Polyvinylidene fluoride resin composition and molded article

By adding ammonium phosphate and/or imidazolium sulfate to the polyvinylidene fluoride resin to form a β-type crystal structure, the problem of dehydrogen fluoride reaction during molding of the polyvinylidene fluoride resin is solved, and transparency and thermal stability are improved. Resin compositions and molded bodies suitable for optical and other uses.

CN118946631APending Publication Date: 2024-11-12KUREHA CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026925.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The conventional polyvinylidene fluoride resin composition is prone to dehydrogenation reaction during molding, which affects the molding device and the environment, and has insufficient transparency.

Method used

The polyvinylidene fluoride resin is added to the ammonium phosphate and/or imidazolium sulfate to form a β-type crystal structure through melting and kneading, which inhibits the dehydrogen fluoride reaction and improves transparency.

Benefits of technology

A low hydrogen fluoride reaction under high transparency is achieved, and resin compositions and molded bodies are suitable for optical and other uses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005037950040000051
    Figure BDA0005037950040000051
  • Figure BDA0005037950040000061
    Figure BDA0005037950040000061
  • Figure BDA0005037950040000101
    Figure BDA0005037950040000101
Patent Text Reader

Abstract

The present invention addresses the problem of providing: a polyvinylidene fluoride resin composition which is not susceptible to a dehydrofluorination reaction derived from a vinylidene fluoride polymer during molding and which has high transparency; and a molded article thereof. The resin composition for solving the problem comprises: a vinylidene fluoride polymer as a main component; and an ammonium phosphate salt and / or an imidazolium sulfate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyvinylidene fluoride resin composition and a molded body. Background Art

[0002] Vinylidene fluoride resins have high strength, chemical resistance, heat resistance, strong dielectric properties, etc., and are therefore used in various fields. For example, Patent Document 1 describes a resin composition containing a polyvinylidene fluoride resin and an alkyl quaternary ammonium sulfate. The resin composition is expected to be used in optical products, etc., because it has very excellent transparency.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2020-105381 Summary of the invention

[0006] Problem that the invention aims to solve

[0007] However, the inventors etc. have conducted in-depth research, and the result clearly shows that the resin combination recorded in the above-mentioned patent document 1 has very good transparency, but the thermal stability used in various applications is insufficient. Specifically, when the resin combination is heated and molded, the vinylidene fluoride polymer interacts with the alkyl quaternary ammonium sulfate, and hydrogen fluoride (HF) (also referred to as " dehydrofluorination " in this specification) is generated by the vinylidene fluoride polymer sometimes. If such hydrogen fluoride is generated, it is possible to affect the environment of molding device and surroundings, so it is required to suppress the generation of dehydrofluorination amount.

[0008] An object of the present invention is to provide a resin composition which is less likely to undergo dehydrofluorination reaction derived from a vinylidene fluoride polymer during molding and has high transparency, and a molded article thereof.

[0009] Technical Solution

[0010] The present invention provides a polyvinylidene fluoride resin composition, which contains: a vinylidene fluoride polymer as a main component; and an ammonium phosphate salt and / or an imidazolium sulfate salt.

[0011] The present invention provides a molded product, which is a molded product of the polyvinylidene fluoride resin composition, and has a haze of 40% or less when the thickness is 2 mm.

[0012] Beneficial Effects

[0013] The polyvinylidene fluoride resin composition of the present invention has high transparency and is not susceptible to dehydrofluorination reaction during molding, so it can be used for various applications including optical applications. DETAILED DESCRIPTION

[0014] 1. Polyvinylidene fluoride resin composition

[0015] The polyvinylidene fluoride resin composition of the present invention (hereinafter also referred to as “resin composition”) contains a vinylidene fluoride polymer and an ammonium phosphate salt or an imidazolium sulfate salt.

[0016] As mentioned above, although the resin composition containing vinylidene fluoride polymer and alkyl quaternary ammonium sulfate has high transparency, dehydrofluorination reaction sometimes occurs during molding. On the contrary, as in the present invention, when ammonium phosphate and / or imidazolium sulfate are combined in vinylidene fluoride polymer, not only the transparency of the resin composition becomes very high, but also the dehydrofluorination reaction during molding is not easy to occur.

[0017] The reason why the transparency of resin composition of the present invention is high can be considered as follows. The crystal structure of vinylidene fluoride polymer has α-type, β-type, γ-type, and common vinylidene fluoride polymer has the crystal structure of α-type. The vinylidene fluoride polymer of α-type crystal structure is usually low in transparency. On the contrary, if ammonium phosphate and imidazolium sulfate as ionic compounds are combined in vinylidene fluoride polymer and melt-mixed, the crystal structure of vinylidene fluoride polymer easily becomes β-type. Therefore, it is believed that the transparency of resin composition becomes very high.

[0018] Furthermore, even when ammonium phosphate and imidazolium sulfate are used in combination, the reason why dehydrofluorination reaction is unlikely to occur in the vinylidene fluoride polymer is considered to be as follows.

[0019] The mechanism of dehydrofluorination reaction is inferred to be that alkyl quaternary ammonium sulfate decomposes when heated, so that amine and sulfide are generated by alkyl quaternary ammonium cation and sulfate anion respectively. It is believed that the generated amine attacks the end of the vinylidene fluoride polymer and dehydrofluorination reaction is carried out to generate a large amount of hydrogen fluoride. On the other hand, it is believed that the generated sulfide is gasified and released outside the system.

[0020] On the other hand, ammonium phosphate decomposes when heated to generate amine and phosphorus oxide. It is believed that the phosphorus oxide generated at this time captures the amine and hinders the amine from attacking the vinylidene fluoride polymer, so that the dehydrofluorination reaction is difficult to proceed and the dehydrofluorination amount is suppressed.

[0021] In addition, it is believed that since the decomposition temperature of imidazolium sulfate is higher than that of ammonium sulfate, chemical species that attack the terminal of the vinylidene fluoride polymer will not be generated, and as a result, the dehydrofluorination reaction can be suppressed. However, in the resin composition of this embodiment, as long as the amount of dehydrofluorination generated from the obtained resin composition is suppressed, the scope of the invention is not limited by its mechanism.

[0022] Hereinafter, the vinylidene fluoride polymer, the ammonium phosphate salt, and the imidazolium sulfate salt contained in the resin composition of the present invention will be described in detail.

[0023] (vinylidene fluoride polymer)

[0024] The resin composition of the present invention is mainly composed of a vinylidene fluoride polymer. In this specification, the term "vinylidene fluoride polymer is mainly composed of" means that the resin composition contains 90 parts by mass or more of the vinylidene fluoride polymer, more preferably 95 parts by mass or more, and even more preferably 98 parts by mass or more, relative to 100 parts by mass of the resin composition.

[0025] The vinylidene fluoride polymer may be a homopolymer of vinylidene fluoride or a copolymer of vinylidene fluoride and other monomers. From the viewpoint of allowing the vinylidene fluoride polymer to fully interact with ammonium phosphate and / or imidazolium sulfate, the vinylidene fluoride polymer preferably contains sufficient constituent units derived from vinylidene fluoride. Specifically, relative to all constituent units constituting the vinylidene fluoride polymer, it is preferred that more than 90 mol% of constituent units derived from vinylidene fluoride are contained, more preferably more than 95 mol%, and further preferably more than 98 mol%. If the amount of constituent units derived from vinylidene fluoride is above the above value, the vinylidene fluoride polymer in the resin composition is likely to become the desired crystal structure (β-type), and the transparency of the resin composition is likely to be improved. In addition, if the amount of constituent units derived from vinylidene fluoride is within the above range, it is easy to obtain the unique properties of vinylidene fluoride, namely chemical resistance, heat resistance, strong dielectric properties, etc. The amount of constituent units derived from vinylidene fluoride in the vinylidene fluoride polymer can be, for example, 19 The results can be confirmed by F-NMR analysis or the like.

[0026] On the other hand, the vinylidene fluoride polymer may include only one constituent unit derived from a monomer other than vinylidene fluoride, or may include two or more. Examples of monomers derived from other than vinylidene fluoride include fluorinated alkyl vinyl compounds having vinyl and fluorinated alkyl groups in one molecule, etc. Examples of fluorinated alkyl vinyl compounds include: vinyl fluoride, trifluoroethylene, tetrafluoroethylene, chlorotrifluoroethylene, hexafluoropropylene, 2,3,3,3-tetrafluoropropylene, pentafluoropropylene, fluoroalkyl vinyl ether, and perfluoromethyl vinyl ether represented by perfluoroalkyl vinyl ether, etc. In addition, in the example of other monomers, (meth) acrylic acid, (meth) acrylate represented by methyl (meth) acrylate, etc. are also included.

[0027] The structure of vinylidene fluoride polymer, i.e. the type of the monomer of combination can be appropriately selected according to the purpose of vinylidene fluoride polymer. For example, from the viewpoint of improving the pollution resistance, ozone resistance, and solvent resistance of the molded body obtained from the resin combination, the homopolymer of vinylidene fluoride is preferably considered. On the other hand, from the viewpoint of improving the flexibility and tear strength of the molded body obtained from the resin combination, the copolymer of vinylidene fluoride and other monomers or the mixture of the copolymer and vinylidene fluoride homopolymer is preferably considered. From the viewpoint of the flexibility of the obtained molded body, the monomer copolymerized with vinylidene fluoride is preferably hexafluoropropylene.

[0028] The molecular weight of the vinylidene fluoride polymer can be appropriately selected based on the desired physical properties of the molded article. The molecular weight of the vinylidene fluoride polymer can be expressed, for example, by inherent viscosity, and is preferably 0.5 to 2.0 dL / g when molding processability is required. The inherent viscosity can be obtained based on a known measurement method, for example, based on the method specified in JIS K7367-1.

[0029] In addition, from the viewpoint of imparting sufficient mechanical strength, gas barrier properties and solvent resistance to the molded body, the melting point of the above-mentioned vinylidene fluoride polymer is preferably 130° C. to 190° C., more preferably 150° C. to 180° C., and particularly preferably 160° C. to 180° C. The melting point of the vinylidene fluoride polymer can be adjusted, for example, by the amount of constituent units derived from vinylidene fluoride in the vinylidene fluoride polymer, the molecular weight of the vinylidene fluoride polymer, etc. The melting point can be measured using a differential scanning calorimeter.

[0030] Here, the method for producing the vinylidene fluoride polymer is not particularly limited, and examples thereof include emulsion polymerization, soap-free emulsion polymerization, seed emulsion polymerization, suspension polymerization, mini-emulsion polymerization, and solution polymerization, etc. Among them, emulsion polymerization or suspension polymerization is preferred.

[0031] Emulsion polymerization is a kind of free radical polymerization method, which refers to a polymerization method in which a medium such as water, a monomer that is insoluble in the medium, and an emulsifier (hereinafter, also referred to as "surfactant") are mixed, and a polymerization initiator that can be dissolved in the medium is added to the mixed solution and carried out with monomers (vinylidene fluoride, other monomers). As surfactants and polymerization initiators, known compounds can be used. When the vinylidene fluoride polymer prepared by emulsion polymerization (also referred to as "emulsion polymerization vinylidene fluoride polymer" in this specification) is combined with the imidazolium sulfate described later, it is particularly easy to improve transparency or reduce the amount of dehydrofluorination.

[0032] On the other hand, suspension polymerization refers to a polymerization method in which an oil-soluble polymerization initiator is dissolved in a water-insoluble monomer in water containing a suspension agent, and mechanical agitation is used to suspend and disperse the polymerized product. In suspension polymerization, polymerization is carried out in monomer droplets to obtain vinylidene fluoride polymer particles. When the vinylidene fluoride polymer prepared by suspension polymerization (also referred to as "suspension polymerization vinylidene fluoride polymer" in this specification) is combined with the ammonium phosphate described later, it is particularly easy to improve transparency or reduce the amount of dehydrofluorination.

[0033] (Ammonium phosphate and imidazolium sulfate)

[0034] The resin composition of the present embodiment may contain only one of the ammonium phosphate salt and the imidazolium sulfate salt, or may contain both of them. However, it is usually preferred to contain either one.

[0035] The ammonium phosphate salt is an ammonium or alkylammonium phosphate salt, and is, for example, a compound represented by the following general formula (1). The resin composition may contain only one type of ammonium phosphate salt, or may contain two or more types.

[0036] [Chemical formula 1]

[0037]

[0038] In the above general formula (1), R 1 ~R 4 represents a hydrogen atom or an alkyl group having 1 or more and 10 or less carbon atoms, which are the same or different from each other. The alkyl group may be linear or branched. Specific examples of the alkyl group include methyl, ethyl, propyl, isopropyl, butyl, pentyl, hexyl, heptyl, octyl, etc. 1 ~R 4 The number of hydrogen atoms in is preferably 52 or less in total. 1 ~R 4 The number of carbon atoms contained is preferably 6 or more and 30 or less in total, more preferably 6 or more and 24 or less, and even more preferably 8 or more and 20 or less. 1 ~R 4 The number of carbon atoms contained is more preferably 2 or more and 6 or less, and specifically, ethyl, propyl, butyl, pentyl, and hexyl are preferred. 1 ~R 4 When the groups are these, the transparency of the obtained resin composition is very likely to be improved.

[0039] On the other hand, in formula (1), R 5 and R 6Each represents a group bonded to the P atom, and each independently represents an alkyl group, a fluoroalkyl group, or a hydrogen atom. The alkyl group is preferably an alkyl group having 1 to 10 carbon atoms, specifically, a straight-chain alkyl group having 1 to 10 carbon atoms such as a methyl group and an ethyl group, or a branched alkyl group such as an isopropyl group and a tert-butyl group. On the other hand, a fluoroalkyl group is a group in which a part or all of the hydrogen in these alkyl groups is replaced by fluorine. Examples thereof include trifluoromethyl, pentafluoroethyl, etc. R is particularly preferred. 5 and R 6 are a hydrogen atom or a tert-butyl group, respectively.

[0040] Specific examples of the ammonium phosphate salt represented by the above general formula (1) include ethyl ammonium phosphate, diethyl ammonium phosphate, trimethyl ammonium phosphate, triethyl ammonium phosphate, tributylammonium pyrophosphate, pentyl triethyl ammonium phosphate, hexyl triethyl ammonium phosphate, octyl triethyl ammonium phosphate, tetramethyl ammonium dihydrogen phosphate, tetraethyl ammonium dihydrogen phosphate, tetrabutyl ammonium phosphate, methyl triethyl dibutyl ammonium phosphate, dodecyl trimethyl ammonium phosphate, hexadecyl trimethyl ammonium dihydrogen phosphate, tetrahexyl ammonium dihydrogen phosphate, etc.

[0041] The imidazolium sulfate is a sulfate of imidazolium, and is, for example, a compound represented by the following general formula (2). The resin composition may contain only one type of imidazolium sulfate, or may contain two or more types.

[0042] [Chemical formula 2]

[0043]

[0044] In the above general formula (2), R 7 and R 8 represents a hydrogen atom, or an alkyl group having 1 to 10 carbon atoms, which is the same or different from each other. The alkyl group may be linear or branched. Specific examples of the alkyl group include methyl, ethyl, propyl, isopropyl, butyl, pentyl, hexyl, heptyl, octyl, etc. Among them, an alkyl group having 1 to 4 carbon atoms is preferred, and specifically, methyl, ethyl, propyl, and butyl are preferred.

[0045] In the above general formula (2), R 9 is an alkyl group, a fluoroalkyl group or a hydrogen atom. The alkyl group is preferably a short-chain alkyl group having 1 to 10 carbon atoms such as a methyl group and an ethyl group. The fluoroalkyl group is preferably CF 3 , C 2 F 5 A short-chain fluoroalkyl group having 1 to 10 carbon atoms. 9 In other words, the imidazolium sulfate is preferably imidazolium hydrogen sulfate.

[0046] Specific examples of preferred imidazolium sulfates (imidazolium hydrogen sulfates) include: 1,3-dimethylimidazolium hydrogen sulfate, 1-methyl-3-propylimidazolium hydrogen sulfate, 1-methyl-3-isopropylimidazolium hydrogen sulfate, 1,3-diethylimidazolium hydrogen sulfate, 1,3-dipropylimidazolium hydrogen sulfate, 1-ethyl-3-propylimidazolium hydrogen sulfate, 1-butyl-3-methylimidazolium hydrogen sulfate, 1-ethyl-3-methylimidazolium hydrogen sulfate, and the like.

[0047] Here, the amount of the above-mentioned ammonium phosphate and / or imidazolium sulfate in the resin combination is not particularly limited. However, relative to the amount 100 mass parts of the above-mentioned vinylidene fluoride polymer, the total content of ammonium phosphate and imidazolium sulfate is preferably more than 0.1 mass part and less than 2 mass parts, more preferably more than 0.3 mass part and less than 1.7 mass parts, further preferably more than 0.4 mass part and less than 1.5 mass parts, particularly preferably more than 0.7 mass part and less than 1.3 mass parts. If the total content of the ammonium phosphate and imidazolium sulfate in the resin combination is within the range, the transparency of the resin combination and its molded body is easily improved, and the dehydrofluorination amount during molding can be reduced.

[0048] (Other ingredients)

[0049] The resin composition of the present embodiment may further contain other components within the scope of obtaining the effect of the present embodiment. The other components may be one or more than one. The content of the additive in the resin composition may be appropriately determined within the scope of both the effect of the present embodiment and the effect generated by the additive. Examples of the above-mentioned other components include additives and polymers other than the above. Examples of additives include heat stabilizers, ultraviolet absorbers, light stabilizers, lubricants, plasticizers, bluing agents, and anti-coloring agents.

[0050] ·Method for producing resin composition

[0051] The above-mentioned vinylidene fluoride polymer and ammonium phosphate and / or imidazolium sulfate are prepared respectively to the above-mentioned resin combination.Then, it is possible to manufacture by mixing them, melt mixing etc. at a temperature above the melting point of the vinylidene fluoride polymer.The temperature during manufacturing the resin combination is preferably more than 160 ℃ and less than 280 ℃.By being heated to this temperature, the crystal structure of the vinylidene fluoride polymer can be made into a β body, it is easy to obtain a resin combination with high transparency, and then obtain a molded body.

[0052] As the device of the material of mixed resin composition, for example, can be listed: Henschel mixer, cylindrical mixer, spiral mixer, spiral extruder, turbulence enhancer, Nauta mixer, V-type mixer, ribbon mixer (Ribbon Blender), double-arm type kneading machine, flow mixer, airflow type mixer, rotating disc type mixer, roller mixer, rolling mixer and Lödige mixer etc. In addition, by the material directly mixed with vinylidene fluoride polymer and ammonium phosphate and / or imidazolium sulfate or the material melt extruded by mixing and drying the aqueous solution of vinylidene fluoride polymer and ammonium phosphate and / or imidazolium sulfate, it is possible to obtain a granular resin composition. As extruder, for example, can be listed single screw extruder, co-rotating twin screw extruder and counter-rotating twin screw extruder etc.

[0053] 2. Molding

[0054] The molded body of the above-mentioned resin composition can be manufactured by heating and molding the above-mentioned resin composition. The method for molding the above-mentioned resin composition is not particularly limited, and can be carried out in the same manner as a known molding method. However, when heated, in order to reduce the amount of dehydrofluorination of the vinylidene fluoride polymer, it is also preferred that the molding temperature is less than 280°C. In addition, at this time, it is preferred that the change in the crystal structure of the vinylidene fluoride polymer in the above-mentioned resin composition is reduced, that is, a state with high transparency can be maintained. Specifically, it is preferably cooled for more than 60 seconds at a temperature below 80°C and molded.

[0055] The shape of the molded body is not particularly limited, and may be, for example, a film, a flat plate, or a three-dimensional structure. The structure of the molded body may be appropriately selected depending on the intended use of the molded body.

[0056] Preferably, the haze of the molded body when the thickness is 2 mm is 40% or less, more preferably 30% or less, and further preferably 20% or less. When the haze of the molded body when the thickness is 2 mm is 40% or less, the molded body can also be used for applications requiring transparency, such as optical products. It should be noted that the above haze is a value measured using a haze meter based on JIS K7136. In addition, for the above haze, even if the thickness of the molded body is other than 2 mm, the haze of the molded body can be measured and calculated from the value based on an empirical formula. Usually, in molded bodies below 8 mm, the relationship between haze and thickness can be expressed by a linear formula. Therefore, an empirical formula can also be created based on the components of the molded body, and calculated from the formula.

[0057] Such a molded product can be used not only for the same purposes as ordinary polyvinylidene fluoride, but also for optical products such as optical films and optical lenses.

[0058] Example

[0059] Hereinafter, specific examples of the present invention will be described together with comparative examples, but the present invention is not limited thereto.

[0060] (Example 1)

[0061] A suspension-polymerized vinylidene fluoride polymer (Polymer A, a vinylidene fluoride homopolymer, inherent viscosity 1.070 dl / g, melting point 171° C.) was prepared by the same method as in Example 4 of International Publication No. 2006 / 061988. 1 part by mass of tetrabutylammonium phosphate (hereinafter also referred to as “N26”) was added to 100 parts by mass of the Polymer A. Next, the mixture was extruded by a co-rotating twin-screw extruder (TEM-26 manufactured by Toshiba Machine Co., Ltd.) at a cylinder temperature of 190° C. to obtain a granular resin composition 1.

[0062] (Example 2)

[0063] 1 part by mass of 1-butyl-3-methylimidazolium hydrogen sulfate (hereinafter also referred to as "I12") was added to 100 parts by mass of an emulsion-polymerized vinylidene fluoride polymer (Kynar (registered trademark) 740, manufactured by Arkema, a vinylidene fluoride homopolymer), and extruded using a co-rotating twin-screw extruder in the same manner as in Example 1 to obtain a granular resin composition 2.

[0064] (Example 3)

[0065] A pelletized resin composition 3 was obtained in the same manner as in Example 2 except that tetrabutylammonium phosphate (N26) was used instead of the 1-butyl-3-methylimidazolium hydrogen sulfate (I12).

[0066] (Example 4)

[0067] A pelletized resin composition 4 was obtained in the same manner as in Example 1 except that the amount of tetrabutylammonium phosphate (N26) was changed to 0.3 parts by mass.

[0068] (Example 5)

[0069] A pelletized resin composition 5 was obtained in the same manner as in Example 1 except that the amount of tetrabutylammonium phosphate (N26) was changed to 0.5 parts by mass.

[0070] (Example 6)

[0071] A pelletized resin composition 6 was obtained in the same manner as in Example 1 except that the amount of tetrabutylammonium phosphate (N26) was changed to 2 parts by mass.

[0072] (Example 7)

[0073] Resin composition 7 was obtained in the same manner as in Example 1 except that the vinylidene fluoride polymer was changed to a suspension-polymerized vinylidene fluoride polymer (KF#2300 manufactured by KUREHA CORPORATION, vinylidene fluoride-hexafluoropropylene copolymer).

[0074] (Example 8)

[0075] A pelletized resin composition 8 was obtained in the same manner as in Example 1 except that 1 part by mass of tetra-n-butylammonium di-tert-butyl phosphate (hereinafter also referred to as "N30") was used instead of tetrabutylammonium phosphate (N26).

[0076] (Comparative Example 1)

[0077] A pelletized resin composition 9 was obtained in the same manner as in Example 1 except that tetrabutylammonium phosphate (N26) was not used.

[0078] (Comparative Example 2)

[0079] A pelletized resin composition 10 was obtained in the same manner as in Example 2 except that 1-butyl-3-methylimidazolium hydrogen sulfate (I12) was not used.

[0080] (Comparative Example 3)

[0081] A pelletized resin composition 11 was obtained in the same manner as in Example 1 except that 1 part by mass of tetrabutylammonium hydrogen sulfate (hereinafter also referred to as "TBAHS") was used instead of tetrabutylammonium phosphate (N26).

[0082] (Comparative Example 4)

[0083] A pelletized resin composition 12 was obtained in the same manner as in Example 2 except that 1 part by mass of tetrabutylammonium hydrogen sulfate (TBHAS) was used instead of 1-butyl-3-methylimidazolium hydrogen sulfate (I12).

[0084] (Method for producing molded article)

[0085] The resin composition prepared in the above-mentioned embodiment and comparative example is clamped with two pieces of aluminum foil, and a stainless steel (SUS) plate is arranged on the outside of the aluminum foil. Then, a compression molding machine (manufactured by Shinto Metal Industries, Ltd., model AYSR-5) is used to press at a pressure of 5MPa at 200°C for 5 minutes. Next, the pressed product is immediately kept under a cold press at 30°C for 3 minutes for cooling (quenching). Thus, a sheet-like molded body is produced. The thickness of the molded body is measured five times for each sample using a thickness meter "DG-925" (manufactured by Ono Test Instruments Co., Ltd.), and the average value is obtained. The average value is used as the thickness of the molded body. They are all 2mm.

[0086] (Haze)

[0087] The haze of each molded article (thickness 2 mm) was measured using a haze meter "NDH4000" (manufactured by Nippon Denshoku Industries) in accordance with JIS K7136. The results are shown in Table 1.

[0088] (Dehydrofluorination amount)

[0089] A sheet-shaped molded body was prepared in the same manner as the above-mentioned molded body. 300 mg of the sheet was placed in a quartz glass boat and heated at 260°C for 2 hours in a nitrogen flow of 100 mL / min using a ceramic electric tubular heating furnace (manufactured by Asahi Rika Seisakusho Co., Ltd.). The generated gas was then purged with 20 mL of NaHCO 3 +Na 2 CO 3 After the aqueous solution is absorbed, the volume is adjusted to 30 mL. It should be noted that the NaHCO 3 and Na 2 CO 3 The initial concentrations of were adjusted to 1.9 mM and 3.2 mM, respectively. Then, the fluoride ion concentration was determined from the solution using an ion chromatograph (manufactured by Tosoh Corporation, model IC-2010). The results are shown in Table 1.

[0090] [Table 1]

[0091]

[0092]

[0093] ※PolymerA and #2300: Suspension polymerization of vinylidene fluoride polymers.

[0094] Kynar740: Emulsion polymerized vinylidene fluoride polymer.

[0095] N26: Tetrabutylammonium phosphate.

[0096] N30: di-tert-butyl phosphate tetra-n-butylammonium salt.

[0097] I12: 1-Butyl-3-methylimidazolium hydrogen sulfate.

[0098] TBAHS: tetrabutylammonium hydrogen sulfate.

[0099] As shown in Table 1 above, when only a vinylidene fluoride polymer is used, the haze is high regardless of the method for producing the vinylidene fluoride polymer (Comparative Examples 1 and 2). In addition, when tetrabutylammonium hydrogen sulfate is added to the vinylidene fluoride polymer, although the haze is reduced, the amount of dehydrofluorination is very large (Comparative Examples 3 and 4). In contrast, when ammonium phosphate or imidazolium sulfate (imidazolium hydrogen sulfate) is added to the vinylidene fluoride polymer, not only the haze of the molded body is reduced, but the amount of dehydrofluorination also becomes very small (Examples 1 to 8).

[0100] This application claims priority based on Japanese Patent Application No. 2022-049939 filed on March 25, 2022. The contents described in the specification of that application are incorporated herein by reference in their entirety.

[0101] Industrial Applicability

[0102] According to the present invention, a resin composition having high transparency and a small amount of dehydrofluorination during molding and a molded product thereof can be obtained. The resin composition and the molded product thereof can be used not only for ordinary resin products but also for products requiring transparency, such as optical products, and are very useful in various industrial fields.

Claims

1. A polyvinylidene fluoride resin composition, comprising: A vinylidene fluoride polymer as a main component; and Ammonium phosphate and / or imidazolium sulfate.

2. The polyvinylidene fluoride resin composition according to claim 1, wherein The total content of the ammonium phosphate and the imidazolium sulfate is 0.1 parts by mass or more and 2 parts by mass or less relative to 100 parts by mass of the vinylidene fluoride polymer.

3. The polyvinylidene fluoride resin composition according to claim 1 or 2, wherein The ammonium phosphate salt contains alkyl quaternary ammonium phosphate.

4. The polyvinylidene fluoride resin composition according to any one of claims 1 to 3, comprising: The ammonium phosphate salt; and Suspension polymerization of vinylidene fluoride polymers.

5. The polyvinylidene fluoride resin composition according to any one of claims 1 to 3, comprising: The imidazolium sulfate; and Emulsion polymerized vinylidene fluoride polymer.

6. The polyvinylidene fluoride resin composition according to any one of claims 1 to 5, wherein The vinylidene fluoride polymer is a homopolymer of vinylidene fluoride.

7. A shaped body, The molded body is a molded body of the polyvinylidene fluoride resin composition according to any one of claims 1 to 6, The haze at a thickness of 2 mm was 40% or less.