Continuous annealing device, continuous hot-dip galvanizing device, and method for producing steel sheet
By applying a stable magnetic field along the width direction of the steel plate in the continuous annealing device and the continuous hot-dip galvanizing device, the problem of difficulty in reducing the amount of hydrogen in the steel plate is solved, and efficient reduction of the amount of hydrogen, maintaining mechanical characteristics, and producing hydrogen embrittlement resistance is achieved. The steel plate with excellent characteristics improves production efficiency.
Patent Information
- Application Number
- CN202380029116.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-03-01
- Publication Date
- 2024-11-12
AI Technical Summary
During the annealing process, the amount of hydrogen in the steel plate is difficult to effectively reduce, resulting in reduced ductility, bending and tensile flange properties, and embrittlement, and traditional methods require a longer Only in time can the hydrogen amount be fully reduced and the production efficiency will be affected.
During the process from cooling to the tension winder after annealing, a stable magnetic field is applied along the plate width direction of the steel plate, and the magnetostrictive effect is used to expand the crystal lattice of the steel plate, thereby promoting hydrogen to detach from the surface of the steel plate and achieving efficient reduction of hydrogen quantity.
Without damaging production efficiency, the amount of hydrogen in the steel plate is effectively reduced, mechanical characteristics are maintained, and steel plates with excellent hydrogen embrittlement resistance are produced, which avoids hydrogen embrittlement problems and shortens the hydrogen reduction time.
Smart Images

Figure CN118946671A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a continuous annealing device and a continuous hot-dip galvanizing device and a method for manufacturing a steel plate. The present invention is particularly suitable for the fields of automobiles, home appliances, building materials, etc., and relates to a continuous annealing device and a continuous hot-dip galvanizing device for manufacturing a steel plate having a small amount of hydrogen inherent in steel and excellent hydrogen embrittlement resistance, and a method for manufacturing a steel plate. Background Art
[0002] For example, when annealing steel sheets and hot-dip galvanizing steel sheets are manufactured in a continuous annealing device and a continuous hot-dip galvanizing device, respectively, the steel sheets are annealed in a reducing atmosphere containing hydrogen, so hydrogen intrudes into the steel sheets during the annealing. The inherent hydrogen in the steel sheets reduces the formability of the steel sheets, such as ductility, bendability, and stretch flangeability. In addition, the inherent hydrogen in the steel sheets can make the steel sheets embrittled, resulting in delayed failure. Therefore, a process to reduce the amount of hydrogen in the steel sheets is required.
[0003] For example, the amount of hydrogen in the steel can be reduced by leaving the product coils manufactured by the continuous annealing device and the continuous hot-dip galvanizing device at room temperature. However, it takes time for hydrogen to move from the inside of the steel plate to the surface and to escape from the surface at room temperature, so it takes several weeks or more to fully reduce the amount of hydrogen in the steel. Therefore, the space and time required for such dehydrogenation treatment become a problem in the manufacturing process.
[0004] In addition, Patent Document 1 discloses a method of reducing the amount of hydrogen in steel by maintaining an annealed steel sheet, a hot-dip galvanized steel sheet, or an alloyed hot-dip galvanized steel sheet in a temperature range of 50° C. to 300° C. for 1800 seconds to 43200 seconds.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2019 / 188642 Summary of the invention
[0008] However, in Patent Document 1, there is a concern that the structural change due to heating may lead to an increase in yield strength and changes in mechanical properties such as temper embrittlement.
[0009] Therefore, in view of the above problems, the present invention aims to provide a continuous annealing apparatus and a continuous hot-dip galvanizing apparatus and a method for producing a steel sheet that can produce a steel sheet having excellent hydrogen embrittlement resistance without impairing production efficiency or changing mechanical properties.
[0010] The inventors of the present invention have repeatedly conducted in-depth research to solve the above-mentioned problems, and as a result, found the following phenomenon. That is, in a continuous annealing device (Continuous Annealing Line: CAL) or a continuous hot-dip galvanizing device (Continuous hot-dip Galvanizing Line: CGL), after annealing the steel plate in a reducing atmosphere containing hydrogen, a stable magnetic field is applied to the steel plate in the plate width direction of the steel plate during the cooling process from the annealing temperature to room temperature, thereby being able to fully and efficiently reduce the hydrogen in the steel plate. It is speculated that this is due to the following mechanism. By applying a stable magnetic field to the steel plate, the shape of the steel plate changes due to the magnetostrictive effect. At this time, since the stable magnetic field applied to the steel plate is along the plate width direction of the steel plate, the lattice spacing of the steel plate is expanded in the direction of the main surface (surface and back) of the steel plate along the plate width direction of the steel plate. As a result, the hydrogen inside the steel plate diffuses to the main surface (surface and back) of the steel plate with low potential energy and detaches from the main surface.
[0011] That is, the present invention has been completed based on the above circumstances, and the gist thereof is as follows.
[0012] [1] A continuous annealing device comprising:
[0013] Uncoiler, unwinding cold-rolled steel sheets from cold-rolled coils;
[0014] an annealing furnace for continuously annealing the cold-rolled steel sheet by passing the sheet through the furnace, wherein the annealing furnace is provided with a heating zone, a soaking zone and a cooling zone from the upstream side of the sheet passing direction, wherein the cold-rolled steel sheet is annealed in a reducing atmosphere containing hydrogen in the heating zone and the soaking zone, and the cold-rolled steel sheet is cooled in the cooling zone;
[0015] Downstream equipment, allowing the cold-rolled steel sheet discharged from the annealing furnace to continue to pass through the plate;
[0016] A tension coiler for coiling the cold-rolled steel sheet in the downstream equipment; and
[0017] The magnetic field applying device applies a stable magnetic field along the sheet width direction of the cold-rolled steel sheet to the cold-rolled steel sheet being passed from the cooling belt to the tension coiler.
[0018] [2] The continuous annealing apparatus according to [1] above, wherein the magnetic field applying device is provided in the cooling zone.
[0019] [3] The continuous annealing apparatus according to [1] or [2] above, wherein the magnetic field applying device is disposed at a position capable of applying a magnetic field to the cold-rolled steel sheet passing through the downstream equipment.
[0020] [4] A continuous annealing device according to any one of [1] to [3] above, wherein the magnetic field application device includes an electromagnet located outside the width direction end of the cold-rolled steel sheet, and the electromagnet has a magnetic pole surface facing the width direction end surface of the cold-rolled steel sheet.
[0021] [5] A continuous annealing device according to any one of [1] to [3] above, wherein the magnetic field application device includes a pair of electromagnets located on the outside of the two end portions in the width direction of the cold-rolled steel sheet, respectively, and the pair of electromagnets respectively have magnetic pole surfaces facing the end surfaces in the width direction of the cold-rolled steel sheet, one of the magnetic pole surfaces is an N pole, and the other is an S pole.
[0022] [6] The continuous annealing apparatus according to any one of [1] to [5] above, wherein the magnetic field applying device is set so that the magnetic flux density in the width direction of the cold-rolled steel sheet is 0.1 to 15 T.
[0023] [7] A continuous hot-dip galvanizing device comprising:
[0024] The continuous annealing apparatus described in [1] above; and
[0025] The hot-dip galvanizing bath as the downstream equipment is located downstream of the annealing furnace in the sheet passing direction, and immerses the cold-rolled steel sheets to perform hot-dip galvanizing on the cold-rolled steel sheets.
[0026] [8] The continuous hot-dip galvanizing apparatus according to [7] above, wherein the magnetic field applying device is provided at a position capable of applying a magnetic field to the cold-rolled steel sheet in the upstream passage of the hot-dip galvanizing bath.
[0027] [9] The continuous hot-dip galvanizing apparatus according to [7] or [8] above, wherein the magnetic field applying device is provided at a position capable of applying a magnetic field to the cold-rolled steel sheet in the downstream passage of the hot-dip galvanizing bath.
[0028]
[10] According to the continuous hot-dip galvanizing apparatus described in [7] above, an alloying furnace is provided as the downstream equipment, and the alloying furnace is located downstream of the hot-dip galvanizing bath in the direction of passing the plate, so that the cold-rolled steel plate passes through the plate and the hot-dip galvanizing is heated and alloyed.
[0029]
[11] The continuous hot-dip galvanizing apparatus according to
[10] above, wherein the magnetic field applying device is provided at a position capable of applying a magnetic field to the cold-rolled steel sheet in the upstream passage of the hot-dip galvanizing bath.
[0030]
[12] The continuous hot-dip galvanizing apparatus according to
[10] or
[11] above, wherein the magnetic field applying device is disposed at a position capable of applying a magnetic field to the cold-rolled steel sheet in the downstream passage of the hot-dip galvanizing bath.
[0031]
[13] A continuous hot-dip galvanizing device according to any one of [7] to
[12] above, wherein the magnetic field application device includes an electromagnet located outside the width direction end of the cold-rolled steel sheet, and the electromagnet has a magnetic pole surface facing the width direction end surface of the cold-rolled steel sheet.
[0032]
[14] A continuous hot-dip galvanizing device according to any one of [7] to
[12] above, wherein the magnetic field application device includes a pair of electromagnets respectively located on the outside of the two end portions in the width direction of the cold-rolled steel sheet, and the pair of electromagnets respectively have magnetic pole surfaces facing the end surfaces in the width direction of the cold-rolled steel sheet, one of the magnetic pole surfaces is an N pole, and the other is an S pole.
[0033]
[15] The continuous hot-dip galvanizing apparatus according to any one of [7] to
[14] above, wherein the magnetic field applying device is set so that the magnetic flux density in the width direction of the cold-rolled steel sheet is 0.1 to 15 T.
[0034]
[16] A method for manufacturing a steel plate, comprising the following steps in sequence:
[0035] (A) A process of unwinding a cold-rolled steel sheet from a cold-rolled coil using an unwinding machine;
[0036] (B) a step of passing the cold-rolled steel sheet through an annealing furnace provided with a heating zone, a soaking zone and a cooling zone on the upstream side of the passing direction, and performing continuous annealing, wherein the continuous annealing comprises (B-1) annealing the cold-rolled steel sheet in a reducing atmosphere containing hydrogen in the heating zone and the soaking zone, and (B-2) cooling the cold-rolled steel sheet in the cooling zone;
[0037] (C) a step of continuing to pass the cold-rolled steel sheet discharged from the annealing furnace; and
[0038] (D) a process of winding the cold-rolled steel sheet using a tension coiler to produce a product coil,
[0039] After step (B-2) and before step (D), the method includes a magnetic field applying step of applying a stable magnetic field to the cold-rolled steel sheet in the sheet along the sheet width direction of the cold-rolled steel sheet.
[0040]
[17] The method for manufacturing a steel plate according to
[16] above, wherein the magnetic field applying step is performed in step (B-2).
[0041]
[18] The method for manufacturing a steel plate according to
[16] or
[17] above, wherein the magnetic field applying step is performed in step (C).
[0042]
[19] The method for manufacturing a steel sheet according to the above-mentioned
[16] , wherein step (C) includes (C-1) a step of immersing the cold-rolled steel sheet in a hot-dip galvanizing bath located downstream in the sheet passing direction of the annealing furnace to perform hot-dip galvanizing on the cold-rolled steel sheet.
[0043]
[20] The method for manufacturing a steel plate according to
[19] above, wherein the magnetic field applying step is performed before the step (C-1).
[0044]
[21] The method for manufacturing a steel plate according to
[19] or
[20] above, wherein the magnetic field applying step is performed after step (C-1).
[0045]
[22] The method for manufacturing a steel sheet according to the above-mentioned
[19] , wherein the above-mentioned step (C) includes, after the above-mentioned step (C-1), a step (C-2) of passing the above-mentioned cold-rolled steel sheet through an alloying furnace downstream in the direction of passing the sheet through the above-mentioned hot-dip galvanizing bath to heat and alloy the above-mentioned hot-dip galvanizing.
[0046]
[23] The method for manufacturing a steel plate according to
[22] above, wherein the magnetic field applying step is performed before the step (C-1).
[0047]
[24] The method for manufacturing a steel plate according to
[22] or
[23] above, wherein the magnetic field applying step is performed after step (C-1).
[0048]
[25] A method for manufacturing a steel plate according to any one of
[16] to
[24] above, wherein in the magnetic field application step, the magnetic flux density in the width direction of the cold-rolled steel plate is set to 0.1 to 15 T.
[0049]
[26] A method for manufacturing a steel plate according to any one of
[16] to
[25] above, wherein, in the magnetic field application step, the stable magnetic field is applied using a magnetic field application device, the magnetic field application device comprising an electromagnet located on the outside of the width direction end of the cold-rolled steel plate, the electromagnet having a magnetic pole surface facing the width direction end surface of the cold-rolled steel plate.
[0050]
[27] A method for manufacturing a steel plate according to any one of
[16] to
[25] above, wherein, in the magnetic field applying step, the stable magnetic field is applied by a magnetic field applying device, the magnetic field applying device comprising a pair of electromagnets respectively located on the outside of both ends in the width direction of the cold-rolled steel plate, the pair of electromagnets respectively having magnetic pole surfaces facing the end surfaces in the width direction of the cold-rolled steel plate, one of the magnetic pole surfaces being an N pole and the other being an S pole.
[0051]
[28] The method for manufacturing a steel plate according to any one of
[16] to
[27] above, wherein the cold-rolled steel plate is a high-strength steel plate having a tensile strength of 590 MPa or more.
[0052]
[29] A method for manufacturing a steel plate according to any one of
[16] to
[28] above, wherein the cold-rolled steel plate has the following composition: in mass %, it contains C: 0.030-0.800%, Si: 0.01-3.00%, Mn: 0.01-10.00%, P: 0.001-0.100%, S: 0.0001-0.0200%, N: 0.0005-0.0100% and Al: 0.001-2.000%, and the remainder is Fe and unavoidable impurities.
[0053]
[30] The method for manufacturing a steel sheet according to the above-mentioned
[29] , wherein the above-mentioned component composition further contains, in terms of mass%, at least one element selected from the group consisting of Ti: less than 0.200%, Nb: less than 0.200%, V: less than 0.500%, W: less than 0.500%, B: less than 0.0050%, Ni: less than 1.000%, Cr: less than 1.000%, Mo: less than 1.000%, Cu: less than 1.000%, Sn: less than 0.200%, Sb: less than 0.200%, Ta: less than 0.100%, Ca: less than 0.0050%, Mg: less than 0.0050%, Zr: less than 0.1000% and REM: less than 0.0050%.
[0054]
[31] A method for manufacturing a steel plate according to any one of
[16] to
[27] above, wherein the cold-rolled steel plate is a stainless steel plate having the following composition, wherein the composition contains, in mass %, C: 0.001-0.400%, Si: 0.01-2.00%, Mn: 0.01-5.00%, P: 0.001-0.100%, S: 0.0001-0.0200%, Cr: 9.0-28.0%, Ni: 0.01-40.0%, N: 0.0005-0.500% and Al: 0.001-3.000%, with the remainder being Fe and unavoidable impurities.
[0055]
[32] The method for manufacturing a steel sheet according to the above-mentioned
[31] , wherein the above-mentioned component composition further contains, in terms of mass%, at least one element selected from the group consisting of Ti: less than 0.500%, Nb: less than 0.500%, V: less than 0.500%, W: less than 2.000%, B: less than 0.0050%, Mo: less than 2.000%, Cu: less than 3.000%, Sn: less than 0.500%, Sb: less than 0.200%, Ta: less than 0.100%, Ca: less than 0.0050%, Mg: less than 0.0050%, Zr: less than 0.1000% and REM: less than 0.0050%.
[0056]
[33] The method for manufacturing a steel sheet according to any one of
[16] to
[32] above, wherein the product coil has a diffusible hydrogen content of 0.50 mass ppm or less.
[0057] According to the continuous annealing apparatus, the continuous hot-dip galvanizing apparatus, and the method for manufacturing a steel sheet of the present invention, a steel sheet having excellent hydrogen embrittlement resistance can be manufactured without impairing production efficiency or changing mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 It is a schematic diagram of a continuous annealing apparatus 100 according to one embodiment of the present invention.
[0059] Figure 2 Schematic diagram of a continuous hot-dip galvanizing apparatus 200 according to an embodiment of the present invention.
[0060] Figure 3 is a schematic diagram of a continuous hot-dip galvanizing device 300 according to another embodiment of the present invention.
[0061] Figure 4 Schematic diagram showing the configuration of a pair of electromagnets 60A and 60B as a magnetic field applying device used in each embodiment of the present invention and magnetic lines of force generated by the electromagnets 60A and 60B.
[0062] Figure 5 (A) and (B) schematically show examples of how a pair of electromagnets 60A and 60B as magnetic field generating means are installed relative to the cold-rolled steel sheet S in the intermediate sheet in each embodiment of the present invention. DETAILED DESCRIPTION
[0063] One embodiment of the present invention relates to a continuous annealing line (CAL), and another embodiment of the present invention relates to a continuous hot-dip galvanizing line (CGL).
[0064] The method for manufacturing a steel sheet according to one embodiment of the present invention is implemented by a continuous annealing line (CAL) or a continuous hot-dip galvanizing line (CGL).
[0065] Reference Figure 1 The continuous annealing device (CAL) 100 of the first embodiment of the present invention comprises an unwinder 10 for releasing a cold-rolled steel sheet S from a cold-rolled coil C; an annealing furnace 20 for passing the cold-rolled steel sheet S through the annealing furnace 20 for continuous annealing; a downstream device 30 for continuing to pass the cold-rolled steel sheet S discharged from the annealing furnace 20; and a tension coiler 50 for winding the cold-rolled steel sheet S passed through the downstream device 30 into a product coil P. In the annealing furnace 20, a heating zone 22, a soaking zone 24, and a cooling zone 26 are provided on the upstream side of the passing direction, and the cold-rolled steel sheet S is annealed in a reducing atmosphere containing hydrogen in the heating zone 22 and the soaking zone 24, and the cold-rolled steel sheet S is cooled in the cooling zone 26. It should be noted that the annealing furnace 20 of CAL 100 preferably has an over-aging treatment zone 28 downstream of the cooling zone 26, but this is not essential. The cold-rolled steel sheet S is subjected to over-aging treatment in the over-aging treatment zone 28. In this embodiment, a product coil of a cold rolled annealed steel sheet (CR) is manufactured using CAL100.
[0066] Reference Figure 1 The first embodiment of the method for manufacturing a steel plate implemented by a continuous annealing device (CAL) 100 has the following steps in sequence: (A) a step of unwinding a cold-rolled steel plate (steel strip) S from a cold-rolled coil C by using an unwinding machine 10; (B) a step of passing the cold-rolled steel plate S through an annealing furnace 20 provided with a heating zone 22, a soaking zone 24 and a cooling zone 26 on the upstream side of the passing direction, and performing continuous annealing, wherein the above-mentioned continuous annealing is (B-1) annealing the cold-rolled steel plate S in a reducing atmosphere containing hydrogen in the heating zone 22 and the soaking zone 24, (B-2) cooling the cold-rolled steel plate S in the cooling zone 26; (C) a step of continuing to pass the cold-rolled steel plate S discharged from the annealing furnace 20; and (D) a step of winding the cold-rolled steel plate S by using a tension coiler 50 to form a product coil P. It should be noted that, in the continuous annealing step (B) of the annealing furnace 20 using CAL100, it is preferred (B-3) to perform overaging treatment on the cold-rolled steel sheet S in the overaging treatment zone 28 arbitrarily provided downstream of the cooling zone 26, but this step is not essential. This embodiment is a method for manufacturing a product coil of a cold-rolled annealed steel sheet (CR) using CAL100.
[0067] Reference Figure 2The continuous hot-dip galvanizing device (CGL) 200 of the second embodiment of the present invention comprises an unwinder 10 for unwinding a cold-rolled steel sheet S from a cold-rolled coil C; an annealing furnace 20 for passing the cold-rolled steel sheet S through a plate to perform continuous annealing; a downstream device 30 for continuing to pass the cold-rolled steel sheet S discharged from the annealing furnace 20 through a plate; and a tension coiler 50 for winding the cold-rolled steel sheet S passed through the plate in the downstream device 30 to form a product coil P. In the annealing furnace 20, a heating zone 22, a soaking zone 24, and a cooling zone 26 are provided on the upstream side of the plate passing direction, and the cold-rolled steel sheet S is annealed in a reducing atmosphere containing hydrogen in the heating zone 22 and the soaking zone 24, and the cold-rolled steel sheet S is cooled in the cooling zone 26. In addition, the CGL200 further comprises, as a downstream device 30, a hot-dip galvanizing bath 31, which is located downstream of the annealing furnace 20 in the sheet passing direction, in which the cold-rolled steel sheet S is immersed and hot-dip galvanized, and an alloying furnace 33, which is located downstream of the hot-dip galvanizing bath 31 in the sheet passing direction, in which the cold-rolled steel sheet S is passed and the hot-dip galvanizing is heated and alloyed. In this embodiment, a product coil of an alloyed hot-dip galvanized steel sheet (GA) whose zinc coating layer is alloyed is manufactured by using the CGL200. It should be noted that, when the steel sheet S is only passed through the alloying furnace 33 without being heated and alloyed, a product coil of a hot-dip galvanized steel sheet (GI) whose zinc coating layer is not alloyed is manufactured.
[0068] Reference Figure 2 The method for manufacturing a steel sheet according to the second embodiment implemented by a continuous hot-dip galvanizing device (CGL) 200 sequentially comprises (A) a step of unwinding a cold-rolled steel sheet (steel strip) S from a cold-rolled coil C by using an unwinding machine 10; (B) a step of passing the cold-rolled steel sheet S through an annealing furnace 20 provided with a heating zone 22, a soaking zone 24 and a cooling zone 26 on the upstream side of the passing direction, and performing continuous annealing, wherein the continuous annealing is (B-1) annealing the cold-rolled steel sheet S in a reducing atmosphere containing hydrogen in the heating zone 22 and the soaking zone 24, and (B-2) cooling the cold-rolled steel sheet S in the cooling zone 26; (C) a step of continuing to pass the cold-rolled steel sheet S discharged from the annealing furnace 20; and (D) a step of winding the cold-rolled steel sheet S to form a product coil P by using a tension coiler 50. Furthermore, the step (C) includes (C-1) a step of immersing the cold-rolled steel sheet S in a hot-dip galvanizing bath 31 located downstream of the annealing furnace 20 in the sheet passing direction, and performing hot-dip galvanizing on the cold-rolled steel sheet S; and then (C-2) a step of passing the cold-rolled steel sheet S through an alloying furnace 33 located downstream of the hot-dip galvanizing bath 31 in the sheet passing direction, and performing heating and alloying on the hot-dip galvanizing. This embodiment is a method for manufacturing a product coil of an alloyed hot-dip galvanized steel sheet (GA) in which the zinc coating layer is alloyed using CGL200.
[0069] Reference Figure 3The continuous hot-dip galvanizing device (CGL) 300 of the third embodiment of the present invention has the same structure as the CGL 200 except that the alloying furnace 33 is not provided. In this embodiment, the CGL 300 is used to manufacture a product coil of a hot-dip galvanized steel sheet (GI) whose zinc coating layer is not alloyed.
[0070] That is, the method for manufacturing a steel sheet of the third embodiment in which the step (C-1) is performed but the step (C-2) is not performed can be realized, for example, by using CGL300 without an alloying furnace 33, or by only passing the steel sheet S through the alloying furnace 33 of CGL200 without performing heating alloying. This embodiment is a method for manufacturing a product coil of a hot-dip galvanized steel sheet (GI) whose zinc coating layer is not alloyed using CGL200 or CGL300.
[0071] Each configuration of the CAL of the first embodiment and the CGL of the second and third embodiments will be described in detail. In addition, each step of the method for manufacturing the steel sheet of the first, second and third embodiments will be described in detail.
[0072] [Uncoiler and equipment from uncoiler to annealing furnace]
[0073] [Step (A)]
[0074] Reference Figures 1 to 3 , the uncoiler 10 unwinds the cold-rolled steel sheet S from the cold-rolled coil C. That is, in step (A), the cold-rolled steel sheet S is unwinded from the cold-rolled coil C by the uncoiler 10. The unwinded cold-rolled steel sheet S is supplied to the annealing furnace 20 through the welding machine 11, the cleaning device 12 and the inlet looper 13. Among them, the upstream equipment between the uncoiler 10 and the annealing furnace 20 is not limited to these welding machines 11, cleaning equipment 12 and inlet looper 13, and can be a known or arbitrary device.
[0075] [Annealing furnace]
[0076] [Process (B)]
[0077] Reference Figures 1 to 3 , the annealing furnace 20 allows the cold-rolled steel sheet S to pass through the inside and perform continuous annealing. In the annealing furnace 20, a heating zone 22, a soaking zone 24 and a cooling zone 26 are provided on the upstream side in the passing direction of the sheet, and the cold-rolled steel sheet S is annealed in a reducing atmosphere containing hydrogen in the heating zone 22 and the soaking zone 24, and the cold-rolled steel sheet S is cooled in the cooling zone 26. That is, in the process (B), the cold-rolled steel sheet S is passed through the annealing furnace 20 in which the heating zone 22, the soaking zone 24 and the cooling zone 26 are provided on the upstream side in the passing direction of the sheet. The cooling zone 26 may be composed of a plurality of cooling zones. In addition, a preheating zone may be provided on the upstream side in the passing direction of the heating zone 22. It should be noted that, Figure 1The annealing furnace 20 of CAL 100 shown preferably has an over-aging zone 28 downstream of the cooling zone 26, but this is not required. Figures 1 to 3 In the figure, each belt is shown as a vertical furnace, but it is not limited to this, and can be a horizontal furnace. In the case of a vertical furnace, adjacent strips are connected via throats (throttling parts) connecting the upper parts or lower parts of each strip.
[0078] (Heating belt)
[0079] In the heating zone 22, the cold rolled steel sheet S can be directly heated by a burner, or indirectly heated by a radiation tube (RT) or an electric heater. In addition, heating can also be performed by induction heating, roller heating, resistance heating, direct electric heating, salt bath heating, electron beam heating, etc. The average temperature inside the heating zone 22 is preferably 500 to 800°C. The gas from the soaking zone 24 flows into the heating zone 22, and a reducing gas is also supplied. As the reducing gas, H 2 -N 2 Mixed gases include, for example, H 2 :1~35vol%,the rest is N 2 A gas composed of one or both of Ar and inevitable impurities (dew point: about -60°C).
[0080] (tropical zone)
[0081] The soaking zone 24 may be used to indirectly heat the cold-rolled steel sheet S using a radiant tube (RT). The average temperature inside the soaking zone 24 is preferably 600 to 950° C. A reducing gas is supplied to the soaking zone 24. As the reducing gas, H 2 -N 2 Mixed gases include, for example, H 2 :1~35vol%,the rest is N 2 A gas composed of one or both of Ar and inevitable impurities (dew point: about -60°C).
[0082] (Cooling Zone)
[0083] In the cooling zone 26, the cold-rolled steel sheet S is cooled by any of gas, a mixture of gas and water, and water. The cold-rolled steel sheet S is cooled to about 100 to 400°C in CAL and about 470 to 530°C in CGL at the stage of leaving the annealing furnace 20. A plurality of cooling nozzles are arranged along the steel sheet conveying path in the cooling zone 26. The cooling nozzle is, for example, a round tube longer than the width of the steel sheet as described in Japanese Patent Publication No. 2010-185101, and is arranged so that the extension direction of the round tube is parallel to the width direction of the steel sheet. The round tube is provided with a plurality of through holes at a predetermined interval along the extension direction of the round tube at a portion facing the steel sheet, and the water in the round tube is sprayed toward the steel sheet from the through holes. The cooling nozzles are arranged in a pair in a manner facing each other on the surface and back of the steel sheet, and a pair of cooling nozzles are arranged in a plurality of pairs (for example, 5 to 10 pairs) at a predetermined interval along the steel sheet conveying path to form a cooling zone. Moreover, the cooling zone is preferably arranged in about 3 to 6 pairs along the steel sheet conveying path.
[0084] (Aging treatment belt)
[0085] Reference Figure 1 In CAL100, the cold-rolled steel sheet S leaving the cooling zone 26 in the over-aging treatment zone 28 is supplied to at least one of isothermal holding, reheating, furnace cooling and cooling, and the cold-rolled steel sheet S is cooled to 100-400°C when leaving the annealing furnace 20.
[0086] [Downstream equipment]
[0087] [Process (C)]
[0088] Reference Figures 1 to 3 In step (C), the cold-rolled steel sheet S discharged from the annealing furnace 20 is continuously passed through the downstream equipment 30. Figure 1 , CAL100 has an outlet looper 35 and a quenching and tempering mill 36 as a downstream device 30. Figure 2 , CGL200 as downstream equipment 30, has hot dip galvanizing bath 31, gas wiping device 32, alloying furnace 33, cooling device 34, outlet looper 35 and tempering mill 36. Figure 3 , CGL300 has a hot-dip galvanizing bath 31, a gas wiping device 32, a cooling device 34, an outlet looper 35, and a quenching and tempering mill 36 as a downstream device 30. However, the downstream device 30 is not limited thereto, and may be a known or arbitrary device. For example, as the downstream device 30, a tension straightener, a chemical treatment device, a surface adjustment device, an oiling device, and an inspection device may be cited.
[0089] (Hot-dip galvanizing bath)
[0090] (Process (C-1))
[0091] Reference Figure 2 , 3 The hot-dip galvanizing bath 31 is located downstream of the annealing furnace 20 in the sheet passing direction, and the cold-rolled steel sheet S is immersed and hot-dip galvanized. That is, in step (C-1), the cold-rolled steel sheet S is immersed in the hot-dip galvanizing bath 31 located downstream of the annealing furnace 20 in the sheet passing direction, and hot-dip galvanizing is performed on the cold-rolled steel sheet S. Figure 2 , 3 The nozzle 29 connected to the cooling belt 26 is a rectangular member perpendicular to the sheet passing direction that divides the space for the cold-rolled steel sheet S to pass through, and its front end is immersed in the hot-dip galvanizing bath 31. Therefore, the annealing furnace 20 is connected to the hot-dip galvanizing bath 31. Hot-dip galvanizing can be performed according to a conventional method.
[0092] The amount of molten zinc deposited on both surfaces of the cold-rolled steel sheet S can be adjusted by blowing gas toward the cold-rolled steel sheet S from a pair of gas wiping devices 32 disposed across the cold-rolled steel sheet S pulled out from the hot-dip galvanizing bath 31 .
[0093] (Alloying furnace)
[0094] (Process (C-2))
[0095] Reference Figure 2 , the alloying furnace 33 is located downstream of the hot-dip galvanizing bath 31 and the gas wiping device 32 in the direction of passing the plate, and the cold-rolled steel sheet S is passed through the plate to heat and alloy the hot-dip galvanizing. That is, in the process (C-2), the cold-rolled steel sheet S is passed through the alloying furnace 33 located downstream of the hot-dip galvanizing bath 31 and the gas wiping device 32 in the direction of passing the plate, and the hot-dip galvanizing is heated and alloyed. The alloying treatment can be carried out according to conventional methods. The heating method in the alloying furnace 33 is not particularly limited, and examples thereof include heating with high-temperature gas and induction heating. However, the alloying furnace 33 is any equipment of the CGL, and the alloying process is any process of the method for manufacturing steel sheets using the CGL.
[0096] (Cooling device)
[0097] Reference Figure 2 , 3 The cooling device 34 is located downstream of the gas wiping device 32 and the alloying furnace 33 in the plate passing direction. The cold rolled steel sheet S can be passed through the cooling device 34 to cool the cold rolled steel sheet S. The cooling device 34 cools the cold rolled steel sheet S by water cooling, air cooling, gas cooling, mist cooling, etc.
[0098] [Tension coiler]
[0099] [Process (D)]
[0100] Reference Figures 1 to 3The cold-rolled steel sheet S passing through the downstream equipment 30 is finally wound into a product coil P by a tension coiler 50 as a winding device.
[0101] [Magnetic field applying device and magnetic field applying step]
[0102] It is important that the CAL100 of the first embodiment, the CGL200 of the second embodiment, and the CGL300 of the third embodiment have a magnetic field applying device 60 for applying a stable magnetic field to the cold-rolled steel sheet S in the sheet passing from the cooling belt 26 to the tension coiler 50 along the sheet width direction of the cold-rolled steel sheet S. That is, it is important that the manufacturing method of the steel sheet of the first embodiment, the second embodiment, and the third embodiment includes a magnetic field applying step of applying a stable magnetic field to the cold-rolled steel sheet S in the sheet passing along the sheet width direction of the cold-rolled steel sheet S after step (B-2) and before step (D). As a result, the hydrogen contained in the cold-rolled steel sheet S during annealing can be sufficiently and efficiently reduced, and a steel sheet with excellent hydrogen embrittlement resistance can be manufactured. In addition, the application of a stable magnetic field is incorporated into the manufacturing process (production line) of the steel sheet of CAL100, CGL200, or CGL300, so that the production efficiency is not impaired. In addition, since hydrogen is desorbed by applying a stable magnetic field instead of heating, there is no worry about changing the mechanical properties of the steel sheet.
[0103] (Magnetic field applying device 60)
[0104] The various embodiments of the present invention can be achieved by Figure 4 and Figure 5 The magnetic field applying device 60 shown in (A) and (B) is installed in CAL100, CGL200 or CGL300, and the magnetic field applying process uses the magnetic field applying device 60 to apply a stable magnetic field to the cold-rolled steel sheet S in the plate. Figure 4, the magnetic field applying device 60 includes a pair of electromagnets 60A and 60B respectively located on the outside of the two ends in the width direction of the cold-rolled steel sheet S. The electromagnets 60A and 60B respectively have iron cores 62A and 62B, coils 64A and 64B wound around these iron cores 62A and 62B, and a driving power supply (not shown) for passing current through these coils 64A and 64B. By turning on the driving power supply and passing a continuous DC current through the coils 64A and 64B, the electromagnets 60A and 60B can be magnetized and a stable magnetic field can be generated. The axial direction of the coils 64A and 64B is consistent with the plate width direction of the cold-rolled steel sheet S. The pair of electromagnets 60A and 60B respectively have magnetic pole faces 66A and 66B that are opposite to the end faces in the width direction of the cold-rolled steel sheet S at a predetermined interval. By controlling the direction of the current flowing through the coils 64A and 64B, one magnetic pole face 66A can be made an N pole and the other magnetic pole face 66B can be made an S pole. The pair of magnetic pole faces 66A and 66B are located at the same position in the through-sheet direction of the cold-rolled steel sheet S and face each other with the cold-rolled steel sheet S interposed therebetween. Figure 4 As shown in FIG. 1 , the main magnetic flux of the stable magnetic field generated by the pair of electromagnets 60A and 60B is directed from the magnetic pole surface 66A (N pole) to the magnetic pole surface 66B (S pole), and its direction is consistent with the width direction of the cold-rolled steel sheet S. Thus, the stable magnetic field can be uniformly applied along the width direction of the cold-rolled steel sheet S. Figure 5 As shown in (A) and (B), by arranging a plurality of such pairs of electromagnets 60A and 60B along the sheet passing direction, it is possible to fully ensure the time for applying the magnetic field to the cold-rolled steel sheet S. It should be noted that in this specification, "continuous direct current" refers to a direct current whose current value is maintained continuously (preferably constant) rather than pulsating. In addition, in this specification, "stable magnetic field" refers to a magnetic field that is maintained continuously rather than pulsating, including a magnetic field formed by a stationary magnet and a magnetic field formed by an electromagnet that supplies a continuous direct current.
[0105] It is important to apply a stable magnetic field rather than a pulsed magnetic field to the cold-rolled steel sheet S. In a pulsed magnetic field, the expansion of the lattice spacing of the steel sheet caused by the magnetostrictive effect is not continuous, and hydrogen cannot be efficiently separated from the cold-rolled steel sheet S. In addition, it is important to apply a magnetic field along the plate width direction of the cold-rolled steel sheet S. For example, when a magnetic field is applied along the plate thickness direction of the cold-rolled steel sheet S, the lattice spacing of the steel sheet expands along the plate thickness direction of the steel sheet. In this case, the hydrogen inside the steel sheet diffuses in the in-plane direction of the steel sheet and can be separated from the end face in the width direction of the steel sheet. However, since the area of the end face in the width direction of the steel sheet is small, a sufficient hydrogen separation effect cannot be obtained. In contrast, if a magnetic field is applied along the plate width direction of the cold-rolled steel sheet S, the lattice spacing of the steel sheet expands in the in-plane direction of the main surface (surface and back) of the steel sheet along the plate width direction of the steel sheet. As a result, the hydrogen inside the steel sheet diffuses to the main surface (surface and back) of the steel sheet with a large area and separates from the main surface. Therefore, a sufficient hydrogen separation effect can be obtained.
[0106] It should be noted that the arrangement of the pair of electromagnets 60A and 60B is preferably as described above, but as long as a stable magnetic field having a magnetic flux component in the plate width direction of the cold-rolled steel sheet S is generated, the arrangement is not limited. In addition, the configuration of the magnetic field applying device 60 is not limited to the pair of electromagnets 60A and 60B as long as a stable magnetic field having a magnetic flux component in the plate width direction of the cold-rolled steel sheet S is generated. For example, the magnetic field applying device 60 may be only one of the electromagnets 60A and 60B. In the case where the magnetic field formed by one electromagnet has a strength to the extent that a magnetic field along the plate width direction is applied to the entire plate width of the cold-rolled steel sheet S, there may be only one.
[0107] In the first, second and third embodiments, the position of the magnetic field applying device 60 is not limited as long as a magnetic field can be applied to the cold-rolled steel sheet S passing from the cooling belt 26 to the tension coiler 50 .
[0108] Reference Figure 1 , the preferred position of the magnetic field applying device 60 in the first embodiment of manufacturing the product coil of the cold-rolled annealed steel sheet (CR) using CAL100, that is, the preferred implementation time of the magnetic field applying process is described. As an example, the magnetic field applying device 60 can be set in the cooling belt 26. In this case, the magnetic field applying process can be performed in the process (B-2). It should be noted that it is not necessary for the magnetic field applying device 60 to be located inside the cooling belt 26 as a whole, and at least the electromagnets 60A and 60B can be located inside the cooling belt 26.
[0109] As another example, the magnetic field applying device 60 may be disposed at a position capable of applying a magnetic field to the cold-rolled steel sheet S in the downstream equipment 30. In this case, the magnetic field applying process may be performed in process (C). Specifically, the magnetic field applying device 60 may be disposed at least one of (i) between the over-aging treatment belt 28 and the exit looper 35, (ii) inside the exit looper 35, (iii) between the exit looper 35 and the quenching and tempering mill 36, and (iv) between the quenching and tempering mill 36 and the tension coiler 50.
[0110] The magnetic field applying device 60 can be provided at both the cooling belt 26 and the position where the magnetic field can be applied to the cold-rolled steel sheet S in the downstream equipment 30. That is, the magnetic field applying process can be performed in both the process (B-2) and the process (C). In addition, the magnetic field applying device 60 can be provided in the over-aging treatment belt 28, and the magnetic field applying process can be performed during the over-aging treatment.
[0111] Next, refer to Figure 2 , the preferred position of the magnetic field applying device 60 in the second embodiment of the product of alloyed hot-dip galvanized steel sheet (GA) manufactured using CGL200, that is, the preferred timing of implementing the magnetic field applying process, is described. As an example, the magnetic field applying device 60 can be set at a first position capable of applying a magnetic field to the cold-rolled steel sheet S in the upstream plate of the hot-dip galvanizing bath 31. In this case, the magnetic field applying process can be performed before the process (C-1). Specifically, the magnetic field applying device 60 can be set in the cooling belt 26. In addition, it is not necessary for the magnetic field applying device 60 to be located in the cooling belt 26 as a whole, and at least the electromagnets 60A and 60B can be located in the cooling belt 26. In addition, at least the electromagnets 60A and 60B of the magnetic field applying device 60 can also be set in the nozzle 29.
[0112] As another example, the magnetic field applying device 60 can be set at a second position capable of applying a magnetic field to the cold-rolled steel sheet S in the downstream plate passing through the hot-dip galvanizing bath 31. In this case, the magnetic field applying step can be performed after step (C-1). Specifically, the magnetic field applying device 60 can be set in at least one of (i) between the hot-dip galvanizing bath 31 and the gas wiping device 32, (ii) between the gas wiping device 32 and the alloying furnace 33, (iii) in the alloying furnace 33, (iv) in the air cooling zone between the alloying furnace 33 and the cooling device 34, (v) between the cooling device 34 and the exit looper 35, (vi) in the exit looper 35, (vii) between the exit looper 35 and the temper mill 36, and (viii) between the temper mill 36 and the tension coiler 50. It is particularly preferred to set the magnetic field applying device 60 in the air cooling zone of (iv).
[0113] From the perspective of making hydrogen more fully separated from the steel plate, the magnetic field applying device 60 is preferably set at the first position rather than the second position. That is, the magnetic field applying process is preferably performed before process (C-1) rather than after process (C-1). However, the magnetic field applying device 60 can also be set at both the first position and the second position. That is, the magnetic field applying process can also be performed both before and after process (C-1).
[0114] Next, refer to Figure 3 , the preferred position of the magnetic field applying device 60 in the third embodiment of the product of hot-dip galvanized steel sheet (GI) manufactured using CGL300, that is, the preferred timing of implementing the magnetic field applying process, is described. As an example, the magnetic field applying device 60 can be set at a first position capable of applying a magnetic field to the cold-rolled steel sheet S in the upstream plate of the hot-dip galvanizing bath 31. In this case, the magnetic field applying process can be performed before the process (C-1). Specifically, the magnetic field applying device 60 can be set in the cooling belt 26. In addition, it is not necessary for the magnetic field applying device 60 to be located inside the cooling belt 26 as a whole, and at least the electromagnets 60A and 60B can be located inside the cooling belt 26. In addition, at least the electromagnets 60A and 60B of the magnetic field applying device 60 can also be set in the nozzle 29.
[0115] As another example, the magnetic field applying device 60 can be set at a second position capable of applying a magnetic field to the cold-rolled steel sheet S in the downstream plate passing through the hot-dip galvanizing bath 31. In this case, the magnetic field applying step can be performed after step (C-1). Specifically, the magnetic field applying device 60 can be set in at least one of (i) between the hot-dip galvanizing bath 31 and the gas wiping device 32, (ii) the air cooling zone between the gas wiping device 32 and the cooling device 34, (iii) between the cooling device 34 and the exit looper 35, (iv) inside the exit looper 35, (v) between the exit looper 35 and the temper mill 36, and (vi) between the temper mill 36 and the tension coiler 50. It is particularly preferred to set the magnetic field applying device 60 in the air cooling zone of (ii).
[0116] From the perspective of making hydrogen more fully separated from the steel plate, the magnetic field applying device 60 is preferably set at the first position rather than the second position. That is, the magnetic field applying process is preferably performed before process (C-1) rather than after process (C-1). However, the magnetic field applying device 60 can also be set at both the first position and the second position. That is, the magnetic field applying process can also be performed both before and after process (C-1).
[0117] (Magnetic flux density)
[0118] From the perspective of promoting the diffusion of hydrogen and fully separating the hydrogen contained in the cold-rolled steel sheet S, the magnetic flux density in the plate width direction of the cold-rolled steel sheet S is preferably 0.1T or more, more preferably 0.2T or more, and further preferably 0.5T or more. On the other hand, considering the performance of a general magnetic field application device, the magnetic flux density in the plate width direction of the cold-rolled steel sheet S is preferably 15T or less, more preferably 14T or less. The magnetic flux density in the plate width direction of the cold-rolled steel sheet S can be adjusted by adjusting the number of turns and current value of the coil. The "magnetic flux density in the plate width direction of the cold-rolled steel sheet S" can be measured online by setting a Tesla meter near the end face of the cold-rolled steel sheet S in the width direction of the plate and near the magnetic field generating surface of the magnetic field application device 60. Alternatively, if the number of turns and current value of the coil in the magnetic field application device 60 are determined, the "magnetic flux density in the plate width direction of the cold-rolled steel sheet S" can also be pre-mastered offline.
[0119] (Magnetic field application time)
[0120] From the viewpoint of more fully reducing hydrogen from the cold-rolled steel sheet S, in the magnetic field application process, the application time of the magnetic field to the cold-rolled steel sheet S is preferably 1 second or more, more preferably 5 seconds or more, and even more preferably 10 seconds or more. On the other hand, from the viewpoint of not hindering productivity, the application time of the magnetic field to the cold-rolled steel sheet S is preferably 3600 seconds or less, more preferably 1800 seconds or less, and even more preferably 900 seconds or less. In this specification, "the application time of the magnetic field to the cold-rolled steel sheet S" refers to the time for applying the magnetic field to each position in the plate width direction of the cold-rolled steel sheet S, and when the magnetic field is applied to each position from a plurality of magnetic field application devices 60, it refers to the cumulative time. Refer to Figure 4 In the case of using a pair of electromagnets 60A and 60B, the portion of the cold-rolled steel sheet S facing the pair of electromagnets 60A and 60B can be regarded as having a magnetic field applied. Therefore, the accumulation of the time that each portion of the cold-rolled steel sheet S faces the pair of electromagnets 60A and 60B can be regarded as the magnetic field application time. The magnetic field application time can be determined by the speed of the cold-rolled steel sheet S and the position of the magnetic field application device 60 (e.g. Figure 4 The number of the pair of electromagnets 60A and 60B shown in the figure along the direction through the plate is adjusted.
[0121] [Cold rolled steel sheet]
[0122] In this embodiment, the cold-rolled steel sheet S supplied to CAL100, CGL200 and CGL300 is not particularly limited. The cold-rolled steel sheet S preferably has a thickness of less than 6 mm, and examples thereof include high-strength steel sheets and stainless steel sheets having a tensile strength of 590 MPa or more.
[0123] [Composition of cold-rolled steel sheets: high-strength steel sheets]
[0124] The component composition in the case where the cold-rolled steel sheet S is a high-strength steel sheet will be described. Hereinafter, "mass %" will be simply referred to as "%".
[0125] C: 0.030~0.800%
[0126] C has the effect of increasing the strength of the steel sheet. From the viewpoint of obtaining this effect, the C content is 0.030% or more, preferably 0.080% or more. However, when the C content is excessive, the steel sheet becomes significantly brittle regardless of the amount of hydrogen in the steel sheet. Therefore, the C content is 0.800% or less, preferably 0.500% or less.
[0127] Si: 0.01~3.00%
[0128] Si has the effect of increasing the strength of the steel sheet. From the viewpoint of obtaining this effect, the amount of Si is 0.01% or more, preferably 0.10% or more. However, when the amount of Si is excessive, the steel sheet becomes brittle and the ductility decreases, or red scale is generated and the surface properties deteriorate, or the plating quality decreases. Therefore, the amount of Si is 3.00% or less, preferably 2.50% or less.
[0129] Mn: 0.01~10.00%
[0130] Mn has the effect of improving the strength of the steel plate by solid solution strengthening. From the viewpoint of obtaining this effect, the amount of Mn is 0.01% or more, preferably 0.5% or more. However, when the amount of Mn is excessive, sometimes unevenness is easily generated in the steel structure due to the segregation of Mn, and hydrogen embrittlement starting from the unevenness becomes obvious. Therefore, the amount of Mn is 10.00% or less, preferably 8.00% or less.
[0131] P: 0.001~0.100%
[0132] P is an element that has a solid solution strengthening effect and can be added according to the desired strength. From the viewpoint of obtaining such an effect, the P content is 0.001% or more, preferably 0.003% or more. However, when the P content is excessive, weldability deteriorates, and when galvanizing is alloyed, the alloying speed decreases, and the quality of galvanizing is impaired. Therefore, the P content is 0.100% or less, preferably 0.050% or less.
[0133] S: 0.0001~0.0200%
[0134] S segregates at grain boundaries and embrittles steel during hot working, and exists as sulfides to reduce local deformability. Therefore, the S content is 0.0200% or less, preferably 0.0100% or less, and more preferably 0.0050% or less. On the other hand, from the perspective of production technology constraints, the S content is 0.0001% or more.
[0135] N: 0.0005~0.0100%
[0136] N is an element that deteriorates the aging resistance of steel. Therefore, the N content is 0.0100% or less, preferably 0.0070% or less. The less the N content, the better. However, considering the constraints of production technology, the N content is 0.0005% or more, preferably 0.0010% or more.
[0137] Al: 0.001~2.000%
[0138] Al is an element that acts as a deoxidizer and is effective for the cleanliness of steel. From the perspective of obtaining this effect, the Al content is 0.001% or more, preferably 0.010% or more. However, when the Al content is excessive, cracks in the steel sheet may occur during continuous casting. Therefore, the Al content is 2.000% or less, preferably 1.200% or less.
[0139] The remainder other than the above components is Fe and inevitable impurities. However, at least one element selected from the following may be arbitrarily contained.
[0140] Ti: 0.200% or less
[0141] Ti contributes to the improvement of the strength of the steel sheet by precipitation strengthening of the steel and fine grain strengthening obtained by suppressing the growth of ferrite grains. Therefore, when adding Ti, the amount of Ti is preferably 0.005% or more, and more preferably 0.010% or more. However, when the amount of Ti is excessive, carbonitrides sometimes precipitate in large quantities, and the formability is reduced. Therefore, when adding Ti, the amount of Ti is set to 0.200% or less, preferably 0.100% or less.
[0142] Nb: 0.200% or less, V: 0.500% or less, W: 0.500% or less
[0143] Nb, V and W are effective for precipitation strengthening of steel. Therefore, when Nb, V and W are added, the content of each element is preferably 0.005% or more, and more preferably 0.010% or more. However, when each content is excessive, carbonitrides sometimes precipitate in large quantities, and formability decreases. Therefore, when Nb is added, the amount of Nb is 0.200% or less, and preferably 0.100% or less. When V and W are added, the content of each element is 0.500% or less, and preferably 0.300% or less.
[0144] B: 0.0050% or less
[0145] B is effective for strengthening the grain boundary and increasing the strength of the steel sheet. Therefore, when B is added, the amount of B is preferably 0.0003% or more. However, when the amount of B is excessive, the formability is sometimes reduced. Therefore, when B is added, the amount of B is 0.0050% or less, preferably 0.0030% or less.
[0146] Ni: 1.000% or less
[0147] Ni is an element that improves the strength of steel by solid solution strengthening. Therefore, when Ni is added, the amount of Ni is preferably 0.005% or more. However, when the amount of Ni is excessive, the area ratio of hard martensite becomes too large, and during a tensile test, micropores at the grain boundaries of martensite increase, and cracks propagate, and sometimes ductility decreases. Therefore, when Ni is added, the amount of Ni is 1.000% or less.
[0148] Cr: 1.000% or less, Mo: 1.000% or less
[0149] Cr and Mo have the effect of improving the balance between strength and formability. Therefore, when adding Cr and Mo, the content of each element is preferably 0.005% or more. However, when the content is excessive, the area ratio of hard martensite becomes too large, and during the tensile test, micropores at the grain boundaries of martensite increase, cracks propagate, and ductility sometimes decreases. Therefore, when adding Cr and Mo, the content of each element is 1.000% or less.
[0150] Cu: 1.000% or less
[0151] Cu is an element effective in strengthening steel. Therefore, when Cu is added, the Cu amount is preferably 0.005% or more. However, when the Cu amount is excessive, the area ratio of hard martensite becomes too large, and during the tensile test, micropores at the grain boundaries of tempered martensite increase, and cracks extend, and sometimes ductility decreases. Therefore, when Cu is added, the Cu amount is 1.000% or less.
[0152] Sn: 0.200% or less, Sb: 0.200% or less
[0153] Sn and Sb are effective in suppressing decarburization of the surface layer of the steel sheet of about tens of μm caused by nitridation and oxidation of the steel sheet surface, and ensuring strength and material stability. Therefore, when Sn and Sb are added, the content of each element is preferably 0.002% or more. However, when the content is excessive, toughness may decrease. Therefore, when Sn and Sb are added, the content of each element is 0.200% or less.
[0154] Ta: 0.100% or less
[0155] Ta, like Ti and Nb, generates alloy carbides and alloy carbonitrides and contributes to high strength. In addition, it is believed that it has the following effects: a part of it is dissolved in Nb carbides and Nb carbonitrides to generate composite precipitates such as (Nb, Ta) (C, N), thereby significantly inhibiting the coarsening of precipitates and stabilizing the precipitation strengthening effect on strength. Therefore, when Ta is added, the amount of Ta is preferably 0.001% or more. However, even if Ta is added excessively, the precipitate stabilization effect is sometimes saturated, and the alloy cost is also increased. Therefore, when Ta is added, the amount of Ta is 0.100% or less.
[0156] Ca: 0.0050% or less, Mg: 0.0050% or less, Zr: 0.1000% or less, REM (Rare Earth Metal): 0.0050% or less
[0157] Ca, Mg, Zr and REM are effective elements for spheroidizing the shape of sulfides and improving the adverse effects of sulfides on formability. When these elements are added, the content of each element is preferably 0.0005% or more. However, when the content is excessive, inclusions and the like may increase, causing surface and internal defects. Therefore, when these elements are added, the content of each element is 0.0050% or less.
[0158] [Composition of cold-rolled steel sheet: stainless steel sheet]
[0159] The component composition in the case where the cold-rolled steel sheet S is a stainless steel sheet will be described. Hereinafter, "mass %" will be simply referred to as "%".
[0160] C: 0.001~0.400%
[0161] C is an indispensable element for obtaining high strength in stainless steel. However, it combines with Cr during tempering in steel production and precipitates as carbides, which deteriorates the corrosion resistance and toughness of the steel. If the C content is less than 0.001%, sufficient strength cannot be obtained, and if it exceeds 0.400%, the above-mentioned deterioration becomes significant. Therefore, the C content is 0.001 to 0.400%.
[0162] Si: 0.01~2.00%
[0163] Si is an element useful as a deoxidizer. From the viewpoint of obtaining this effect, the amount of Si is 0.01% or more. However, when the amount of Si is excessive, Si dissolved in the steel reduces the workability of the steel. Therefore, Si is 2.00% or less.
[0164] Mn: 0.01~5.00%
[0165] Mn has the effect of increasing the strength of steel. From the viewpoint of obtaining this effect, the amount of Mn is 0.01% or more. However, when the amount of Mn is excessive, the workability of steel decreases. Therefore, the amount of Mn is 5.00% or less.
[0166] P: 0.001~0.100%
[0167] P is an element that promotes grain boundary destruction due to grain boundary segregation. Therefore, the lower the P content, the better, and it is 0.100% or less, preferably 0.030% or less, and more preferably 0.020% or less. On the other hand, the P content is 0.001% or more in view of the constraints of production technology.
[0168] S: 0.0001~0.0200%
[0169] S exists as sulfide inclusions such as MnS, which reduces ductility, corrosion resistance, etc. Therefore, the lower the S content, the better, and is 0.0200% or less, preferably 0.0100% or less, and more preferably 0.0050% or less. On the other hand, the S content is 0.0001% or more in view of the constraints of production technology.
[0170] Cr: 9.0~28.0%
[0171] Cr is a basic element constituting stainless steel and an important element showing corrosion resistance. Considering the corrosion resistance in a harsh environment above 180°C, if the Cr content is less than 9.0%, sufficient corrosion resistance cannot be obtained, and if it exceeds 28.0%, the effect is saturated, which is problematic from an economic point of view. Therefore, the Cr content is 9.0 to 28.0%.
[0172] Ni: 0.01~40.0%
[0173] Ni is an element that improves the corrosion resistance of stainless steel. If the Ni content is less than 0.01%, this effect cannot be fully exerted. On the other hand, if the Ni content is excessive, the formability is deteriorated and stress corrosion cracking is easily generated. Therefore, the Ni content is 0.01 to 40.0%.
[0174] N: 0.0005~0.500%
[0175] N is an element that is harmful to the improvement of the corrosion resistance of stainless steel. Therefore, the amount of N is 0.500% or less, preferably 0.200% or less. The less the amount of N, the better, but considering the constraints of production technology, the amount of N is 0.0005% or more.
[0176] Al: 0.001~3.000%
[0177] Al acts as a deoxidizer and also has the effect of inhibiting oxide scale peeling. From the perspective of obtaining these effects, the Al content is 0.001% or more. However, excessive Al content leads to a decrease in elongation and deterioration of surface quality. Therefore, the Al content is 3.000% or less.
[0178] The remainder other than the above components is Fe and inevitable impurities. However, at least one element selected from the following may be arbitrarily contained.
[0179] Ti: 0.500% or less
[0180] Ti combines with C, N and S to improve corrosion resistance, intergranular corrosion resistance and deep drawability. However, when the amount of Ti exceeds 0.500%, the toughness deteriorates due to solid solution Ti. Therefore, when Ti is added, the amount of Ti is 0.500% or less.
[0181] Nb: 0.500% or less
[0182] Nb, like Ti, combines with C, N, and S to improve corrosion resistance, intergranular corrosion resistance, and deep drawing properties. In addition, in addition to improving workability and high temperature strength, it promotes the suppression of crevice corrosion and repassivation. However, excessive addition leads to hardening and deteriorates formability. Therefore, when Nb is added, the amount of Nb is 0.500% or less.
[0183] V: 0.500% or less
[0184] V suppresses crevice corrosion. However, excessive addition deteriorates formability. Therefore, when V is added, the amount of V is 0.500% or less.
[0185] W: 2.000% or less
[0186] W contributes to the improvement of corrosion resistance and high temperature strength. However, excessive addition leads to deterioration of toughness during steel plate production and increased costs. Therefore, when W is added, the amount of W is 2.000% or less.
[0187] B: 0.0050% or less
[0188] B improves the secondary workability of the product by segregating at the grain boundaries. However, excessive addition leads to a decrease in workability and corrosion resistance. Therefore, when B is added, the amount of B is 0.0050% or less.
[0189] Mo: 2.000% or less
[0190] Mo is an element that improves corrosion resistance, and in particular suppresses crevice corrosion. However, excessive addition deteriorates formability. Therefore, when Mo is added, the amount of Mo is 2.000% or less.
[0191] Cu: 3.000% or less
[0192] Cu is an austenite stabilizing element like Ni and Mn, and is effective for the refinement of grains caused by phase transformation. In addition, it promotes the suppression of crevice corrosion and repassivation. However, excessive addition deteriorates toughness and formability. Therefore, when Cu is added, the amount of Cu is 3.000% or less.
[0193] Sn: 0.500% or less
[0194] Sn contributes to the improvement of corrosion resistance and high temperature strength. However, excessive addition may cause slab cracks during steel sheet production. Therefore, when Sn is added, the amount of Sn is 0.500% or less.
[0195] Sb: 0.200% or less
[0196] Sb has the effect of segregating at grain boundaries to improve high temperature strength. However, excessive addition may cause cracks during welding due to Sb segregation. Therefore, when Sb is added, the Sb amount is 0.200% or less.
[0197] Ta: 0.100% or less
[0198] Ta combines with C and N to contribute to the improvement of toughness. However, excessive addition saturates this effect, resulting in an increase in manufacturing cost. Therefore, when Ta is added, the amount of Ta is 0.100% or less.
[0199] Ca: 0.0050% or less, Mg: 0.0050% or less, Zr: 0.1000% or less, REM (Rare Earth Metal): 0.0050% or less
[0200] Ca, Mg, Zr and REM are effective elements for spheroidizing the shape of sulfides and improving the adverse effects of sulfides on formability. When these elements are added, the content of each element is preferably 0.0005% or more. However, when the content is excessive, inclusions and the like may increase, causing surface and internal defects. Therefore, when these elements are added, the content of each element is 0.0050% or less.
[0201] [Diffusible hydrogen content]
[0202] In this embodiment, in order to ensure good ductility, the amount of diffusible hydrogen in the product coil is preferably 0.50 mass ppm or less, more preferably 0.30 mass ppm or less, and further preferably 0.20 mass ppm or less. It should be noted that there is no particular lower limit for the amount of diffusible hydrogen in the product coil, but considering the constraints of production technology, the amount of diffusible hydrogen in the product coil may be 0.01 mass ppm or more.
[0203] Here, the method for determining the amount of diffusible hydrogen in the product coil is as follows. Take a test piece with a length of 30 mm and a width of 5 mm from the product coil. In the case of a product coil of hot-dip galvanized steel sheet or alloyed hot-dip galvanized steel sheet, remove the hot-dip galvanized layer or alloyed hot-dip galvanized layer of the test piece by grinding or alkali. Then, the amount of hydrogen released from the test piece is measured by thermal desorption spectroscopy (TDS). Specifically, the test piece is continuously heated from room temperature to 300°C at a heating rate of 200°C / h, and then cooled to room temperature. The cumulative amount of hydrogen released from the test piece from room temperature to 210°C is measured to obtain the diffusible hydrogen amount of the product coil.
[0204] Example
[0205] Steel having a composition containing the elements shown in Table 1 and the remainder consisting of Fe and inevitable impurities was melted in a converter and made into slabs by continuous casting. The obtained slabs were hot rolled and cold rolled to obtain cold rolled coils. As shown in Table 2, in some levels, the steel was Figure 1 The CAL shown manufactures cold rolled annealed steel (CR) product coils, among other levels, using Figure 2 The CGL shown here does not perform heat alloying to produce hot-dip galvanized steel (GI) product coils. In the remaining levels, Figure 2 The CGL shown manufactures product coils of alloyed hot-dip galvannealed steel (GA).
[0206] Use at each level Figure 4 and Figure 5 The magnetic field applying devices shown in (A) and (B) apply a stable magnetic field to the cold-rolled steel sheet in the plate along the plate width direction under the conditions of the magnetic flux density (plate width direction) and magnetic field application time shown in Table 2. The "magnetic field application location" in Table 2 indicates the area where the magnetic field application process of CAL or CGL is performed, that is, the place where the magnetic field applying device is installed.
[0207] “(B-2)” means that a magnetic field applying device is provided in the cooling zone in CAL and CGL, and the magnetic field applying step is performed using the cooling zone in step (B-2).
[0208] “(C)” means that a magnetic field applying device is provided at a position in the CAL where a magnetic field can be applied to the cold-rolled steel sheet in the downstream equipment, and means that a magnetic field applying device is provided at a position downstream of the cooling zone and upstream of the tension coiler, specifically, at least one of (i) between the overaging zone 28 and the exit looper 35, (ii) inside the exit looper 35, (iii) between the exit looper 35 and the temper mill 36, and (iv) between the temper mill 36 and the tension coiler 50. That is, “(C)” means that step (C) is performed in the CAL, specifically, the magnetic field applying step is performed at at least one of the above-mentioned (i) to (iv).
[0209] “Before (C-1)” means that a magnetic field applying device is provided at a position downstream of the cooling zone and upstream of the hot dip galvanizing bath in the CGL, specifically at the nozzle 29, and a magnetic field applying step is performed after step (B-2) and before step (C-1).
[0210] “After (C-1)” means that a magnetic field applying device is provided at a position downstream of the hot-dip galvanizing bath and upstream of the tension coiler in the CGL, specifically, at least one of (i) between the hot-dip galvanizing bath 31 and the gas wiping device 32, (ii) between the gas wiping device 32 and the alloying furnace 33, (iii) inside the alloying furnace 33, (iv) in the air cooling zone between the alloying furnace 33 and the cooling device 34, (v) between the cooling device 34 and the exit looper 35, (vi) inside the exit looper 35, (vii) between the exit looper 35 and the temper mill 36, and (viii) between the temper mill 36 and the tension coiler 50. After step (C-1), specifically, a magnetic field applying step is performed at at least one of the above-mentioned positions (i) to (viii).
[0211] Steel sheet samples were taken from the product coils obtained at each level, and their tensile properties and hydrogen embrittlement resistance were evaluated as follows. The results are shown in Table 2.
[0212] The tensile test was conducted according to JIS Z 2241 (2011) using a JIS No. 5 test piece in which a sample was taken so that the tensile direction was perpendicular to the rolling direction of the steel sheet, and TS (tensile strength) and EL (total elongation) were measured.
[0213] The hydrogen embrittlement resistance is evaluated as follows according to the tensile test. When the value obtained by dividing the EL of the steel sheet after the magnetic field is applied measured above by the EL' when the hydrogen content in the steel of the same steel sheet is 0.00 mass ppm is 0.70 or more, the hydrogen embrittlement resistance is judged to be good. It should be noted that EL' is measured by leaving the same steel sheet in the atmosphere for a long time to reduce the hydrogen in the steel inside, and then confirming that the hydrogen content in the steel is 0.00 mass ppm by TDS and then conducting a tensile test.
[0214] The amount of diffusible hydrogen in the product coils obtained at each level was measured according to the method described above, and the results are shown in Table 2.
[0215] In the examples of the present invention, since the magnetic field application step is performed, a steel sheet having excellent hydrogen embrittlement resistance can be manufactured.
[0216]
[0217]
[0218]
[0219] Industrial Applicability
[0220] According to the continuous annealing apparatus, the continuous hot-dip galvanizing apparatus, and the method for manufacturing a steel sheet of the present invention, a steel sheet having excellent hydrogen embrittlement resistance can be manufactured without impairing production efficiency or changing mechanical properties.
[0221] Explanation of symbols
[0222] 100 continuous annealing device
[0223] 200 continuous hot dip galvanizing device
[0224] 300 continuous hot dip galvanizing device
[0225] 10 Unwinding machine
[0226] 11Welding Machine
[0227] 12. Cleaning Equipment
[0228] 13 Entrance Looper
[0229] 20 Annealing furnace
[0230] 22 Heating belt
[0231] 24 Tropical
[0232] 26 Cooling belt
[0233] 28 Over-aging treatment belt
[0234] 29 Nozzle
[0235] 30 Downstream equipment
[0236] 31 Hot dip galvanizing bath
[0237] 32 Gas wiping device
[0238] 33 Alloying furnace
[0239] 34Cooling device
[0240] 35 Export Looper
[0241] 36Quenching and Tempering Mill
[0242] 50 tension coiler
[0243] 60 Magnetic field application device
[0244] 60A electromagnet (magnetic field applying device)
[0245] 60B electromagnet (magnetic field applying device)
[0246] 62A core
[0247] 62B core
[0248] 64A Coil
[0249] 64B Coil
[0250] 66A magnetic pole surface (N pole)
[0251] 66B magnetic pole surface (S pole)
[0252] C Cold Rolled Coil
[0253] S cold rolled steel sheet
[0254] P Product Coil
Claims
1. A continuous annealing device, comprising: Unwinding machine, unwinding cold rolled steel sheets from cold rolled coils, an annealing furnace, wherein the cold-rolled steel sheet is passed through the annealing furnace to perform continuous annealing, wherein a heating zone, a soaking zone, and a cooling zone are provided on the upstream side of the passing direction of the annealing furnace, wherein the cold-rolled steel sheet is annealed in a reducing atmosphere containing hydrogen in the heating zone and the soaking zone, and the cold-rolled steel sheet is cooled in the cooling zone; Downstream equipment, allowing the cold-rolled steel sheet discharged from the annealing furnace to continue to pass through the plate; A tension coiler, for coiling the cold-rolled steel plate in the downstream equipment; as well as The magnetic field applying device applies a stable magnetic field along the sheet width direction of the cold-rolled steel sheet to the cold-rolled steel sheet being passed from the cooling belt to the tension coiler.
2. The continuous annealing device according to claim 1, in, The magnetic field applying device is disposed in the cooling zone.
3. The continuous annealing device according to claim 1 or 2, in, The magnetic field applying device is disposed at a position capable of applying a magnetic field to the cold-rolled steel sheet passing through the downstream equipment.
4. The continuous annealing device according to any one of claims 1 to 3, in, The magnetic field applying device includes an electromagnet located outside an end portion in the width direction of the cold-rolled steel sheet, and the electromagnet has a magnetic pole surface facing an end surface in the width direction of the cold-rolled steel sheet.
5. The continuous annealing device according to any one of claims 1 to 3, in, The magnetic field application device includes a pair of electromagnets respectively located on the outside of the two ends of the cold-rolled steel plate in the width direction, and the pair of electromagnets respectively have magnetic pole surfaces facing the end surfaces of the cold-rolled steel plate in the width direction, one of the magnetic pole surfaces is an N pole and the other is an S pole.
6. The continuous annealing device according to any one of claims 1 to 5, in, The magnetic field applying device is set so that the magnetic flux density in the sheet width direction of the cold-rolled steel sheet is 0.1 to 15 T.
7. A continuous hot-dip galvanizing device, comprising: The continuous annealing device according to claim 1; and The hot-dip galvanizing bath, as the downstream equipment, is located downstream of the annealing furnace in the sheet passing direction, and immerses the cold-rolled steel sheets to perform hot-dip galvanizing on the cold-rolled steel sheets.
8. The continuous hot-dip galvanizing device according to claim 7, in, The magnetic field applying device is provided at a position capable of applying a magnetic field to the cold-rolled steel sheet passing through the upstream side of the hot-dip galvanizing bath.
9. The continuous hot-dip galvanizing device according to claim 7 or 8, in, The magnetic field applying device is provided at a position capable of applying a magnetic field to the cold-rolled steel sheet passing through the downstream of the hot-dip galvanizing bath.
10. The continuous hot-dip galvanizing device according to claim 7, in, As the downstream equipment, an alloying furnace is provided. The alloying furnace is located downstream of the hot-dip galvanizing bath in the direction of passing the hot-dip galvanizing bath, and the cold-rolled steel sheet is passed through to heat and alloy the hot-dip galvanizing.
11. The continuous hot-dip galvanizing device according to claim 10, in, The magnetic field applying device is provided at a position capable of applying a magnetic field to the cold-rolled steel sheet passing through the upstream side of the hot-dip galvanizing bath.
12. The continuous hot-dip galvanizing device according to claim 10 or 11, in, The magnetic field applying device is provided at a position capable of applying a magnetic field to the cold-rolled steel sheet passing through the downstream of the hot-dip galvanizing bath.
13. The continuous hot-dip galvanizing device according to any one of claims 7 to 12, in, The magnetic field applying device includes an electromagnet located outside an end portion in the width direction of the cold-rolled steel sheet, and the electromagnet has a magnetic pole surface facing an end surface in the width direction of the cold-rolled steel sheet.
14. The continuous hot-dip galvanizing device according to any one of claims 7 to 12, in, The magnetic field application device includes a pair of electromagnets respectively located on the outside of the two ends of the cold-rolled steel plate in the width direction, and the pair of electromagnets respectively have magnetic pole surfaces facing the end surfaces of the cold-rolled steel plate in the width direction, one of the magnetic pole surfaces is an N pole and the other is an S pole.
15. The continuous hot-dip galvanizing device according to any one of claims 7 to 14, in, The magnetic field applying device is set so that the magnetic flux density in the sheet width direction of the cold-rolled steel sheet is 0.1 to 15 T.
16. A method for manufacturing a steel plate, comprising the following steps in sequence: (A) A process of unwinding a cold-rolled steel sheet from a cold-rolled coil using an unwinding machine; (B) a step of passing the cold-rolled steel sheet through an annealing furnace provided with a heating zone, a soaking zone and a cooling zone on the upstream side of the passing direction, and performing continuous annealing, wherein the continuous annealing is (B-1) annealing the cold-rolled steel sheet in a reducing atmosphere containing hydrogen in the heating zone and the soaking zone, and (B-2) cooling the cold-rolled steel sheet in the cooling zone; (C) a step of continuing to pass the cold-rolled steel sheet discharged from the annealing furnace; and (D) a step of winding the cold-rolled steel sheet using a tension coiler to produce a product coil, After step (B-2) and before step (D), the method further includes a magnetic field applying step of applying a stable magnetic field to the cold-rolled steel sheet in the sheet width direction of the cold-rolled steel sheet.
17. The method for manufacturing a steel plate according to claim 16, in, The magnetic field application step is performed in step (B-2).
18. The method for manufacturing a steel plate according to claim 16 or 17, in, The magnetic field application step is performed in step (C).
19. The method for manufacturing a steel plate according to claim 16, in, The step (C) includes (C-1) the step of immersing the cold-rolled steel sheet in a hot-dip galvanizing bath located downstream in the sheet-passing direction of the annealing furnace to perform hot-dip galvanizing on the cold-rolled steel sheet.
20. The method for manufacturing a steel plate according to claim 19, in, The magnetic field application step is performed before the step (C-1).
21. The method for manufacturing a steel plate according to claim 19 or 20, in, The magnetic field application step is performed after the step (C-1).
22. The method for manufacturing a steel plate according to claim 19, in, The step (C) includes, after the step (C-1), the step (C-2): passing the cold-rolled steel sheet through an alloying furnace located downstream in the direction of passing the hot-dip galvanizing bath to heat and alloy the hot-dip galvanized sheet.
23. The method for manufacturing a steel plate according to claim 22, in, The magnetic field application step is performed before the step (C-1).
24. The method for manufacturing a steel plate according to claim 22 or 23, in, The magnetic field application step is performed after the step (C-1).
25. The method for producing a steel plate according to any one of claims 16 to 24, in, In the magnetic field applying step, the magnetic flux density of the cold-rolled steel sheet in the sheet width direction is set to 0.1 to 15 T.
26. The method for producing a steel plate according to any one of claims 16 to 25, in, In the magnetic field applying step, the stable magnetic field is applied by a magnetic field applying device including an electromagnet located outside the widthwise end of the cold-rolled steel sheet, the electromagnet having a magnetic pole surface facing the widthwise end surface of the cold-rolled steel sheet.
27. The method for producing a steel plate according to any one of claims 16 to 25, in, In the magnetic field application process, the stable magnetic field is applied using a magnetic field application device, which includes a pair of electromagnets located on the outside of the two end portions in the width direction of the cold-rolled steel plate, respectively. The pair of electromagnets respectively have magnetic pole surfaces facing the end surfaces in the width direction of the cold-rolled steel plate, one of the magnetic pole surfaces is an N pole, and the other is an S pole.
28. The method for producing a steel plate according to any one of claims 16 to 27, in, The cold-rolled steel sheet is a high-strength steel sheet having a tensile strength of 590 MPa or more.
29. The method for producing a steel plate according to any one of claims 16 to 28, in, The cold-rolled steel sheet has the following composition: in mass %, it contains C: 0.030-0.800%, Si: 0.01-3.00%, Mn: 0.01-10.00%, P: 0.001-0.100%, S: 0.0001-0.0200%, N: 0.0005-0.0100% and Al: 0.001-2.000%, and the remainder is composed of Fe and inevitable impurities.
30. The method for manufacturing a steel plate according to claim 29, in, The component composition further contains, in mass%, at least one element selected from the group consisting of Ti: 0.200% or less, Nb: 0.200% or less, V: 0.500% or less, W: 0.500% or less, B: 0.0050% or less, Ni: 1.000% or less, Cr: 1.000% or less, Mo: 1.000% or less, Cu: 1.000% or less, Sn: 0.200% or less, Sb: 0.200% or less, Ta: 0.100% or less, Ca: 0.0050% or less, Mg: 0.0050% or less, Zr: 0.1000% or less, and REM: 0.0050% or less.
31. The method for producing a steel plate according to any one of claims 16 to 27, in, The cold-rolled steel sheet is a stainless steel sheet having the following composition, which contains, by mass%, C: 0.001-0.400%, Si: 0.01-2.00%, Mn: 0.01-5.00%, P: 0.001-0.100%, S: 0.0001-0.0200%, Cr: 9.0-28.0%, Ni: 0.01-40.0%, N: 0.0005-0.500% and Al: 0.001-3.000%, and the remainder is composed of Fe and inevitable impurities.
32. The method for manufacturing a steel plate according to claim 31, in, The component composition further contains, in mass %, at least one element selected from the group consisting of Ti: 0.500% or less, Nb: 0.500% or less, V: 0.500% or less, W: 2.000% or less, B: 0.0050% or less, Mo: 2.000% or less, Cu: 3.000% or less, Sn: 0.500% or less, Sb: 0.200% or less, Ta: 0.100% or less, Ca: 0.0050% or less, Mg: 0.0050% or less, Zr: 0.1000% or less, and REM: 0.0050% or less.
33. The method for producing a steel plate according to any one of claims 16 to 32, in, The product coil has a diffusible hydrogen content of 0.50 mass ppm or less.