinum, platinum-carbon, platinum-alumina, platinum-silica and other supported catalysts.

[0076] Among these, from the viewpoint of selectivity during hydrosilylation, a zero-valent platinum complex is preferred, and a toluene or xylene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex is more preferred.

[0077] The amount of the catalyst containing the platinum compound is not particularly limited. From the perspective of reactivity, productivity, etc., it is preferred that the amount of platinum atoms contained is 1×10 -8 ~1×10 -2 The molar amount is more preferably 1×10 -7 ~1×10 -3 The amount of moles.

[0078] In the above-mentioned hydrosilylation reaction, a co-catalyst may be used. Examples of the co-catalyst include ammonium salts of inorganic acids, amide compounds, and carboxylic acids.

[0079] Specific examples of ammonium salts of inorganic acids include ammonium chloride, ammonium sulfate, ammonium amidosulfate, ammonium nitrate, monoammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, diammonium phosphite, ammonium carbonate, ammonium bicarbonate, ammonium sulfide, ammonium borate, and ammonium borofluoride. Among them, ammonium salts of inorganic acids having a pKa of 2 or more are preferred, and ammonium carbonate and ammonium bicarbonate are more preferred.

[0080] Specific examples of the amide compound include formamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, propionamide, acrylamide, malonamide, succinamide, maleamide, fumaramide, benzamide, phthalamide, palmitamide, and stearamide.

[0081] Specific examples of the carboxylic acid include acetic acid, propionic acid, butyric acid, methoxyacetic acid, valeric acid, hexanoic acid, heptanoic acid, octanoic acid, lactic acid, glycolic acid, and the like. Among them, formic acid, acetic acid, and lactic acid are preferred, and acetic acid is more preferred.

[0082] When a co-catalyst is used, its amount is not particularly limited. From the viewpoint of reactivity, selectivity, and cost, it is preferably 1×10 -5 ~1×10 -1 mole, more preferably 1×10 -4 ~5×10 -1 Moore.

[0083] The above reaction can be carried out without a solvent, but a solvent can also be used.

[0084] Specific examples of usable solvents include hydrocarbon solvents such as pentane, hexane, cyclohexane, heptane, isooctane, benzene, toluene, and xylene; ether solvents such as diethyl ether, tetrahydrofuran, and dioxane; ester solvents such as ethyl acetate and butyl acetate; aprotic polar solvents such as N,N-dimethylformamide; chlorinated hydrocarbon solvents such as dichloromethane and chloroform, etc. These solvents may be used alone or in combination of two or more.

[0085] The reaction temperature in the hydrosilylation reaction is not particularly limited, and the reaction can be carried out at a temperature ranging from 0°C to 200°C, preferably 0°C to 200°C.

[0086] In order to obtain an appropriate reaction rate, it is preferred to carry out the reaction under heating. From such a viewpoint, the reaction temperature is more preferably 40 to 110°C, and further preferably 40 to 90°C.

[0087] The reaction time is not particularly limited, but is usually about 1 to 60 hours, preferably 1 to 30 hours, and more preferably 1 to 20 hours.

[0088] Generally, epoxy-containing organosilicon compounds have good adhesion to inorganic substrates such as glass and metal. The silane-modified copolymer of the present invention can be suitably used as an adhesion enhancer for organic substrates such as resins and rubbers in addition to inorganic substrates such as glass and metal.

[0089] [3] Composition

[0090] The composition of the present invention contains the above-mentioned silane-modified copolymer. The silane-modified copolymer of the present invention is a compound with a large molecular weight and has a plurality of hydrolyzable silyl groups and epoxy groups in one molecule. Therefore, by adding a predetermined amount to an epoxy resin composition; a polyurethane resin composition; an acrylic resin composition; a polyimide resin composition; an organosilicon composition such as an organosilicon resin composition and a modified organosilicon resin composition, it is expected that the adhesion and tackiness are equal to or higher than those of an existing organosilicon compound containing an epoxy group. Among them, it is preferably added to an organosilicon composition.

[0091] The content of the silane-modified copolymer contained in the composition of the present invention is not particularly limited, but is preferably 0.1 to 20% by mass, more preferably 0.1 to 10% by mass, based on the entire composition.

[0092] When the silane-modified copolymer of the present invention is blended in a silicone composition, a known silicone composition can be used as the silicone composition, for example, a silicone composition containing a linear organopolysiloxane having both molecular chain terminals blocked with hydroxyl groups and a curing catalyst can be used.

[0093] Specific examples of the linear organopolysiloxane having both molecular chain terminals blocked with hydroxyl groups include dimethylpolysiloxane having both molecular chain terminals blocked with hydroxyl groups, methylphenylpolysiloxane having both molecular chain terminals blocked with hydroxyl groups, and methylvinylpolysiloxane having both molecular chain terminals blocked with hydroxyl groups.

[0094] The viscosity of these organopolysiloxanes at 25° C. is preferably 300 to 500,000 mPa·s, more preferably 500 to 100,000 mPa·s, and further preferably 1,000 to 80,000 mPa·s. It should be noted that the above viscosity can be measured using a rotational viscometer. They may be used alone or in combination of two or more having different structures and / or molecular weights.

[0095] As a curing catalyst, an organic metal catalyst is preferably used. As an organic metal catalyst, alkyl tin ester compounds such as dibutyltin diacetate, dibutyltin dilaurate, and dibutyltin dioctoate can be listed; titanates or titanium chelate compounds such as tetraisopropoxytitanium, tetra-n-butoxytitanium, tetra(2-ethylhexyloxy)titanium, dipropoxybis(acetylacetonate)titanium, and isopropoxyoctanediol titanium; zinc naphthenate, zinc stearate, and zinc 2-ethyloctoate; iron 2-ethylhexanoate; cobalt 2-ethylhexanoate, cobalt naphthenate; manganese 2-ethylhexanoate; alkoxyaluminum compounds, aluminum chelate compounds, etc. These can be used alone or in combination of two or more.

[0096] The amount of the curing catalyst to be added is preferably 0.01 to 15 parts by mass, more preferably 0.01 to 5 parts by mass, based on 100 parts by mass of the organopolysiloxane.

[0097] The composition of the present invention may contain, if necessary, hydrolyzable silanes such as methyltris(methylethylketoxime)silane and / or partial hydrolysis condensates thereof, fillers such as silica, silane coupling agents, organopolysiloxanes other than those mentioned above, and the like.

[0098] The composition of the present invention can be prepared by mixing the above-mentioned components according to a conventional method.

[0099] By applying the composition of the present invention to the surface of various substrates and curing them to form a coating layer, a coated substrate can be obtained. In addition, by applying the composition of the present invention to the surface of a substrate, and then stacking other substrates thereon, the composition is cured to form an adhesive layer, thereby obtaining an adhesive laminate.

[0100] The coating method of the composition of the present invention is not particularly limited, and specific examples thereof include known methods such as spray coating, spin coating, dip coating, roll coating, brush coating, bar coating, and flow coating, and any method can be appropriately selected from these methods for use.

[0101] The substrate is not particularly limited, and specific examples thereof include organic resin substrates such as polypropylene resin, poly(ethylene terephthalate), poly(butylene terephthalate) and other polyester resins, polystyrene resin, poly(methyl methacrylate) and other acrylic resins, polyethylene resin, polyamide resins such as nylon, acrylonitrile-butadiene-styrene resin, polyphenylene sulfide resin and the like; rubber substrates such as polyurethane rubber and butadiene rubber; metal substrates; paint-coated surfaces; glass; ceramics; concrete; stone slabs; fabrics; inorganic fillers such as (hollow) silica, titania, zirconia, and alumina; and glass fiber products such as glass cloth, glass tape, glass felt, and glass paper, led by glass fiber. The shape of the substrate is not particularly limited.

[0102] The curing reaction temperature and time can be appropriately changed according to the substrate used. The curing reaction temperature is usually preferably a room temperature around 23°C from the viewpoint of workability. In order to promote the curing reaction, the curing reaction can be heated within a range not exceeding the heat resistance temperature of the substrate used. The curing reaction time is usually about 1 minute to 1 week from the viewpoint of workability.

[0103] Example

[0104] The present invention will be described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples.

[0105] In the following examples, "parts" means parts by mass. The molecular weight is a polystyrene-equivalent number average molecular weight determined by GPC measurement. The viscosity is a value measured at 25°C using a rotational viscometer.

[0106] [1] Production of silane-modified copolymers

[0107] [Example 1-1]

[0108] In a 1 L separable flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, 540 g of Ricon 657 (manufactured by Cray Valley Co., Ltd., number average molecular weight 2200, composed of structural units represented by the following formulae (1), (3), (4) and (5), (1) / [(3)+(4)] / (5)=30 / 20 / 50 (molar ratio)) and a toluene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (1×10 -5mol), 244 g of trimethoxysilane was dripped in at an internal temperature of 75 to 85° C. for 1 hour. Then, it was aged at 80° C. for 3 hours. After the aging, it was concentrated under reduced pressure and filtered to obtain a silane-modified copolymer A of a pale yellow liquid with a viscosity of 300,000 mPa·s and a number average molecular weight of 3,200. The obtained silane-modified copolymer A is composed of structural units represented by the following formulas (1), (2'), (3), (4) and (5), (1) / [(3)+(4)] / (2') / (5)=30 / 20 / 20 / 30 (molar ratio).

[0109] [Chemistry 11]

[0110]

[0111] (In the formula, the asterisk * has the same meaning as above.)

[0112] [Example 1-2]

[0113] In a 1 L separable flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, 540 g of Ricon 657 (manufactured by Cray Valley Co., Ltd., number average molecular weight 2200, composed of structural units represented by the above formulae (1), (3), (4) and (5), (1) / [(3)+(4)] / (5)=30 / 20 / 50 (molar ratio)) and a toluene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (1×10 -5 122 g of trimethoxysilane was added dropwise at an internal temperature of 75 to 85° C. for 1 hour. Then, the mixture was aged at 80° C. for 3 hours. After the aging, the mixture was concentrated under reduced pressure and filtered to obtain a silane-modified copolymer B having a light yellow liquid with a viscosity of 270,000 mPa·s and a number average molecular weight of 2,700. The obtained silane-modified copolymer B is composed of the structural units represented by the above formulas (1), (2′), (3), (4) and (5), and (1) / [(3)+(4)] / (2′) / (5)=30 / 20 / 10 / 40 (molar ratio).

[0114] [Examples 1-3]

[0115] In a 1 L separable flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, 540 g of a partially epoxidized copolymer of Ricon 130 (manufactured by Cray Valley Co., Ltd.) (number average molecular weight 2700, composed of structural units represented by the above formulae (1), (3), (4) and (5), (1) / [(3)+(4)] / (5)=71 / 1 / 28 (molar ratio)) and a toluene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (1×10-5 mol), 244 g of trimethoxysilane was dripped in at an internal temperature of 75 to 85° C. for 1 hour. Then, it was aged at 80° C. for 3 hours. After the aging, it was concentrated under reduced pressure and filtered to obtain a silane-modified copolymer C of a pale yellow liquid with a viscosity of 1800 mPa·s and a number average molecular weight of 3800. The obtained silane-modified copolymer C is composed of the structural units represented by the above formulas (1), (2'), (3), (4) and (5), (1) / [(3)+(4)] / (2') / (5)=71 / 1 / 18 / 10 (molar ratio).

[0116] [Examples 1-4]

[0117] In a 1 L separable flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, 540 g of a partially epoxidized copolymer of Ricon 130 (manufactured by Cray Valley Co., Ltd.) (number average molecular weight 2700, composed of structural units represented by the above formulae (1), (3), (4) and (5), (1) / [(3)+(4)] / (5)=71 / 1 / 28 (molar ratio)) and a toluene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (1×10 -5 122 g of trimethoxysilane was added dropwise at an internal temperature of 75 to 85° C. for 1 hour. Then, the mixture was aged at 80° C. for 3 hours. After the aging, the mixture was concentrated under reduced pressure and filtered to obtain a silane-modified copolymer D of a pale yellow liquid having a viscosity of 1800 mPa·s and a number average molecular weight of 3300. The obtained silane-modified copolymer D is composed of structural units represented by the above formulas (1), (2′), (3), (4) and (5), and (1) / [(3)+(4)] / (2′) / (5)=71 / 1 / 9 / 19 (molar ratio).

[0118] [Examples 1-5]

[0119] In a 1 L separable flask equipped with a stirrer, a reflux condenser, a dropping funnel and a thermometer, 540 g of a partially epoxidized copolymer of Ricon 130 (manufactured by Cray Valley Co., Ltd.) (number average molecular weight 2700, composed of structural units represented by the above formulae (1), (3), (4) and (5), (1) / [(3)+(4)] / (5)=71 / 1 / 28 (molar ratio)) and a toluene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (1×10 -5mol), 61 g of trimethoxysilane was dripped in at an internal temperature of 75 to 85°C for 1 hour. Then, it was aged at 80°C for 3 hours. After the aging, it was concentrated under reduced pressure and filtered to obtain a silane-modified copolymer E with a light yellow liquid having a viscosity of 1700 mPa·s and a number average molecular weight of 3000. The obtained silane-modified copolymer E is composed of the structural units represented by the above formulas (1), (2'), (3), (4) and (5), (1) / [(3)+(4)] / (2') / (5)=71 / 1 / 5 / 23 (molar ratio).

[0120] [2] Evaluation of volatility of silane-modified copolymers

[0121] The volatility of the silane-modified copolymers A to E obtained in Examples 1-1 to 1-5 and the following organosilicon compound F (Comparative Example 1-1) was evaluated.

[0122] Organic silicon compound F: 3-glycidyloxypropyltrimethoxysilane (KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.)

[0123] As an evaluation method, the residual rate of each compound in an aluminum dish dripped with 1 g was left in an open system at 150° C. for 3 hours and evaluated as nonvolatile content. The larger the nonvolatile content, the lower the volatility of the compound. The evaluation results are shown in Table 1.

[0124] [Table 1]

[0125] Compound Non-volatile components (%) Example 1-1 Silane modified copolymer A 99 Example 1-2 Silane modified copolymer B 99 Examples 1-3 Silane modified copolymer C 99 Examples 1-4 Silane modified copolymer D 99 Examples 1-5 Silane modified copolymer E 99 Comparative Example 1-1 Organic Silicon Compound F 0

[0126] As shown in Table 1, it is found that the silane-modified copolymers of the present invention obtained in Examples 1-1 to 1-5 have low volatility.

[0127] Therefore, the silane-modified copolymer of the present invention can suppress volatilization during high-temperature coating, and can exhibit necessary properties with the minimum necessary amount, so it is economical. Furthermore, it can suppress contamination of peripheral equipment and can also be expected to improve productivity.

[0128] [3] Preparation of composition

[0129] [Example 2-1]

[0130] 60 parts of dimethylpolysiloxane with a molecular chain viscosity of 50000 mPa·s and hydroxyl-terminated at both ends, 25 parts of dimethylpolysiloxane with a molecular chain viscosity of 100 mPa·s and trimethylsilyl-terminated at both ends, and 10 parts of surface-treated silica were added, mixed at normal pressure for 30 minutes, and then mixed again at reduced pressure for 15 minutes. 0.5 parts of silane-modified copolymer A and 4 parts of methyltri(methylethylketoxime)silane were added, mixed at atmospheric pressure for 10 minutes, and then mixed at reduced pressure for 30 minutes. After the reduced pressure mixing was completed, 0.1 parts of dioctyltin dilaurate were added, and mixed at reduced pressure for 60 minutes to obtain composition I.

[0131] [Example 2-2]

[0132] Composition II was prepared in the same manner as in Example 2-1 except that 0.5 parts of silane-modified copolymer B was added instead of silane-modified copolymer A.

[0133] [Example 2-3]

[0134] Composition III was prepared in the same manner as in Example 2-1 except that 0.5 parts of silane-modified copolymer C was added instead of silane-modified copolymer A.

[0135] [Examples 2-4]

[0136] Composition IV was prepared in the same manner as in Example 2-1 except that 0.5 parts of silane-modified copolymer D was added instead of silane-modified copolymer A.

[0137] [Example 2-5]

[0138] A composition V was prepared in the same manner as in Example 2-1 except that 0.5 parts of the silane-modified copolymer E was added instead of the silane-modified copolymer A.

[0139] [Comparative Example 2-1]

[0140] Composition VI was prepared in the same manner as in Example 2-1 except that the silane-modified copolymer A was not added.

[0141] [Comparative Example 2-2]

[0142] Composition VI was prepared in the same manner as in Example 2-1 except that 0.5 parts of the organosilicon compound F was added instead of the silane-modified copolymer A.

[0143] [4] Evaluation of the adhesiveness of the composition

[0144] Each composition prepared in Examples 2-1 to 2-5 and Comparative Examples 2-1 and 2-2 was applied to a plate-shaped adherend (material: polyester resin, 6-nylon resin, polyurethane rubber, ABS resin), and after aging at 23° C. and 50% RH for 7 days, the adhesiveness was confirmed.

[0145] The adhesiveness was examined by the cross-cut method (25-liter grid tape peeling test) of JIS K-5600. In this case, the evaluation was performed as follows: ○: adhesion (no peeling), △: partial peeling (peeling area less than 30%), and ×: peeling (peeling area exceeding 30%). The results are shown in Table 2 below.

[0146] [Table 2]

[0147]

[0148] As shown in Table 2, it is found that the silane-modified copolymers of Examples 2-1 to 2-5 can exhibit adhesiveness equal to or higher than that of the conventional epoxy group-containing organosilicon compound (3-glycidyloxypropyltrimethoxysilane) of Comparative Example 2-2.

Claims

1. A silane-modified copolymer comprising structural units represented by the following formulae (1) and (2) and a structural unit containing an epoxy group, [Chemistry 1] In the formula, the asterisk * indicates the bond with the adjacent structural unit. In formula (2), R 1 each independently represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 20 carbon atoms, and R 2 independently represent an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 20 carbon atoms, and m represents an integer of 1 to 3, wherein The order of the structural units is arbitrary.

2. The silane-modified copolymer according to claim 1, wherein The epoxy group-containing structural unit is one or more structural units selected from the group consisting of structural units represented by the following formula (3) and formula (4), [Chemistry 2] In the formula, the asterisk * has the same meaning as above.

3. The method for producing a silane-modified copolymer according to claim 1, comprising the step of: subjecting a copolymer comprising structural units represented by the following formulae (1) and (5) and a structural unit containing an epoxy group to a reaction mixture in the presence of a catalyst containing a platinum compound. The order of each structural unit is arbitrary) is subjected to a hydrosilylation reaction with an organic silicon compound represented by the following formula (6), [Chemistry 3] In the formula, the asterisk * has the same meaning as above. [Chemistry 4] In the formula, R 1 , R 2 and m represent the same meanings as above.

4. The method for producing a silane-modified copolymer according to claim 3, wherein: The epoxy group-containing structural unit is one or more structural units selected from the group consisting of structural units represented by the following formula (3) and formula (4), [Chemistry 5] In the formula, the asterisk * has the same meaning as above.

5. A composition comprising the silane-modified copolymer according to claim 1 or 2. The composition according to claim 5 , comprising an organopolysiloxane.