Ethylene-vinyl alcohol copolymer composition, method for producing ethylene-vinyl alcohol copolymer composition, pellet, multilayer structure, and method for producing multilayer structure

By adding titanium compounds and other metal compounds to the EVOH resin, the thermal deterioration and coloring problems of EVOH resin during melt forming are solved, the long-term operation and appearance quality of the product are improved, and the disadvantages of unsaturated aldehydes are avoided.

CN118946627APending Publication Date: 2024-11-12MITSUBISHI CHEM CORP

Patent Information

Application Number
CN202380030856.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When melt-forming, EVOH resin is prone to color changes due to thermal deterioration, which affects the long-term operation and appearance quality of the product. The prior art uses unsaturated aldehydes to suppress it, but has foul odor and environmental problems.

Method used

A specific trace amount of titanium compound is added to the EVOH resin, and combined with alkaline earth metal compounds, alkali metal compounds, lubricants, antioxidants, etc., the moisture content and component ratio of the composition are controlled to suppress coloring changes during melt forming.

Benefits of technology

It effectively suppresses the coloring changes caused by thermal deterioration of EVOH resin, improves long-term operation and appearance quality, and avoids the foul odor and environmental problems caused by the use of unsaturated aldehydes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005062075840001061
    Figure BDA0005062075840001061
  • Figure BDA0005062075840001091
    Figure BDA0005062075840001091
  • Figure BDA0005062075840001111
    Figure BDA0005062075840001111
Patent Text Reader

Abstract

Provided is an ethylene-vinyl alcohol copolymer composition which is suppressed in color change due to thermal degradation during melt molding. This ethylene-vinyl alcohol copolymer composition contains an ethylene-vinyl alcohol copolymer and a titanium compound, and the content of the titanium compound in terms of metal is 0.001 ppm or more but less than 5 ppm relative to the mass of the ethylene-vinyl alcohol copolymer composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an ethylene-vinyl alcohol copolymer composition, a method for producing the ethylene-vinyl alcohol copolymer composition, a pellet, a multilayer structure, and a method for producing the multilayer structure. Background Art

[0002] Ethylene-vinyl alcohol copolymers (hereinafter sometimes referred to as "EVOH resins") are excellent in transparency, oxygen and other gas barrier properties, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and are formed into films, sheets, bottles, etc. and are widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials.

[0003] However, EVOH resin has a relatively active hydroxyl group in the molecule and tends to be easily degraded by heat, and is prone to coloring during melt molding.

[0004] Regarding the above-mentioned problems, for example, Patent Document 1 discloses that by making EVOH resin contain a specific amount of unsaturated aldehyde, oxidative degradation during melt molding can be suppressed and coloration can be suppressed.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2013 / 146961 Summary of the invention

[0008] In recent years, molding equipment has tended to be more functional, with the diversification of the feed blocks and die shapes of molding equipment, the thinning of multilayer structures in the final products, the increase in the number of layers, and other requirements for higher functionality. However, on the other hand, the productivity of the product tends to decrease due to thermal degradation and coloration of the resin in the molding equipment that has become more complex due to higher functionality.

[0009] In the above-mentioned Patent Document 1, unsaturated aldehydes are used to suppress coloration during melt molding, but such aldehyde compounds can cause bad odor even in a trace amount. In particular, when exposed to high-temperature melt molding, the aldehyde compounds volatilize, which may deteriorate the working environment. Therefore, an EVOH resin composition is sought that suppresses coloration during the melt molding process without using such volatile compounds, that is, has excellent long-run performance.

[0010] An object of the present invention is to provide an EVOH resin composition in which color change due to thermal degradation during melt molding is suppressed.

[0011] However, in view of this situation, the present inventors have found that by adding a specific trace amount of a titanium compound to an EVOH resin, an EVOH resin composition can be obtained in which color change due to thermal degradation during melt molding is suppressed, that is, an EVOH resin composition having excellent long-term operating properties can be obtained.

[0012] The present inventors have found that long-term operating performance is further improved by using at least one selected from an alkaline earth metal compound, an alkali metal compound, a lubricant, and an antioxidant in addition to the titanium compound and / or by reducing the water content of the EVOH resin composition to a specific value or less.

[0013] Furthermore, the present inventors have found that by using at least one selected from a compound having a conjugated polyene structure, a boron compound, and a styrene derivative in addition to the above-mentioned titanium compound, long-term operating performance is excellent and coloring of the EVOH resin composition itself can be suppressed.

[0014] That is, the present invention has the following aspects.

[0015] [1] An EVOH resin composition comprising an EVOH resin and a titanium compound, wherein the EVOH resin has an ethylene structural unit content of 20 to 60 mol %, and the titanium compound has a metal-converted content of 0.001 ppm or more and less than 5 ppm relative to the mass of the EVOH resin composition.

[0016] [2] The EVOH resin composition according to [1], further comprising at least one selected from the group consisting of an alkaline earth metal compound, an alkali metal compound, a lubricant, a compound having a conjugated polyene structure, a boron compound, an antioxidant, and a styrene derivative.

[0017] [3] The EVOH resin composition according to [1], wherein the water content of the EVOH resin composition is 1% by mass or less.

[0018] [4] The EVOH resin composition according to [2], wherein the metal conversion content of the alkaline earth metal compound is 0.1 to 500 ppm based on the mass of the EVOH resin composition.

[0019] [5] The EVOH resin composition according to [2], wherein the metal conversion content of the alkali metal compound is 1 to 1000 ppm based on the mass of the EVOH resin composition.

[0020] [6] The EVOH resin composition according to [2], wherein the content of the lubricant is 500 ppm or less relative to the mass of the EVOH resin composition.

[0021] [7] The EVOH resin composition according to [2], wherein the content of the compound having a conjugated polyene structure is 1 to 1000 ppm based on the mass of the EVOH resin composition.

[0022] [8] The EVOH resin composition according to [2], wherein the boron-equivalent content of the boron compound is 5 to 400 ppm based on the mass of the EVOH resin composition.

[0023] [9] The EVOH resin composition according to [2], wherein the content of the antioxidant is 1 to 30,000 ppm based on the mass of the EVOH resin composition.

[0024]

[10] The EVOH resin composition according to [2], wherein the content of the styrene derivative is 1 to 1000 ppm based on the mass of the EVOH resin composition.

[0025]

[11] A method for producing an EVOH resin composition, which is the method for producing the EVOH resin composition according to any one of [1] to

[10] , comprising the step of melt-mixing raw materials of the EVOH resin composition.

[0026]

[12] A pellet comprising the EVOH resin composition according to any one of [1] to

[10] .

[0027]

[13] A multilayer structure comprising at least one layer comprising the EVOH resin composition according to any one of [1] to

[10] .

[0028]

[14] A method for producing a multilayer structure, which is the method for producing a multilayer structure according to

[13] , comprising the step of melt-molding the layer composed of the EVOH resin composition.

[0029] The EVOH resin composition of the present invention containing a specific amount of a titanium compound can suppress the color change of the EVOH resin during melt molding and has excellent long-term operating properties.

[0030] In addition, the EVOH resin composition of the present invention further contains at least one selected from an alkaline earth metal compound, an alkali metal compound, a lubricant, and an antioxidant in addition to the above-mentioned titanium compound and / or the water content of the EVOH resin composition is below a specific value, and has better long-term operating performance.

[0031] Furthermore, the EVOH resin composition of the present invention further containing at least one selected from a compound having a conjugated polyene structure, a boron compound, and a styrene derivative in addition to the above-mentioned titanium compound has excellent long-term operating performance and can suppress the coloring of the EVOH resin composition itself. DETAILED DESCRIPTION

[0032] Hereinafter, the present invention will be described in more detail based on the embodiments of the present invention, but the present invention is not limited to these embodiments.

[0033] In the present invention, when "X to Y" (X and Y are arbitrary numbers) is expressed, unless otherwise specified, it means "more than X and less than Y", and also includes the meaning of "preferably greater than X" or "preferably less than Y".

[0034] Furthermore, when expressed as "X or more" (X is an arbitrary number) or "Y or less" (Y is an arbitrary number), it also includes the meaning of "preferably greater than X" or "preferably smaller than Y".

[0035] In the present invention, "x and / or y (x and y are arbitrary structures or components)" means only x, only y, or a combination of three types of x and y.

[0036] The EVOH resin composition of the present invention has the following modes: a "first mode" containing an EVOH resin and a specific trace amount of a titanium compound, a "second mode" further containing an alkaline earth metal compound, a "third mode" containing an alkali metal compound, a "fourth mode" containing a lubricant, a "fifth mode" containing a compound having a conjugated polyene structure, a "sixth mode" containing a boron compound, a "seventh mode" containing an antioxidant, an "eighth mode" containing a styrene derivative, and a "ninth mode" in which the water content of the EVOH resin composition is 1% by mass or less. Each mode is described below.

[0037] <<Method 1>>

[0038] <EVOH resin composition>

[0039] The EVOH resin composition according to one embodiment of the present invention (hereinafter referred to as "the present EVOH resin composition") contains EVOH resin as a main component and a specific trace amount of a titanium compound.

[0040] That is, the present invention has the following aspects.

[0041] [1-1] An EVOH resin composition comprising an EVOH resin and a titanium compound, wherein the metal-equivalent content of the titanium compound is 0.001 ppm or more and less than 5 ppm based on the mass of the EVOH resin composition.

[0042] [1-2] A pellet comprising the EVOH resin composition described in [1-1].

[0043] [1-3] A multilayer structure comprising at least one layer comprising the EVOH resin composition according to [1-1].

[0044] [1-4] A method for producing an EVOH resin composition, which is a method for producing the EVOH resin composition described in [1-1].

[0045] The method comprises the step of melt-mixing a composition raw material containing the EVOH resin and the titanium compound.

[0046] [1-5] A method for producing a multilayer structure, which is a method for producing the multilayer structure described in [1-3],

[0047] The process comprises melt-molding the layer composed of the EVOH resin composition.

[0048] The base resin in the present EVOH resin composition is EVOH resin, and the content of EVOH resin in the present EVOH resin composition is usually 70% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 95% by mass or more.

[0049] Hereinafter, each component will be described.

[0050] [EVOH resin]

[0051] The EVOH resin used in the present invention is generally a resin obtained by saponifying a copolymer of ethylene and a vinyl ester monomer, that is, an ethylene-vinyl ester copolymer, and is a water-insoluble thermoplastic resin.

[0052] In view of market availability and good impurity treatment efficiency during production, vinyl acetate is typically used as the vinyl ester monomer. As other vinyl ester monomers other than vinyl acetate, for example, aliphatic vinyl esters such as vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl trimethylacetate, vinyl caprate, vinyl laurate, vinyl stearate, and vinyl versatate, and aromatic vinyl esters such as vinyl benzoate can be mentioned. Usually, aliphatic vinyl esters having 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms are used. These are usually used alone, but multiple types may be used simultaneously as needed.

[0053] The polymerization method for copolymerizing the above-mentioned ethylene and vinyl ester monomers can be carried out by any known polymerization method, such as solution polymerization, suspension polymerization, emulsion polymerization, etc. Generally speaking, solution polymerization using methanol as a solvent is used. In addition, the saponification of the obtained ethylene-vinyl ester copolymer can also be carried out by a known method.

[0054] The EVOH resin produced in this way mainly contains structural units derived from ethylene and vinyl alcohol, and contains a certain amount of vinyl ester structural units which remain without being saponified.

[0055] The content of the ethylene structural unit in the EVOH resin is 20 to 60 mol%, preferably 25 to 50 mol%, and particularly preferably 25 to 35 mol%. The content of the ethylene structural unit can be controlled by the pressure of ethylene when copolymerizing the vinyl ester monomer with ethylene. When the content is too low, the gas barrier properties and melt moldability under high humidity tend to decrease, whereas when it is too high, the gas barrier properties tend to decrease.

[0056] In addition, the content of the ethylene structural unit can be measured based on ISO14663.

[0057] The saponification degree of the EVOH resin is usually 90 to 100 mol%, preferably 95 to 100 mol%, and particularly preferably 99 to 100 mol%. The saponification degree can be controlled by the amount of a saponification catalyst (usually a basic catalyst such as sodium hydroxide is used) when saponifying the ethylene-vinyl ester copolymer, temperature, time, etc. When the saponification degree is too low, the gas barrier properties, thermal stability, moisture resistance, etc. tend to be reduced.

[0058] The saponification degree of the EVOH resin can be measured according to JIS K6726 (wherein the EVOH resin is used in the form of a solution uniformly dissolved in a water / methanol solvent).

[0059] In the above-mentioned EVOH resin, the melt flow rate (MFR) (210°C, load 2160g) is usually 0.5 to 100g / 10min, preferably 1 to 50g / 10min, and particularly preferably 3 to 35g / 10min. If the MFR is too large, the stability during film formation tends to be impaired, and if it is too small, the viscosity becomes too high, and there is a tendency that melt extrusion becomes difficult.

[0060] The MFR is an index of the degree of polymerization of the EVOH resin, and can be adjusted by the amount of the polymerization initiator and the amount of the solvent when ethylene and the vinyl ester monomer are copolymerized.

[0061] The EVOH resin may further contain a structural unit derived from the following comonomer (for example, 10 mol% or less of the EVOH resin) within a range not impairing the effects of the present invention.

[0062] Examples of the comonomer include olefins such as propylene, 1-butene, and isobutylene; hydroxyl-containing α-olefins such as 3-butene-1-ol, 3-butene-1,2-diol, 4-pentene-1-ol, and 5-hexene-1,2-diol; and derivatives thereof such as esters and acylates; hydroxyalkyl vinylides such as 2-methylenepropane-1,3-diol and 3-methylenepentane-1,5-diol; 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2- Hydroxyalkyl vinylene diacetates such as methylenepropane and 1,3-dibutyryloxy-2-methylenepropane; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, phthalic acid (anhydride), maleic acid (anhydride), itaconic acid (anhydride) or their salts or mono- or di-alkyl esters having 1 to 18 carbon atoms in the alkyl group; acrylamide, N-alkyl acrylamide having 1 to 18 carbon atoms in the alkyl group, N,N-dimethylacrylamide, 2-acrylamidopropanesulfonic acid or its salts, acrylamidopropyl dimethylamine or its salts acrylamides such as methacrylamide, N-alkylmethacrylamide with an alkyl group having 1 to 18 carbon atoms, N,N-dimethylmethacrylamide, 2-methacrylamidepropanesulfonic acid or its salt, methacrylamidepropyldimethylamine or its acid salt or its quaternary ammonium salt; N-vinylamides such as N-vinylpyrrolidone, N-vinylformamide, N-vinylacetamide; vinyl cyanides such as acrylonitrile and methacrylonitrile; 18 alkyl vinyl ethers, hydroxyalkyl vinyl ethers, alkoxyalkyl vinyl ethers and other vinyl ethers; halogenated vinyl compounds such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, vinyl bromide, etc.; vinyl silanes such as trimethoxyvinylsilane; halogenated allyl compounds such as allyl acetate and allyl chloride; allyl alcohols such as allyl alcohol and dimethoxyallyl alcohol; comonomers such as trimethyl-(3-acrylamide-3-dimethylpropyl)-ammonium chloride and acrylamide-2-methylpropanesulfonic acid. These can be used alone or in combination of two or more.

[0063] Among them, α-olefins containing hydroxyl groups are preferred, and 3-butene-1,2-diol and 5-hexene-1,2-diol are particularly preferred. When the above α-olefins containing hydroxyl groups are copolymerized, the obtained EVOH resin has a primary hydroxyl group in the side chain. Such EVOH resins having a primary hydroxyl group in the side chain, especially EVOH resins having a 1,2-diol structure in the side chain, are preferred in terms of maintaining gas barrier properties and improving secondary moldability.

[0064] When the EVOH resin has a primary hydroxyl group in the side chain, the content of the structural unit derived from the monomer having the primary hydroxyl group is usually 0.1 to 20 mol %, preferably 0.5 to 15 mol %, particularly preferably 1 to 10 mol % of the EVOH resin.

[0065] In addition, the EVOH resin may be “post-modified” by esterification, urethanization, acetalization, cyanoethylation, oxyalkyleneization or the like.

[0066] When the post-modified EVOH resin is used, the modification rate is usually 10 mol% or less, preferably 4 mol% or less. If the modification rate of the EVOH resin is too high, it is easily thermally degraded, and the long-term operating performance tends to decrease.

[0067] Furthermore, the EVOH resin may be a mixture of EVOH resins having different contents of ethylene structural units, saponification degrees, polymerization degrees, copolymer components, and the like.

[0068] [Titanium compounds]

[0069] Examples of the titanium compound include inorganic titanium compounds and organic titanium compounds. The titanium compound may be used alone or in combination of two or more. Among them, inorganic titanium compounds are preferred.

[0070] Examples of the inorganic titanium compound include titanium oxide, titanium hydroxide, titanium chloride, and inorganic titanium salts.

[0071] Examples of the titanium oxide include titanium (II) oxide, titanium (III) oxide, titanium (IV) oxide, and titanium oxyoxide.

[0072] Examples of the titanium hydroxide include titanium (II) hydroxide and titanium (III) hydroxide.

[0073] Examples of the titanium chloride include titanium (II) chloride and titanium (III) chloride.

[0074] Examples of the inorganic salt of titanium include titanium phosphate and titanium sulfate.

[0075] Among them, titanium oxide is preferred, titanium (IV) oxide is more preferred, and rutile titanium (IV) oxide is particularly preferred.

[0076] Examples of the organic titanium compound include titanium acetate, titanium butyrate, titanium stearate and other titanium carboxylates.

[0077] In addition, the titanium compound may exist in the EVOH resin composition as a titanium compound or in an ionized state or in a complex state interacting with the EVOH resin or other ligands.

[0078] The average particle size of the titanium compound is usually 0.001 to 100 μm, preferably 0.01 to 50 μm, and more preferably 0.015 to 20 μm. When the average particle size of the titanium compound is within the above range, the coloration suppressing effect tends to be excellent.

[0079] The metal conversion content of the titanium compound is greater than 0.001ppm and less than 5ppm relative to the mass of the EVOH resin composition. It is preferably 0.01 to 3ppm, more preferably 0.03 to 1ppm, and particularly preferably 0.05 to 0.5ppm. By making the metal conversion content of the titanium compound within the above range, the color change caused by thermal degradation during melt molding can be suppressed, and long-term operation performance is excellent. In addition, if the metal conversion content of the titanium compound is too small, the effect of suppressing color change is reduced, and if the metal conversion content is too much, thermal decomposition of the EVOH resin becomes easy to occur, and it is easy to color.

[0080] The metal conversion content of the above-mentioned titanium compound can be obtained by weighing the EVOH resin composition into a platinum crucible, ashing it with a burner and an electric furnace in sequence, heating and decomposing the ashed material with nitric acid and hydrofluoric acid, treating it with a mixed acid of dilute nitric acid and dilute hydrofluoric acid and fixing the volume, and quantitatively measuring the titanium in the obtained fixed volume solution by ICP mass spectrometry using an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800).

[0081] Generally speaking, EVOH resin will be colored due to thermal degradation. It is believed that this is because the thermal degradation of EVOH resin generates free radicals, and these free radicals dehydrate the hydroxyl groups of EVOH resin, forming double bonds in the main chain of EVOH resin. This site becomes the starting point of the reaction, further promoting dehydration and forming a conjugated polyene structure in the main chain of EVOH resin.

[0082] On the other hand, the EVOH resin composition contains a specific trace amount of the titanium compound, so that the color change of the EVOH resin due to thermal degradation is suppressed and the long-term operating performance is excellent.

[0083] Generally, when an EVOH resin composition contains a titanium compound, it is believed that the EVOH resin composition is colored due to titanium ions, so it is common knowledge for those skilled in the art to avoid using titanium compounds. However, contrary to such common knowledge, the present invention has found that when a specific trace amount of a titanium compound is used, an EVOH resin composition in which color change due to thermal degradation is suppressed can be obtained.

[0084] That is, it is presumed that the tetravalent ion form of titanium is stable and even a trace amount thereof coordinates to the double bonds of the main chain of the EVOH resin described above to form a chelate complex or the like, thereby stabilizing and suppressing the formation of a polyene structure.

[0085] [Other thermoplastic resins]

[0086] The present EVOH resin composition may contain a thermoplastic resin other than EVOH resin within a range not impairing the effects of the present invention (for example, generally 30% by mass or less, preferably 20% by mass or less, particularly preferably 10% by mass or less of the present EVOH resin composition).

[0087] As other thermoplastic resins, known thermoplastic resins can be used, for example, polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, ionomers, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0088] [Other compounding ingredients]

[0089] In addition, the EVOH resin composition may contain a compounding agent generally added to EVOH resin within a range that does not hinder the effect of the present invention. As the above-mentioned compounding agent, for example, inorganic complex salts (such as hydrotalcite), plasticizers (such as aliphatic polyols such as ethylene glycol, glycerol, hexanediol, etc.), oxygen absorbers [such as inorganic oxygen absorbers such as aluminum powder and potassium sulfite; ascorbic acid, and further its fatty acid esters, metal salts, etc., gallic acid, polyphenols such as hydroxyl-containing phenolic resins, terpene compounds, blends of tertiary hydrogen-containing resins and transition metals (such as a combination of polypropylene and cobalt), blends of carbon-carbon unsaturated bond-containing resins and transition metals] can be added. The invention discloses a kind of photopolymerization agent, which is a kind of polymerized oxygen absorber, and is a kind of photopolymerization agent. The polymerized oxygen absorber is a kind of polymerized oxygen absorber, and is a kind of polymerized oxygen absorber ...

[0090] [Method for producing EVOH resin composition]

[0091] The present EVOH resin composition can be prepared, for example, by mixing the above-mentioned EVOH resin and the titanium compound by a known method, such as a dry blending method, a melt blending method, a solution blending method, an impregnation method, etc. Among these, it is preferably prepared by a process of melt blending the composition raw materials containing the above-mentioned EVOH resin and the titanium compound. In addition, these manufacturing methods can also be arbitrarily combined.

[0092] Examples of the dry blending method include (i) a method of dry blending a pelletized EVOH resin and a titanium compound using a tumbler or the like.

[0093] Examples of the melt mixing method include (ii) a method of melt kneading a dry blend of pelletized EVOH resin and a titanium compound; and (iii) a method of adding a titanium compound to a molten EVOH resin and melt kneading the mixture.

[0094] Examples of the solution mixing method include (iv) a method in which a solution is prepared using a commercially available EVOH resin, a titanium compound is added thereto, the solution is solidified into a shape, and then the solution is separated into solid and liquid by known means and dried; and (v) a method in which, during the manufacturing process of the EVOH resin, a solution of an ethylene-vinyl ester copolymer before saponification or a uniform solution of the EVOH resin (water / alcohol solution, etc.) is added with a titanium compound, the solution is solidified into a shape, and then the solution is separated into solid and liquid by known means and dried.

[0095] Examples of the impregnation method include (vi) a method of bringing pelletized EVOH resin into contact with an aqueous solution containing a titanium compound to impregnate the EVOH resin with the titanium compound and then drying the mixture.

[0096] As the aqueous solution containing a titanium compound, an aqueous solution of a titanium compound or an aqueous solution obtained by immersing a titanium compound in water containing various chemicals to dissolve titanium ions can be used.

[0097] In the above-mentioned impregnation method, the content (metal conversion) of the titanium compound can be controlled by the concentration of the titanium compound in the aqueous solution for impregnating the EVOH resin, the impregnation temperature, the impregnation time, and the like.

[0098] The immersion temperature and immersion time are usually 0.5 to 48 hours, preferably 1 to 36 hours, and the immersion temperature is usually 10 to 40°C, preferably 20 to 35°C.

[0099] The drying method in each of the above-mentioned production methods can adopt various drying methods, and can be any of static drying and fluidized drying. In addition, these methods can also be combined.

[0100] As described above, the above different methods can be combined in the present invention. Among them, considering productivity and the viewpoint of obtaining a resin composition with more significant effects of the present invention, the melt mixing method is preferred, and the method (ii) is particularly preferred. In addition, when using the above other thermoplastic resins and other compounding ingredients, they can be compounded in a conventional manner according to the above manufacturing method.

[0101] The present EVOH resin composition obtained by the above-mentioned respective production methods may be in any shape, but is preferably in the form of pellets.

[0102] The pellets may be spherical, elliptical, cylindrical, cubic, or rectangular, and are usually elliptical or cylindrical. Considering the convenience of using the pellets as molding materials, the pellets are usually 1 to 10 mm in diameter, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm in diameter, and usually 1.5 to 30 mm in diameter, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm in diameter, in the case of elliptical pellets. In the case of cylindrical pellets, the bottom diameter is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm.

[0103] In addition, the shape and size of the pelletized EVOH resin used in each of the above-mentioned production methods are also preferably the same.

[0104] Even when the EVOH resin composition is heated during melt molding, the color change is still suppressed, and the long-term operation is excellent. The ratio of the YI value after heating to the YI value (yellow index) before heating (YI value after heating / YI value before heating) is usually 4.5 or less, preferably 4.2 or less, and particularly preferably 3.9 or less. If the ratio of the YI value after heating to the YI value before heating is within the above range, there is a tendency to further suppress coloring. By the way, if the ratio of the YI value after heating to the YI value before heating exceeds 4.8, it is judged that the coloring caused by thermal degradation is large, which is not preferred. It should be noted that the lower limit of the ratio of the YI value after heating to the YI value before heating is usually 1.

[0105] The YI value before heating is obtained by grinding the EVOH resin composition into 1 to 5 mm square pieces, filling the ground product into a cylinder with an inner diameter of 32 mm and a height of 30 mm, and then scraping off the ground product. In this state, the YI value is measured using a spectrocolorimeter SE6000 (manufactured by Nippon Denshoku Industries Co., Ltd.).

[0106] The YI value after heating is obtained by heating the EVOH resin composition crushed into 1 to 5 mm square pieces in an oven under air atmosphere at 150°C for 5 hours and then measuring the same method.

[0107] The water content of the present EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0108] The water content of the EVOH resin composition is measured and calculated by the following method.

[0109] The mass (W1) of the EVOH resin composition before drying was weighed with an electronic balance, dried in a hot air dryer at 150°C for 5 hours, and the mass (W2) after cooling in the dryer for 30 minutes was weighed and calculated according to the following formula.

[0110] Water content (mass %) = [(W1-W2) / W1] × 100

[0111] When the EVOH resin composition is in the form of pellets, it is preferred to attach a known lubricant to the surface of the pellets from the viewpoint of stabilizing the feedability during melt molding. Examples of the lubricant include higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters of higher fatty acids, etc.), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauramide, myristic acid, palmitic acid, stearic acid, behenic acid, etc.; unsaturated higher fatty acid amides such as oleamide and erucic acid, bis-higher fatty acid amides such as ethylene bisstearamide, ethylene bisoleamide, ethylene biserucic acid, ethylene bislauramide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene having a molecular weight of about 500 to 10,000, or low molecular weight polypropylene, etc., or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluorinated vinyl resins, etc. These compounds can be used alone or in combination with two or more thereof. In addition, the content of the lubricant is usually below 5% by mass of the EVOH resin composition, preferably below 1% by mass. In addition, the lower limit is usually 0% by mass.

[0112] The EVOH resin composition thus obtained can be prepared into various forms such as pellets, powders, and liquids, and provided as molding materials for various molded products. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to obtain the effects of the present invention with better efficiency, which is preferred.

[0113] In addition, the present EVOH resin composition also includes a resin composition obtained by mixing a resin other than the EVOH resin used in the present EVOH resin composition.

[0114] The molded product is, for example, a multilayer structure having a layer composed of the present EVOH resin composition, such as a single-layer film molded from the present EVOH resin composition.

[0115] [Multilayer structure]

[0116] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present EVOH resin composition. The layer composed of the present EVOH resin composition (hereinafter referred to as "the present EVOH resin composition layer") can be further provided with strength, or the present EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating it with other substrates having a thermoplastic resin as a main component other than the present EVOH resin composition (hereinafter, the resin used in the substrate is sometimes referred to as "substrate resin").

[0117] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polybutene, polypentene, (unmodified) polyolefin resins including polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and these polyolefin resins. Modified olefin resins in a broad sense include polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by graft modification with unsaturated carboxylic acid or its ester, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, chlorinated polyethylene, chlorinated polypropylene and other halogenated polyolefins, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.

[0118] Among these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred as hydrophobic resins, and polyethylene resins, polypropylene resins, polycyclic olefin resins, and polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred.

[0119] When the EVOH resin composition layer is a (a1, a2, ...) and the substrate resin layer is b (b1, b2, ...), the layer structure of the multilayer structure can be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the recovered layer including the mixture of the EVOH resin composition and the thermoplastic resin other than the EVOH resin composition obtained by remelting and molding the end parts and defective products generated in the production process of the multilayer structure is taken as R, it can be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is usually 2 to 15 in total, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be inserted between the layers as needed.

[0120] As the above-mentioned adhesive resin, a known adhesive resin can be used, and it can be appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins by addition reaction, grafting reaction, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. They can be used alone or in combination of two or more.

[0121] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present EVOH resin composition layer, it is preferred to use an adhesive resin having excellent hydrophobicity.

[0122] The above-mentioned base resin and adhesive resin may contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating materials, antiblocking agents, waxes, etc., within the range that does not hinder the gist of the present invention (for example, 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These can be used alone or in combination of two or more.

[0123] The lamination of the above-mentioned EVOH resin composition layer and the above-mentioned substrate resin layer (including the case where an adhesive resin layer is inserted) can be carried out according to a known method. For example: a method of melt-extrusion laminating the substrate resin on a film, sheet, etc. of the present EVOH resin composition, a method of melt-extrusion laminating the present EVOH resin composition on a substrate resin layer, a method of co-extruding the present EVOH resin composition and the substrate resin, a method of dry laminating the present EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc., a method of applying a solution of the present EVOH resin composition on the substrate resin and then removing the solvent, etc. Among these, considering the viewpoints of cost and environment, it is preferred to manufacture by a process of melting the present EVOH resin composition layer, and specifically, a co-extrusion method is preferred.

[0124] The present multilayer structure may also be subjected to (heating) stretching treatment as required. The stretching treatment may be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, the stretching may be performed simultaneously or sequentially. In addition, the stretching method may be a method with a higher stretching ratio such as a roller stretching method, a tenter stretching method, a belt stretching method, a stretch blow molding method, and a vacuum pressure molding method. The stretching temperature is a temperature near the melting point of the multilayer structure, and is selected from a range of usually 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is too low, the stretchability is poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0125] In addition, the multilayer structure after the stretching treatment may be heat-fixed in order to impart dimensional stability. Heat-fixing may be performed by known means, for example, the multilayer structure after the stretching treatment is maintained in a tensile state and heat-treated at a temperature of usually 80 to 180° C., preferably 100 to 165° C., for usually 2 to 600 seconds.

[0126] When the stretched multilayer structure is used as a shrink film, in order to impart heat shrinkage, the stretched multilayer structure may be cooled and fixed by blowing cold air instead of the heat setting.

[0127] The thickness of the present multilayer structure (including the stretched multilayer structure), and further the thickness of the present EVOH resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure, depends on the layer constitution, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., and cannot be generalized, but the thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0128] Furthermore, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the substrate resin layer (present EVOH resin composition layer / substrate resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, calculated as the ratio of the thickest layers. In addition, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer (present EVOH resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, calculated as the ratio of the thickest layers.

[0129] In addition, the present multilayer structure can be used to obtain a cup or tray-shaped multilayer container. In this case, a drawing molding method is usually used, and specifically, for example, vacuum molding, pressure molding, vacuum pressure molding, plug-assisted vacuum pressure molding, etc. can be cited. Furthermore, when a tubular or bottle-shaped multilayer container (laminated structure) is obtained from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, for example, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulation type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion cold parison biaxial stretch blow molding, injection cold parison biaxial stretch blow molding, injection molding online biaxial stretch blow molding, etc.), etc. The obtained laminate can be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, deep drawing processing, box processing, tube processing, splitting processing, etc. as needed.

[0130] The single-layer film formed from the present EVOH resin composition, the bags and cups, trays, tubes, bottles and other containers and lids formed from the present multilayer structure are useful as various packaging material containers for general foods, seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oils, beverages, cosmetics, pharmaceuticals, etc.

[0131] <<Method 2>>

[0132] EVOH resin has excellent transparency, oxygen and other gas barrier properties, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and is molded into films, sheets, bottles, etc. and widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials.

[0133] However, EVOH resin has a relatively active hydroxyl group in the molecule and tends to be easily degraded by heat, and is prone to coloring during melt molding.

[0134] Regarding the above-mentioned problems, for example, Patent Document 1 discloses a resin composition characterized in that it contains EVOH resin (A), acetic acid (B), magnesium acetate and / or calcium acetate (C), wherein the content of (B) is 0.05 weight part or less relative to 100 weight parts of (A), and the content of (C) is 0.001 to 0.02 weight part relative to 100 weight parts of (A) in terms of metal conversion. It is also disclosed that by using the resin composition, long-term operation performance during melt molding is excellent, and a molded product with less fish eyes, streaks, and coloring and excellent appearance can be obtained, and when the molded product is made into a laminate, the odor is reduced, and the interlayer adhesion of the laminate is still excellent after secondary processing such as stretching and deep drawing.

[0135] [Patent Document 1] Japanese Patent Application Laid-Open No. 11-106592

[0136] The technology disclosed in the above-mentioned patent document 1 has excellent long-term operation performance during melt molding, and can obtain molded products with less fish eyes, streaks, and coloring, and excellent appearance. However, in recent years, with the diversification of the feed block and die head shapes of molding devices, the thin filmization of multilayer structures in the final products, the increase in the number of layers, and other requirements for high functionality, the molding devices tend to be highly functional. Therefore, there is a tendency for the resin to undergo thermal degradation and coloring in the molding devices that have become complicated due to high functionality, which reduces the productivity (long-term operation performance) of the product, and further improvement is sought.

[0137] The present invention provides an EVOH resin composition in which the color change of the EVOH resin during heating such as melt molding is suppressed.

[0138] [Methods to solve the problem]

[0139] However, the present inventors have found that, in view of the above circumstances, an EVOH resin composition can be obtained in which the color change of the EVOH resin during heating such as melt molding is suppressed by adding an alkaline earth metal compound and a specific trace amount of a titanium compound to the EVOH resin.

[0140] That is, the present invention has the following aspects.

[0141] [2-1] An EVOH resin composition comprising an EVOH resin, an alkaline earth metal compound and a titanium compound, wherein the metal-converted content of the titanium compound is 0.001 ppm or more and less than 5 ppm based on the mass of the EVOH resin composition.

[0142] [2-2] The EVOH resin composition according to [2-1], wherein the metal-equivalent content of the alkaline earth metal compound is 0.1 to 500 ppm relative to the mass of the EVOH resin composition.

[0143] [2-3] The EVOH resin composition according to [2-1] or [2-2], wherein the mass ratio of the metal-converted content of the alkaline earth metal compound to the metal-converted content of the titanium compound is 0.02 to 500,000.

[0144] [2-4] A pellet comprising the EVOH resin composition according to any one of [2-1] to [2-3].

[0145] [2-5] A multilayer structure comprising at least one layer comprising the EVOH resin composition according to any one of [2-1] to [2-3].

[0146] [2-6] A method for producing an EVOH resin composition, the method being a method for producing the EVOH resin composition described in any one of [2-1] to [2-3],

[0147] The method comprises the step of melt-mixing a composition raw material containing the EVOH resin and the titanium compound.

[0148] [2-7] A method for producing a multilayer structure, which is a method for producing the multilayer structure described in [2-5],

[0149] The process comprises melt-molding the layer composed of the EVOH resin composition.

[0150] [Effects of the Invention]

[0151] The EVOH resin composition of the present invention can suppress the color change of the EVOH resin during melt molding and has excellent long-term operating properties. [Specific implementation method]

[0153] Hereinafter, the present invention will be described in more detail based on the embodiments of the present invention, but the present invention is not limited to these embodiments.

[0154] <EVOH resin composition>

[0155] The EVOH resin composition according to one embodiment of the present invention (hereinafter referred to as "the present EVOH resin composition") contains EVOH resin as a main component and an alkaline earth metal compound and a specific trace amount of a titanium compound.

[0156] That is, the base resin in the present EVOH resin composition is EVOH resin, and the content of EVOH resin in the present EVOH resin composition is usually 70 mass % or more, preferably 80 mass % or more, more preferably 90 mass % or more, particularly preferably 95 mass % or more.

[0157] Hereinafter, each component will be described.

[0158] [EVOH resin]

[0159] The EVOH resin used in the present invention is generally a resin obtained by saponifying an ethylene-vinyl ester copolymer which is a copolymer of ethylene and a vinyl ester monomer, and the same EVOH resin as described in the first embodiment can be used.

[0160] [Alkaline earth metal compounds]

[0161] As the above-mentioned alkaline earth metal compound, for example, salts, oxides, hydroxides, etc. of alkaline earth metals can be cited. They can be used alone or in combination of two or more. Among them, considering the viewpoints of economy and dispersibility, alkaline earth metal salts and alkaline earth metal oxides are preferred, and alkaline earth metal oxides are particularly preferred.

[0162] Examples of the alkaline earth metal salt include inorganic salts of alkaline earth metals and carboxylates of alkaline earth metals.

[0163] Examples of the inorganic salt of the alkaline earth metal include carbonates, hydrogen carbonates, phosphates, borates, sulfates, chlorides and the like of the alkaline earth metal.

[0164] Examples of the alkaline earth metal carboxylates include saturated or unsaturated carboxylates having 2 to 25 carbon atoms, preferably 2 to 22 carbon atoms, and particularly preferably 6 to 20 carbon atoms. Specifically, examples include monovalent carboxylates such as acetate, butyrate, propionate, heptanoate, caprate, laurate, palmitate, stearate, 12-hydroxystearate, behenic acid, and montanate, and divalent carboxylates such as oxalate, malonate, succinate, adipate, suberate, and sebacate. Among these, linear saturated carboxylates are preferred, and monovalent carboxylates are more preferred from the viewpoint of market availability.

[0165] Examples of the alkaline earth metal species of the alkaline earth metal compound include beryllium, magnesium, calcium, strontium, barium, and radium. Among them, magnesium and calcium are preferred, and magnesium is particularly preferred, from the viewpoint of market availability and economic efficiency.

[0166] Among them, magnesium oxide is preferred as the alkaline earth metal compound. In addition, the alkaline earth metal compound preferably excludes layered inorganic compounds such as montmorillonite and complex salts such as hydrotalcite from the viewpoints of economy and dispersibility.

[0167] The alkaline earth metal compound may be in any form, such as solid (powder, fine powder, flake, etc.), semisolid, liquid, paste, solution, emulsion (aqueous dispersion), etc. Among them, powder is preferred.

[0168] The content of the alkaline earth metal compound is usually 0.1 to 1000 ppm, preferably 1 to 800 ppm, more preferably 5 to 500 ppm, and particularly preferably 10 to 200 ppm, based on the mass of the EVOH resin composition.

[0169] When the content of the alkaline earth metal compound is too large, the thermal stability tends to decrease, and when it is too small, the moldability of the EVOH resin composition tends to decrease.

[0170] The metal conversion content of the alkaline earth metal compound is preferably 0.1 to 500 ppm, more preferably 0.5 to 300 ppm, further preferably 1 to 200 ppm, particularly preferably 2 to 150 ppm, even more preferably 3 to 80 ppm, and most preferably 5 to 40 ppm, relative to the mass of the EVOH resin composition.

[0171] When the metal conversion content of the alkaline earth metal compound is too large, the thermal stability tends to decrease, and when it is too small, the moldability of the EVOH resin composition tends to decrease.

[0172] The metal conversion content of the alkaline earth metal compound can be measured by, for example, heating the EVOH resin composition to ashing and then treating it with an acid such as hydrochloric acid to obtain a solution, adding pure water to the obtained solution to make it constant to volume and using it as a detection solution with an atomic absorption spectrophotometer.

[0173] [Titanium compounds]

[0174] Examples of the titanium compound include inorganic titanium compounds and organic titanium compounds. As the titanium compound, the same titanium compound as that described in the first embodiment can be used.

[0175] The metal conversion content of the titanium compound is greater than 0.001ppm and less than 5ppm relative to the mass of the EVOH resin composition. It is preferably 0.01 to 3ppm, more preferably 0.03 to 1ppm, and particularly preferably 0.05 to 0.5ppm. By making the metal conversion content of the titanium compound within the above range, the color change caused by thermal degradation during melt molding can be suppressed, and long-term operation performance is excellent. In addition, if the metal conversion content of the titanium compound is too small, the effect of suppressing color change is reduced, and if the metal conversion content is too much, thermal decomposition of the EVOH resin becomes easy to occur, and it is easy to color.

[0176] The metal conversion content of the above-mentioned titanium compound can be obtained by weighing the EVOH resin composition into a platinum crucible, ashing it with a burner and an electric furnace in sequence, heating and decomposing the ashed material with nitric acid and hydrofluoric acid, treating it with a mixed acid of dilute nitric acid and dilute hydrofluoric acid and fixing the volume, and quantitatively measuring the titanium in the obtained fixed volume solution by ICP mass spectrometry using an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800).

[0177] The mass ratio of the alkaline earth metal compound content to the metal equivalent content of the titanium compound is usually 0.06 to 180,000, preferably 2 to 36,000, particularly preferably 7 to 15,000, more particularly preferably 15 to 1,500, and most preferably 100 to 800.

[0178] When the mass ratio is within the above range, there is a tendency for coloration changes due to thermal degradation to be further suppressed.

[0179] The mass ratio of the metal conversion content of the alkaline earth metal compound to the metal conversion content of the titanium compound is preferably 0.02 to 500,000, more preferably 0.03 to 50,000, more preferably 0.5 to 10,000, particularly preferably 2 to 4,000, even more preferably 9 to 1,000, and most preferably 50 to 500.

[0180] If the mass ratio is within the above range, there is a tendency to further suppress the color change due to thermal degradation. In addition, when the mass ratio is too large, the thermal stability tends to decrease, and when it is too small, the molded product tends to be colored.

[0181] Generally speaking, it is known that when EVOH resin is added with alkaline earth metal compounds, the viscosity tends to decrease over time when heated. The mechanism is not clear, but it is speculated that the EVOH resin composition becomes alkaline by adding alkaline earth metal compounds, and some anions become nucleophiles, taking away hydrogen bonded to the main chain carbon of the EVOH resin, etc., and causing the main chain decomposition reaction to cut the main chain of the EVOH resin. It is speculated that the color change of EVOH resin after heating is due to the formation of a double bond structure in the main chain of the EVOH resin during the above reaction, and this structure becomes the starting point of the reaction again, causing a dehydration reaction, etc., and forming a polyene structure in the main chain of the EVOH resin.

[0182] On the other hand, the present EVOH resin composition contains an alkaline earth metal compound and a specific trace amount of a titanium compound, thereby suppressing the color change of the EVOH resin due to thermal degradation.

[0183] Generally, when an EVOH resin composition contains a titanium compound, it is believed that the EVOH resin composition is colored due to titanium ions, so it is common knowledge for those skilled in the art to avoid using titanium compounds. However, contrary to such common knowledge, the present invention has found that when a specific trace amount of a titanium compound is used, an EVOH resin composition in which color change due to thermal degradation is suppressed can be obtained.

[0184] That is, it is presumed that the tetravalent ion form of titanium is stable and even a trace amount thereof coordinates to the double bonds of the main chain of the EVOH resin described above to form a chelate complex or the like, thereby stabilizing and suppressing the formation of a polyene structure.

[0185] On the other hand, if the amount of the titanium compound is too large, it is considered that the EVOH resin may be thermally decomposed by titanium and thus be colored.

[0186] [Other thermoplastic resins]

[0187] The present EVOH resin composition may contain a thermoplastic resin other than EVOH resin within a range not impairing the effects of the present invention (for example, generally 30% by mass or less, preferably 20% by mass or less, particularly preferably 10% by mass or less of the present EVOH resin composition).

[0188] As other thermoplastic resins, known thermoplastic resins can be used, for example, polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, ionomers, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0189] [Other compounding ingredients]

[0190] The EVOH resin composition may contain a compounding agent generally compounded in EVOH resin within a range not hindering the effects of the present invention. As the compounding agent, the same compounding agent as described in the first embodiment can be used.

[0191] [Method for producing EVOH resin composition]

[0192] The EVOH resin composition can be prepared by mixing the above-mentioned EVOH resin, alkaline earth metal compound and titanium compound by a known method, such as dry mixing, melt mixing, solution mixing, impregnation, etc. Among these, it is preferably prepared by a process of melt mixing the composition raw materials containing the above-mentioned EVOH resin and titanium compound. In addition, these production methods can also be arbitrarily combined.

[0193] Examples of the dry blending method include (i) a method of dry blending a pelletized EVOH resin and an alkaline earth metal compound and / or a titanium compound using a tumbler or the like.

[0194] Examples of the melt mixing method include (ii) a method of melt-kneading a dry blend of EVOH resin in pellet form and an alkaline earth metal compound and / or a titanium compound; and (iii) a method of adding an alkaline earth metal compound and / or a titanium compound to a molten EVOH resin and melt-kneading the mixture.

[0195] Examples of the solution mixing method include (iv) a method in which a solution is prepared using a commercially available EVOH resin, an alkaline earth metal compound and / or a titanium compound is added thereto, the solution is solidified into a shape, and then the solution is separated into solid and liquid by known means and dried; (v) in the manufacturing process of the EVOH resin, an ethylene-vinyl ester copolymer solution before saponification and a uniform solution of the EVOH resin (water / alcohol solution, etc.) are made to contain an alkaline earth metal compound and / or a titanium compound, and then the solution is solidified into a shape, and then the solution is separated into solid and liquid by known means and dried.

[0196] Examples of the impregnation method include (vi) a method of bringing pelletized EVOH resin into contact with an aqueous solution containing an alkaline earth metal compound and / or a titanium compound to allow the EVOH resin to contain the alkaline earth metal compound and / or the titanium compound, followed by drying.

[0197] As the aqueous solution containing a titanium compound, an aqueous solution of a titanium compound or an aqueous solution obtained by immersing a titanium compound in water containing various chemicals to dissolve titanium ions can be used.

[0198] In the above impregnation method, the content (metal conversion) of the alkaline earth metal compound and the titanium compound can be controlled by the concentration of the alkaline earth metal compound and the titanium compound in the aqueous solution for impregnating the EVOH resin, the impregnation temperature, the impregnation time, etc.

[0199] The immersion temperature and immersion time are usually 0.5 to 48 hours, preferably 1 to 36 hours, and the immersion temperature is usually 10 to 40°C, preferably 20 to 35°C.

[0200] The drying method in each of the above-mentioned production methods can adopt various drying methods, and can be any of static drying and fluidized drying. In addition, these methods can also be combined.

[0201] As described above, the above different methods can be combined in the present invention. Among them, considering productivity and the viewpoint of obtaining a resin composition with more significant effects of the present invention, the melt mixing method is preferred, and the method (ii) is particularly preferred. In addition, when using the above other thermoplastic resins and other compounding ingredients, they can be compounded in a conventional manner according to the above manufacturing method.

[0202] The present EVOH resin composition obtained by the above-mentioned respective production methods may be in any shape, but is preferably in the form of pellets.

[0203] The pellets may be spherical, elliptical, cylindrical, cubic, or rectangular, and are usually elliptical or cylindrical. Considering the convenience of using the pellets as molding materials, the pellets are usually 1 to 10 mm in diameter, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm in diameter, and usually 1.5 to 30 mm in diameter, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm in diameter, in the case of elliptical pellets. In the case of cylindrical pellets, the bottom diameter is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm.

[0204] In addition, the shape and size of the pelletized EVOH resin used in each of the above-mentioned production methods are also preferably the same.

[0205] Even when the EVOH resin composition is heated during melt molding, the color change is still suppressed, and the long-term operation is excellent. The ratio of the YI value after heating to the YI value (yellow index) before heating (YI value after heating / YI value before heating) is usually less than 3.2, preferably below 3.1, and particularly preferably below 2.7. If the ratio of the YI value after heating to the YI value before heating is within the above range, there is a tendency to further suppress the color change. In addition, the lower limit of the ratio of the YI value after the above heating to the YI value before heating is usually 1.

[0206] In addition, even a difference of 0.1 in the ratio of the above-mentioned YI values ​​will show a significant difference in yield in actual production, and therefore the difference is very large.

[0207] The YI value before heating is obtained by grinding the EVOH resin composition into 1 to 5 mm square pieces, filling the ground product into a cylinder with an inner diameter of 32 mm and a height of 30 mm, and then scraping off the ground product. In this state, the YI value is measured using a spectrocolorimeter SE6000 (manufactured by Nippon Denshoku Industries Co., Ltd.).

[0208] The YI value after heating is obtained by heating the EVOH resin composition crushed into 1 to 5 mm square pieces in an oven under air atmosphere at 150°C for 5 hours and then measuring the same method.

[0209] The water content of the present EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0210] The water content of the EVOH resin composition is measured and calculated by the following method.

[0211] The mass (W1) of the EVOH resin composition before drying was weighed with an electronic balance, dried in a hot air dryer at 150°C for 5 hours, and the mass (W2) after cooling in the dryer for 30 minutes was weighed and calculated according to the following formula.

[0212] Water content (mass %) = [(W1-W2) / W1] × 100

[0213] When the EVOH resin composition is in the form of pellets, it is preferred to attach a known lubricant to the surface of the pellets from the viewpoint of stabilizing the feedability during melt molding. Examples of the lubricant include higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters of higher fatty acids, etc.), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauramide, myristic acid, palmitic acid, stearic acid, behenic acid, etc.; unsaturated higher fatty acid amides such as oleamide and erucic acid, bis-higher fatty acid amides such as ethylene bisstearamide, ethylene bisoleamide, ethylene biserucic acid, ethylene bislauramide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene having a molecular weight of about 500 to 10,000, or low molecular weight polypropylene, etc., or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluorinated vinyl resins, etc. These compounds can be used alone or in combination with two or more thereof. In addition, the content of the lubricant is usually below 5% by mass of the EVOH resin composition, preferably below 1% by mass. In addition, the lower limit is usually 0% by mass.

[0214] The EVOH resin composition thus obtained can be prepared into various forms such as pellets, powders, and liquids, and provided as molding materials for various molded products. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to obtain the effects of the present invention with better efficiency, which is preferred.

[0215] In addition, the present EVOH resin composition also includes a resin composition obtained by mixing a resin other than the EVOH resin used in the present EVOH resin composition.

[0216] The molded product is, for example, a multilayer structure having a layer composed of the present EVOH resin composition, such as a single-layer film molded from the present EVOH resin composition.

[0217] [Multilayer structure]

[0218] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present EVOH resin composition. The layer composed of the present EVOH resin composition (hereinafter referred to as "the present EVOH resin composition layer") can be further provided with strength, or the present EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating it with other substrates having a thermoplastic resin as a main component other than the present EVOH resin composition (hereinafter, the resin used in the substrate is sometimes referred to as "substrate resin").

[0219] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polybutene, polypentene, (unmodified) polyolefin resins including polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and these polyolefin resins. Modified olefin resins in a broad sense include polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by graft modification with unsaturated carboxylic acid or its ester, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, chlorinated polyethylene, chlorinated polypropylene and other halogenated polyolefins, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.

[0220] Among these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred as hydrophobic resins, and polyethylene resins, polypropylene resins, polycyclic olefin resins, and polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred.

[0221] When the EVOH resin composition layer is a (a1, a2, ...) and the substrate resin layer is b (b1, b2, ...), the layer structure of the multilayer structure can be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the recovered layer including the mixture of the EVOH resin composition and the thermoplastic resin other than the EVOH resin composition obtained by remelting and molding the end parts and defective products generated in the production process of the multilayer structure is taken as R, it can be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is usually 2 to 15 in total, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be inserted between the layers as needed.

[0222] As the above-mentioned adhesive resin, a known adhesive resin can be used, and it can be appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins by addition reaction, grafting reaction, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. They can be used alone or in combination of two or more.

[0223] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present EVOH resin composition layer, it is preferred to use an adhesive resin having excellent hydrophobicity.

[0224] The above-mentioned base resin and adhesive resin may contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating materials, antiblocking agents, waxes, etc., within the range that does not hinder the gist of the present invention (for example, 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These can be used alone or in combination of two or more.

[0225] The lamination of the above-mentioned EVOH resin composition layer and the above-mentioned substrate resin layer (including the case where an adhesive resin layer is inserted) can be carried out according to a known method. For example: a method of melt-extrusion laminating the substrate resin on a film, sheet, etc. of the present EVOH resin composition, a method of melt-extrusion laminating the present EVOH resin composition on a substrate resin layer, a method of co-extruding the present EVOH resin composition and the substrate resin, a method of dry laminating the present EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc., a method of applying a solution of the present EVOH resin composition on the substrate resin and then removing the solvent, etc. Among these, considering the viewpoints of cost and environment, it is preferred to manufacture by a process of melting the present EVOH resin composition layer, and specifically, a co-extrusion method is preferred.

[0226] The present multilayer structure may also be subjected to (heating) stretching treatment as required. The stretching treatment may be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, the stretching may be performed simultaneously or sequentially. In addition, the stretching method may be a method with a higher stretching ratio such as a roller stretching method, a tenter stretching method, a belt stretching method, a stretch blow molding method, and a vacuum pressure molding method. The stretching temperature is a temperature near the melting point of the multilayer structure, and is selected from a range of usually 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is too low, the stretchability is poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0227] In addition, the multilayer structure after the stretching treatment may be heat-fixed in order to impart dimensional stability. Heat-fixing may be performed by known means, for example, the multilayer structure after the stretching treatment is maintained in a tensile state and heat-treated at a temperature of usually 80 to 180° C., preferably 100 to 165° C., for usually 2 to 600 seconds.

[0228] When the stretched multilayer structure is used as a shrink film, in order to impart heat shrinkage, the stretched multilayer structure may be cooled and fixed by blowing cold air instead of the heat setting.

[0229] The thickness of the present multilayer structure (including the stretched multilayer structure), and further the thickness of the present EVOH resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure, depends on the layer constitution, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., and cannot be generalized, but the thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0230] Furthermore, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the substrate resin layer (present EVOH resin composition layer / substrate resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, calculated as the ratio of the thickest layers. In addition, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer (present EVOH resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, calculated as the ratio of the thickest layers.

[0231] In addition, the present multilayer structure can be used to obtain a cup or tray-shaped multilayer container. In this case, a pull molding method is usually used, and specifically, for example, vacuum molding, pressure molding, vacuum pressure molding, plug-assisted vacuum pressure molding, etc. can be cited. Furthermore, when a tubular or bottle-shaped multilayer container (laminated structure) is obtained from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, for example, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulation type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion type cold parison biaxial stretch blow molding, injection type cold parison biaxial stretch blow molding, injection molding online biaxial stretch blow molding, etc.), etc. The obtained laminate can be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, deep drawing processing, box processing, tube processing, splitting processing, etc. as needed.

[0232] The single-layer film formed from the present EVOH resin composition, the bags and cups, trays, tubes, bottles and other containers and lids formed from the present multilayer structure are useful as various packaging material containers for general foods, seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oils, beverages, cosmetics, pharmaceuticals, etc.

[0233] <<Method 3>>

[0234] EVOH resin has excellent transparency, oxygen and other gas barrier properties, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and is molded into films, sheets, bottles, etc. and widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials.

[0235] However, EVOH resin has a relatively active hydroxyl group in the molecule and tends to be easily degraded by heat, and is prone to coloring during melt molding.

[0236] Regarding the above-mentioned problems, for example, Patent Document 1 discloses a resin composition characterized in that it contains EVOH resin (A), acetic acid (B), magnesium acetate and / or calcium acetate (C), wherein the content of (B) is 0.05 weight part or less relative to 100 weight parts of (A), and the content of (C) is 0.001 to 0.02 weight part relative to 100 weight parts of (A) in terms of metal conversion. It is also disclosed that by using the resin composition, long-term operation performance during melt molding is excellent, and a molded product with less fish eyes, streaks, and coloring and excellent appearance can be obtained, and when the molded product is made into a laminate, the odor is reduced, and the interlayer adhesion of the laminate is still excellent after secondary processing such as stretching and deep drawing.

[0237] [Patent Document 1] Japanese Patent Application Laid-Open No. 11-106592

[0238] The technology disclosed in the above-mentioned patent document 1 has excellent long-term operation performance during melt molding, and can obtain molded products with less fish eyes, streaks, and coloring, and excellent appearance. However, in recent years, with the diversification of the feed block and die head shapes of molding devices, the thin filmization of multilayer structures in the final products, the increase in the number of layers, and other requirements for high functionality, the molding devices tend to be highly functional. Therefore, there is a tendency for the resin to undergo thermal degradation and coloring in the molding devices that have become complicated due to high functionality, which reduces the productivity (long-term operation performance) of the product, and further improvement is sought.

[0239] The present invention provides an EVOH resin composition in which the color change of the EVOH resin during heating such as melt molding is suppressed.

[0240] [Methods to solve the problem]

[0241] However, the present inventors have found that, in view of the above circumstances, an EVOH resin composition can be obtained in which the color change of the EVOH resin during heating such as melt molding is suppressed by adding an alkali metal compound and a specific trace amount of a titanium compound to the EVOH resin.

[0242] That is, the present invention has the following aspects.

[0243] [3-1] An EVOH resin composition comprising an EVOH resin, an alkali metal compound and a titanium compound, wherein the metal-equivalent content of the titanium compound is 0.001 ppm or more and less than 5 ppm based on the mass of the EVOH resin composition.

[0244] [3-2] The EVOH resin composition according to [3-1], wherein the metal-equivalent content of the alkali metal compound is 1 to 1000 ppm based on the mass of the EVOH resin composition.

[0245] [3-3] The EVOH resin composition according to [3-1] or [3-2], wherein the mass ratio of the metal content of the alkali metal compound to the metal-equivalent content of the titanium compound is 0.2 to 1,000,000.

[0246] [3-4] The EVOH resin composition according to any one of [3-1] to [3-3], wherein the alkali metal compound is a carboxylate of an alkali metal.

[0247] [3-5] A pellet comprising the EVOH resin composition according to any one of [3-1] to [3-4].

[0248] [3-6] A multilayer structure comprising at least one layer comprising the EVOH resin composition according to any one of [3-1] to [3-4].

[0249] [3-7] A method for producing an EVOH resin composition, the method comprising producing the EVOH resin composition described in any one of [3-1] to [3-4].

[0250] The method comprises the step of melt-mixing a composition raw material containing the EVOH resin and the titanium compound.

[0251] [3-8] A method for producing a multilayer structure, which is a method for producing the multilayer structure described in [3-6],

[0252] The process comprises melt-molding the layer composed of the EVOH resin composition.

[0253] [Effects of the Invention]

[0254] The EVOH resin composition of the present invention can suppress the color change of the EVOH resin during melt molding and has excellent long-term operating properties. [Specific implementation method]

[0256] Hereinafter, the present invention will be described in more detail based on the embodiments of the present invention, but the present invention is not limited to these embodiments.

[0257] <EVOH resin composition>

[0258] The EVOH resin composition according to one embodiment of the present invention (hereinafter referred to as "the present EVOH resin composition") contains EVOH resin as a main component and an alkali metal compound and a specific trace amount of a titanium compound.

[0259] That is, the base resin in the present EVOH resin composition is EVOH resin, and the content of EVOH resin in the present EVOH resin composition is usually 70 mass % or more, preferably 80 mass % or more, more preferably 90 mass % or more, particularly preferably 95 mass % or more.

[0260] Hereinafter, each component will be described.

[0261] [EVOH resin]

[0262] The EVOH resin used in the present invention is generally a resin obtained by saponifying an ethylene-vinyl ester copolymer which is a copolymer of ethylene and a vinyl ester monomer, and the same EVOH resin as described in the first embodiment can be used.

[0263] [Alkali metal compounds]

[0264] As the above-mentioned alkali metal compound, for example, salts and hydroxides of alkali metals can be mentioned. They can be used alone or in combination of two or more. Among them, as the alkali metal compound, it is preferably water-soluble, and considering the viewpoint of dispersibility, it is preferably an alkali metal salt.

[0265] Examples of the alkali metal salt include inorganic salts of alkali metals and carboxylates of alkali metals. Among them, carboxylates of alkali metals are preferred.

[0266] Examples of the inorganic salt of an alkali metal include carbonates, hydrogen carbonates, phosphates, borates, sulfates, and chloride salts of an alkali metal.

[0267] Examples of the alkali metal carboxylates include monocarboxylates having 2 to 11 carbon atoms such as acetates, butyrates, propionates, heptanoates and decanoates, dicarboxylates having 2 to 11 carbon atoms such as oxalates, malonates, succinates, adipates, suberates and sebacates, monocarboxylates having 12 or more carbon atoms such as laurates, palmitates, stearates, 12-hydroxystearates, behenic acid and montanates, and carboxylates with the terminal carboxyl group of the polymerization terminal of the EVOH resin.

[0268] Among them, monocarboxylates having 2 to 11 carbon atoms are preferred, and acetates are particularly preferred.

[0269] Examples of the alkali metal species of the alkali metal compound include lithium, sodium, potassium, rubidium, and cesium. Among them, sodium and potassium are preferred, and sodium is particularly preferred.

[0270] The molecular weight of the alkali metal compound is usually 20 to 10,000, preferably 20 to 1,000, and particularly preferably 20 to 500.

[0271] Among them, sodium acetate is preferred as the alkali metal compound. In view of economic efficiency and dispersibility, inorganic layered compounds and complex salts are preferably excluded from the alkali metal compound.

[0272] The metal conversion content of the alkali metal compound is preferably 1 to 1000 ppm, more preferably 5 to 800 ppm, further preferably 10 to 700 ppm, particularly preferably 100 to 600 ppm, and even more preferably 150 to 400 ppm, based on the mass of the EVOH resin composition.

[0273] When the content of the alkali metal compound is too large, the thermal stability tends to decrease, and when it is too small, the moldability of the EVOH resin composition tends to decrease.

[0274] The metal conversion content of the alkali metal compound can be measured by, for example, heating the EVOH resin composition to ashing and then treating it with an acid such as hydrochloric acid to obtain a solution, adding pure water to the obtained solution to make it constant to volume, and using the solution as a detection solution for measurement using an atomic absorption spectrophotometer.

[0275] [Titanium compounds]

[0276] Examples of the titanium compound include inorganic titanium compounds and organic titanium compounds. As the titanium compound, the same titanium compound as that described in the first embodiment can be used.

[0277] The metal conversion content of the titanium compound is greater than 0.001ppm and less than 5ppm relative to the mass of the EVOH resin composition. It is preferably 0.01 to 3ppm, more preferably 0.03 to 1ppm, and particularly preferably 0.05 to 0.5ppm. By making the metal conversion content of the titanium compound within the above range, the color change caused by thermal degradation during melt molding can be suppressed, and long-term operation performance is excellent. In addition, if the metal conversion content of the titanium compound is too small, the effect of suppressing color change is reduced, and if the metal conversion content is too much, thermal decomposition of the EVOH resin becomes easy to occur, and it is easy to color.

[0278] The metal conversion content of the above-mentioned titanium compound can be obtained by weighing the EVOH resin composition into a platinum crucible, ashing it with a burner and an electric furnace in sequence, heating and decomposing the ashed material with nitric acid and hydrofluoric acid, treating it with a mixed acid of dilute nitric acid and dilute hydrofluoric acid and fixing the volume, and quantitatively measuring the titanium in the obtained fixed volume solution by ICP mass spectrometry using an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800).

[0279] The mass ratio of the content of the alkali metal compound to the metal-equivalent content of the titanium compound is usually 1 to 360,000, preferably 18 to 100,000, and particularly preferably 100 to 50,000.

[0280] When the mass ratio is within the above range, there is a tendency for coloration changes due to thermal degradation to be further suppressed.

[0281] The mass ratio of the metal conversion content of the alkali metal compound to the metal conversion content of the titanium compound is preferably 0.2 to 1,000,000, more preferably 0.3 to 100,000, more preferably 5 to 27,000, particularly preferably 20 to 14,000, even more preferably 100 to 7,000, and most preferably 300 to 4,000.

[0282] If the mass ratio is within the above range, there is a tendency to further suppress the color change due to thermal degradation. In addition, when the mass ratio is too large, the thermal stability tends to decrease, and when it is too small, the molded product tends to be colored.

[0283] Generally, it is known that when EVOH resin is added with an alkali metal compound, the viscosity tends to decrease over time when heated. The mechanism is not clear, but it is speculated that the EVOH resin composition becomes alkaline by adding an alkali metal compound, and some anions become nucleophiles, which take away hydrogen bonded to the main chain carbon of the EVOH resin, etc., and cause the main chain decomposition reaction to cut the main chain of the EVOH resin. It is speculated that the color change of EVOH resin after heating is due to the formation of a double bond structure in the main chain of the EVOH resin during the above reaction, and this structure becomes the starting point of the reaction again, causing a dehydration reaction, etc., and forming a polyene structure in the main chain of the EVOH resin.

[0284] On the other hand, the present EVOH resin composition contains an alkali metal compound and a specific trace amount of a titanium compound, thereby suppressing the color change of the EVOH resin due to thermal degradation.

[0285] Generally, when an EVOH resin composition contains a titanium compound, it is believed that the EVOH resin composition is colored due to titanium ions, so it is common knowledge for those skilled in the art to avoid using titanium compounds. However, contrary to such common knowledge, the present invention has found that when a specific trace amount of a titanium compound is used, an EVOH resin composition in which color change due to thermal degradation is suppressed can be obtained.

[0286] That is, it is presumed that the tetravalent ion form of titanium is stable and even a trace amount thereof coordinates to the double bonds of the main chain of the EVOH resin described above to form a chelate complex or the like, thereby stabilizing and suppressing the formation of a polyene structure.

[0287] On the other hand, if the amount of the titanium compound is too large, it is considered that the EVOH resin may be thermally decomposed by titanium and thus be colored.

[0288] [Other thermoplastic resins]

[0289] The present EVOH resin composition may contain a thermoplastic resin other than EVOH resin within a range not impairing the effects of the present invention (for example, generally 30% by mass or less, preferably 20% by mass or less, particularly preferably 10% by mass or less of the present EVOH resin composition).

[0290] As other thermoplastic resins, known thermoplastic resins can be used, for example, polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, ionomers, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0291] [Other compounding ingredients]

[0292] The EVOH resin composition may contain a compounding agent generally compounded in EVOH resin within a range not hindering the effects of the present invention. As the compounding agent, the same compounding agent as described in the first embodiment can be used.

[0293] [Method for producing EVOH resin composition]

[0294] The present EVOH resin composition can be prepared, for example, by mixing the above-mentioned EVOH resin, alkali metal compound and titanium compound by a known method, such as dry blending, melt blending, solution blending, impregnation, etc. Among these, it is preferably prepared by a process of melt blending the composition raw materials containing the above-mentioned EVOH resin and titanium compound. In addition, these production methods can also be arbitrarily combined.

[0295] Examples of the dry blending method include (i) a method of dry blending a pelletized EVOH resin with an alkali metal compound and / or a titanium compound using a tumbler or the like.

[0296] Examples of the melt mixing method include (ii) a method of melt kneading a dry blend of pelletized EVOH resin and an alkali metal compound and / or a titanium compound; and (iii) a method of adding an alkali metal compound and / or a titanium compound to a molten EVOH resin and melt kneading the dry blend.

[0297] Examples of the solution mixing method include (iv) a method in which a solution is prepared using a commercially available EVOH resin, an alkali metal compound and / or a titanium compound is added thereto, the solution is solidified into a shape, and then the solution is separated into a solid and a liquid and dried by known means; (v) a method in which, during the manufacture of the EVOH resin, an ethylene-vinyl ester copolymer solution before saponification or a uniform solution of the EVOH resin (water / alcohol solution, etc.) is made to contain an alkali metal compound and / or a titanium compound, the solution is solidified into a shape, and then the solution is separated into a solid and a liquid and dried by known means.

[0298] Examples of the impregnation method include (vi) a method of bringing pelletized EVOH resin into contact with an aqueous solution containing an alkali metal compound and / or a titanium compound to allow the EVOH resin to contain the alkali metal compound and / or the titanium compound, followed by drying.

[0299] As the aqueous solution containing a titanium compound, an aqueous solution of a titanium compound or an aqueous solution obtained by immersing a titanium compound in water containing various chemicals to dissolve titanium ions can be used.

[0300] In the above impregnation method, the content (metal conversion) of the alkali metal compound and the titanium compound can be controlled by the concentration of the alkali metal compound and the titanium compound in the aqueous solution for impregnating the EVOH resin, the impregnation temperature, the impregnation time, etc.

[0301] The immersion temperature and immersion time are usually 0.5 to 48 hours, preferably 1 to 36 hours, and the immersion temperature is usually 10 to 40°C, preferably 20 to 35°C.

[0302] The drying method in each of the above-mentioned production methods can adopt various drying methods, and can be any of static drying and fluidized drying. In addition, these methods can also be combined.

[0303] As described above, the above different methods can be combined in the present invention. Among them, considering productivity and the viewpoint of obtaining a resin composition with more significant effects of the present invention, the melt mixing method is preferred, and the method (ii) is particularly preferred. In addition, when using the above other thermoplastic resins and other compounding ingredients, they can be compounded in a conventional manner according to the above manufacturing method.

[0304] The present EVOH resin composition obtained by the above-mentioned respective production methods may be in any shape, but is preferably in the form of pellets.

[0305] The pellets may be spherical, elliptical, cylindrical, cubic, or rectangular, and are usually elliptical or cylindrical. Considering the convenience of using the pellets as molding materials, the pellets are usually 1 to 10 mm in diameter, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm in diameter, and usually 1.5 to 30 mm in diameter, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm in diameter, in the case of elliptical pellets. In the case of cylindrical pellets, the bottom diameter is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm.

[0306] In addition, the shape and size of the pelletized EVOH resin used in each of the above-mentioned production methods are also preferably the same.

[0307] Even when this EVOH resin composition is heated during melt molding, the coloration change can still be suppressed, and the long-term operation is excellent. The ratio of the YI value after heating to the YI value (yellow index) before heating (YI value after heating / YI value before heating) is usually below 3.9, preferably below 3.7, and more preferably below 3.2. If the ratio of the YI value after heating to the YI value before heating is the above range, there is a tendency to further suppress the coloration change. In addition, the lower limit of the ratio of the YI value after the above-mentioned heating to the YI value before heating is usually 1.

[0308] In addition, even a difference of 0.1 in the ratio of the above-mentioned YI values ​​will show a significant difference in yield in actual production, and therefore the difference is very large.

[0309] The YI value before heating is obtained by grinding the EVOH resin composition into 1 to 5 mm square pieces, filling the ground product into a cylinder with an inner diameter of 32 mm and a height of 30 mm, and then scraping off the ground product. In this state, the YI value is measured using a spectrocolorimeter SE6000 (manufactured by Nippon Denshoku Industries Co., Ltd.).

[0310] The YI value after heating is obtained by heating the EVOH resin composition crushed into 1 to 5 mm square pieces in an oven under air atmosphere at 150°C for 5 hours and then measuring the same method.

[0311] The water content of the present EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0312] The water content of the EVOH resin composition is measured and calculated by the following method.

[0313] The mass (W1) of the EVOH resin composition before drying was weighed with an electronic balance, dried in a hot air dryer at 150°C for 5 hours, and the mass (W2) after cooling in the dryer for 30 minutes was weighed and calculated according to the following formula.

[0314] Water content (mass %) = [(W1-W2) / W1] × 100

[0315] In addition, when the EVOH resin composition is in the form of pellets, it is preferred to attach a known lubricant to the surface of the pellets from the viewpoint of stabilizing the feeding property during melt molding. Examples of lubricants include: higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters, etc. of higher fatty acids), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauramide, myristic acid, palmitic acid, stearic acid, behenic acid, etc.; unsaturated higher fatty acid amides such as oleamide and erucic acid, bis-higher fatty acid amides such as ethylene bisstearamide, ethylene bisoleamide, ethylene biserucic acid, ethylene bislauramide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene having a molecular weight of about 500 to 10,000, or low molecular weight polypropylene, etc., or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluorinated vinyl resins, etc. These compounds may be used alone or in combination of two or more. The content of the lubricant is usually 5% by mass or less, preferably 1% by mass or less, of the EVOH resin composition, and the lower limit is usually 0% by mass.

[0316] The EVOH resin composition thus obtained can be prepared into various forms such as pellets, powders, and liquids, and provided as molding materials for various molded products. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to obtain the effects of the present invention with better efficiency, which is preferred.

[0317] In addition, the present EVOH resin composition also includes a resin composition obtained by mixing a resin other than the EVOH resin used in the present EVOH resin composition.

[0318] The molded product is, for example, a multilayer structure having a layer composed of the present EVOH resin composition, such as a single-layer film molded from the present EVOH resin composition.

[0319] [Multilayer structure]

[0320] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present EVOH resin composition. The layer composed of the present EVOH resin composition (hereinafter referred to as "the present EVOH resin composition layer") can be further provided with strength, or the present EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating it with other substrates having a thermoplastic resin as a main component other than the present EVOH resin composition (hereinafter, the resin used in the substrate is sometimes referred to as "substrate resin").

[0321] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polybutene, polypentene, (unmodified) polyolefin resins including polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and these polyolefin resins. Modified olefin resins in a broad sense include polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by graft modification with unsaturated carboxylic acid or its ester, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, chlorinated polyethylene, chlorinated polypropylene and other halogenated polyolefins, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.

[0322] Among these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred as hydrophobic resins, and polyethylene resins, polypropylene resins, polycyclic olefin resins, and polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred.

[0323] When the EVOH resin composition layer is a (a1, a2, ...) and the substrate resin layer is b (b1, b2, ...), the layer structure of the multilayer structure can be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the recovered layer including the mixture of the EVOH resin composition and the thermoplastic resin other than the EVOH resin composition obtained by remelting and molding the end parts and defective products generated in the production process of the multilayer structure is taken as R, it can be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is usually 2 to 15 in total, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be inserted between the layers as needed.

[0324] As the above-mentioned adhesive resin, a known adhesive resin can be used, and it can be appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins by addition reaction, grafting reaction, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. They can be used alone or in combination of two or more.

[0325] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present EVOH resin composition layer, it is preferred to use an adhesive resin having excellent hydrophobicity.

[0326] The above-mentioned base resin and adhesive resin may contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating materials, antiblocking agents, waxes, etc., within the range that does not hinder the gist of the present invention (for example, 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These can be used alone or in combination of two or more.

[0327] The lamination of the above-mentioned EVOH resin composition layer and the above-mentioned substrate resin layer (including the case where an adhesive resin layer is inserted) can be carried out according to a known method. For example: a method of melt-extrusion laminating the substrate resin on a film, sheet, etc. of the present EVOH resin composition, a method of melt-extrusion laminating the present EVOH resin composition on a substrate resin layer, a method of co-extruding the present EVOH resin composition and the substrate resin, a method of dry laminating the present EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc., a method of applying a solution of the present EVOH resin composition on the substrate resin and then removing the solvent, etc. Among these, considering the viewpoints of cost and environment, it is preferred to manufacture by a process of melting the present EVOH resin composition layer, and specifically, a co-extrusion method is preferred.

[0328] The present multilayer structure may also be subjected to (heating) stretching treatment as required. The stretching treatment may be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, the stretching may be performed simultaneously or sequentially. In addition, the stretching method may be a method with a higher stretching ratio such as a roller stretching method, a tenter stretching method, a belt stretching method, a stretch blow molding method, and a vacuum pressure molding method. The stretching temperature is a temperature near the melting point of the multilayer structure, and is selected from a range of usually 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is too low, the stretchability is poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0329] In addition, the multilayer structure after the stretching treatment may be heat-fixed in order to impart dimensional stability. Heat-fixing may be performed by known means, for example, the multilayer structure after the stretching treatment is maintained in a tensile state and heat-treated at a temperature of usually 80 to 180° C., preferably 100 to 165° C., for usually 2 to 600 seconds.

[0330] When the stretched multilayer structure is used as a shrink film, in order to impart heat shrinkage, the stretched multilayer structure may be cooled and fixed by blowing cold air instead of the heat setting.

[0331] The thickness of the present multilayer structure (including the stretched multilayer structure), and further the thickness of the present EVOH resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure, depends on the layer constitution, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., and cannot be generalized, but the thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0332] Furthermore, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the substrate resin layer (present EVOH resin composition layer / substrate resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, calculated as the ratio of the thickest layers. In addition, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer (present EVOH resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, calculated as the ratio of the thickest layers.

[0333] In addition, the present multilayer structure can be used to obtain a cup or tray-shaped multilayer container. In this case, a pull molding method is usually used, and specifically, for example, vacuum molding, pressure molding, vacuum pressure molding, plug-assisted vacuum pressure molding, etc. can be cited. Furthermore, when a tubular or bottle-shaped multilayer container (laminated structure) is obtained from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, for example, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulation type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion type cold parison biaxial stretch blow molding, injection type cold parison biaxial stretch blow molding, injection molding online biaxial stretch blow molding, etc.), etc. The obtained laminate can be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, deep drawing processing, box processing, tube processing, splitting processing, etc. as needed.

[0334] The single-layer film formed from the present EVOH resin composition, the bags and cups, trays, tubes, bottles and other containers and lids formed from the present multilayer structure are useful as various packaging material containers for general foods, seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oils, beverages, cosmetics, pharmaceuticals, etc.

[0335] <<Method 4>>

[0336] EVOH resin has excellent transparency, oxygen and other gas barrier properties, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and is molded into films, sheets, bottles, etc. and widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials.

[0337] However, EVOH resin has a relatively active hydroxyl group in the molecule and tends to be easily degraded by heat, and is prone to coloring during melt molding.

[0338] Regarding the above-mentioned problems, for example, Patent Document 1 discloses that by making EVOH resin contain a specific amount of unsaturated aldehyde, oxidative degradation during melt molding can be suppressed and coloration can be suppressed.

[0339] [Patent Document 1] International Publication No. 2013 / 146961

[0340] In recent years, molding equipment has tended to be more functional, with the diversification of the feed blocks and die shapes of molding equipment, the thinning of multilayer structures in the final products, the increase in the number of layers, and other requirements for higher functionality. However, on the other hand, the productivity of the product tends to decrease due to thermal degradation and coloration of the resin in the molding equipment that has become more complex due to higher functionality.

[0341] In the above-mentioned Patent Document 1, unsaturated aldehydes are used to suppress coloration during melt molding, but such aldehyde compounds can cause bad odor even in a trace amount. In particular, when exposed to high-temperature melt molding, the aldehyde compounds volatilize, which may deteriorate the working environment. Therefore, an EVOH resin composition is sought that suppresses coloration during the melt molding process without using such volatile compounds, that is, has excellent long-run performance.

[0342] The present invention provides an EVOH resin composition in which color change due to thermal degradation during melt molding is suppressed.

[0343] [Methods to solve the problem]

[0344] However, in view of the above circumstances, the present inventors have found that an EVOH resin composition in which color change due to thermal degradation during melt molding is suppressed can be obtained by adding a lubricant and a specific trace amount of a titanium compound to an EVOH resin.

[0345] That is, the present invention has the following aspects.

[0346] [4-1] An EVOH resin composition comprising an EVOH resin, a lubricant, and a titanium compound, wherein the metal-equivalent content of the titanium compound is 0.001 ppm or more and less than 5 ppm based on the mass of the EVOH resin composition.

[0347] [4-2] The EVOH resin composition according to [4-1], wherein the content of the lubricant is 500 ppm or less relative to the mass of the EVOH resin composition.

[0348] [4-3] The EVOH resin composition according to [4-1] or [4-2], wherein the mass ratio of the content of the lubricant to the metal-equivalent content of the titanium compound is 0.2 to 500,000.

[0349] [4-4] A pellet comprising the EVOH resin composition according to any one of [4-1] to [4-3].

[0350] [4-5] A multilayer structure comprising at least one layer comprising the ethylene-vinyl alcohol copolymer composition according to any one of [4-1] to [4-3].

[0351] [4-6] A method for producing an EVOH resin composition, the method comprising producing the EVOH resin composition described in any one of [4-1] to [4-3].

[0352] The method comprises the step of melt-mixing a composition raw material containing an EVOH resin and a titanium compound.

[0353] [4-7] A method for producing a multilayer structure, which is a method for producing the multilayer structure described in [4-5],

[0354] The process comprises melt-molding the layer composed of the EVOH resin composition.

[0355] [Effects of the Invention]

[0356] The EVOH resin composition of the present invention can suppress the color change of the EVOH resin during melt molding and has excellent long-term operating properties. [Specific implementation method]

[0358] Hereinafter, the present invention will be described in more detail based on the embodiments of the present invention, but the present invention is not limited to these embodiments.

[0359] <EVOH resin composition>

[0360] The EVOH resin composition according to one embodiment of the present invention (hereinafter referred to as "the present EVOH resin composition") contains EVOH resin as a main component and contains a lubricant and a specific trace amount of a titanium compound.

[0361] That is, the base resin in the present EVOH resin composition is EVOH resin, and the content of EVOH resin in the present EVOH resin composition is usually 70 mass % or more, preferably 80 mass % or more, more preferably 90 mass % or more, particularly preferably 95 mass % or more.

[0362] Hereinafter, each component will be described.

[0363] [EVOH resin]

[0364] The EVOH resin used in the present invention is generally a resin obtained by saponifying an ethylene-vinyl ester copolymer which is a copolymer of ethylene and a vinyl ester monomer, and the same EVOH resin as described in the first embodiment can be used.

[0365] [Lubricant]

[0366] Examples of the lubricant include higher fatty acids having 12 to 25 carbon atoms, preferably 13 to 23 carbon atoms, and more preferably 15 to 20 carbon atoms.

[0367] Examples of the higher fatty acids include higher fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, and oleic acid; metal salts of these higher fatty acids such as aluminum salts, calcium salts, zinc salts, magnesium salts, and barium salts; esters of these higher fatty acids such as methyl esters, isopropyl esters, butyl esters, and octyl esters; saturated higher fatty acid amides such as stearamide and behenamide; unsaturated higher fatty acid amides such as oleamide and erucamide; and amides of higher fatty acids such as bis-higher fatty acid amides such as ethylene bisstearamide, ethylene bisoleamide, ethylene biserucamide, and ethylene bislauramide.

[0368] Examples of lubricants other than the higher fatty acids include low molecular weight polyethylene and low molecular weight polypropylene having a molecular weight of about 500 to 10,000, low molecular weight polyolefins such as acid-modified products thereof, higher alcohols, ester oligomers, and fluorinated vinyl resins.

[0369] These lubricants may be used alone or in combination of two or more.

[0370] In addition, from the viewpoint of extrusion stability and market availability, the valence of the higher fatty acids is usually 1 to 5, preferably 1 to 3, and particularly preferably 1 to 2. The valence refers to the number of structures derived from higher fatty acids in one molecule of the compound used in the lubricant. For example, when bis-stearamide is used as a lubricant, there are two structures derived from higher fatty acid molecules with 18 carbon atoms in one molecule, so it is an amide of a higher fatty acid with 18 carbon atoms, and the valence of the higher fatty acid is 2.

[0371] Among the above lubricants, higher fatty acids, metal salts of higher fatty acids, esters of higher fatty acids, and amides of higher fatty acids are preferred, and metal salts of higher fatty acids and amides of higher fatty acids are particularly preferred. From the viewpoint of extrusion stability, amides of higher fatty acids are more preferred, and ethylene bisstearamide is particularly preferred.

[0372] As the form of the lubricant, any form such as solid (powder, fine powder, flake, etc.), semi-solid, liquid, paste, solution, emulsion (aqueous dispersion) can be used. Among them, powder is preferred. The particle size of the powder lubricant is usually 0.1 to 100 μm, preferably 1 to 75 μm, and particularly preferably 5 to 50 μm.

[0373] The content of the lubricant is preferably 500 ppm or less, more preferably 300 ppm or less, and particularly preferably 200 ppm or less relative to the mass of the EVOH resin composition. If the content of the lubricant exceeds the above value, the thermal stability tends to decrease. It should be noted that the lower limit of the content of the lubricant is usually 1 ppm, preferably 10 ppm, and particularly preferably 50 ppm. When the lubricant is too little, the moldability of the EVOH resin composition tends to decrease.

[0374] The content of the lubricant can be measured, for example, by the following method.

[0375] When the lubricant adheres to the surface of the EVOH resin, the amount of lubricant added can be regarded as the content.

[0376] In addition, when the EVOH resin composition contains a lubricant, if the lubricant is, for example, a higher fatty amide, the lubricant content in the EVOH resin composition can be determined by measuring the total nitrogen content in the EVOH resin composition using a micro total nitrogen analyzer and converting it into the lubricant content.

[0377] [Titanium compounds]

[0378] Examples of the titanium compound include inorganic titanium compounds and organic titanium compounds. As the titanium compound, the same titanium compound as that described in the first embodiment can be used.

[0379] The metal conversion content of the titanium compound is greater than 0.001ppm and less than 5ppm relative to the mass of the EVOH resin composition. It is preferably 0.01 to 3ppm, more preferably 0.03 to 1ppm, and particularly preferably 0.05 to 0.5ppm. By making the metal conversion content of the titanium compound within the above range, the color change caused by thermal degradation during melt molding can be suppressed, and long-term operation performance is excellent. In addition, if the metal conversion content of the titanium compound is too small, the effect of suppressing color change is reduced, and if the metal conversion content is too much, thermal decomposition of the EVOH resin becomes easy to occur, and it is easy to color.

[0380] The metal conversion content of the above-mentioned titanium compound can be obtained by weighing the EVOH resin composition into a platinum crucible, ashing it with a burner and an electric furnace in sequence, heating and decomposing the ashed material with nitric acid and hydrofluoric acid, treating it with a mixed acid of dilute nitric acid and dilute hydrofluoric acid and fixing the volume, and quantitatively measuring the titanium in the obtained fixed volume solution by ICP mass spectrometry using an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800).

[0381] The mass ratio of the lubricant content to the metal-converted content of the titanium compound [lubricant content / metal-converted content of the titanium compound] is usually 0.2 to 500,000, preferably 0.3 to 50,000, more preferably 10 to 10,000, particularly preferably 100 to 4,000, and even more preferably 900 to 3,000. If this value is too large, thermal stability tends to be impaired, and if it is too small, the molded product tends to be colored.

[0382] Generally speaking, EVOH resin will be colored due to thermal degradation. It is believed that this is because the thermal degradation of EVOH resin generates free radicals, and these free radicals dehydrate the hydroxyl groups of EVOH resin, forming double bonds in the main chain of EVOH resin. This site becomes the starting point of the reaction, further promoting dehydration and forming a conjugated polyene structure in the main chain of EVOH resin.

[0383] On the other hand, the EVOH resin composition contains a specific trace amount of the titanium compound, so that the color change of the EVOH resin due to thermal degradation is suppressed and the long-term operating performance is excellent.

[0384] Generally, when an EVOH resin composition contains a titanium compound, it is believed that the EVOH resin composition is colored due to titanium ions, so it is common knowledge for those skilled in the art to avoid using titanium compounds. However, contrary to such common knowledge, the present invention has found that when a specific trace amount of a titanium compound is used, an EVOH resin composition in which color change due to thermal degradation is suppressed can be obtained.

[0385] That is, it is presumed that the tetravalent ion form of titanium is stable and even a trace amount thereof coordinates to the double bonds of the main chain of the EVOH resin described above to form a chelate complex or the like, thereby stabilizing and suppressing the formation of a polyene structure.

[0386] [Other thermoplastic resins]

[0387] The present EVOH resin composition may contain a thermoplastic resin other than EVOH resin within a range not impairing the effects of the present invention (for example, generally 30% by mass or less, preferably 20% by mass or less, particularly preferably 10% by mass or less of the present EVOH resin composition).

[0388] As other thermoplastic resins, known thermoplastic resins can be used, for example, polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, ionomers, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0389] [Other compounding ingredients]

[0390] The EVOH resin composition may contain a compounding agent generally compounded in EVOH resin within a range not hindering the effects of the present invention. As the compounding agent, the same compounding agent as described in the first embodiment can be used.

[0391] [Method for producing EVOH resin composition]

[0392] The present EVOH resin composition can be prepared, for example, by mixing the above-mentioned EVOH resin and the titanium compound by a known method, such as a dry blending method, a melt blending method, a solution blending method, an impregnation method, etc. Among these, it is preferably prepared by a process of melt blending the composition raw materials containing the above-mentioned EVOH resin and the titanium compound. In addition, these manufacturing methods can also be arbitrarily combined.

[0393] Examples of the dry blending method include (i) a method of dry blending a pelletized EVOH resin with a lubricant and / or a titanium compound using a tumbler or the like.

[0394] Examples of the melt mixing method include (ii) a method of melt kneading a dry blend of EVOH resin in pellet form with a lubricant and / or a titanium compound; and (iii) a method of adding a lubricant and / or a titanium compound to molten EVOH resin and melt kneading the mixture.

[0395] Examples of the solution mixing method include (iv) a method in which a solution is prepared using a commercially available EVOH resin, a lubricant and / or a titanium compound is added thereto, the solution is solidified into a shape, and then the solution is separated into solid and liquid by known means and dried; (v) in the manufacturing process of the EVOH resin, a lubricant and / or a titanium compound is added to an ethylene-vinyl ester copolymer solution before saponification or a uniform solution of the EVOH resin (water / alcohol solution, etc.), and then the solution is solidified into a shape, and then the solution is separated into solid and liquid by known means and dried.

[0396] Examples of the impregnation method include (vi) a method of bringing pelletized EVOH resin into contact with an aqueous solution containing a lubricant and / or a titanium compound to allow the EVOH resin to contain the lubricant and / or the titanium compound, followed by drying.

[0397] As the aqueous solution containing a titanium compound, an aqueous solution of a lubricant and / or a titanium compound, or an aqueous solution obtained by immersing a lubricant and / or a titanium compound in water containing various chemicals to dissolve titanium ions can be used.

[0398] In the above-mentioned impregnation method, the content (metal conversion) of the titanium compound can be controlled by the concentration of the titanium compound in the aqueous solution for impregnating the EVOH resin, the impregnation temperature, the impregnation time, and the like.

[0399] The immersion temperature and immersion time are usually 0.5 to 48 hours, preferably 1 to 36 hours, and the immersion temperature is usually 10 to 40°C, preferably 20 to 35°C.

[0400] The drying method in each of the above-mentioned production methods can adopt various drying methods, and can be any of static drying and fluidized drying. In addition, these methods can also be combined.

[0401] As described above, the above different methods can be combined in the present invention. Among them, considering productivity and the viewpoint of obtaining a resin composition with more significant effects of the present invention, the melt mixing method is preferred, and the method (ii) is particularly preferred. In addition, when using the above other thermoplastic resins and other compounding ingredients, they can be compounded in a conventional manner according to the above manufacturing method.

[0402] The present EVOH resin composition obtained by the above-mentioned respective production methods may be in any shape, but is preferably in the form of pellets.

[0403] The pellets may be spherical, elliptical, cylindrical, cubic, or rectangular, and are usually elliptical or cylindrical. Considering the convenience of using the pellets as molding materials, the pellets are usually 1 to 10 mm in diameter, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm in diameter, and usually 1.5 to 30 mm in diameter, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm in diameter, in the case of elliptical pellets. In the case of cylindrical pellets, the bottom diameter is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm.

[0404] In addition, the shape and size of the pelletized EVOH resin used in each of the above-mentioned production methods are also preferably the same.

[0405] Even when the EVOH resin composition is heated during melt molding, the color change is still suppressed, and the long-term operation is excellent. The ratio of the YI value after heating to the YI value (yellow index) before heating (YI value after heating / YI value before heating) is usually 3.9 or less, preferably 3.6 or less, and more preferably 3.0 or less. If the ratio of the YI value after heating to the YI value before heating is within the above range, there is a tendency to further suppress the color change. It should be noted that the lower limit of the ratio of the YI value after heating to the YI value before heating is usually 1.

[0406] The YI value before heating is obtained by grinding the EVOH resin composition into 1 to 5 mm square pieces, filling the ground product into a cylinder with an inner diameter of 32 mm and a height of 30 mm, and then scraping off the ground product. In this state, the YI value is measured using a spectrocolorimeter SE6000 (manufactured by Nippon Denshoku Industries Co., Ltd.).

[0407] The YI value after heating is obtained by heating the EVOH resin composition crushed into 1 to 5 mm square pieces in an oven under air atmosphere at 150°C for 5 hours and then measuring the same method.

[0408] The water content of the present EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0409] The water content of the EVOH resin composition is measured and calculated by the following method.

[0410] The mass (W1) of the EVOH resin composition before drying was weighed with an electronic balance, dried in a hot air dryer at 150°C for 5 hours, and the mass (W2) after cooling in the dryer for 30 minutes was weighed and calculated according to the following formula.

[0411] Water content (mass %) = [(W1-W2) / W1] × 100

[0412] The EVOH resin composition thus obtained can be prepared into various forms such as pellets, powders, and liquids, and provided as molding materials for various molded products. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to obtain the effects of the present invention with better efficiency, which is preferred.

[0413] In addition, the present EVOH resin composition also includes a resin composition obtained by mixing a resin other than the EVOH resin used in the present EVOH resin composition.

[0414] The molded product is, for example, a multilayer structure having a layer composed of the present EVOH resin composition, such as a single-layer film molded from the present EVOH resin composition.

[0415] [Multilayer structure]

[0416] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present EVOH resin composition. The layer composed of the present EVOH resin composition (hereinafter referred to as "the present EVOH resin composition layer") can be further provided with strength, or the present EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating it with other substrates having a thermoplastic resin as a main component other than the present EVOH resin composition (hereinafter, the resin used in the substrate is sometimes referred to as "substrate resin").

[0417] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polybutene, polypentene, (unmodified) polyolefin resins including polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and these polyolefin resins. Modified olefin resins in a broad sense include polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by graft modification with unsaturated carboxylic acid or its ester, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, chlorinated polyethylene, chlorinated polypropylene and other halogenated polyolefins, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.

[0418] Among these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred as hydrophobic resins, and polyethylene resins, polypropylene resins, polycyclic olefin resins, and polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred.

[0419] When the EVOH resin composition layer is a (a1, a2, ...) and the substrate resin layer is b (b1, b2, ...), the layer structure of the multilayer structure can be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the recovered layer including the mixture of the EVOH resin composition and the thermoplastic resin other than the EVOH resin composition obtained by remelting and molding the end parts and defective products generated in the production process of the multilayer structure is taken as R, it can be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is usually 2 to 15 in total, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be inserted between the layers as needed.

[0420] As the above-mentioned adhesive resin, a known adhesive resin can be used, and it can be appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins by addition reaction, grafting reaction, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. They can be used alone or in combination of two or more.

[0421] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present EVOH resin composition layer, it is preferred to use an adhesive resin having excellent hydrophobicity.

[0422] The above-mentioned base resin and adhesive resin may contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating materials, antiblocking agents, waxes, etc., within the range that does not hinder the gist of the present invention (for example, 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These can be used alone or in combination of two or more.

[0423] The lamination of the above-mentioned EVOH resin composition layer and the above-mentioned substrate resin layer (including the case where an adhesive resin layer is inserted) can be carried out according to a known method. For example: a method of melt-extrusion laminating the substrate resin on a film, sheet, etc. of the present EVOH resin composition, a method of melt-extrusion laminating the present EVOH resin composition on a substrate resin layer, a method of co-extruding the present EVOH resin composition and the substrate resin, a method of dry laminating the present EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc., a method of applying a solution of the present EVOH resin composition on the substrate resin and then removing the solvent, etc. Among these, considering the viewpoints of cost and environment, it is preferred to manufacture by a process of melting the present EVOH resin composition layer, and specifically, a co-extrusion method is preferred.

[0424] The present multilayer structure may also be subjected to (heating) stretching treatment as required. The stretching treatment may be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, the stretching may be performed simultaneously or sequentially. In addition, the stretching method may be a method with a higher stretching ratio such as a roller stretching method, a tenter stretching method, a belt stretching method, a stretch blow molding method, and a vacuum pressure molding method. The stretching temperature is a temperature near the melting point of the multilayer structure, and is selected from a range of usually 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is too low, the stretchability is poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0425] In addition, the multilayer structure after the stretching treatment may be heat-fixed in order to impart dimensional stability. Heat-fixing may be performed by known means, for example, the multilayer structure after the stretching treatment is maintained in a tensile state and heat-treated at a temperature of usually 80 to 180° C., preferably 100 to 165° C., for usually 2 to 600 seconds.

[0426] When the stretched multilayer structure is used as a shrink film, in order to impart heat shrinkage, the stretched multilayer structure may be cooled and fixed by blowing cold air instead of the heat setting.

[0427] The thickness of the present multilayer structure (including the stretched multilayer structure), and further the thickness of the present EVOH resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure, depends on the layer constitution, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., and cannot be generalized, but the thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0428] Furthermore, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the substrate resin layer (present EVOH resin composition layer / substrate resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, calculated as the ratio of the thickest layers. In addition, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer (present EVOH resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, calculated as the ratio of the thickest layers.

[0429] In addition, the present multilayer structure can be used to obtain a cup or tray-shaped multilayer container. In this case, a pull molding method is usually used, and specifically, for example, vacuum molding, pressure molding, vacuum pressure molding, plug-assisted vacuum pressure molding, etc. can be cited. Furthermore, when a tubular or bottle-shaped multilayer container (laminated structure) is obtained from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, for example, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulation type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion type cold parison biaxial stretch blow molding, injection type cold parison biaxial stretch blow molding, injection molding online biaxial stretch blow molding, etc.), etc. The obtained laminate can be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, deep drawing processing, box processing, tube processing, splitting processing, etc. as needed.

[0430] The single-layer film formed from the present EVOH resin composition, the bags and cups, trays, tubes, bottles and other containers and lids formed from the present multilayer structure are useful as various packaging material containers for general foods, seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oils, beverages, cosmetics, pharmaceuticals, etc.

[0431] <<Method 5>>

[0432] EVOH resin has excellent transparency, oxygen and other gas barrier properties, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and is molded into films, sheets, bottles, etc. and widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials.

[0433] However, EVOH resin has a relatively active hydroxyl group in the molecule and tends to be easily degraded by heat, and is prone to coloring during melt molding.

[0434] Regarding the above-mentioned problems, for example, Patent Document 1 discloses that by making EVOH resin contain a specific amount of unsaturated aldehyde, oxidative degradation during melt molding can be suppressed and coloration can be suppressed.

[0435] [Patent Document 1] International Publication No. 2013 / 146961

[0436] In recent years, molding equipment has tended to be more functional, with the diversification of the feed blocks and die shapes of molding equipment, the thinning of multilayer structures in the final products, the increase in the number of layers, and other requirements for higher functionality. However, on the other hand, the productivity of the product tends to decrease due to thermal degradation and coloration of the resin in the molding equipment that has become more complex due to higher functionality.

[0437] In the above-mentioned Patent Document 1, unsaturated aldehydes are used to suppress coloration during melt molding, but such aldehyde compounds can cause bad odor even in a trace amount. In particular, when exposed to high-temperature melt molding, the aldehyde compounds volatilize, which may deteriorate the working environment. Therefore, an EVOH resin composition is sought that suppresses coloration during the melt molding process without using such volatile compounds, that is, has excellent long-run performance.

[0438] An object of the present invention is to provide an EVOH resin composition in which color change due to thermal degradation during melt molding is suppressed.

[0439] [Methods to solve the problem]

[0440] However, in view of this situation, the present inventors have found that an EVOH resin composition in which color change due to thermal degradation during melt molding is suppressed can be obtained by adding a compound having a conjugated polyene structure and a specific trace amount of a titanium compound to an EVOH resin.

[0441] That is, the present invention has the following aspects.

[0442] [5-1] An EVOH resin composition comprising an EVOH resin, a compound having a conjugated polyene structure, and a titanium compound, wherein the metal-equivalent content of the titanium compound is 0.001 ppm or more and less than 5 ppm based on the mass of the EVOH resin composition.

[0443] [5-2] The EVOH resin composition according to [5-1], wherein the content of the compound having a conjugated polyene structure is 1 to 1000 ppm based on the mass of the EVOH resin composition.

[0444] [5-3] The EVOH resin composition according to [5-1] or [5-2], wherein the mass ratio of the content of the compound having a conjugated polyene structure to the metal equivalent content of the titanium compound is 0.2 to 1,000,000.

[0445] [5-4] The EVOH resin composition according to any one of [5-1] to [5-3], wherein the compound having a conjugated polyene structure is sorbic acid.

[0446] [5-5] A pellet comprising the EVOH resin composition according to any one of [5-1] to [5-4].

[0447] [5-6] A multilayer structure comprising at least one layer comprising the EVOH resin composition according to any one of [5-1] to [5-4].

[0448] [5-7] A method for producing an EVOH resin composition, the method comprising producing the EVOH resin composition described in any one of [5-1] to [5-4].

[0449] The method comprises the step of melt-mixing a composition raw material containing the EVOH resin and the titanium compound.

[0450] [5-8] A method for producing a multilayer structure, which is a method for producing the multilayer structure described in [5-6],

[0451] The process comprises melt-molding the layer composed of the EVOH resin composition.

[0452] [Effects of the Invention]

[0453] The EVOH resin composition of the present invention can suppress the color change of the EVOH resin during melt molding and has excellent long-term operating properties. [Specific implementation method]

[0455] Hereinafter, the present invention will be described in more detail based on the embodiments of the present invention, but the present invention is not limited to these embodiments.

[0456] <EVOH resin composition>

[0457] The EVOH resin composition according to one embodiment of the present invention (hereinafter referred to as "the present EVOH resin composition") contains EVOH resin as a main component and a compound having a conjugated polyene structure and a specific trace amount of a titanium compound.

[0458] That is, the base resin in the present EVOH resin composition is EVOH resin, and the content of EVOH resin in the present EVOH resin composition is usually 70 mass % or more, preferably 80 mass % or more, more preferably 90 mass % or more, particularly preferably 95 mass % or more.

[0459] Hereinafter, each component will be described.

[0460] [EVOH resin]

[0461] The EVOH resin used in the present invention is generally a resin obtained by saponifying an ethylene-vinyl ester copolymer which is a copolymer of ethylene and a vinyl ester monomer, and the same EVOH resin as described in the first embodiment can be used.

[0462] [Compounds having a conjugated polyene structure]

[0463] The compound having a conjugated polyene structure is a compound having a structure in which carbon-carbon double bonds and carbon-carbon single bonds are alternately connected, and the number of carbon-carbon double bonds is 2 or more, that is, a so-called conjugated double bond.

[0464] The compound having a conjugated polyene structure may be a conjugated diene compound having a structure in which two carbon-carbon double bonds are alternately connected with one carbon-carbon single bond, a conjugated triene compound having a structure in which three carbon-carbon double bonds are alternately connected with two carbon-carbon single bonds, or a conjugated polyene compound having a structure in which a greater number of carbon-carbon double bonds are alternately connected with a carbon-carbon single bond. Among them, the compound having a conjugated polyene structure does not include aromatic carboxylic acids such as cinnamic acid, and quinones such as hydroquinone and benzoquinone.

[0465] In addition, in the compound having a conjugated polyene structure, if the number of conjugated carbon-carbon double bonds is 8 or more, there is a concern that the color of the conjugated polyene compound itself may cause coloring of the molded product, so the number of conjugated carbon-carbon double bonds is preferably 7 or less. Furthermore, in the compound having a conjugated polyene structure, the conjugated double bonds consisting of two or more carbon-carbon double bonds may be non-conjugated to each other and may have multiple groups in one molecule. For example, a compound having three conjugated trienes in the same molecule, such as tung oil, is also included in the compound having a conjugated polyene structure.

[0466] The molecular weight of the compound having a conjugated polyene structure is usually 30 to 500, preferably 50 to 400, and particularly preferably 100 to 300 from the viewpoint of productivity and handling.

[0467] The compound having a conjugated polyene structure has generally 4 to 30 carbon atoms, preferably 4 to 20 carbon atoms, and particularly preferably 4 to 10 carbon atoms in one molecule from the viewpoint of productivity and handling properties.

[0468] Examples of such compounds having a conjugated polyene structure include isoprene, 2,3-dimethyl-1,3-butadiene, 2,3-diethyl-1,3-butadiene, 2-tert-butyl-1,3-butadiene, 1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 2,4-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-pentadiene, 3-ethyl-1,3-pentadiene, 2-methyl-1,3-pentadiene, 3-methyl-1,3-pentadiene, 4-methyl-1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 2,5-dimethyl-2,4-hexadiene, 1,3-octadiene, 1,3-cyclopentadiene, 1,3-cyclohexadiene, 1-phenyl-1,3-butadiene, 1 ,4-diphenyl-1,3-butadiene, 1-methoxy-1,3-butadiene, 2-methoxy-1,3-butadiene, 1-ethoxy-1,3-butadiene, 2-ethoxy-1,3-butadiene, 2-nitro-1,3-butadiene, chloroprene, 1-chloro-1,3-butadiene, 1-bromo-1,3-butadiene, 2-bromo-1,3-butadiene, fulvene, tropone, ocimene, phllandrene, myrcene, farnesene, cembrene; sorbic acid, sorbic acid esters, sorbates and other sorbic acids, abietic acid ( A conjugated diene compound composed of a conjugated structure of two carbon-carbon double bonds, such as 1,3,5-hexatriene, 2,4,6-octatriene-1-carboxylic acid, eleostearic acid, tung oil, cholecalciferol, etc.; a conjugated triene compound composed of a conjugated structure of three carbon-carbon double bonds, such as cyclooctatetraene, 2,4,6,8-decatetraene-1-carboxylic acid, retinol, retinoic acid, etc., having a conjugated polyene structure composed of a conjugated structure of four or more carbon-carbon double bonds. In addition, for compounds having multiple stereoisomers such as 1,3-pentadiene, myrcene, and farnesene, any one can be used. The above-mentioned compounds having a conjugated polyene structure can be used alone or in combination of two or more.

[0469] Among these compounds having a conjugated polyene structure, compounds having a carboxyl group are preferred from the viewpoint of high affinity with water, and chain compounds having a carboxyl group are more preferred. Sorbic acids, particularly sorbic acid, are particularly preferred.

[0470] The content of the compound having a conjugated polyene structure is preferably 1 to 1000 ppm, more preferably 10 to 700 ppm, particularly preferably 50 to 600 ppm, and even more particularly preferably 70 to 300 ppm relative to the mass of the EVOH resin composition. When the content of the compound having a conjugated polyene structure is too much, productivity tends to be impaired, and when it is too little, thermal stability tends to be reduced.

[0471] The content of the above-mentioned compound with conjugated polyene structure can for example use liquid chromatography-ultraviolet spectroscopic detector, and measures by the following steps.It should be noted that the following steps are recorded as an example with the situation of using sorbic acid, but for other compounds with conjugated polyene structure, it is also possible to measure by the same steps by using an extraction solvent that is suitable for this compound.

[0472] [Method for determining the content of a compound having a conjugated polyene structure]

[0473] (1) 8 mL of an extraction solvent (distilled water:methanol=1:1, volume ratio) was added to 1 g of freeze-pulverized powder of the present EVOH resin composition.

[0474] (2) The solution was subjected to ultrasonic treatment at 20°C for 1 hour in a static state to extract the sorbic acid in the resin, and after cooling, the volume was fixed to 10 mL with the extraction solvent. In addition, it can be diluted to any multiple as needed.

[0475] (3) After filtering the above solution through a filter with a pore size of 0.45 μm, the sorbic acid in the extract solution was determined by liquid chromatography-ultraviolet spectrophotometry.

[0476] (4) A calibration curve is prepared using a standard solution of sorbic acid prepared using the above-mentioned extraction solvent, and the content of sorbic acid is quantified using the absolute calibration curve method.

[0477] [HPLC measurement conditions]

[0478] LC system: Agilent 1260 / 1290 [Agilent Technologies]

[0479] Detector: Agilent 1260 infinity diode array detector [Agilent Technologies, Inc.]

[0480] Column: Cadenza CD-C18 (100×3.0 mm, 3 μm) [manufactured by Imtakt]

[0481] Column temperature: 40°C

[0482] Mobile phase A: 5% acetonitrile in water containing 0.05% formic acid

[0483] Mobile phase B: 95% acetonitrile in water containing 0.05% formic acid

[0484] Time program: 0.0→5.0 minutes B%=30%

[0485] 5.0→8.0 minutes B%=30%→50%

[0486] 8.0→10.0 minutes B%=50%

[0487] 10.0→13.0 minutes B%=50%→30%

[0488] 13.0→15.0 minutes B%=30%

[0489] Flow rate: 0.2mL / min

[0490] UV detection wavelength: 190~400nm

[0491] Quantitative wavelength: 262nm

[0492] In addition, "%" in the above-mentioned HPLC measurement conditions means volume %.

[0493] [Titanium compounds]

[0494] Examples of the titanium compound include inorganic titanium compounds and organic titanium compounds. As the titanium compound, the same titanium compound as that described in the first embodiment can be used.

[0495] The metal conversion content of the titanium compound is greater than 0.001ppm and less than 5ppm relative to the mass of the EVOH resin composition. It is preferably 0.01 to 3ppm, more preferably 0.03 to 1ppm, and particularly preferably 0.05 to 0.5ppm. By making the metal conversion content of the titanium compound within the above range, the color change caused by thermal degradation during melt molding can be suppressed, and long-term operation performance is excellent. In addition, if the metal conversion content of the titanium compound is too small, the effect of suppressing color change is reduced, and if the metal conversion content is too much, thermal decomposition of the EVOH resin becomes easy to occur, and it is easy to color.

[0496] In addition, the mass ratio of the content of the compound having a conjugated polyene structure to the metal-converted content of the titanium compound (the content of the compound having a conjugated polyene structure / the metal-converted content of the titanium compound) is preferably 0.2 to 1,000,000, further preferably 0.3 to 100,000, more preferably 10 to 23,000, particularly preferably 50 to 12,000, even more preferably 100 to 5,000, and most preferably 150 to 3,000. When the mass ratio is too large, thermal stability tends to be impaired, and when it is too small, the molded product tends to be colored.

[0497] The metal conversion content of the above-mentioned titanium compound can be obtained by measuring the EVOH resin composition into a platinum crucible, ashing it with a burner and an electric furnace in sequence, heating and decomposing the ashed material with nitric acid and hydrofluoric acid, treating it with a mixed acid of dilute nitric acid and dilute hydrofluoric acid and fixing the volume, and quantitatively measuring the titanium in the obtained fixed volume solution by ICP mass spectrometry using an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800).

[0498] Generally speaking, EVOH resin will be colored due to thermal degradation. It is believed that this is because the thermal degradation of EVOH resin generates free radicals, and these free radicals dehydrate the hydroxyl groups of EVOH resin, forming double bonds in the main chain of EVOH resin. This site becomes the starting point of the reaction, further promoting dehydration and forming a conjugated polyene structure in the main chain of EVOH resin.

[0499] On the other hand, the present EVOH resin composition contains a compound having a conjugated polyene structure and a specific trace amount of a titanium compound, so that the color change of the EVOH resin due to thermal degradation is suppressed and the long-term operating performance is excellent.

[0500] Generally, when an EVOH resin composition contains a titanium compound, it is believed that the EVOH resin composition is colored due to titanium ions, so it is common knowledge for those skilled in the art to avoid using titanium compounds. However, contrary to such common knowledge, the present invention has found that when a specific trace amount of a titanium compound is used, an EVOH resin composition in which color change due to thermal degradation is suppressed can be obtained.

[0501] The reason why the effect of the present invention is obtained by using a compound having a conjugated polyene structure and a trace amount of a titanium compound in combination is that titanium can exist in the form of trivalent and tetravalent ions, and the compound having a conjugated polyene structure reduces the tetravalent titanium ions to generate trivalent titanium ions. Furthermore, it is presumed that the trivalent titanium ions again reduce the compound having a conjugated polyene structure, thereby generating a cycle of recovering the activity of the compound having a conjugated polyene structure.

[0502] It is also presumed that the tetravalent ion form of titanium is stable and even a trace amount thereof coordinates to the double bonds of the main chain of the EVOH resin described above to form a chelate complex or the like, thereby stabilizing and inhibiting the formation of a polyene structure.

[0503] On the other hand, if the content of the titanium compound is too large, it is considered that thermal decomposition of the EVOH resin by the titanium compound occurs, resulting in coloration.

[0504] [Other thermoplastic resins]

[0505] The present EVOH resin composition may contain a thermoplastic resin other than EVOH resin within a range not impairing the effects of the present invention (for example, generally 30% by mass or less, preferably 20% by mass or less, particularly preferably 10% by mass or less of the present EVOH resin composition).

[0506] As other thermoplastic resins, known thermoplastic resins can be used, for example, polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, ionomers, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0507] [Other compounding ingredients]

[0508] The EVOH resin composition may contain a compounding agent generally compounded in EVOH resin within a range not hindering the effects of the present invention. As the compounding agent, the same compounding agent as described in the first embodiment can be used.

[0509] [Method for producing EVOH resin composition]

[0510] The present EVOH resin composition can be prepared, for example, by mixing the above-mentioned EVOH resin, a compound having a conjugated polyene structure and a titanium compound by a known method, such as a dry blending method, a melt blending method, a solution blending method, an impregnation method, etc. Among these, it is preferably prepared by a process of melt blending a composition raw material containing the above-mentioned EVOH resin and the titanium compound. In addition, these manufacturing methods can also be arbitrarily combined.

[0511] Examples of the dry blending method include (i) a method of dry blending a pelletized EVOH resin with a compound having a conjugated polyene structure and / or a titanium compound using a tumbler or the like.

[0512] Examples of the melt mixing method include (ii) a method of melt-kneading a pelletized EVOH resin and a compound having a conjugated polyene structure and / or a titanium compound; and (iii) a method of adding a compound having a conjugated polyene structure and / or a titanium compound to a molten EVOH resin and melt-kneading the dry blend.

[0513] Examples of the solution mixing method include (iv) a method in which a solution is prepared using a commercially available EVOH resin, a compound having a conjugated polyene structure and / or a titanium compound is added thereto, the solution is solidified into a shape, and then the solution is separated into solid and liquid by known means and dried; (v) a method in which, during the manufacture of the EVOH resin, a solution of an ethylene-vinyl ester copolymer before saponification or a uniform solution of the EVOH resin (water / alcohol solution, etc.) is made to contain a compound having a conjugated polyene structure and / or a titanium compound, the solution is solidified into a shape, and then the solution is separated into solid and liquid by known means and dried.

[0514] Examples of the impregnation method include (vi) contacting pelletized EVOH resin with an aqueous solution containing a compound having a conjugated polyene structure and / or a titanium compound to allow the EVOH resin to contain the compound having a conjugated polyene structure and / or a titanium compound, followed by drying.

[0515] As the aqueous solution containing the compound having a conjugated polyene structure and / or a titanium compound, an aqueous solution of a compound having a conjugated polyene structure and / or a titanium compound, or an aqueous solution in which titanium ions are dissolved by immersing the compound having a conjugated polyene structure and / or a titanium compound in water containing various reagents can be used.

[0516] In the above-mentioned impregnation method, the content (metal conversion) of the titanium compound can be controlled by the concentration of the titanium compound in the aqueous solution for impregnating the EVOH resin, the impregnation temperature, the impregnation time, and the like.

[0517] The immersion temperature and immersion time are usually 0.5 to 48 hours, preferably 1 to 36 hours, and the immersion temperature is usually 10 to 40°C, preferably 20 to 35°C.

[0518] The drying method in each of the above-mentioned production methods can adopt various drying methods, and can be any of static drying and fluidized drying. In addition, these methods can also be combined.

[0519] As described above, the above different methods can be combined in the present invention. Among them, considering productivity and the viewpoint of obtaining a resin composition with more significant effects of the present invention, the melt mixing method is preferred, and the method (ii) is particularly preferred. In addition, when using the above other thermoplastic resins and other compounding ingredients, they can be compounded in a conventional manner according to the above manufacturing method.

[0520] The present EVOH resin composition obtained by the above-mentioned respective production methods may be in any shape, but is preferably in the form of pellets.

[0521] The pellets may be spherical, elliptical, cylindrical, cubic, or rectangular, and are usually elliptical or cylindrical. Considering the convenience of using the pellets as molding materials, the pellets are usually 1 to 10 mm in diameter, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm in diameter, and usually 1.5 to 30 mm in diameter, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm in diameter, in the case of elliptical pellets. In the case of cylindrical pellets, the bottom diameter is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm.

[0522] In addition, the shape and size of the pelletized EVOH resin used in each of the above-mentioned production methods are also preferably the same.

[0523] Even when the EVOH resin composition is heated during melt molding, the color change is still suppressed, and the long-term operation is excellent. The ratio of the YI value after heating to the YI value (yellow index) before heating (YI value after heating / YI value before heating) is usually less than 5.0, preferably less than 4.9, and more preferably less than 4.5. If the ratio of the YI value after heating to the YI value before heating is within the above range, there is a tendency to further suppress the color change. It should be noted that the lower limit of the ratio of the YI value after heating to the YI value before heating is usually 1.

[0524] In the above-mentioned ratio of YI values, even a difference of 0.1 will show a significant difference in yield in actual production, so the difference is very large.

[0525] The YI value before heating is obtained by grinding the EVOH resin composition into 1 to 5 mm square pieces, filling the ground product into a cylinder with an inner diameter of 32 mm and a height of 30 mm, and then scraping off the ground product. In this state, the YI value is measured using a spectrocolorimeter SE6000 (manufactured by Nippon Denshoku Industries Co., Ltd.).

[0526] The YI value after heating is obtained by heating the EVOH resin composition crushed into 1 to 5 mm square pieces in an oven under air atmosphere at 150°C for 5 hours and then measuring the same method.

[0527] The water content of the present EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0528] The water content of the EVOH resin composition is measured and calculated by the following method.

[0529] The mass (W1) of the EVOH resin composition before drying was weighed with an electronic balance, dried in a hot air dryer at 150°C for 5 hours, and the mass (W2) after cooling in the dryer for 30 minutes was weighed and calculated according to the following formula.

[0530] Water content (mass %) = [(W1-W2) / W1] × 100

[0531] In addition, when the EVOH resin composition is in the form of pellets, it is preferred to attach a known lubricant to the surface of the pellets from the viewpoint of stabilizing the feeding property during melt molding. Examples of lubricants include: higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters, etc. of higher fatty acids), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauramide, myristic acid, palmitic acid, stearic acid, behenic acid, etc.; unsaturated higher fatty acid amides such as oleamide and erucic acid, bis-higher fatty acid amides such as ethylene bisstearamide, ethylene bisoleamide, ethylene biserucic acid, ethylene bislauramide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene having a molecular weight of about 500 to 10,000, or low molecular weight polypropylene, etc., or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluorinated vinyl resins, etc. These compounds may be used alone or in combination of two or more. The content of the lubricant is usually 5% by mass or less, preferably 1% by mass or less, of the EVOH resin composition, and the lower limit is usually 0% by mass.

[0532] The EVOH resin composition thus obtained can be prepared into various forms such as pellets, powders, and liquids, and provided as molding materials for various molded products. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to obtain the effects of the present invention with better efficiency, which is preferred.

[0533] In addition, the present EVOH resin composition also includes a resin composition obtained by mixing a resin other than the EVOH resin used in the present EVOH resin composition.

[0534] The molded product is, for example, a multilayer structure having a layer composed of the present EVOH resin composition, such as a single-layer film molded from the present EVOH resin composition.

[0535] [Multilayer structure]

[0536] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present EVOH resin composition. The layer composed of the present EVOH resin composition (hereinafter referred to as "the present EVOH resin composition layer") can be further provided with strength, or the present EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating it with other substrates having a thermoplastic resin as a main component other than the present EVOH resin composition (hereinafter, the resin used in the substrate is sometimes referred to as "substrate resin").

[0537] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polybutene, polypentene, (unmodified) polyolefin resins including polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and these polyolefin resins. Modified olefin resins in a broad sense include polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by graft modification with unsaturated carboxylic acid or its ester, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, chlorinated polyethylene, chlorinated polypropylene and other halogenated polyolefins, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.

[0538] Among these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred as hydrophobic resins, and polyethylene resins, polypropylene resins, polycyclic olefin resins, and polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred.

[0539] When the EVOH resin composition layer is a (a1, a2, ...) and the substrate resin layer is b (b1, b2, ...), the layer structure of the multilayer structure can be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the recovered layer including the mixture of the EVOH resin composition and the thermoplastic resin other than the EVOH resin composition obtained by remelting and molding the end parts and defective products generated in the production process of the multilayer structure is taken as R, it can be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is usually 2 to 15 in total, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be inserted between the layers as needed.

[0540] As the above-mentioned adhesive resin, a known adhesive resin can be used, and it can be appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins by addition reaction, grafting reaction, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. They can be used alone or in combination of two or more.

[0541] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present EVOH resin composition layer, it is preferred to use an adhesive resin having excellent hydrophobicity.

[0542] The above-mentioned base resin and adhesive resin may contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating materials, antiblocking agents, waxes, etc., within the range that does not hinder the gist of the present invention (for example, 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These can be used alone or in combination of two or more.

[0543] The lamination of the above-mentioned EVOH resin composition layer and the above-mentioned substrate resin layer (including the case where an adhesive resin layer is inserted) can be carried out according to a known method. For example: a method of melt-extrusion laminating the substrate resin on a film, sheet, etc. of the present EVOH resin composition, a method of melt-extrusion laminating the present EVOH resin composition on a substrate resin layer, a method of co-extruding the present EVOH resin composition and the substrate resin, a method of dry laminating the present EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc., a method of applying a solution of the present EVOH resin composition on the substrate resin and then removing the solvent, etc. Among these, considering the viewpoints of cost and environment, it is preferred to manufacture by a process of melting the present EVOH resin composition layer, and specifically, a co-extrusion method is preferred.

[0544] The present multilayer structure may also be subjected to (heating) stretching treatment as required. The stretching treatment may be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, the stretching may be performed simultaneously or sequentially. In addition, the stretching method may be a method with a higher stretching ratio such as a roller stretching method, a tenter stretching method, a belt stretching method, a stretch blow molding method, and a vacuum pressure molding method. The stretching temperature is a temperature near the melting point of the multilayer structure, and is selected from a range of usually 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is too low, the stretchability is poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0545] In addition, the multilayer structure after the stretching treatment may be heat-fixed in order to impart dimensional stability. Heat-fixing may be performed by known means, for example, the multilayer structure after the stretching treatment is maintained in a tensile state and heat-treated at a temperature of usually 80 to 180° C., preferably 100 to 165° C., for usually 2 to 600 seconds.

[0546] When the stretched multilayer structure is used as a shrink film, in order to impart heat shrinkage, the stretched multilayer structure may be cooled and fixed by blowing cold air instead of the heat setting.

[0547] The thickness of the present multilayer structure (including the stretched multilayer structure), and further the thickness of the present EVOH resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure, depends on the layer constitution, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., and cannot be generalized, but the thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0548] Furthermore, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the substrate resin layer (present EVOH resin composition layer / substrate resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, calculated as the ratio of the thickest layers. In addition, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer (present EVOH resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, calculated as the ratio of the thickest layers.

[0549] In addition, the present multilayer structure can be used to obtain a cup or tray-shaped multilayer container. In this case, a pull molding method is usually used, and specifically, for example, vacuum molding, pressure molding, vacuum pressure molding, plug-assisted vacuum pressure molding, etc. can be cited. Furthermore, when a tubular or bottle-shaped multilayer container (laminated structure) is obtained from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, for example, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulation type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion type cold parison biaxial stretch blow molding, injection type cold parison biaxial stretch blow molding, injection molding online biaxial stretch blow molding, etc.), etc. The obtained laminate can be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, deep drawing processing, box processing, tube processing, splitting processing, etc. as needed.

[0550] The single-layer film formed from the present EVOH resin composition, the bags and cups, trays, tubes, bottles and other containers and lids formed from the present multilayer structure are useful as various packaging material containers for general foods, seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oils, beverages, cosmetics, pharmaceuticals, etc.

[0551] <<Method 6>>

[0552] EVOH resin has excellent transparency, oxygen and other gas barrier properties, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and is molded into films, sheets, bottles, etc. and widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials.

[0553] However, EVOH resin has a relatively active hydroxyl group in the molecule and tends to be easily degraded by heat, and is prone to coloring during melt molding.

[0554] Regarding the above-mentioned problems, for example, Patent Document 1 discloses that by making EVOH resin contain a specific amount of unsaturated aldehyde, oxidative degradation during melt molding can be suppressed and coloration can be suppressed.

[0555] [Patent Document 1] International Publication No. 2013 / 146961

[0556] In recent years, molding equipment has tended to be more functional, with the diversification of the feed blocks and die shapes of molding equipment, the thinning of multilayer structures in the final products, the increase in the number of layers, and other requirements for higher functionality. However, on the other hand, the productivity of the product tends to decrease due to thermal degradation and coloration of the resin in the molding equipment that has become more complex due to higher functionality.

[0557] In the above-mentioned Patent Document 1, unsaturated aldehydes are used to suppress coloration during melt molding, but such aldehyde compounds can cause bad odor even in a trace amount. In particular, when exposed to high-temperature melt molding, aldehyde compounds volatilize, which may deteriorate the working environment. Therefore, an EVOH resin composition is sought that suppresses coloration during the melt molding process without using such volatile compounds, that is, has excellent long-term operating performance.

[0558] An object of the present invention is to provide an EVOH resin composition in which color change due to thermal degradation during melt molding is suppressed.

[0559] [Methods to solve the problem]

[0560] However, in view of the above circumstances, the present inventors have found that an EVOH resin composition in which color change due to thermal degradation during melt molding is suppressed can be obtained by adding a boron compound and a specific trace amount of a titanium compound to an EVOH resin.

[0561] That is, the present invention has the following aspects.

[0562] [6-1] An EVOH resin composition comprising an EVOH resin, a boron compound, and a titanium compound, wherein the metal-equivalent content of the titanium compound is 0.001 ppm or more and less than 5 ppm based on the mass of the EVOH resin composition.

[0563] [6-2] The EVOH resin composition according to [6-1], wherein the boron-equivalent content of the boron compound is 5 to 400 ppm relative to the mass of the EVOH resin composition.

[0564] [6-3] The EVOH resin composition according to [6-1] or [6-2], wherein the mass ratio of the boron-equivalent content of the boron compound to the metal content of the titanium compound is 1 to 400,000.

[0565] [6-4] A pellet comprising the EVOH resin composition according to any one of [6-1] to [6-3].

[0566] [6-5] A multilayer structure comprising at least one layer comprising the EVOH resin composition according to any one of [6-1] to [6-3].

[0567] [6-6] A method for producing an EVOH resin composition, the method comprising producing the EVOH resin composition described in any one of [6-1] to [6-3].

[0568] The method comprises the step of melt-mixing a composition raw material containing the EVOH resin and the titanium compound.

[0569] [6-7] A method for producing a multilayer structure, which is a method for producing the multilayer structure described in [6-5],

[0570] The process comprises melt-molding the layer composed of the EVOH resin composition.

[0571] [Effects of the Invention]

[0572] The EVOH resin composition of the present invention can suppress the color change of the EVOH resin during melt molding and has excellent long-term operating properties. [Specific implementation method]

[0574] Hereinafter, the present invention will be described in more detail based on the embodiments of the present invention, but the present invention is not limited to these embodiments.

[0575] <EVOH resin composition>

[0576] The EVOH resin composition according to one embodiment of the present invention (hereinafter referred to as "the present EVOH resin composition") contains EVOH resin as a main component and a boron compound and a specific trace amount of a titanium compound.

[0577] That is, the base resin in the present EVOH resin composition is EVOH resin, and the content of EVOH resin in the present EVOH resin composition is usually 70 mass % or more, preferably 80 mass % or more, more preferably 90 mass % or more, particularly preferably 95 mass % or more.

[0578] Hereinafter, each component will be described.

[0579] [EVOH resin]

[0580] The EVOH resin used in the present invention is generally a resin obtained by saponifying an ethylene-vinyl ester copolymer which is a copolymer of ethylene and a vinyl ester monomer, and the same EVOH resin as described in the first embodiment can be used.

[0581] [Boron compounds]

[0582] Examples of the boron compound include boric acid or metal salts thereof, for example, sodium borate (sodium metaborate, sodium diborate, sodium tetraborate, sodium pentaborate, sodium hexaborate, sodium octaborate, etc.), potassium borate (potassium metaborate, potassium tetraborate, potassium pentaborate, potassium hexaborate, potassium octaborate, etc.), lithium borate (lithium metaborate, lithium tetraborate, lithium pentaborate, etc.), calcium borate, barium borate (barium orthoborate, barium metaborate, barium diborate, barium tetraborate, etc.), magnesium borate (magnesium orthoborate, magnesium diborate, magnesium metaborate, trimagnesium tetraborate, pentamagnesium tetraborate, etc.), manganese borate (manganous borate, manganese metaborate, manganese tetraborate, etc.), cobalt borate, zinc borate (zinc tetraborate, zinc metaborate, etc.) The present invention relates to a kind of borate minerals, such as borax, cahnite, inyoite, suanite, szaibelyite, etc., and ...

[0583] As the properties of the boron compound, any boron compound in any form such as solid (powder, fine powder, flake, etc.), semi-solid, liquid, paste, solution, emulsion (aqueous dispersion) can be used, and powder is preferred. When the boron compound is in powder form, the particle size of the boron compound is usually 0.1 to 100 μm, preferably 1 to 75 μm, and particularly preferably 5 to 50 μm.

[0584] The content of the boron compound is preferably 5 to 400 ppm, more preferably 10 to 300 ppm, and even more preferably 50 to 200 ppm based on the mass of the EVOH resin composition in terms of boron. If the content is too low, the moldability of the EVOH resin composition tends to decrease.

[0585] The boron-equivalent content of the boron compound can be measured by, for example, heating the EVOH resin composition to ashing and then treating it with an acid such as hydrochloric acid to obtain a solution, adding pure water to the obtained solution to make it constant to volume, and using the solution as a test solution for measurement using an atomic absorption spectrophotometer.

[0586] [Titanium compounds]

[0587] Examples of the titanium compound include inorganic titanium compounds and organic titanium compounds. As the titanium compound, the same titanium compound as that described in the first embodiment can be used.

[0588] The metal conversion content of the above-mentioned titanium compound is greater than 0.001ppm and less than 5ppm relative to the mass of the EVOH resin composition. It is preferably 0.01 to 3ppm, more preferably 0.03 to 2ppm, and particularly preferably 0.05 to 1ppm. By making the metal conversion content of the titanium compound within the above range, the color change caused by thermal degradation during melt molding can be suppressed, and long-term operation performance is excellent. In addition, if the metal conversion content of the titanium compound is too small, the effect of suppressing color change is reduced, and if the metal conversion content is too much, thermal decomposition of the EVOH resin becomes easy to occur, and it is easy to color.

[0589] The metal conversion content of the above-mentioned titanium compound can be obtained by measuring the EVOH resin composition into a platinum crucible, ashing it with a burner and an electric furnace in sequence, heating and decomposing the ashed material with nitric acid and hydrofluoric acid, treating it with a mixed acid of dilute nitric acid and dilute hydrofluoric acid and fixing the volume, and quantitatively measuring the titanium in the obtained fixed volume solution by ICP mass spectrometry using an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800).

[0590] The mass ratio of the boron-converted content of the above-mentioned boron compound to the metal-converted content of the above-mentioned titanium compound (metal-converted content of the titanium compound / boron-converted content of the boron compound) is preferably 1 to 400,000, further preferably 2 to 40,000, more preferably 5 to 10,000, particularly preferably 30 to 4,000, even more preferably 50 to 2,000, and most preferably 70 to 900.

[0591] When the mass ratio is too large, the coloration prevention effect tends to be reduced, and when it is too small, the molded product tends to be colored.

[0592] Generally speaking, EVOH resin will be colored due to thermal degradation. It is believed that this is because the thermal degradation of EVOH resin generates free radicals, and these free radicals dehydrate the hydroxyl groups of EVOH resin, forming double bonds in the main chain of EVOH resin. This site becomes the starting point of the reaction, further promoting dehydration and forming a conjugated polyene structure in the main chain of EVOH resin.

[0593] On the other hand, the present EVOH resin composition contains a boron compound and a specific trace amount of a titanium compound, so that the color change of the EVOH resin due to thermal degradation is suppressed and the long-term operating performance is excellent.

[0594] Generally, when an EVOH resin composition contains a titanium compound, it is believed that the EVOH resin composition is colored due to titanium ions, so it is common knowledge for those skilled in the art to avoid using titanium compounds. However, contrary to such common knowledge, the present invention has found that when a specific trace amount of a titanium compound is used, an EVOH resin composition in which color change due to thermal degradation is suppressed can be obtained.

[0595] That is, it is presumed that the tetravalent ion form of titanium is stable and even a trace amount thereof coordinates to the double bonds of the main chain of the EVOH resin described above to form a chelate complex or the like, thereby stabilizing and suppressing the formation of a polyene structure.

[0596] On the other hand, if the content of the titanium compound is too large, it is considered that thermal decomposition of the EVOH resin by the titanium compound occurs, resulting in coloration.

[0597] [Other thermoplastic resins]

[0598] The present EVOH resin composition may contain a thermoplastic resin other than EVOH resin within a range not impairing the effects of the present invention (for example, generally 30% by mass or less, preferably 20% by mass or less, particularly preferably 10% by mass or less of the present EVOH resin composition).

[0599] As other thermoplastic resins, known thermoplastic resins can be used, for example, polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, ionomers, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0600] [Other compounding ingredients]

[0601] The EVOH resin composition may contain a compounding agent generally compounded in EVOH resin within a range not hindering the effects of the present invention. As the compounding agent, the same compounding agent as described in the first embodiment can be used.

[0602] [Method for producing EVOH resin composition]

[0603] The present EVOH resin composition can be prepared, for example, by mixing the above-mentioned EVOH resin, boron compound and titanium compound by a known method, such as dry blending, melt blending, solution blending, impregnation, etc. Among these, it is preferably prepared by a process of melt blending the composition raw materials containing the above-mentioned EVOH resin and titanium compound. In addition, these manufacturing methods can also be arbitrarily combined.

[0604] Examples of the dry blending method include (i) a method of dry blending a pelletized EVOH resin with a boron compound and / or a titanium compound using a tumbler or the like.

[0605] Examples of the melt mixing method include (ii) a method of melt kneading a dry blend of pelletized EVOH resin and a boron compound and / or a titanium compound; and (iii) a method of adding a boron compound and / or a titanium compound to a molten EVOH resin and melt kneading the mixture.

[0606] Examples of the solution mixing method include (iv) a method in which a solution is prepared using a commercially available EVOH resin, a boron compound and / or a titanium compound is added thereto, the solution is solidified into a shape, and then the solution is separated into solid and liquid by known means and dried; (v) in the manufacturing process of the EVOH resin, a method in which a boron compound and / or a titanium compound is added to an ethylene-vinyl ester copolymer solution before saponification or a uniform solution of the EVOH resin (water / alcohol solution, etc.) is solidified into a shape, and then the solution is separated into solid and liquid by known means and dried.

[0607] Examples of the impregnation method include (vi) a method of bringing pelletized EVOH resin into contact with an aqueous solution containing a boron compound and / or a titanium compound to allow the EVOH resin to contain the boron compound and / or the titanium compound, followed by drying.

[0608] As the aqueous solution containing a boron compound and / or a titanium compound, an aqueous solution of a boron compound and / or a titanium compound or an aqueous solution obtained by immersing a boron compound and / or a titanium compound in water containing various chemicals to dissolve titanium ions can be used.

[0609] In the above impregnation method, the content of the boron compound (boron conversion) and the content of the titanium compound (metal conversion) can be controlled by the concentration of the boron compound and the titanium compound in the aqueous solution for impregnating the EVOH resin, the impregnation temperature, the impregnation time, etc.

[0610] The immersion temperature and immersion time are usually 0.5 to 48 hours, preferably 1 to 36 hours, and the immersion temperature is usually 10 to 40°C, preferably 20 to 35°C.

[0611] The drying method in each of the above-mentioned production methods can adopt various drying methods, and can be any of static drying and fluidized drying. In addition, these methods can also be combined.

[0612] As described above, the above different methods can be combined in the present invention. Among them, considering productivity and the viewpoint of obtaining a resin composition with more significant effects of the present invention, the melt mixing method is preferred, and the method (ii) is particularly preferred. In addition, when using the above other thermoplastic resins and other compounding ingredients, they can be compounded in a conventional manner according to the above manufacturing method.

[0613] The present EVOH resin composition obtained by the above-mentioned respective production methods may be in any shape, but is preferably in the form of pellets.

[0614] The pellets may be spherical, elliptical, cylindrical, cubic, or rectangular, and are usually elliptical or cylindrical. Considering the convenience of using the pellets as molding materials, the pellets are usually 1 to 10 mm in diameter, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm in diameter, and usually 1.5 to 30 mm in diameter, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm in diameter, in the case of elliptical pellets. In the case of cylindrical pellets, the bottom diameter is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm.

[0615] In addition, the shape and size of the pelletized EVOH resin used in each of the above-mentioned production methods are also preferably the same.

[0616] Even when the EVOH resin composition is heated during melt molding, the color change is still suppressed, and the long-term operation is excellent. The ratio of the YI value after heating to the YI value before heating (yellow index) (YI value after heating / YI value before heating) is usually 5.0 or less, and more preferably 4.9 or less. If the ratio of the YI value after heating to the YI value before heating is within the above range, there is a tendency to further suppress the color change. It should be noted that the lower limit of the ratio of the YI value after heating to the YI value before heating is usually 1.

[0617] In addition, even a difference of 0.1 in the ratio of the above-mentioned YI values ​​will show a significant difference in yield in actual production, and therefore the difference is very large.

[0618] The YI value before heating is obtained by grinding the EVOH resin composition into 1 to 5 mm square pieces, filling the ground product into a cylinder with an inner diameter of 32 mm and a height of 30 mm, and then scraping off the ground product. In this state, the YI value is measured using a spectrocolorimeter SE6000 (manufactured by Nippon Denshoku Industries Co., Ltd.).

[0619] The YI value after heating is obtained by heating the EVOH resin composition crushed into 1 to 5 mm square pieces in an oven under air atmosphere at 150°C for 5 hours and then measuring the same method.

[0620] The water content of the present EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0621] The water content of the EVOH resin composition is measured and calculated by the following method.

[0622] The mass (W1) of the EVOH resin composition before drying was weighed with an electronic balance, dried in a hot air dryer at 150°C for 5 hours, and the mass (W2) after cooling in the dryer for 30 minutes was weighed and calculated according to the following formula.

[0623] Water content (mass %) = [(W1-W2) / W1] × 100

[0624] In addition, when the EVOH resin composition is in the form of pellets, it is preferred to attach a known lubricant to the surface of the pellets from the viewpoint of stabilizing the feeding property during melt molding. Examples of lubricants include: higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters, etc. of higher fatty acids), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauramide, myristic acid, palmitic acid, stearic acid, behenic acid, etc.; unsaturated higher fatty acid amides such as oleamide and erucic acid, bis-higher fatty acid amides such as ethylene bisstearamide, ethylene bisoleamide, ethylene biserucic acid, ethylene bislauramide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene having a molecular weight of about 500 to 10,000, or low molecular weight polypropylene, etc., or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluorinated vinyl resins, etc. These compounds may be used alone or in combination of two or more. The content of the lubricant is usually 5% by mass or less, preferably 1% by mass or less, of the EVOH resin composition, and the lower limit is usually 0% by mass.

[0625] The EVOH resin composition thus obtained can be prepared into various forms such as pellets, powders, and liquids, and provided as molding materials for various molded products. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to obtain the effects of the present invention with better efficiency, which is preferred.

[0626] In addition, the present EVOH resin composition also includes a resin composition obtained by mixing a resin other than the EVOH resin used in the present EVOH resin composition.

[0627] The molded product is, for example, a multilayer structure having a layer composed of the present EVOH resin composition, such as a single-layer film molded from the present EVOH resin composition.

[0628] [Multilayer structure]

[0629] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present EVOH resin composition. The layer composed of the present EVOH resin composition (hereinafter referred to as "the present EVOH resin composition layer") can be further provided with strength, or the present EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating it with other substrates having a thermoplastic resin as a main component other than the present EVOH resin composition (hereinafter, the resin used in the substrate is sometimes referred to as "substrate resin").

[0630] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polybutene, polypentene, (unmodified) polyolefin resins including polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and these polyolefin resins. Modified olefin resins in a broad sense include polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by graft modification with unsaturated carboxylic acid or its ester, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, chlorinated polyethylene, chlorinated polypropylene and other halogenated polyolefins, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.

[0631] Among these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred as hydrophobic resins, and polyethylene resins, polypropylene resins, polycyclic olefin resins, and polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred.

[0632] When the EVOH resin composition layer is a (a1, a2, ...) and the substrate resin layer is b (b1, b2, ...), the layer structure of the multilayer structure can be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the recovered layer including the mixture of the EVOH resin composition and the thermoplastic resin other than the EVOH resin composition obtained by remelting and molding the end parts and defective products generated in the production process of the multilayer structure is taken as R, it can be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is usually 2 to 15 in total, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be inserted between the layers as needed.

[0633] As the above-mentioned adhesive resin, a known adhesive resin can be used, and it can be appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins by addition reaction, grafting reaction, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. They can be used alone or in combination of two or more.

[0634] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present EVOH resin composition layer, it is preferred to use an adhesive resin having excellent hydrophobicity.

[0635] The above-mentioned base resin and adhesive resin may contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating materials, antiblocking agents, waxes, etc., within the range that does not hinder the gist of the present invention (for example, 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These can be used alone or in combination of two or more.

[0636] The lamination of the above-mentioned EVOH resin composition layer and the above-mentioned substrate resin layer (including the case where an adhesive resin layer is inserted) can be carried out according to a known method. For example: a method of melt-extrusion laminating the substrate resin on a film, sheet, etc. of the present EVOH resin composition, a method of melt-extrusion laminating the present EVOH resin composition on a substrate resin layer, a method of co-extruding the present EVOH resin composition and the substrate resin, a method of dry laminating the present EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc., a method of applying a solution of the present EVOH resin composition on the substrate resin and then removing the solvent, etc. Among these, considering the viewpoints of cost and environment, it is preferred to manufacture by a process of melting the present EVOH resin composition layer, and specifically, a co-extrusion method is preferred.

[0637] The present multilayer structure may also be subjected to (heating) stretching treatment as required. The stretching treatment may be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, the stretching may be performed simultaneously or sequentially. In addition, the stretching method may be a method with a higher stretching ratio such as a roller stretching method, a tenter stretching method, a belt stretching method, a stretch blow molding method, and a vacuum pressure molding method. The stretching temperature is a temperature near the melting point of the multilayer structure, and is selected from a range of usually 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is too low, the stretchability is poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0638] In addition, the multilayer structure after the stretching treatment may be heat-fixed in order to impart dimensional stability. Heat-fixing may be performed by known means, for example, the multilayer structure after the stretching treatment is maintained in a tensile state and heat-treated at a temperature of usually 80 to 180° C., preferably 100 to 165° C., for usually 2 to 600 seconds.

[0639] When the stretched multilayer structure is used as a shrink film, in order to impart heat shrinkage, the stretched multilayer structure may be cooled and fixed by blowing cold air instead of the heat setting.

[0640] The thickness of the present multilayer structure (including the stretched multilayer structure), and further the thickness of the present EVOH resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure, depends on the layer constitution, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., and cannot be generalized, but the thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0641] Furthermore, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the substrate resin layer (present EVOH resin composition layer / substrate resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, calculated as the ratio of the thickest layers. In addition, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer (present EVOH resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, calculated as the ratio of the thickest layers.

[0642] In addition, the present multilayer structure can be used to obtain a cup or tray-shaped multilayer container. In this case, a pull molding method is usually used, and specifically, for example, vacuum molding, pressure molding, vacuum pressure molding, plug-assisted vacuum pressure molding, etc. can be cited. Furthermore, when a tubular or bottle-shaped multilayer container (laminated structure) is obtained from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, for example, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulation type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion type cold parison biaxial stretch blow molding, injection type cold parison biaxial stretch blow molding, injection molding online biaxial stretch blow molding, etc.), etc. The obtained laminate can be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, deep drawing processing, box processing, tube processing, splitting processing, etc. as needed.

[0643] The single-layer film formed from the present EVOH resin composition, the bags and cups, trays, tubes, bottles and other containers and lids formed from the present multilayer structure are useful as various packaging material containers for general foods, seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oils, beverages, cosmetics, pharmaceuticals, etc.

[0644] <<Method 7>>

[0645] EVOH resin has excellent transparency, oxygen and other gas barrier properties, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and is molded into films, sheets, bottles, etc. and widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials.

[0646] Furthermore, in a multi-layer pipe used in a floor heating system utilizing a warm water circulation method, EVOH resin is also used as a molding material for one layer constituting the multi-layer pipe in order to prevent corrosion and the like.

[0647] However, EVOH resin has a tendency to deteriorate easily due to heat because of its relatively active hydroxyl groups in the molecule. Therefore, problems such as coloration and gelation may occur during melt molding, and the melt stability tends to decrease. In this regard, there is a known method of solving this problem by adding various heat stabilizers (for example, see Patent Document 1).

[0648] On the other hand, when EVOH resin moldings are used for a long period of time, the resin may deteriorate and develop odor or cracks depending on the use environment. For example, in the case of the above-mentioned multilayer tube, due to long-term exposure to high temperatures, there is a tendency for degradation to proceed due to oxygen in the air. In order to suppress such degradation, a technology of using a specific amount of an antioxidant and a conjugated polyene compound in combination is known (for example, see Patent Document 2).

[0649] In addition, agricultural materials (silage films, mulch films, etc.) tend to be easily degraded by oxygen in the air due to long-term outdoor use and exposure to sunlight, geothermal heat, wind and rain, etc. In order to suppress such degradation, it is known that a silage film with good weather resistance can be obtained by adding a specific amount of hindered amine compounds (for example, see Patent Document 3).

[0650] [Patent Document 1] Japanese Patent Application Laid-Open No. 63-286459

[0651] [Patent Document 2] International Publication No. 2011 / 125736

[0652] [Patent Document 3] Japanese Patent Application Publication No. 2014-172928

[0653] However, the methods of the above-mentioned patent documents are still insufficient for suppressing the above-mentioned degradation due to oxygen and the like.

[0654] In addition, in recent years, there is a trend of molding devices becoming more functional, with the diversification of the feed blocks and die shapes of molding devices, the thinning of multilayer structures in the final products, the increase in the number of layers, and other requirements for higher functionality. On the other hand, the molding devices that have become more complex due to higher functionality tend to have thermal degradation and coloration of the resin, which may reduce the productivity of the product, and further improvements are sought.

[0655] An object of the present invention is to provide an EVOH resin composition in which the color change of the EVOH resin during heating such as melt molding is suppressed.

[0656] [Methods to solve the problem]

[0657] However, in view of the above circumstances, the present inventors have found that an EVOH resin composition in which the color change of the EVOH resin during heating such as melt molding is suppressed can be obtained by adding an antioxidant and a specific trace amount of a titanium compound to the EVOH resin.

[0658] That is, the present invention has the following aspects.

[0659] [7-1] An EVOH resin composition comprising an EVOH resin, an antioxidant, and a titanium compound, wherein the metal-equivalent content of the titanium compound is 0.001 ppm or more and less than 5 ppm based on the mass of the EVOH resin composition.

[0660] [7-2] The EVOH resin composition according to [7-1], wherein the content of the antioxidant is 1 to 30,000 ppm based on the mass of the EVOH resin composition.

[0661] [7-3] The EVOH resin composition according to [7-1] or [7-2], wherein the mass ratio of the content of the antioxidant to the metal-equivalent content of the titanium compound is 0.2 to 30,000,000.

[0662] [7-4] A pellet comprising the EVOH resin composition according to any one of [7-1] to [7-3].

[0663] [7-5] A multilayer structure comprising at least one layer comprising the EVOH resin composition according to any one of [7-1] to [7-3].

[0664] [7-6] A tube comprising at least one layer comprising the EVOH resin composition according to any one of [7-1] to [7-3].

[0665] [7-7] A method for producing an EVOH resin composition, the method comprising producing the EVOH resin composition described in any one of [7-1] to [7-3].

[0666] The method comprises the step of melt-mixing a composition raw material containing the EVOH resin and the titanium compound.

[0667] [7-8] A method for producing a multilayer structure, which is a method for producing the multilayer structure described in [7-5],

[0668] The process comprises melt-molding the layer composed of the EVOH resin composition.

[0669] [Effects of the Invention]

[0670] The EVOH resin composition of the present invention can suppress the color change of the EVOH resin during melt molding and has excellent long-term operating properties. [Specific implementation method]

[0672] Hereinafter, the present invention will be described in more detail based on the embodiments of the present invention, but the present invention is not limited to these embodiments.

[0673] <EVOH resin composition>

[0674] The EVOH resin composition according to one embodiment of the present invention (hereinafter referred to as "the present EVOH resin composition") contains EVOH resin as a main component and an antioxidant and a specific trace amount of a titanium compound.

[0675] That is, the base resin in the present EVOH resin composition is EVOH resin, and the content of EVOH resin in the present EVOH resin composition is usually 70 mass % or more, preferably 80 mass % or more, more preferably 90 mass % or more, particularly preferably 95 mass % or more.

[0676] Hereinafter, each component will be described.

[0677] [EVOH resin]

[0678] The EVOH resin used in the present invention is generally a resin obtained by saponifying an ethylene-vinyl ester copolymer which is a copolymer of ethylene and a vinyl ester monomer, and the same EVOH resin as described in the first embodiment can be used.

[0679] [Antioxidant]

[0680] The antioxidant does not include quinone compounds and compounds having a conjugated polyene structure. Other than these, any compound having a function of capturing free radicals generated by resin deterioration is not particularly limited, and various antioxidants for resins can be used.

[0681] The melting point of the antioxidant is usually 200° C. or less, preferably 170° C. or less. The lower limit of the melting point of the antioxidant is usually 30° C. If the melting point of the antioxidant is too high, the antioxidant will not melt in the extruder, so the antioxidant will be localized in the molded product, and the quality tends to be reduced.

[0682] The molecular weight of the antioxidant is usually 100 to 8000, preferably 200 to 6000, and particularly preferably 300 to 4000. When the molecular weight of the antioxidant is too low, the antioxidant tends to ooze out from the surface of the obtained molded product, and when the molecular weight is too high, the antioxidant tends to be localized in the molded product, and the quality tends to be reduced.

[0683] As the above-mentioned antioxidant, for example, hindered phenol antioxidants, phosphite antioxidants, thioether antioxidants, hindered amine antioxidants, benzotriazole antioxidants, diphenyl ketone antioxidants, etc. can be mentioned. These can be used alone or in combination of two or more. Among them, considering the excellent effect of degradation resistance, hindered phenol antioxidants and hindered amine antioxidants are preferred, and hindered phenol antioxidants are particularly preferred.

[0684] The hindered phenol antioxidant itself has excellent thermal stability and has the ability to capture oxygen radicals, which are the cause of oxidative degradation. When it is added as an antioxidant to an EVOH resin composition, it has an excellent effect of preventing oxidative degradation.

[0685] In addition, the hindered amine antioxidant not only has the effect of preventing the thermal degradation of the EVOH resin, but also has the effect of capturing aldehydes generated by the thermal decomposition of the EVOH resin, thereby reducing the generation of decomposition gas, thereby inhibiting the generation of bubbles during molding. Furthermore, by capturing aldehydes, when the EVOH resin composition is used as a food packaging container material, for example, the problem of the odor of aldehydes damaging the taste of the contents can be improved.

[0686] Examples of the hindered phenol antioxidant include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] ("IRGANOX 1010" manufactured by BASF: melting point 110 to 125°C, molecular weight 1178), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate ("IRGANOX 1076" manufactured by BASF: melting point 50 to 55°C, molecular weight 531), N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide] ("IRGANOX 1098" manufactured by BASF: melting point 156 to 161°C, molecular weight 637), triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate] ("IRGANOX 1098" manufactured by BASF: melting point 156 to 161°C, molecular weight 637), and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate. 245": melting point 76-79°C, molecular weight 587), 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] ("IRGANOX 259" manufactured by BASF: melting point 104-108°C, molecular weight 639), 2,2'-methylene-bis(4-methyl-6-tert-butylphenol) ("Sumilizer MDP-s" manufactured by Sumitomo Chemical: melting point about 128°C, molecular weight 341), 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate ("Sumilizer GM": melting point of about 128°C, molecular weight 395), 3,9-bis[2-{3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane (Sumitomo Chemical Co., Ltd. "Sumilizer GA-80": melting point of about 110°C, molecular weight 741), etc. Among them, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] is preferred from the viewpoint of excellent degradation resistance.

[0687] As the hindered amine antioxidant, preferably a piperidine derivative is used. In particular, a 2,2,6,6-tetraalkylpiperidine derivative having a substituent at position 4 is preferably used. Examples of the substituent at position 4 include a carboxyl group, an alkoxy group, and an alkylamino group.

[0688] In the above-mentioned hindered amine antioxidant, the N position of the hindered amine group may be substituted with an alkyl group, but it is more preferable to use a hindered amine antioxidant having a hydrogen atom bond from the viewpoint of excellent thermal stabilization effect.

[0689] Examples of the hindered amine antioxidant include bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (“TINUVIN 770” manufactured by BASF: melting point 81-85° C., molecular weight 481), bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate and 1,2,2,6,6-pentamethyl-4-piperidinyl sebacate (mixture) (“TINUVIN 765” manufactured by BASF: liquid compound, molecular weight 509), dimethyl succinate·1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate (“TINUVIN 765” manufactured by BASF: liquid compound, molecular weight 509), 622LD": melting point 55-70°C, molecular weight 3100-4000), N,N'-bis(3-aminopropyl)ethylenediamine·2,4-bis[N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidinyl)amino]-6-chloro-1,3,5-triazine condensate (BASF "CHIMASSORB 119FL": melting point 130-140°C, molecular weight 2000 or more), poly[[6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]hexamethylene[(2,2,6,6-tetramethyl-4-piperidinyl)imino]] (BASF "CHIMASSORB 944LD": melting point 100-135°C, molecular weight 2000-3100), bis(1,2,2,6,6-pentamethyl-4-piperidinyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butylmalonate (BASF "TINUVIN 144": melting point 146-150°C, molecular weight 685), N,N'-1,6-hexanediylbis{N-(2,2,6,6-tetramethyl-4-piperidinyl)-formamide} (BASF "UVINUL 4050H": melting point 157°C, molecular weight 450), BASF "UVINUL 5050H" (melting point 104-112°C, molecular weight about 3500), etc.

[0690] The antioxidant may be in any form such as powder, granule, liquid, paste, or emulsion.

[0691] The content of the antioxidant is preferably 1 to 30,000 ppm, more preferably 100 to 10,000 ppm, particularly preferably 1,000 to 5,000 ppm, and even more preferably 2,000 to 4,000 ppm relative to the mass of the EVOH resin composition. If the content is too small, the degradation resistance tends to decrease, and if the content is too large, the antioxidant tends to ooze out from the surface of the molded product.

[0692] When two or more antioxidants having different structures, compositions, molecular weights, etc. are used in combination, the total mass (total content) thereof may be within the above range.

[0693] The content of the above antioxidant can be measured in the following manner. First, the EVOH resin composition is freeze-pulverized, and 1 g of the obtained sample is extracted with an extraction solvent. The extract is fixed to volume and measured using a liquid chromatography-ultraviolet spectrophotometer. A calibration curve can be prepared from a standard solution of the antioxidant, and the content of the antioxidant can be quantified using the absolute calibration curve method.

[0694] [Titanium compounds]

[0695] Examples of the titanium compound include inorganic titanium compounds and organic titanium compounds. As the titanium compound, the same titanium compound as that described in the first embodiment can be used.

[0696] The metal conversion content of the titanium compound is greater than 0.001ppm and less than 5ppm relative to the mass of the EVOH resin composition. It is preferably 0.01 to 3ppm, more preferably 0.03 to 1ppm, and particularly preferably 0.05 to 0.5ppm. By making the metal conversion content of the titanium compound within the above range, the color change caused by thermal degradation during melt molding can be suppressed, and long-term operation performance is excellent. In addition, if the metal conversion content of the titanium compound is too small, the effect of suppressing color change is reduced, and if the metal conversion content is too much, thermal decomposition of the EVOH resin becomes easy to occur, and it is easy to color.

[0697] The metal conversion content of the above-mentioned titanium compound can be obtained by measuring the EVOH resin composition into a platinum crucible, ashing it with a burner and an electric furnace in sequence, heating and decomposing the ashed material with nitric acid and hydrofluoric acid, treating it with a mixed acid of dilute nitric acid and dilute hydrofluoric acid and fixing the volume, and quantitatively measuring the titanium in the obtained fixed volume solution by ICP mass spectrometry using an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800).

[0698] The mass ratio of the content of the antioxidant to the metal-converted content of the titanium compound [the content of the antioxidant / the metal-converted content of the titanium compound] is preferably 0.2 to 30,000,000, more preferably 0.3 to 3,000,000, more preferably 100 to 300,000, particularly preferably 500 to 100,000, even more preferably 2,000 to 80,000, and most preferably 5,000 to 50,000. If the mass ratio is too large, the thermal stability tends to decrease, and if it is too small, the molded product tends to be colored.

[0699] Generally speaking, EVOH resin will be colored due to thermal degradation. It is believed that this is because the thermal degradation of EVOH resin generates free radicals, and these free radicals dehydrate the hydroxyl groups of EVOH resin, forming double bonds in the main chain of EVOH resin. This site becomes the starting point of the reaction, further promoting dehydration and forming a conjugated polyene structure in the main chain of EVOH resin.

[0700] On the other hand, the present EVOH resin composition contains an antioxidant and a specific trace amount of a titanium compound, so that the color change of the EVOH resin due to thermal degradation is suppressed and the long-term operating performance is excellent.

[0701] Generally, when an EVOH resin composition contains a titanium compound, it is believed that the EVOH resin composition is colored due to titanium ions, so it is common knowledge for those skilled in the art to avoid using titanium compounds. However, contrary to such common knowledge, the present invention has found that when a specific trace amount of a titanium compound is used, an EVOH resin composition in which color change due to thermal degradation is suppressed can be obtained.

[0702] That is, it is presumed that the tetravalent ion form of titanium is stable and even a trace amount thereof coordinates to the double bonds of the main chain of the EVOH resin described above to form a chelate complex or the like, thereby stabilizing and suppressing the formation of a polyene structure.

[0703] On the other hand, if the content of the titanium compound is too large, it is considered that thermal decomposition of the EVOH resin by the titanium compound occurs, resulting in coloration.

[0704] [Other thermoplastic resins]

[0705] The present EVOH resin composition may contain a thermoplastic resin other than EVOH resin within a range not impairing the effects of the present invention (for example, generally 30% by mass or less, preferably 20% by mass or less, particularly preferably 10% by mass or less of the present EVOH resin composition).

[0706] As other thermoplastic resins, known thermoplastic resins can be used, for example, polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, ionomers, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0707] [Other compounding ingredients]

[0708] The EVOH resin composition may contain a compounding agent generally compounded in EVOH resin within a range not hindering the effects of the present invention. As the compounding agent, the same compounding agent as described in the first embodiment can be used.

[0709] [Method for producing EVOH resin composition]

[0710] The present EVOH resin composition can be prepared, for example, by mixing the above-mentioned EVOH resin, antioxidant and titanium compound by a known method, such as dry blending, melt blending, solution blending, impregnation, etc. Among these, it is preferably prepared by a process of melt blending the composition raw materials containing the above-mentioned EVOH resin and titanium compound. In addition, these manufacturing methods can also be arbitrarily combined.

[0711] Examples of the dry blending method include (i) a method of dry blending a pelletized EVOH resin with an antioxidant and / or a titanium compound using a tumbler or the like.

[0712] Examples of the melt mixing method include (ii) a method of melt kneading a dry blend of EVOH resin in pellet form with an antioxidant and / or a titanium compound; and (iii) a method of adding an antioxidant and / or a titanium compound to EVOH resin in a molten state and melt kneading the mixture.

[0713] Examples of the solution mixing method include (iv) a method in which a solution is prepared using a commercially available EVOH resin, an antioxidant and / or a titanium compound is added thereto, the solution is solidified into a shape, and then the solution is separated into a solid and a liquid and dried by known means; (v) a method in which, during the manufacture of the EVOH resin, an ethylene-vinyl ester copolymer solution before saponification or a uniform solution of the EVOH resin (water / alcohol solution, etc.) is made to contain an antioxidant and / or a titanium compound, the solution is solidified into a shape, and then the solution is separated into a solid and a liquid and dried by known means.

[0714] Examples of the impregnation method include (vi) a method of bringing pelletized EVOH resin into contact with an aqueous solution containing an antioxidant and / or a titanium compound to allow the EVOH resin to contain the antioxidant and / or the titanium compound, followed by drying.

[0715] As the aqueous solution containing a titanium compound, an aqueous solution of a titanium compound or an aqueous solution obtained by immersing a titanium compound in water containing various chemicals to dissolve titanium ions can be used.

[0716] In the above impregnation method, the content (metal conversion) of the antioxidant and the titanium compound can be controlled by the concentration of the antioxidant and the titanium compound in the aqueous solution for impregnating the EVOH resin, the impregnation temperature, the impregnation time, and the like.

[0717] The immersion temperature and immersion time are usually 0.5 to 48 hours, preferably 1 to 36 hours, and the immersion temperature is usually 10 to 40°C, preferably 20 to 35°C.

[0718] The drying method in each of the above-mentioned production methods can adopt various drying methods, and can be any of static drying and fluidized drying. In addition, these methods can also be combined.

[0719] As described above, the above different methods can be combined in the present invention. Among them, considering productivity and the viewpoint of obtaining a resin composition with more significant effects of the present invention, the melt mixing method is preferred, and the method (ii) is particularly preferred. In addition, when using the above other thermoplastic resins and other compounding ingredients, they can be compounded in a conventional manner according to the above manufacturing method.

[0720] The present EVOH resin composition obtained by the above-mentioned respective production methods may be in any shape, but is preferably in the form of pellets.

[0721] The pellets may be spherical, elliptical, cylindrical, cubic, or rectangular, and are usually elliptical or cylindrical. Considering the convenience of using the pellets as molding materials, the pellets are usually 1 to 10 mm in diameter, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm in diameter, and usually 1.5 to 30 mm in diameter, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm in diameter, in the case of elliptical pellets. In the case of cylindrical pellets, the bottom diameter is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm.

[0722] In addition, the shape and size of the pelletized EVOH resin used in each of the above-mentioned production methods are also preferably the same.

[0723] Even when the EVOH resin composition is heated during melt molding, the color change is still suppressed, and the long-term operation is excellent. The ratio of the YI value after heating to the YI value (yellow index) before heating (YI value after heating / YI value before heating) is usually 4.1 or less, preferably 4.0 or less, and more preferably 3.7 or less. If the ratio of the YI value after heating to the YI value before heating is within the above range, there is a tendency to further suppress coloring. It should be noted that the lower limit of the ratio of the YI value after heating to the YI value before heating is usually 1.

[0724] In addition, even a difference of 0.1 in the ratio of the above-mentioned YI values ​​will show a significant difference in yield in actual production, and therefore the difference is very large.

[0725] The YI value before heating is obtained by grinding the EVOH resin composition into 1 to 5 mm square pieces, filling the ground product into a cylinder with an inner diameter of 32 mm and a height of 30 mm, and then scraping off the ground product. In this state, the YI value is measured using a spectrocolorimeter SE6000 (manufactured by Nippon Denshoku Industries Co., Ltd.).

[0726] The YI value after heating is obtained by heating the EVOH resin composition crushed into 1 to 5 mm square pieces in an oven under air atmosphere at 150°C for 5 hours and then measuring the same method.

[0727] The water content of the present EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0728] The water content of the EVOH resin composition is measured and calculated by the following method.

[0729] The mass (W1) of the EVOH resin composition before drying was weighed with an electronic balance, dried in a hot air dryer at 150°C for 5 hours, and the mass (W2) after cooling in the dryer for 30 minutes was weighed and calculated according to the following formula.

[0730] Water content (mass %) = [(W1-W2) / W1] × 100

[0731] In addition, when the EVOH resin composition is in the form of pellets, it is preferred to attach a known lubricant to the surface of the pellets from the viewpoint of stabilizing the feeding property during melt molding. Examples of lubricants include: higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters, etc. of higher fatty acids), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauramide, myristic acid, palmitic acid, stearic acid, behenic acid, etc.; unsaturated higher fatty acid amides such as oleamide and erucic acid, bis-higher fatty acid amides such as ethylene bisstearamide, ethylene bisoleamide, ethylene biserucic acid, ethylene bislauramide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene having a molecular weight of about 500 to 10,000, or low molecular weight polypropylene, etc., or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluorinated vinyl resins, etc. These compounds may be used alone or in combination of two or more. The content of the lubricant is usually 5% by mass or less, preferably 1% by mass or less, of the EVOH resin composition, and the lower limit is usually 0% by mass.

[0732] The EVOH resin composition thus obtained can be prepared into various forms such as pellets, powders, and liquids, and provided as molding materials for various molded products. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to obtain the effects of the present invention with better efficiency, which is preferred.

[0733] In addition, the present EVOH resin composition also includes a resin composition obtained by mixing a resin other than the EVOH resin used in the present EVOH resin composition.

[0734] The molded product is, for example, a multilayer structure having a layer composed of the present EVOH resin composition, such as a single-layer film molded from the present EVOH resin composition.

[0735] [Multilayer structure]

[0736] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present EVOH resin composition. The layer composed of the present EVOH resin composition (hereinafter referred to as "the present EVOH resin composition layer") can be further provided with strength, or the present EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating it with other substrates having a thermoplastic resin as a main component other than the present EVOH resin composition (hereinafter, the resin used in the substrate is sometimes referred to as "substrate resin").

[0737] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polybutene, polypentene, (unmodified) polyolefin resins including polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and these polyolefin resins. Modified olefin resins in a broad sense include polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by graft modification with unsaturated carboxylic acid or its ester, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, chlorinated polyethylene, chlorinated polypropylene and other halogenated polyolefins, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.

[0738] Among these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred as hydrophobic resins, and polyethylene resins, polypropylene resins, polycyclic olefin resins, and polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred.

[0739] When the EVOH resin composition layer is a (a1, a2, ...) and the substrate resin layer is b (b1, b2, ...), the layer structure of the multilayer structure can be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the recovered layer including the mixture of the EVOH resin composition and the thermoplastic resin other than the EVOH resin composition obtained by remelting and molding the end parts and defective products generated in the production process of the multilayer structure is taken as R, it can be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is usually 2 to 15 in total, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be inserted between the layers as needed.

[0740] As the above-mentioned adhesive resin, a known adhesive resin can be used, and it can be appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins by addition reaction, grafting reaction, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. They can be used alone or in combination of two or more.

[0741] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present EVOH resin composition layer, it is preferred to use an adhesive resin having excellent hydrophobicity.

[0742] The above-mentioned base resin and adhesive resin may contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating materials, antiblocking agents, waxes, etc., within the range that does not hinder the gist of the present invention (for example, 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These can be used alone or in combination of two or more.

[0743] The lamination of the above-mentioned EVOH resin composition layer and the above-mentioned substrate resin layer (including the case where an adhesive resin layer is inserted) can be carried out according to a known method. For example: a method of melt-extrusion laminating the substrate resin on a film, sheet, etc. of the present EVOH resin composition, a method of melt-extrusion laminating the present EVOH resin composition on a substrate resin layer, a method of co-extruding the present EVOH resin composition and the substrate resin, a method of dry laminating the present EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc., a method of applying a solution of the present EVOH resin composition on the substrate resin and then removing the solvent, etc. Among these, considering the viewpoints of cost and environment, it is preferred to manufacture by a process of melting the present EVOH resin composition layer, and specifically, a co-extrusion method is preferred.

[0744] The present multilayer structure may also be subjected to (heating) stretching treatment as required. The stretching treatment may be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, the stretching may be performed simultaneously or sequentially. In addition, the stretching method may be a method with a higher stretching ratio such as a roller stretching method, a tenter stretching method, a belt stretching method, a stretch blow molding method, and a vacuum pressure molding method. The stretching temperature is a temperature near the melting point of the multilayer structure, and is selected from a range of usually 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is too low, the stretchability is poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0745] In addition, the multilayer structure after the stretching treatment may be heat-fixed in order to impart dimensional stability. Heat-fixing may be performed by known means, for example, the multilayer structure after the stretching treatment is maintained in a tensile state and heat-treated at a temperature of usually 80 to 180° C., preferably 100 to 165° C., for usually 2 to 600 seconds.

[0746] When the stretched multilayer structure is used as a shrink film, in order to impart heat shrinkage, the stretched multilayer structure may be cooled and fixed by blowing cold air instead of the heat setting.

[0747] The thickness of the present multilayer structure (including the stretched multilayer structure), and further the thickness of the present EVOH resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure, depends on the layer constitution, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., and cannot be generalized, but the thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0748] Furthermore, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the substrate resin layer (present EVOH resin composition layer / substrate resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, calculated as the ratio of the thickest layers. In addition, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer (present EVOH resin composition layer / adhesive resin layer) is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10, calculated as the ratio of the thickest layers.

[0749] In addition, the present multilayer structure can be used to obtain a cup or tray-shaped multilayer container. In this case, a pull molding method is usually used, and specifically, for example, vacuum molding, pressure molding, vacuum pressure molding, plug-assisted vacuum pressure molding, etc. can be cited. Furthermore, when a tubular or bottle-shaped multilayer container (laminated structure) is obtained from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, for example, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulation type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion type cold parison biaxial stretch blow molding, injection type cold parison biaxial stretch blow molding, injection molding online biaxial stretch blow molding, etc.), etc. The obtained laminate can be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, deep drawing processing, box processing, tube processing, splitting processing, etc. as needed.

[0750] The monolayer film formed from the present EVOH resin composition, the containers and covers composed of bags, cups, trays, tubes, bottles, etc. composed of the present multilayer structure are useful as various packaging material containers for general foods, seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, pharmaceuticals, etc. Furthermore, the layer composed of the present EVOH resin composition has excellent resistance to degradation, and is therefore particularly useful as agricultural materials such as silage films and multilayer films.

[0751] [Multilayer tube]

[0752] A multilayer tube according to one embodiment of the present invention (hereinafter referred to as "the present multilayer tube") is a tube having a multilayer structure of the present EVOH resin composition layer. The present EVOH resin composition layer can be further provided with strength, or the present EVOH resin composition layer can be protected from moisture or the like, or other functions can be provided by laminating with a layer composed of another resin composition having a resin other than the present EVOH resin composition as a main component.

[0753] In the present multilayer tube, the present EVOH resin composition layer constituting the present multilayer tube has EVOH resin as a main component, and thus has excellent gas barrier properties. In addition, even if the present multilayer tube is exposed to high temperature for a long time, since the present EVOH resin composition layer has excellent resistance to degradation, even if the multilayer tube is used at high temperature for a long time, the generation of cracks in the present EVOH resin composition layer due to oxidation degradation can be suppressed. Due to such characteristics, the present multilayer tube is suitable for use as, for example, a warm water circulation pipe and a heat-insulating multilayer pipe for regional cooling and heating rooms.

[0754] The layer structure of the present multilayer tube can adopt the layer structure of the above-mentioned multilayer structure. When the present multilayer tube is used as, for example, a warm water circulation tube, a three-layer multilayer tube having a layer structure of the present EVOH resin composition layer / adhesive resin layer / thermoplastic resin layer is generally used, wherein the outermost layer is the present EVOH resin composition layer, the middle layer is a layer formed of an adhesive resin, and the innermost layer is a layer formed of a thermoplastic resin.

[0755] Examples of the thermoplastic resin include polyolefins such as polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, etc. Among them, polyethylene is preferred, and high-density polyethylene is particularly preferred.

[0756] In addition, examples of the adhesive resin include, similarly to the adhesive resin used in the multilayer structure, carboxyl group-containing modified polyolefin polymers obtained by chemically bonding unsaturated carboxylic acid or its anhydride to a polyolefin resin by addition reaction, graft reaction, etc.

[0757] When the multilayer tube is used as a hot water circulation tube such as a floor heating tube, it is preferable to arrange the EVOH resin composition layer as the outermost layer from the viewpoint of gas barrier properties as described above. That is, the multilayer tube is advantageous from the viewpoint of barrier properties as a multilayer tube by arranging the EVOH resin composition layer having excellent gas barrier properties and also excellent degradation resistance as the outermost layer.

[0758] Furthermore, the present multilayer tube uses the present EVOH resin composition having excellent long-term operating properties as a molding material for the outermost layer in direct contact with air, and therefore can be a multilayer tube having excellent barrier properties and in which cracking due to oxidative degradation is suppressed.

[0759] Next, a method for producing the multilayer tube of the present invention will be described.

[0760] The present multilayer tube can be produced by, for example, coextrusion coating the present EVOH resin composition and the adhesive resin on the outer peripheral surface of a single-layer tube composed of a thermoplastic resin such as a cross-linked polyolefin. When the present EVOH resin composition and the adhesive resin are coextrusion coated on the outer peripheral surface of the above-mentioned single-layer tube, a film of the present EVOH resin composition and the adhesive resin melted can be simply coated on the outer peripheral surface of the single-layer tube, but sometimes the adhesion between the above-mentioned single-layer tube and the coating layer is insufficient, and there is a possibility that the coating layer will peel off and lose the gas barrier property when used for a long period of time. In this way, before coextrusion coating, it is preferred to preliminarily treat the outer peripheral surface of the single-layer tube with a flame treatment and / or a corona discharge treatment.

[0761] As another multilayer molding method for manufacturing the multilayer tube, for example, there can be cited a method of manufacturing by using extruders of a number corresponding to the types (number of layers) of the layer molding materials, and simultaneously extruding and molding the molten layer molding materials in a flowing layer state in the overlapping extruders, i.e., so-called co-extrusion molding. In addition, a multilayer molding method such as dry lamination can also be used.

[0762] The method for producing the multilayer tube preferably includes a step of cooling with water at 10 to 70° C. immediately after molding. That is, the EVOH resin composition layer is preferably solidified by cooling with water at 10 to 70° C. after melt molding and before solidification of the EVOH resin composition layer.

[0763] The temperature of the cooling water is preferably 15 to 60° C., particularly preferably 20 to 50° C. If the temperature of the cooling water is too low, when the multilayer tube is bent in the subsequent secondary processing step, the EVOH resin composition layer may be prone to cracking due to strain at the bent portion. In addition, if the temperature of the cooling water is too high, the EVOH resin composition layer may be prone to cracking due to strain at the bent portion during the secondary processing.

[0764] The multilayer tube obtained by the above method can be subjected to secondary processing to obtain various molded bodies. There is no particular limitation on the secondary processing method, and a known secondary processing method can be used appropriately. For example, a method in which the multilayer tube is heated to 80 to 160° C. and fixed for 1 minute to 2 hours in a state of being deformed into a desired shape, and then processed.

[0765] Since the multilayer tube has the EVOH resin composition layer, it is excellent in degradation resistance and is therefore particularly useful as a warm water circulation tube or the like.

[0766] <<Method 8>>

[0767] EVOH resin has excellent transparency, oxygen and other gas barrier properties, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and is molded into films, sheets, bottles, etc. and widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials.

[0768] However, EVOH resin has a relatively active hydroxyl group in the molecule and tends to be easily degraded by heat, and is prone to coloring during melt molding.

[0769] In order to solve the above-mentioned problems, for example, Patent Document 1 discloses that EVOH resin may contain an unsaturated aldehyde to suppress oxidative degradation during melt molding and thereby suppress coloration.

[0770] [Patent Document 1] International Publication No. 2013 / 146961

[0771] However, even a trace amount of aldehyde compounds such as the above-mentioned unsaturated aldehydes may sometimes cause bad odors, and they may volatilize in particular in a molding process exposed to high temperatures, and there is a concern that the working environment may deteriorate. In addition, the improvement effects on long-term operation moldability such as color suppression during heating such as melt kneading and melt molding cannot be said to be sufficient. Therefore, there is an urgent need for an EVOH resin composition that can suppress color changes during heating without deteriorating the working environment and can obtain high-quality molded products.

[0772] An object of the present invention is to provide an EVOH resin composition in which the color change of the EVOH resin during heating such as melt molding is suppressed.

[0773] [Methods to solve the problem]

[0774] However, the present inventors have found that, in view of the above circumstances, by adding a styrene derivative and a specific trace amount of a titanium compound to an EVOH resin, an EVOH resin composition can be obtained in which the color change of the EVOH resin during heating such as melt molding is suppressed.

[0775] That is, the present invention has the following aspects.

[0776] [8-1] An EVOH resin composition comprising an EVOH resin (A), a styrene derivative (B) and a titanium compound (C), wherein the metal-equivalent content of the titanium compound (C) is 0.001 ppm or more and less than 5 ppm relative to the mass of the EVOH resin composition.

[0777] [8-2] The EVOH resin composition according to [8-1], wherein the content of the styrene derivative (B) is 1 to 1000 ppm based on the mass of the EVOH resin composition.

[0778] [8-3] The EVOH resin composition according to [8-1] or [8-2], wherein the mass ratio of the content of the styrene derivative (B) to the metal-equivalent content of the titanium compound (C) is 0.3 to 100,000.

[0779] [8-4] The EVOH resin composition according to any one of [8-1] to [8-3], wherein the styrene derivative (B) is a cinnamic acid derivative.

[0780] [8-5] A pellet comprising the EVOH resin composition according to any one of [8-1] to [8-4].

[0781] [8-6] A multilayer structure comprising at least one layer comprising the EVOH resin composition according to any one of [8-1] to [8-4].

[0782] [8-7] A method for producing an EVOH resin composition, the method being a method for producing the EVOH resin composition described in any one of [8-1] to [8-4],

[0783] The method comprises the step of melt-mixing a composition raw material containing the EVOH resin and the titanium compound.

[0784] [8-8] A method for producing a multilayer structure, which is a method for producing the multilayer structure described in [8-6],

[0785] The process comprises melt-molding the layer composed of the EVOH resin composition.

[0786] [Effects of the Invention]

[0787] The EVOH resin composition of the present invention has excellent thermal stability, can suppress the color change of the EVOH resin during heating such as melt molding, and has excellent long-term operating properties. [Specific implementation method]

[0789] Hereinafter, the present invention will be described in more detail based on the embodiments of the present invention, but the present invention is not limited to these embodiments.

[0790] <EVOH resin composition>

[0791] The EVOH resin composition according to one embodiment of the present invention (hereinafter referred to as "the present EVOH resin composition") contains EVOH resin as a main component and a styrene derivative and a specific trace amount of a titanium compound.

[0792] That is, the base resin in the present EVOH resin composition is EVOH resin, and the content of EVOH resin in the present EVOH resin composition is usually 70 mass % or more, preferably 80 mass % or more, more preferably 90 mass % or more, particularly preferably 95 mass % or more.

[0793] Hereinafter, each component will be described.

[0794] [EVOH resin]

[0795] The EVOH resin (A) used in the present invention is generally a resin obtained by saponifying a copolymer of ethylene and a vinyl ester monomer, that is, an ethylene-vinyl ester copolymer, and the same EVOH resin as described in the first embodiment can be used.

[0796] [Styrene derivatives]

[0797] Examples of the styrene derivatives used in the present invention include various styrene derivatives having a styrene molecular structure as a molecular skeleton and a substituent at the α position and a substituent at the β position, among aromatic compounds having the ability to resonance stabilize and capture free radicals.

[0798] As the styrene derivative having a substituent at the α-position among the above-mentioned styrene derivatives, from the viewpoint of resonance stabilization of the free radical at the benzyl position, for example, a styrene compound having a substituent at the α-position such as 2,4-diphenyl-4-methyl-1-pentene is preferably mentioned.

[0799] In addition, the styrene derivative having a substituent at the β-position is preferably a styrene compound having a carbonyl group at the β-position, for example, cinnamic acid derivatives such as cinnamic acid, cinnamic alcohol, cinnamic acid esters, and cinnamic acid salts, from the viewpoint of having an enone structure and resonance stabilization of the free radical.

[0800] It should be noted that in the present EVOH resin composition, as the above-mentioned styrene derivative, it is preferred to use a styrene derivative without a substituent at the α position as compared to a styrene derivative with a substituent at the α position, because the coloration suppression effect is more excellent. It is particularly preferred to use a styrene derivative with a substituent at the β position, and among them, a cinnamic acid derivative is preferred. Moreover, among the cinnamic acid derivatives, cinnamic acid is the most preferred from the viewpoint of effect.

[0801] The molecular weight of the styrene derivative is usually 100 to 100,000, preferably 100 to 10,000, particularly preferably 100 to 1,000, and particularly preferably 130 to 300. When the molecular weight is within the above range, the effects of the present invention tend to be more effectively obtained.

[0802] The content of the styrene derivative is preferably 1 to 1000 ppm, more preferably 10 to 800 ppm, particularly preferably 50 to 700 ppm, and even more particularly preferably 200 to 650 ppm relative to the mass of the EVOH resin composition. If the content is too high, productivity tends to decrease, and if the content is too low, thermal stability decreases and the coloration suppression effect tends to decrease.

[0803] The EVOH resin composition serving as a basis for the content ratio of the styrene derivative is an EVOH resin composition as a final product containing EVOH resin, a styrene derivative, a titanium compound, and various additives blended as necessary.

[0804] The content of the styrene derivative in the EVOH resin composition of the present invention can be measured by, for example, liquid chromatography-mass spectrometry (LC / MS / MS) according to the following procedure. It should be noted that the following procedure is described using cinnamic acid as an example, but other styrene derivatives (B) can also be measured by the same procedure.

[0805] <Method for determining the content of styrene derivatives>

[0806] [Preparation of standard solution]

[0807] Weigh cinnamic acid (10.89 mg) into a 10 mL volumetric flask and dissolve in methanol to make a 10 mL solution (standard stock solution; 1089 μg / mL). Then, dilute the prepared standard stock solution with methanol to prepare mixed standard solutions of multiple concentrations (0.109 μg / mL, 0.218 μg / mL, 0.545 μg / mL, 1.09 μg / mL, 2.18 μg / mL). Use these mixed standard solutions to perform LC / MS / MS analysis and create a calibration curve.

[0808] [Preparation of sample solution]

[0809] (1) Pellets (1 g) of the pulverized EVOH resin composition of the present invention were weighed into a 10 mL volumetric flask, and 9 mL of methanol was added.

[0810] (2) After ultrasonic treatment for 120 minutes, the mixture was allowed to cool at room temperature (25°C).

[0811] (3) Add methanol to adjust the volume to 10 mL (sample solution (I)).

[0812] (4) After sampling 1 mL of the sample solution (I) into a 10 mL volumetric flask, methanol was added to adjust the volume to 10 mL (sample solution (II)).

[0813] (5) After the sample solution (I) or the sample solution (II) is filtered through a PTFE filter membrane (0.45 μm), the filtrate is used as a measurement solution for LC / MS / MS analysis.

[0814] The detection concentration of cinnamic acid was calculated from the peak area value detected by LC / MS / MS analysis and the calibration curve of the standard solution.

[0815] [LC / MS / MS measurement conditions]

[0816] LC system: LC-20A [manufactured by Shimadzu Corporation]

[0817] Mass spectrometer: API4000 [AB / MDS Sciex]

[0818] Analytical column: Scherzo SM-C18 (3.0×75mm, 3μm)

[0819] Column temperature: 45℃

[0820] Mobile phase: A 10mmol / L ammonium acetate aqueous solution

[0821] B Methanol

[0822] Time program:

[0823] 0.0→5.0 minutes B%=30%→95%

[0824] 5.0→10.0 minutes B%=95%

[0825] 10.1→15.0 minutes B%=30%

[0826] Flow rate: 0.4mL / min

[0827] Switching valve: 2.0 to 6.0 minutes: to MS

[0828] Injection volume: 5μL

[0829] Ionization: ESI method

[0830] Detection: Negative ion detection (SRM method)

[0831] Monitor ions: Q1 = 147.0 → Q3 = 102.9 (CE: -15 eV)

[0832] [Titanium compounds]

[0833] Examples of the titanium compound used in the present invention include inorganic titanium compounds and organic titanium compounds. As the titanium compound, the same titanium compound as that described in the first embodiment can be used.

[0834] The metal conversion content of the titanium compound (C) is greater than 0.001ppm and less than 5ppm relative to the mass of the EVOH resin composition. It is preferably 0.01 to 3ppm, more preferably 0.03 to 1ppm, and particularly preferably 0.05 to 0.5ppm. By making the metal conversion content of the titanium compound (C) within the above range, thermal degradation during melt molding can be suppressed, and long-term operation performance is excellent. In addition, if the metal conversion content of the titanium compound (C) is too little, the effect of suppressing thermal degradation is reduced, and if the metal conversion content is too much, thermal decomposition of the EVOH resin is likely to occur, and there is a tendency to be easily colored.

[0835] The metal conversion content of the above-mentioned titanium compound (C) can be obtained by weighing the EVOH resin composition into a platinum crucible, ashing it with a burner and an electric furnace in sequence, heating and decomposing the ashed material with nitric acid and hydrofluoric acid, treating it with a mixed acid of dilute nitric acid and dilute hydrofluoric acid and fixing the volume, and quantitatively measuring the titanium in the obtained fixed volume solution by ICP mass spectrometry using an ICP mass spectrometer (manufactured by Agilent Technologies, Agilent 8800).

[0836] The mass ratio of the content of the styrene derivative (B) to the metal conversion content of the titanium compound (C) is preferably 0.3 to 100,000, more preferably 10 to 30,000, particularly preferably 100 to 12,000, even more preferably 300 to 10,000, and most preferably 600 to 8,000.

[0837] When this value is too large, the ultraviolet absorption ability of the present EVOH resin composition tends to be reduced, and when it is too small, the molded product tends to be colored.

[0838] Here, it is generally known that EVOH resin will be colored due to thermal degradation. This can be considered as follows. It can be considered that: the EVOH resin deteriorates due to heat and generates free radicals, and the hydroxyl groups possessed by the EVOH resin undergo a dehydration reaction due to these free radicals, thereby generating a double bond structure in the main chain of the EVOH resin. Moreover, this site becomes the starting point of the reaction, further causing a dehydration reaction, etc., to form a polyene structure in the main chain of the EVOH resin.

[0839] Furthermore, generally, when an EVOH resin composition contains a titanium compound, it is considered that the EVOH resin composition is colored due to titanium ions, and therefore it is common knowledge for those skilled in the art to avoid using titanium compounds.

[0840] However, the present invention, contrary to such common technical knowledge, has found that when a styrene derivative (B) and a specific trace amount of a titanium compound (C) are used in combination, an EVOH resin composition in which thermal degradation is significantly suppressed and coloration is suppressed can be obtained.

[0841] That is, it is presumed that the tetravalent ion form of titanium is stable, and even if it is in a trace amount, it coordinates to the double bonds of the main chain of the EVOH resin as described above to form a chelate or the like to stabilize, thereby inhibiting the formation of a polyene structure. Furthermore, it is presumed that the stabilizing effect of the titanium compound (C) is more effectively exerted by the coexistence of the styrene derivative (B) and the titanium compound (C).

[0842] On the other hand, if the content of the titanium compound (C) is too high, thermal decomposition of the EVOH resin due to the titanium compound (C) may occur, resulting in coloration. Therefore, the content of the titanium compound (C) is limited to a specific trace amount in the present invention.

[0843] [Other thermoplastic resins]

[0844] The present EVOH resin composition may contain a thermoplastic resin other than the EVOH resin (A) within a range not impairing the effects of the present invention (for example, generally 30% by mass or less, preferably 20% by mass or less, particularly preferably 10% by mass or less of the present EVOH resin composition).

[0845] As other thermoplastic resins, known thermoplastic resins can be used, for example, polyester resins, polystyrene resins, polyvinyl chloride resins, polycarbonate resins, ionomers, polyvinylidene chloride, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0846] [Other compounding ingredients]

[0847] The EVOH resin composition may contain a compounding agent generally compounded in EVOH resin within a range not hindering the effects of the present invention. As the compounding agent, the same compounding agent as described in the first embodiment can be used.

[0848] [Method for producing EVOH resin composition]

[0849] The present EVOH resin composition can be produced, for example, by mixing the above-mentioned EVOH resin (A), styrene derivative (B) and titanium compound (C) by a known method, such as dry blending, melt mixing, solution mixing, impregnation, etc. Among these, it is preferably produced by a process of melt mixing the composition raw materials containing the above-mentioned EVOH resin and titanium compound. In addition, these production methods can also be arbitrarily combined.

[0850] Examples of the dry blending method include (i) a method of dry blending a pelletized EVOH resin (A) and a styrene derivative (B) and / or a titanium compound (C) using a tumbler or the like.

[0851] As the above-mentioned melt mixing method, for example, there can be cited (ii) a method in which a pelletized EVOH resin (A), a styrene derivative (B) and a titanium compound (C) are dry-mixed and melt-kneaded to obtain pellets or a molded product; (iii) a method in which a styrene derivative (B) and / or a titanium compound (C) are added to a molten EVOH resin (A) and melt-kneaded to obtain pellets or a molded product.

[0852] As the above-mentioned solution mixing method, for example, there can be cited the following method: (iv) a solution is prepared using a granular EVOH resin (A), a styrene derivative (B) and / or a titanium compound (C) is added thereto, the solution is solidified and granulated, and then the solid-liquid separation and drying are carried out by known means; (v) in the manufacturing process of the EVOH resin (A), a uniform solution of the EVOH resin before saponification (water / alcohol solution, etc.) is made to contain a styrene derivative (B) and / or a titanium compound (C), the solution is solidified and granulated, and then the solid-liquid separation and drying are carried out by known means, etc.

[0853] As the above-mentioned impregnation method, for example, there can be mentioned a method of (vi) contacting a pelletized EVOH resin (A) with an aqueous solution containing a styrene derivative (B) and / or a titanium compound (C), allowing the EVOH resin (A) to contain a styrene derivative (B) and / or a titanium compound (C), and then drying the mixture.

[0854] As the aqueous solution containing the titanium compound (C), an aqueous solution of the titanium compound (C) or an aqueous solution obtained by immersing the titanium compound (C) in water containing various chemicals to dissolve titanium ions can be used. The same applies to the aqueous solution containing the styrene derivative (B).

[0855] It should be noted that in the above-mentioned impregnation method, the content (metal conversion) of the styrene derivative (B) and the titanium compound (C) can be controlled by the concentration of the styrene derivative (B) and the titanium compound (C) in the aqueous solution in which the EVOH resin (A) is impregnated, the impregnation temperature, the impregnation time, etc.

[0856] The immersion temperature and immersion time are usually 0.5 to 48 hours, preferably 1 to 36 hours, and the immersion temperature is usually 10 to 40°C, preferably 20 to 35°C.

[0857] In addition, the drying method in each of the above-mentioned production methods can adopt various drying methods, and can be any of static drying and fluidized drying. In addition, these methods can also be combined.

[0858] As described above, in order to obtain the present EVOH resin composition, the above-mentioned various methods can be combined. Among them, considering the productivity and the viewpoint of obtaining a resin composition with more significant effects of the present invention, the melt mixing method is preferred, and the method (ii) is particularly preferred. In addition, when using the above-mentioned other thermoplastic resins and other compounding agents, they can be compounded in a conventional manner according to the above-mentioned manufacturing method.

[0859] The EVOH resin composition thus obtained may be in any shape, but is preferably in the form of pellets.

[0860] The pellets may be spherical, elliptical, cylindrical, cubic, or rectangular, and are usually elliptical or cylindrical. Considering the convenience of using the pellets as molding materials, the pellets are usually 1 to 10 mm in diameter, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm in diameter, and usually 1.5 to 30 mm in diameter, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm in diameter, in the case of elliptical pellets. In the case of cylindrical pellets, the bottom diameter is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm.

[0861] Furthermore, the shape and size of the pelletized EVOH resin (A) used in the above-mentioned respective production methods are also preferably the same.

[0862] It should be noted that when the EVOH resin composition is in the form of pellets, it is preferred to attach a known lubricant to the surface of the pellets from the viewpoint of stabilizing the feeding property during melt molding. Examples of the lubricant include: higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters, etc. of higher fatty acids), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauramide, myristic acid, palmitic acid, stearic acid, behenic acid, etc.; unsaturated higher fatty acid amides such as oleamide and erucic acid, bis-higher fatty acid amides such as ethylene bisstearamide, ethylene bisoleamide, ethylene biserucic acid, ethylene bislauramide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene having a molecular weight of about 500 to 10,000, or low molecular weight polypropylene, etc., or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluorinated vinyl resins, etc. These compounds may be used alone or in combination of two or more. The content of the lubricant is usually 5% by mass or less, preferably 1% by mass or less, of the EVOH resin composition, and the lower limit is usually 0% by mass.

[0863] The EVOH resin composition thus obtained has a color change that is suppressed even when heated during melt molding, etc., and has excellent long-term operability. The ratio of the YI value after heating to the YI value (yellow index) before heating (YI value after heating / YI value before heating) is usually less than 6.5, preferably less than 6.0, and particularly preferably less than 5.5. If the ratio of the YI value after heating to the YI value before heating is within the above range, the color suppression effect is excellent. In addition, the lower limit of the ratio of the YI value after heating to the YI value before heating is usually 1.

[0864] In addition, even a difference of 0.1 in the ratio of the above-mentioned YI values ​​will show a significant difference in yield in actual production, and therefore the difference is very large.

[0865] The YI value before heating is obtained by grinding the EVOH resin composition into 1 to 5 mm square pieces, filling the ground product into a cylinder with an inner diameter of 32 mm and a height of 30 mm, and then scraping off the ground product. In this state, the YI value is measured using a spectrocolorimeter SE6000 (manufactured by Nippon Denshoku Industries Co., Ltd.).

[0866] The YI value after heating is obtained by heating the EVOH resin composition crushed into 1 to 5 mm square pieces in an oven under air atmosphere at 150°C for 5 hours and then measuring the same method.

[0867] The water content of the present EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0868] The water content of the present EVOH resin composition is measured and calculated by the following method.

[0869] The mass (W1) of the EVOH resin composition before drying was weighed with an electronic balance, dried in a hot air dryer at 150°C for 5 hours, and the mass (W2) after cooling in the dryer for 30 minutes was weighed and calculated according to the following formula.

[0870] <Formula>

[0871] Water content (mass %) = [(W1-W2) / W1] × 100

[0872] In addition to being prepared into pellets, the EVOH resin composition can also be prepared into various forms such as powder and liquid, and provided as a molding material for various molded objects. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to obtain the effect of the present invention with better efficiency, which is preferred.

[0873] In addition, the present EVOH resin composition also includes a resin composition obtained by mixing a resin other than the EVOH resin (A) used in the present EVOH resin composition.

[0874] The molded product is, for example, a multilayer structure having a layer composed of the present EVOH resin composition, such as a single-layer film molded from the present EVOH resin composition.

[0875] [Multilayer structure]

[0876] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present EVOH resin composition. The layer composed of the present EVOH resin composition (hereinafter referred to as "the present EVOH resin composition layer") can be further provided with strength, or the present EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating it with other substrates having a thermoplastic resin as a main component other than the present EVOH resin composition (hereinafter, the resin used in the substrate is sometimes referred to as "substrate resin").

[0877] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polybutene, polypentene, (unmodified) polyolefin resins including polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and these polyolefin resins. Modified olefin resins in a broad sense include polyolefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by graft modification with unsaturated carboxylic acids or their esters, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, halogenated polyolefins such as chlorinated polyethylene and chlorinated polypropylene, and aromatic or aliphatic polyketones.

[0878] Among these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred as hydrophobic resins, and polyolefin resins such as polyethylene resins, polypropylene resins, polycyclic olefin resins, and unsaturated carboxylic acid-modified polyolefin resins thereof are more preferred; in particular, polycyclic olefin resins are preferably used as the hydrophobic resin.

[0879] When the EVOH resin composition layer is a (a1, a2, ...) and the substrate resin layer is b (b1, b2, ...), the layer structure of the multilayer structure can be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the recovered layer including the mixture of the EVOH resin composition and the thermoplastic resin other than the EVOH resin composition obtained by remelting and molding the end parts and defective products generated in the production process of the multilayer structure is taken as R, it can be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is usually 2 to 15 in total, preferably 3 to 10. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be inserted between the layers as needed.

[0880] As the above-mentioned adhesive resin, a known adhesive resin can be used, and it can be appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins by addition reaction, grafting reaction, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. They can be used alone or in combination of two or more.

[0881] In the present multilayer structure, when an adhesive resin layer is used between the present EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present EVOH resin composition layer, it is preferred to use an adhesive resin having excellent hydrophobicity.

[0882] The above-mentioned base resin and adhesive resin may contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating materials, antiblocking agents, waxes, etc., within the range that does not hinder the gist of the present invention (for example, 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These can be used alone or in combination of two or more.

[0883] The lamination of the above-mentioned EVOH resin composition layer and the above-mentioned substrate resin layer (including the case where an adhesive resin layer is inserted) can be carried out according to a known method. For example: a method of melt-extrusion laminating the substrate resin on a film, sheet, etc. of the present EVOH resin composition, a method of melt-extrusion laminating the present EVOH resin composition on a substrate resin layer, a method of co-extruding the present EVOH resin composition and the substrate resin, a method of dry laminating the present EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc., a method of applying a solution of the present EVOH resin composition on the substrate resin and then removing the solvent, etc. Among these, considering the viewpoints of cost and environment, it is preferred to manufacture by a process of melting the present EVOH resin composition layer, and specifically, a co-extrusion method is preferred.

[0884] The present multilayer structure may also be subjected to (heating) stretching treatment as required. The stretching treatment may be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, the stretching may be performed simultaneously or sequentially. In addition, the stretching method may be a method with a higher stretching ratio such as a roller stretching method, a tenter stretching method, a belt stretching method, a stretch blow molding method, and a vacuum pressure molding method. The stretching temperature is a temperature near the melting point of the multilayer structure, and is selected from a range of usually 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is too low, the stretchability is poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0885] In addition, the multilayer structure after the stretching treatment may be heat-fixed in order to impart dimensional stability. Heat-fixing may be performed by known means, for example, the multilayer structure after the stretching treatment is maintained in a tensile state and heat-treated at a temperature of usually 80 to 180° C., preferably 100 to 165° C., for usually 2 to 600 seconds.

[0886] When the stretched multilayer structure is used as a shrink film, in order to impart heat shrinkage, the stretched multilayer structure may be cooled and fixed by blowing cold air instead of the heat setting.

[0887] The thickness of the present multilayer structure (including the stretched multilayer structure), and further the thickness of the present EVOH resin composition layer, the base resin layer and the adhesive resin layer constituting the multilayer structure, depends on the layer constitution, the type of base resin, the type of adhesive resin, the application, the packaging form, the required physical properties, etc., and cannot be generalized, but the thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0888] Furthermore, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the substrate resin layer (present EVOH resin composition layer / substrate resin layer) is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60, calculated as the ratio of the thickest layers. In addition, in the present multilayer structure, when there are multiple layers, the thickness ratio of the present EVOH resin composition layer to the adhesive resin layer (present EVOH...

Claims

1. An ethylene-vinyl alcohol copolymer composition, comprising an ethylene-vinyl alcohol copolymer and a titanium compound; the ethylene structural unit content of the ethylene-vinyl alcohol copolymer is 20 to 60 mol%, and the metal conversion content of the titanium compound is greater than 0.001 ppm and less than 5 ppm relative to the mass of the ethylene-vinyl alcohol copolymer composition.

2. The ethylene-vinyl alcohol copolymer composition according to claim 1, wherein The invention further contains at least one selected from the group consisting of an alkaline earth metal compound, an alkali metal compound, a lubricant, a compound having a conjugated polyene structure, a boron compound, an antioxidant, and a styrene derivative.

3. The ethylene-vinyl alcohol copolymer composition according to claim 1, wherein The water content of the ethylene-vinyl alcohol copolymer composition is 1% by mass or less.

4. The ethylene-vinyl alcohol copolymer composition according to claim 2, wherein The metal conversion content of the alkaline earth metal compound is 0.1 to 500 ppm based on the mass of the ethylene-vinyl alcohol copolymer composition.

5. The ethylene-vinyl alcohol copolymer composition according to claim 2, wherein The metal conversion content of the alkali metal compound is 1 to 1000 ppm based on the mass of the ethylene-vinyl alcohol copolymer composition.

6. The ethylene-vinyl alcohol copolymer composition according to claim 2, wherein The content of the lubricant is 500 ppm or less based on the mass of the ethylene-vinyl alcohol copolymer composition.

7. The ethylene-vinyl alcohol copolymer composition according to claim 2, wherein The content of the compound having a conjugated polyene structure is 1 to 1000 ppm based on the mass of the ethylene-vinyl alcohol copolymer composition.

8. The ethylene-vinyl alcohol copolymer composition according to claim 2, wherein The boron-equivalent content of the boron compound is 5 to 400 ppm based on the mass of the ethylene-vinyl alcohol copolymer composition.

9. The ethylene-vinyl alcohol copolymer composition according to claim 2, wherein The content of the antioxidant is 1 to 30000 ppm based on the mass of the ethylene-vinyl alcohol copolymer composition.

10. The ethylene-vinyl alcohol copolymer composition according to claim 2, wherein The content of the styrene derivative is 1 to 1000 ppm based on the mass of the ethylene-vinyl alcohol copolymer composition.

11. A method for producing an ethylene-vinyl alcohol copolymer composition, the method comprising the step of melt-mixing raw materials of the ethylene-vinyl alcohol copolymer composition. 12 . Pellets comprising the ethylene-vinyl alcohol copolymer composition according to claim 1 . 13 . A multilayer structure comprising at least one layer comprising the ethylene-vinyl alcohol copolymer composition according to claim 1 .

14. A method for producing a multilayer structure, which is the method for producing a multilayer structure according to claim 13, comprising the step of melt-molding the layer composed of the ethylene-vinyl alcohol copolymer composition.

Citation Information

Patent Citations

  • Resin composition

    JP1988286459A

  • Resin composition and its laminate

    JP1999106592A

  • Silage film

    JP2014172928A

  • Resin composition, molded article, multilayered pipe and method for producing the same

    WO2011125736A1

  • Resin composition containing ethylene-vinyl alcohol copolymer

    WO2013146961A1

Cited By

  • Ethylene-vinyl alcohol copolymer and preparation method thereof

    CN120737239A