Coated electric wire
By using fluorine-containing copolymers containing tetrafluoroethylene, hexafluoropropylene and fluoroalkyl vinyl ether units, the melt flow rate is adjusted to form a coating with uniform thickness, and the coating wires in the prior art are solved at high temperature heat in the high temperature in the prior art The problem of insufficient heat resistance in water achieves excellent tensile creep resistance and ductility, and reduces crack occurrence.
Patent Information
- Application Number
- CN202380029089.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-08-26
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-12
AI Technical Summary
When the existing coated wire is used in high-temperature hot water for a long time, it is difficult to maintain excellent tensile creep resistance and ductility, and it is easy to cause cracks when heated in a winding state.
The fluorine-containing copolymer containing tetrafluoroethylene, hexafluoropropylene and fluoroalkyl vinyl ether units is used as the coating material, and the melt flow rate is adjusted within the range of 5.6 g/10 minutes to 8.9 g/10 minutes, and then the melt flow rate is adjusted. The extrusion molding method forms a coating with uniform thickness.
It realizes excellent tensile creep resistance and ductility of 150°C after long use in high-temperature hot water, reduces cracks during heating in the winding state, and ensures heat resistance and stability of the coating. sex.
Smart Images

Figure BDA0005051980750000071 
Figure BDA0005051980750000161 
Figure BDA0005051980750000201
Abstract
Description
Technical Field
[0001] The present invention relates to a covered electric wire. Background Art
[0002] Patent document 1 describes an electric wire or cable coated with a fluorine-containing polymer, wherein the total amount (ppm) of alkali metals and alkaline earth metals contained in the fluorine-containing polymer does not exceed the value calculated by the melt flow rate (MFR) (g / 10 min, ASTM D2116) at 372° C. according to the following formula (1) and exceeds the value calculated by the following formula (2).
[0003] 5.2×e 0.125(MFR) +2 (1)
[0004] 0.35×e 0.125(MFR) (2)
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 01 / 018076 Summary of the invention
[0008] Problems to be solved by the invention
[0009] An object of the present invention is to provide a covered electric wire having a covering layer which has a uniform thickness and can be easily formed by an extrusion molding method, wherein the covering layer can maintain excellent tensile creep resistance at 150°C, excellent ductility to a tensile force applied at 150°C, and excellent deformation resistance to a tensile load applied at 150°C even after being placed in hot water at high temperature for a long time, and is unlikely to crack even if the covering layer is heated for a long time in a state of being wound around a cylinder with a small diameter after being placed in hot water at high temperature for a long time.
[0010] Means for solving problems
[0011] According to the present invention, there is provided a covered electric wire comprising a core wire and a covering layer provided around the core wire, wherein the covering layer contains a fluorinated copolymer, the fluorinated copolymer containing a tetrafluoroethylene unit, a hexafluoropropylene unit and a fluoro(alkyl vinyl ether) unit, the content of the hexafluoropropylene unit in the fluorinated copolymer is 9.5% by mass to 10.5% by mass relative to all monomer units, the content of the fluoro(alkyl vinyl ether) unit in the fluorinated copolymer is 0% by mass to 0.3% by mass relative to all monomer units, and the melt flow rate of the fluorinated copolymer at 372° C. is 5.6 g / 10 min to 8.9 g / 10 min.
[0012] Effects of the Invention
[0013] According to the present invention, there can be provided a covered electric wire having a covering layer which has a uniform thickness and can be easily formed by an extrusion molding method, wherein the covering layer can maintain excellent tensile creep resistance at 150°C, excellent ductility to a tensile force applied at 150°C, and excellent deformation resistance to a tensile load applied at 150°C even after being placed in hot water at high temperature for a long time, and is unlikely to cause cracks even when the covering layer is heated for a long time in a state of being wound around a cylinder with a small diameter after being placed in hot water at high temperature for a long time. DETAILED DESCRIPTION
[0014] Hereinafter, specific embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments.
[0015] The covered electric wire of the present invention comprises a core wire and a covering layer provided around the core wire, wherein the covering layer contains a tetrafluoroethylene (TFE) unit, a hexafluoropropylene (HFP) unit and a fluoro(alkyl vinyl ether) (FAVE) unit.
[0016] Fluororesins are excellent in electrical properties and are therefore used as a covering material for electric wires as described in Patent Document 1. Fluororesins are also excellent in heat resistance and are therefore also used as a covering material for heat-resistant electric wires used in high-temperature environments.
[0017] However, fluororesins conventionally used as covering materials for electric wires are only assumed to be used in high-temperature environments, and have a problem of not having sufficient heat resistance when used as covering materials for electric wires placed in hot water for a long time.
[0018] Therefore, the present inventors have conducted intensive studies on a fluororesin that can easily form a coating layer with no thickness fluctuation and can form a coating layer that can protect an electric wire even when left in hot water for a long time. As a result, the present inventors have found that, by using a fluorinated copolymer containing a TFE unit, an HFP unit, and a FAVE unit, and adjusting the contents of the HFP unit and the FAVE unit and the melt flow rate to extremely limited ranges as a coating material, the electric wire can be protected at a high level that has not been achieved before, even when used as a coating material for an electric wire left in hot water for a long time, thereby completing the present invention.
[0019] That is, the covered electric wire of the present invention has a coating layer containing a fluorinated copolymer in which the content of the HFP unit and the FAVE unit and the melt flow rate are appropriately adjusted. The coating layer is formed by such a fluorinated copolymer, so it can be easily formed by extruding the molten fluorinated copolymer onto the core wire, and it is also easy to make the thickness of the coating layer uniform. In addition, even after the coating layer is placed in hot water at a high temperature of 150°C for a long time, it can maintain excellent 150°C tensile creep resistance, excellent ductility to tensile force applied at 150°C, and excellent deformation resistance to tensile loads loaded at 150°C. Furthermore, after being placed in hot water at a high temperature for a long time, it is not easy to crack even if it is further heated for a long time when it is further wound in a cylinder with a small diameter.
[0020] The copolymer contained in the coating layer is a melt-processable fluororesin. Melt-processability means that the polymer can be melted and processed using existing processing machines such as an extruder and an injection molding machine.
[0021] Examples of FAVE constituting the FAVE unit include those selected from the general formula (1):
[0022] CF 2 =CFO(CF 2 CFY 1 O) p -(CF 2 CF 2 CF 2 O) q -Rf (1)
[0023] (Where Y 1 Indicates F or CF 3 , Rf represents a perfluoroalkyl group having 1 to 5 carbon atoms. p represents an integer of 0 to 5, and q represents an integer of 0 to 5. ) and the general formula (2):
[0024] CFX=CXOCF 2 OR 1 (2)
[0025] (wherein, X is the same or different and represents H, F or CF 3 , R 1 It represents a linear or branched fluoroalkyl group having 1 to 6 carbon atoms which may contain 1 to 2 atoms of at least one kind selected from the group consisting of H, Cl, Br and I, or a cyclic fluoroalkyl group having 5 or 6 carbon atoms which may contain 1 to 2 atoms of at least one kind selected from the group consisting of H, Cl, Br and I. At least one of the group consisting of monomers represented by ).
[0026] Among them, as the above-mentioned FAVE, the monomer represented by the general formula (1) is preferred, more preferably at least one selected from the group consisting of perfluoro(methyl vinyl ether), perfluoro(ethyl vinyl ether) (PEVE) and perfluoro(propyl vinyl ether) (PPVE), further preferably at least one selected from the group consisting of PEVE and PPVE, and particularly preferably PPVE.
[0027] The content of the HFP unit of the fluorinated copolymer is 9.5% to 10.5% by mass relative to the total monomer units, preferably 9.6% by mass or more, preferably 10.4% by mass or less, more preferably 10.2% by mass or less, and further preferably 10.1% by mass or less. When the content of the HFP unit is too small, it is impossible to obtain a coating layer having excellent ductility and excellent crack resistance to a tensile force applied at 150° C. after being placed in hot water at high temperature for a long time. When the content of the HFP unit is too large, it is impossible to obtain a coating layer having excellent tensile creep resistance at 150° C. and excellent deformation resistance to a tensile load applied at 150° C. after being placed in hot water at high temperature for a long time.
[0028] The content of the FAVE unit of the fluorinated copolymer is 0% to 0.3% by mass relative to the total monomer units, preferably 0.2% by mass or less, and more preferably 0.1% by mass or less. When the content of the FAVE unit is too much, it is impossible to obtain a coating layer having excellent tensile creep resistance at 150° C. and excellent deformation resistance to a tensile load applied at 150° C. after being placed in hot water for a long time at high temperature.
[0029] The content of the TFE unit of the fluorinated copolymer is preferably 89.2% by mass or more relative to all monomer units, more preferably 89.3% by mass or more, further preferably 89.4% by mass or more, further preferably 89.5% by mass or more, particularly preferably 89.6% by mass or more, most preferably 89.8% by mass or more, preferably 90.5% by mass or less, more preferably 90.4% by mass or less, and further preferably 90.3% by mass or less. In addition, the content of the TFE unit can be selected so that the total content of the HFP unit, the FAVE unit, the TFE unit and other monomer units is 100% by mass.
[0030] The fluorinated copolymer may contain the above three monomer units, and may be a copolymer containing only the above three monomer units or a copolymer containing the above three monomer units and other monomer units.
[0031] The other monomer is not particularly limited as long as it is a monomer copolymerizable with TFE, HFP and FAVE, and may be a fluorine-containing monomer or a non-fluorine-containing monomer.
[0032] The fluorine-containing monomer is preferably selected from chlorotrifluoroethylene, vinyl fluoride, vinylidene fluoride, trifluoroethylene, hexafluoroisobutylene, CH 2 =CZ 1 (CF 2 ) n Z 2 (Where Z 1 H or F, Z 2 is H, F or Cl, n is an integer of 1 to 10), CF 2 =CF-O-CH 2 -Rf 2 (Where Rf 2 At least one selected from the group consisting of an alkyl perfluorovinyl ether derivative represented by a perfluoroalkyl group having 1 to 5 carbon atoms, perfluoro-2,2-dimethyl-1,3-dioxole [PDD], and perfluoro-2-methylene-4-methyl-1,3-dioxolane [PMD].
[0033] As CH 2 =CZ 1 (CF 2 ) n Z 2 The monomers shown in FIG. 2 =CFCF 3 , CH 2 =CH-C 4 F 9 , CH 2 =CH-C 6 F 13 , CH 2 =CF-C 3 F 6 H et al.
[0034] As non-fluorine-containing monomers, hydrocarbon monomers that can be copolymerized with TFE, HFP and FAVE can be cited. As hydrocarbon monomers, for example, olefins such as ethylene, propylene, butylene, and isobutylene can be cited; alkyl vinyl ethers such as ethyl vinyl ether, propyl vinyl ether, butyl vinyl ether, isobutyl vinyl ether, and cyclohexyl vinyl ether can be cited; vinyl acetate, vinyl propionate, vinyl n-butyrate, vinyl isobutyrate, vinyl valerate, vinyl pivalate, vinyl hexanoate, vinyl octanoate, vinyl decanoate, vinyl versatate, vinyl laurate, vinyl myristate, vinyl palmitate, vinyl stearate, vinyl benzoate, vinyl p-tert-butylbenzoate, vinyl cyclohexanecarboxylate, vinyl monochloroacetate , vinyl adipate, vinyl acrylate, vinyl methacrylate, vinyl crotonate, vinyl sorbate, vinyl cinnamate, vinyl undecylenate, vinyl hydroxyacetate, vinyl hydroxypropionate, vinyl hydroxybutyrate, vinyl hydroxyvalerate, vinyl hydroxyisobutyrate, vinyl hydroxycyclohexanecarboxylate and other vinyl esters; alkyl allyl ethers such as ethyl allyl ether, propyl allyl ether, butyl allyl ether, isobutyl allyl ether, cyclohexyl allyl ether; alkyl allyl esters such as ethyl allyl ester, propyl allyl ester, butyl allyl ester, isobutyl allyl ester, cyclohexyl allyl ester, etc.
[0035] As a non-fluorine-containing monomer, it can also be a hydrocarbon monomer containing a functional group that can be copolymerized with TFE, HFP and FAVE. As a hydrocarbon monomer containing a functional group, for example, hydroxyalkyl vinyl ethers such as hydroxyethyl vinyl ether, hydroxypropyl vinyl ether, hydroxybutyl vinyl ether, hydroxyisobutyl vinyl ether, and hydroxycyclohexyl vinyl ether can be cited; non-fluorine-containing monomers having a glycidyl group such as glycidyl vinyl ether and glycidyl allyl ether; non-fluorine-containing monomers having an amino group such as aminoalkyl vinyl ether and aminoalkyl allyl ether; non-fluorine-containing monomers having an amide group such as (methyl) acrylamide and hydroxymethyl acrylamide; bromine-containing olefins, iodine-containing olefins, bromine-containing vinyl ethers, iodine-containing vinyl ethers; non-fluorine-containing monomers having a nitrile group, etc.
[0036] The content of other monomer units in the fluorinated copolymer is preferably 0 to 1.3 mass %, more preferably 1.0 mass % or less, further preferably 0.5 mass % or less, particularly preferably 0.1 mass % or less, based on the total monomer units.
[0037] The melt flow rate (MFR) of the fluorinated copolymer is 5.6 g / 10 minutes to 8.9 g / 10 minutes. The MFR of the fluorinated copolymer is preferably 5.7 g / 10 minutes or more, more preferably 5.8 g / 10 minutes or more, further preferably 5.9 g / 10 minutes or more, particularly preferably 6.0 g / 10 minutes or more, and most preferably 6.1 g / 10 minutes or more, preferably 8.7 g / 10 minutes or less, more preferably 8.6 g / 10 minutes or less, further preferably 8.5 g / 10 minutes or less, further preferably 8.4 g / 10 minutes or less, particularly preferably 8.3 g / 10 minutes or less, particularly preferably 8.2 g / 10 minutes or less, and most preferably 8.1 g / 10 minutes or less. If the MFR is too low, it is impossible to obtain a coating layer having excellent deformation resistance to a tensile load applied at 150° C. after being placed in high-temperature hot water for a long time. If the MFR is too high, it is impossible to obtain a coating layer that has excellent tensile creep resistance at 150°C after being placed in hot water for a long time, excellent ductility to a tensile force applied at 150°C, and is not prone to cracking even when heated for a long time in a state of being wound around a cylinder with a small diameter. In addition, if the MFR is too high or too low, it is difficult to form a coating layer with uniform thickness.
[0038] In the present invention, the melt flow rate is a value obtained as the mass (g / 10 minutes) of a polymer flowing out from a die having an inner diameter of 2 mm and a length of 8 mm at 372° C. and a load of 5 kg per 10 minutes using a melt flow indexer G-01 (manufactured by Toyo Seiki Seisaku-sho, Ltd.) in accordance with ASTM D-1238.
[0039] The MFR can be adjusted by adjusting the type and amount of the polymerization initiator, the type and amount of the chain transfer agent, etc., used when polymerizing the monomers.
[0040] The fluorinated copolymer may have a carbonyl-containing terminal group, -CF=CF 2 or -CH 2 OH, or may not have. In the fluorinated copolymer, the carbonyl terminal group, -CF=CF 2 and -CH 2 The total number of OH per 10 6 The number of carbon atoms in the main chain is preferably 70 or less. 2 and -CH 2 The total number of OH groups is preferably 60 or less, 50 or less, 40 or less, and 30 or less. 2 and -CH 2 When the total number of OH groups is within the above range, a coating layer having better heat resistance and further reduced molding defects can be obtained. 2and -CH 2 The total number of OH groups can be adjusted, for example, by appropriately selecting the type of the polymerization initiator or the chain transfer agent, or by wet heat treatment or fluorination treatment of the fluorinated copolymer described later.
[0041] Examples of carbonyl-containing terminal groups are -COF, -COOH, -COOR (R is an alkyl group), -CONH 2 The type of the alkyl group (R) in -COOR and -O(C=O)OR is determined by the polymerization initiator, chain transfer agent, etc. used in the production of the fluorinated copolymer. For example, -CH 3 Alkyl groups having 1 to 6 carbon atoms.
[0042] The fluorinated copolymer may have -CF 2 H, or may not have it. From the perspective of being able to obtain a coating layer that can further suppress molding defects and has better heat resistance, the fluorinated copolymer preferably has -CF 2 H. Fluorinated copolymers -CF 2 The number of H is relative to every 10 6 The number of carbon atoms in the main chain may be 50 or more, preferably 60 or more, more preferably more than 90, further preferably more than 120, further preferably more than 150, particularly preferably more than 200, and most preferably more than 250. 2 The upper limit of the number of H is not particularly limited, and may be, for example, 800. 2 The number of H can be adjusted, for example, by appropriately selecting the type of the polymerization initiator or the chain transfer agent, or by wet heat treatment or fluorination treatment of the fluorinated copolymer described later.
[0043] The identification of the types of the functional groups and the measurement of the number of the functional groups can be performed using infrared spectroscopy.
[0044] The number of functional groups is specifically determined by the following method. First, the fluorinated copolymer is formed by cold pressing to produce a film with a thickness of 0.25 mm to 0.30 mm. The film is analyzed by Fourier transform infrared spectroscopy to obtain an infrared absorption spectrum of the fluorinated copolymer and a differential spectrum from a background spectrum of a fully fluorinated copolymer without functional groups. The number of functional groups in the fluorinated copolymer relative to each 1×10 6 The number of functional groups N per carbon atom.
[0045] N=I×K / t(A)
[0046] I: Absorbance
[0047] K: Correction coefficient
[0048] t: film thickness (mm)
[0049] For reference, absorption frequencies, molar absorption coefficients, and correction coefficients for some functional groups are shown in Table 1. The molar absorption coefficients were determined from FT-IR measurement data of low-molecular model compounds.
[0050] [Table 1]
[0051] Table 1
[0052]
[0053] -CH 2 CF 2 H, -CH 2 COF, -CH 2 COOH, -CH 2 COOCH 3 、-CH 2 CONH 2 The absorption frequency ratios are shown in Table -CF 2 H, -COF, free -COOH and bonded -COOH, -COOCH 3 、-CONH 2 The absorption frequency is several tens of cm lower. -1 ).
[0054] For example, the functional group number of -COF refers to the number of functional groups derived from -CF 2 The absorption frequency of COF is 1883 cm -1 The number of functional groups obtained from the absorption peak at -CH 2 The absorption frequency of COF is 1840 cm -1 The total number of functional groups found from the absorption peak at .
[0055] In addition, -CF 2 The number of H groups can also be determined using a nuclear magnetic resonance apparatus at a temperature of (melting point of the polymer + 20)°C. 19 F-NMR determination, by -CF 2 The peak integral value of the H group was obtained.
[0056] -CF 2 The functional groups such as H groups are functional groups present at the ends of the main chain or side chains of the fluorinated copolymer and functional groups present in the main chain or side chains. These functional groups are introduced into the fluorinated copolymer by, for example, chain transfer agents or polymerization initiators used in the manufacture of the fluorinated copolymer. For example, alcohol is used as a chain transfer agent, or a -CH 2 When the peroxide with OH structure is used as the polymerization initiator, -CH2 OH is introduced into the main chain terminal of the fluorinated copolymer. In addition, by polymerizing a monomer having a functional group, the above functional group is introduced into the side chain terminal of the fluorinated copolymer.
[0057] By subjecting the fluorinated copolymer having such functional groups to a wet heat treatment, a fluorination treatment or the like, a fluorinated copolymer having the number of functional groups within the above range can be obtained. The fluorinated copolymer is more preferably subjected to a wet heat treatment.
[0058] The melting point of the fluorinated copolymer is preferably from 220 to 290°C, more preferably from 255 to 275°C, further preferably from 264 to 271°C, from the viewpoint of further improving the characteristics of the coating layer.
[0059] In the present invention, the melting point can be measured using a differential scanning calorimeter [DSC].
[0060] The fluorinated copolymer of the present invention can also be produced by any polymerization method such as bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, etc. In these polymerization methods, various conditions such as temperature and pressure, polymerization initiator, chain transfer agent, solvent, and other additives can be appropriately set according to the desired composition and amount of the fluorinated copolymer.
[0061] As the polymerization initiator, an oil-soluble radical polymerization initiator or a water-soluble radical initiator can be used.
[0062] The oil-soluble radical polymerization initiator may be a known oil-soluble peroxide, and the following may be cited as representative examples:
[0063] Dialkyl peroxycarbonates such as di-n-propyl peroxydicarbonate, di-isopropyl peroxydicarbonate and di-sec-butyl peroxydicarbonate;
[0064] Peroxyesters such as tert-butyl peroxyisobutyrate and tert-butyl peroxypivalate;
[0065] Dialkyl peroxides such as di-tert-butyl peroxide;
[0066] Di[fluoro(or chlorofluoro)acyl]peroxides; etc.
[0067] Examples of di[fluoro(or chlorofluoro)acyl]peroxides include [(RfCOO)-] 2 (Rf is a perfluoroalkyl group, an ω-hydroperfluoroalkyl group or a fluorochloroalkyl group).
[0068] Examples of the di[fluoro(or chlorofluoro)acyl]peroxides include di(ω-hydroperfluorohexanoyl)peroxide, di(ω-hydro-dodecafluoroheptanoyl)peroxide, di(ω-hydro-tetrafluorooctanoyl)peroxide, di(ω-hydro-hexafluorononanoyl)peroxide, di(perfluorobutyryl)peroxide, di(perfluorovaleranoyl)peroxide, di(perfluorohexanoyl)peroxide, di(perfluoroheptanoyl)peroxide, di(perfluorooctanoyl)peroxide, di(perfluorononanoyl)peroxide, and di(ω-chloro-hexafluorobutyryl)peroxide. , di(ω-chloro-decafluorohexanoyl)peroxide, di(ω-chloro-tetrafluorooctanoyl)peroxide, ω-hydro-dodecafluoroheptanoyl-ω-hydrohexafluorononanoyl-peroxide, ω-chloro-hexafluorobutyryl-ω-chloro-decafluorohexanoyl-peroxide, ω-hydro-dodecafluoroheptanoyl-peroxide, ω-hydro-dodecafluoroheptanoyl-perfluorobutyryl-peroxide, di(dichloropentafluorobutyryl)peroxide, di(trichlorooctafluorohexanoyl)peroxide, di(tetrachloroundecanoyl)peroxide, di(pentachlorotetrafluorodecanoyl)peroxide, di(undecachlorotriacontanoyl)peroxide, and the like.
[0069] As the water-soluble free radical polymerization initiator, it can be a known water-soluble peroxide, for example, ammonium salts, potassium salts, sodium salts of persulfuric acid, perboric acid, perchloric acid, perphosphoric acid, percarbonic acid, etc., tert-butyl peroxymaleate, tert-butyl hydroperoxide, etc. It can also contain a reducing agent such as sulfites, and its amount can be 0.1 to 20 times that of the peroxide.
[0070] If an oil-soluble free radical polymerization initiator is used as the polymerization initiator, the generation of -COF and -COOH can be avoided, and the total amount of -COF and -COOH in the fluorinated copolymer can be easily adjusted to the above range, which is preferred. In addition, if an oil-soluble free radical polymerization initiator is used, it is also easy to convert the terminal group containing a carbonyl group and -CH 2 OH is adjusted to the tendency of above-mentioned scope.Particularly, preferably make fluorinated copolymer by the suspension polymerization using oil-soluble free radical polymerization initiator.As oil-soluble free radical polymerization initiator, preferably at least one in the group consisting of dialkyl peroxycarbonates and two [fluorine (or chlorine) acyl] peroxides, more preferably at least one in the group consisting of di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate and two (ω-hydrogen-dodecanoyl) peroxides.
[0071] Examples of chain transfer agents include hydrocarbons such as ethane, isopentane, n-hexane, and cyclohexane; aromatics such as toluene and xylene; ketones such as acetone; acetates such as ethyl acetate and butyl acetate; alcohols such as methanol, ethanol, and 2,2,2-trifluoroethanol; mercaptans such as methyl mercaptan; halogenated hydrocarbons such as carbon tetrachloride, chloroform, dichloromethane, and chloromethane; 3-fluorobenzotrifluoride, etc. The amount added can vary depending on the chain transfer constant of the compound used, and is usually used in the range of 0.01 to 20 parts by mass relative to 100 parts by mass of the solvent.
[0072] For example, when dialkyl peroxycarbonates, di[fluoro(or chlorofluoro)acyl]peroxides, etc. are used as polymerization initiators, the molecular weight of the obtained fluorinated copolymer becomes too high, and it is sometimes difficult to adjust the desired melt flow rate, but a chain transfer agent can be used to adjust the molecular weight. It is particularly preferred to manufacture the fluorinated copolymer by suspension polymerization using a chain transfer agent such as alcohols and an oil-soluble free radical polymerization initiator.
[0073] Examples of the solvent include water, a mixed solvent of water and alcohol, etc. Alternatively, a monomer used for polymerization of the fluorinated copolymer may be used as the solvent.
[0074] In suspension polymerization, a fluorinated solvent may be used in addition to water. Examples of the fluorinated solvent include CH 3 CClF 2 , CH 3 CCl 2 F. CF 3 CF 2 CCl 2 H.CF 2 CCF 2 CFHCl and other hydrochlorofluoroalkanes; CF 2 ClCFClCF 2 CF 3 CF 3 CFClCFClCF 3 Chlorofluoroalkanes, such as perfluorocyclobutane, CF 3 CF 2 CF 2 CF 3 CF 3 CF 2 CF 2 CF 2 CF 3 CF 3 CF 2 CF 2 CF 2 CF 2 CF 3The amount of the fluorinated solvent used is preferably 10 to 100 parts by mass based on 100 parts by mass of the solvent from the viewpoint of suspending property and economic efficiency.
[0075] The polymerization temperature is not particularly limited and may be 0° C. to 100° C. In addition, when the decomposition rate of the polymerization initiator is too fast, such as when dialkyl peroxycarbonates, di[fluoro(or chlorofluoro)acyl]peroxides, etc. are used as the polymerization initiator, it is preferred to adopt a relatively low polymerization temperature such as a range of 0° C. to 35° C.
[0076] The polymerization pressure is appropriately determined according to other polymerization conditions such as the type of solvent used, the amount of solvent, the vapor pressure, the polymerization temperature, etc., and can generally be 0 MPaG to 9.8 MPaG. The polymerization pressure is preferably 0.1 MPaG to 5 MPaG, more preferably 0.5 MPaG to 2 MPaG, and further preferably 0.5 MPaG to 1.5 MPaG. In addition, when the polymerization pressure is 1.5 MPaG or more, the production efficiency can be improved.
[0077] As the additive in the polymerization, for example, a suspension stabilizer can be cited. As a suspension stabilizer, as long as it is an existing known suspension stabilizer, there is no particular limitation, and methylcellulose, polyvinyl alcohol, etc. can be used. If a suspension stabilizer is used, the suspended particles generated by the polymerization reaction are stably dispersed in the aqueous medium, so even if a reaction tank made of SUS that is not subjected to anti-adhesion treatments such as glass lining is used, the suspended particles are not easily attached to the reaction tank. Therefore, a reaction tank that withstands high pressure can be used, so polymerization under high pressure can be carried out, and production efficiency can be improved. In contrast, when polymerization is carried out without using a suspension stabilizer, if a reaction tank made of SUS that is not subjected to anti-adhesion treatment is used, the suspended particles are likely to adhere and reduce production efficiency. The concentration of the suspension stabilizer relative to the aqueous medium can be appropriately adjusted according to the conditions.
[0078] In the case of obtaining an aqueous dispersion containing a fluoropolymer by polymerization, the dry fluoropolymer can be recovered by precipitating, cleaning, and drying the fluoropolymer contained in the aqueous dispersion. In addition, in the case of obtaining a fluoropolymer in the form of a slurry by polymerization, the dry fluoropolymer can be recovered by taking out the slurry from the reaction vessel and cleaning and drying. By drying, the fluoropolymer can be recovered in the form of a powder.
[0079] The fluorinated copolymer obtained by polymerization can be formed into pellets. There is no particular limitation on the molding method for forming the pellets, and a conventionally known method can be used. For example, there can be cited a method in which the fluorinated copolymer is melt-extruded using a single-screw extruder, a twin-screw extruder, or a tandem extruder, and the fluorinated copolymer is cut into a predetermined length to form pellets. The extrusion temperature during melt extrusion needs to be changed according to the melt viscosity and the manufacturing method of the fluorinated copolymer, and is preferably the melting point of the fluorinated copolymer + 20°C to the melting point of the fluorinated copolymer + 140°C. There is no particular limitation on the cutting method of the fluorinated copolymer, and conventionally known methods such as a wire cutting method, a heat cutting method, an underwater cutting method, and a sheet cutting method can be used. The volatile components in the pellets can also be removed by heating the obtained pellets (degassing treatment). The obtained pellets can also be treated by contacting with warm water at 30°C to 200°C, steam at 100°C to 200°C, or hot air at 40°C to 200°C.
[0080] The fluorinated copolymer obtained by polymerization can also be heated to a temperature of 100°C or higher in the presence of air and water (wet heat treatment). As a method of wet heat treatment, for example, the following method can be cited: using an extruder, while supplying air and water, the fluorinated copolymer obtained by polymerization is melted and extruded. By wet heat treatment, the thermally unstable functional groups such as -COF and -COOH of the fluorinated copolymer can be converted into thermally more stable -CF 2 H, the total number of -COF and -COOH of the fluorinated copolymer, as well as the terminal groups containing carbonyl groups and -CH 2 The total number of OH groups is adjusted to the above range. By heating the fluorinated copolymer in the presence of an alkali metal salt in addition to air and water, the conversion to -CF 2 Conversion reaction of H. However, it should be noted that, depending on the use of the fluorinated copolymer, contamination by alkali metal salts should be avoided.
[0081] The fluorinated copolymer obtained by polymerization may or may not be fluorinated. From the perspective of avoiding time and economic burden, it is preferred not to fluorinate the fluorinated copolymer. The fluorination treatment can be carried out by contacting the unfluorinated fluorinated copolymer with a fluorinated compound. The fluorination treatment can be used to convert the carbonyl-containing terminal groups, -CH 2 Thermally unstable functional groups such as OH and thermally stable -CF 2 H and other functional groups are converted into thermally extremely stable -CF 3 As a result, the carbonyl-containing terminal group of the fluorinated copolymer and -CH 2 The total number of OH is adjusted to the above range.
[0082] The fluorine-containing compound is not particularly limited, and examples thereof include a fluorine radical source that generates fluorine radicals under fluorination treatment conditions. Examples of the fluorine radical source include F 2 Gas, CoF 3 , AgF 2 、UF 6 、OF 2 、N 2 F 2 CF 3 OF, fluorinated halogens (such as IF 5 , ClF 3 )wait.
[0083] F 2 The fluorine radical source such as gas can be 100% concentration, but from the aspect of safety, it is preferably mixed with an inert gas and diluted to 5% to 50% by mass for use, and more preferably diluted to 15% to 30% by mass for use. As the above-mentioned inert gas, nitrogen, helium, argon, etc. can be cited, and nitrogen is preferred from the aspect of economy.
[0084] The conditions for the fluorination treatment are not particularly limited, and the fluorinated copolymer in a molten state may be brought into contact with the fluorinated compound. However, the treatment may be generally carried out at a temperature below the melting point of the fluorinated copolymer, preferably at 20°C to 220°C, and more preferably at 100°C to 200°C. The fluorination treatment is generally carried out for 1 to 30 hours, preferably for 5 to 25 hours. The fluorination treatment is preferably carried out by bringing the unfluorinated fluorinated copolymer into contact with fluorine gas (F 2 Gas) contact treatment.
[0085] The coating layer may contain other components as required. Other components include fillers, plasticizers, processing aids, mold release agents, pigments, flame retardants, lubricants, light stabilizers, weather stabilizers, conductive agents, antistatic agents, ultraviolet absorbers, antioxidants, foaming agents, fragrances, oils, softeners, dehydrofluorination agents, etc.
[0086] As fillers, for example, silicon dioxide, kaolin, clay, organic clay, talc, mica, aluminum oxide, calcium carbonate, calcium terephthalate, titanium oxide, calcium phosphate, calcium fluoride, lithium fluoride, cross-linked polystyrene, potassium titanate, carbon, boron nitride, carbon nanotubes, glass fibers, etc. can be cited. As conductive agents, carbon black, etc. can be cited. As plasticizers, dioctyl phthalate, pentaerythritol, etc. can be cited. As processing aids, carnauba wax, sulfone compounds, low molecular weight polyethylene, fluorine-based additives, etc. can be cited. As dehydrofluorination agents, organic onium, amidines, etc. can be cited.
[0087] In addition, as the above-mentioned other components, other polymers other than the above-mentioned copolymers may be used. Examples of other polymers include fluororesins other than the above-mentioned copolymers, fluororubbers, and non-fluorinated polymers.
[0088] The coated electric wire of the present invention comprises a core wire and a coating layer disposed around the core wire and containing the above-mentioned copolymer. For example, an extrusion molding formed by melt-extruding the above-mentioned copolymer on the core wire can be used as the above-mentioned coating layer. The coated electric wire is suitable for LAN cables (Ethernet Cables), high-frequency transmission cables, flat cables, heat-resistant cables, etc., and is suitable for transmission cables such as LAN cables (Ethernet Cables) and high-frequency transmission cables.
[0089] As the material of the core wire, a metal conductor material such as copper or aluminum can be used. The core wire preferably has a diameter of 0.02 mm to 3 mm. The core wire diameter is more preferably 0.04 mm or more, further preferably 0.05 mm or more, and particularly preferably 0.1 mm or more. The core wire diameter is more preferably 2 mm or less.
[0090] As specific examples of the core wire, AWG (American Wire Gauge)-46 (solid copper wire with a diameter of 40 μm), AWG-26 (solid copper wire with a diameter of 404 μm), AWG-24 (solid copper wire with a diameter of 510 μm), AWG-22 (solid copper wire with a diameter of 635 μm), etc. can be used.
[0091] The thickness of the coating layer is preferably 0.1 mm to 3.0 mm, and the thickness of the coating layer is also preferably 2.0 mm or less.
[0092] As a high-frequency transmission cable, a coaxial cable can be cited. A coaxial cable generally has a structure in which an inner conductor, an insulating coating, an outer conductor layer, and a protective coating are stacked in order from the core to the periphery. The thickness of each layer in the above structure is not particularly limited. Generally, the diameter of the inner conductor is about 0.1 mm to 3 mm, the thickness of the insulating coating is about 0.3 mm to 3 mm, the thickness of the outer conductor layer is about 0.5 mm to 10 mm, and the thickness of the protective coating is about 0.5 mm to 2 mm.
[0093] The coating layer may contain air bubbles, and the air bubbles are preferably uniformly distributed in the coating layer.
[0094] The average bubble diameter of the bubbles is not limited, and is, for example, preferably 60 μm or less, more preferably 45 μm or less, further preferably 35 μm or less, further preferably 30 μm or less, particularly preferably 25 μm or less, and particularly preferably 23 μm or less. In addition, the average bubble diameter is preferably 0.1 μm or more, more preferably 1 μm or more. The average bubble diameter can be obtained by obtaining an electron microscope image of a cross section of the wire, calculating the diameter of each bubble by image processing, and averaging them.
[0095] The foaming rate of the coating layer may be 20% or more. More preferably, it is 30% or more, further preferably, it is 33% or more, and further preferably, it is 35% or more. The upper limit is not particularly limited, for example, it is 80%. The upper limit of the foaming rate may be 60%. The foaming rate is a value calculated as ((specific gravity of the wire coating material - specific gravity of the coating layer) / specific gravity of the wire coating material) × 100. The foaming rate can be appropriately adjusted according to the application by, for example, adjusting the amount of gas inserted in the extruder described later, or by selecting the type of dissolved gas.
[0096] The covered electric wire may also have other layers between the core wire and the covering layer, and may further have other layers (outer layers) around the covering layer. When the covering layer contains bubbles, the covered electric wire of the present invention may also be a two-layer structure (skin-foam) in which a non-foam layer is inserted between the core wire and the covering layer; a two-layer structure (foam-skin) in which a non-foam layer is covered on the outer layer; and a three-layer structure (skin-foam-skin) in which a non-foam layer is covered on the outer layer of the skin-foam. The non-foam layer is not particularly limited, and may be a resin layer composed of TFE / HFP copolymers, TFE / PAVE copolymers, TFE / ethylene copolymers, vinylidene fluoride polymers, polyolefin resins such as polyethylene [PE], polyvinyl chloride [PVC] and other resins.
[0097] The covered electric wire can be produced, for example, by heating a copolymer using an extruder and extruding the copolymer onto a core wire in a molten state to form a covering layer.
[0098] When forming the coating, it is also possible to heat the copolymer and, under the state where the copolymer is molten, introduce gas into the copolymer to form the above-mentioned coating containing bubbles. As the gas, for example, a mixture of gases such as chlorodifluoromethane, nitrogen, carbon dioxide or the like or the above-mentioned gases can be used. The gas can be introduced into the heated copolymer in the form of pressurized gas, or it can be produced by mixing a chemical foaming agent in the copolymer. The gas dissolves in the copolymer in a molten state.
[0099] Although the embodiments have been described above, it should be understood that various modifications may be made to the embodiments and details without departing from the spirit and scope of the claims.
[0100] <1> According to a first aspect of the present invention, there is provided a covered electric wire comprising a core wire and a covering layer provided around the core wire, wherein:
[0101] The coating layer contains a fluorinated copolymer containing tetrafluoroethylene units, hexafluoropropylene units and fluoro(alkyl vinyl ether) units.
[0102] The content of the hexafluoropropylene unit in the fluorinated copolymer is 9.5 to 10.5% by mass based on the total monomer units.
[0103] The content of the fluorinated (alkyl vinyl ether) unit in the fluorinated copolymer is 0% by mass to 0.3% by mass based on the total monomer units.
[0104] The melt flow rate of the fluorinated copolymer at 372° C. is 5.6 g / 10 min to 8.9 g / 10 min.
[0105] <2> According to a second aspect of the present invention, there is provided a covered electric wire according to the first aspect, wherein a content of the hexafluoropropylene unit in the fluorinated copolymer is 9.6% by mass to 10.4% by mass based on all monomer units.
[0106] <3> According to a third aspect of the present invention, there is provided a covered electric wire according to the first aspect or the second aspect, wherein a content of the fluorinated (alkyl vinyl ether) unit in the fluorinated copolymer is 0 mass % to 0.1 mass % based on all monomer units.
[0107] <4> According to a fourth aspect of the present invention, there is provided a covered electric wire according to any one of the first to third aspects, wherein the fluoro(alkyl vinyl ether) unit is a perfluoro(propyl vinyl ether) unit.
[0108] <5> According to a fifth aspect of the present invention, there is provided a covered electric wire according to any one of the first to fourth aspects, wherein the fluorinated copolymer has a melt flow rate at 372° C. of 6.1 g / 10 min to 8.1 g / 10 min.
[0109] <6> According to a sixth aspect of the present invention, there is provided a covered electric wire according to any one of the first to fifth aspects, wherein the carbonyl-containing terminal group of the fluorinated copolymer, -CF=CF 2 and -CH 2 The total number of OH per 10 6 The number of carbon atoms in the main chain is 70 or less.
[0110] <7> According to a seventh aspect of the present invention, there is provided a covered electric wire according to any one of the first to sixth aspects, wherein -CF2 The number of H is relative to every 10 6 The number of carbon atoms in the main chain is 50 or more.
[0111] Example
[0112] Next, embodiments of the present invention will be described with reference to examples, but the present invention is not limited to the examples.
[0113] Each numerical value in the examples was measured by the following method.
[0114] (Content of monomer units)
[0115] The content of each monomer unit of the fluorinated copolymer is measured using an NMR analyzer (for example, AVANCE300 high temperature probe manufactured by Bruker BioSpin) or an infrared absorption analyzer (Spectrum One manufactured by Perkin Elmer).
[0116] (Melt Flow Rate (MFR))
[0117] The MFR of the fluorinated copolymer was determined by measuring the mass (g / 10 minutes) of the polymer flowing out from a die having an inner diameter of 2 mm and a length of 8 mm at 372°C and a load of 5 kg using a melt flow indexer G-01 (manufactured by Toyo Seiki Seisaku-sho, Ltd.) in accordance with ASTM D-1238.
[0118] (-CF 2 Number of H)
[0119] Fluorinated copolymer -CF 2 The number of H groups was determined using a nuclear magnetic resonance apparatus AVANCE-300 (manufactured by Bruker BioSpin) at a temperature of (melting point of polymer + 20)°C. 19 F-NMR determination, by -CF 2 The peak integral value of the H group was obtained.
[0120] (-COOH, -COOCH 3 、-CH 2 OH, -COF, -CF=CF 2 、-CONH 2 Quantity)
[0121] The dry powder or pellets obtained in the examples and comparative examples are formed by cold pressing to produce films with a thickness of 0.25 mm to 0.3 mm. The film is scanned 40 times by a Fourier transform infrared spectrometer [FT-IR (Spectrum One, manufactured by PerkinElmer)] and analyzed to obtain an infrared absorption spectrum. The obtained infrared absorption spectrum is compared with the infrared absorption spectrum of a known film to determine the type of terminal group. In addition, the absorption peak of a specific functional group that appears in the differential spectrum between the obtained infrared absorption spectrum and the infrared absorption spectrum of a known film is calculated according to the following formula (A) for every 1×10 6 The number of functional groups N per carbon atom.
[0122] N=I×K / t (A)
[0123] I: Absorbance
[0124] K: Correction coefficient
[0125] t: film thickness (mm)
[0126] For reference, the absorption frequency, molar absorption coefficient and correction coefficient of the functional groups in the examples are shown in Table 2. The molar absorption coefficient was determined from the FT-IR measurement data of the low molecular model compound.
[0127] [Table 2]
[0128] Table 2
[0129]
[0130] (-OC(=O)OR(carbonate group) number)
[0131] The analysis was performed by the method described in International Publication No. 2019 / 220850. The absorption frequency was set to 1817 cm -1 The number of -OC(=O)OR (carbonate groups) was calculated in the same manner as the method for calculating the number of functional groups N, except that the molar absorptivity coefficient was set to 170 (l / cm / mol) and the correction factor was set to 1426.
[0132] (Melting Point)
[0133] Regarding the melting point of the fluorinated copolymer, a differential scanning calorimeter (trade name: X-DSC7000, manufactured by Hitachi High-Tech Science Co., Ltd.) was used to perform the first temperature increase from 200°C to 350°C at a temperature increase rate of 10°C / min, then cooled from 350°C to 200°C at a cooling rate of 10°C / min, and then the second temperature increase from 200°C to 350°C was performed again at a temperature increase rate of 10°C / min. The melting point was determined from the peak of the melting curve generated in the second temperature increase process.
[0134] Comparative Example 1
[0135] 40.25 kg of deionized water and 0.251 kg of methanol were added to an autoclave with a stirrer of a volume of 174 L, and the autoclave was fully replaced with vacuum nitrogen. After that, the autoclave was vacuum degassed, 40.25 kg of HFP was added to the autoclave in a vacuum state, and the autoclave was heated to 30.0 ° C. Next, TFE was added until the internal pressure of the autoclave reached 0.909 MPa, and then 0.63 kg of 8% by mass di(ω-hydroperfluorohexanoyl) peroxide solution (hereinafter referred to as DHP) was added to the autoclave to start polymerization. The internal pressure of the autoclave at the start of polymerization was set to 0.909 MPa, and the set pressure was maintained by continuously adding TFE. 0.251 kg of methanol was added 1.5 hours after the start of polymerization. 2 hours and 4 hours after the start of polymerization, 0.63 kg of DHP was added and the internal pressure was reduced by 0.001 MPa. 6 hours later, 0.48 kg was added and the internal pressure was reduced by 0.001 MPa. Thereafter, 0.13 kg of DHP was added every 2 hours until the reaction was completed, and the internal pressure was reduced by 0.001 MPa each time.
[0136] In addition, when the additional amount of TFE reached 6.0 kg and 18.1 kg, 0.251 kg of methanol was added to the autoclave, respectively. Then, when the additional amount of TFE reached 40.25 kg, the polymerization was terminated. After the polymerization was completed, unreacted TFE and HFP were released to obtain a wet powder. Then, the wet powder was washed with pure water and dried at 150°C for 10 hours to obtain 45.6 kg of dry powder.
[0137] The obtained powder was melt-extruded at 370°C using a screw extruder (trade name: PCM46, manufactured by Ikegai Co., Ltd.) to obtain pellets of the copolymer. Various physical properties were measured using the obtained pellets by the above-mentioned methods. The results are shown in Table 3.
[0138] Comparative Example 2
[0139] The amount of methanol added before the start of polymerization was changed to 0.263 kg, the amount of methanol added in batches after the start of polymerization was changed to 0.263 kg, and the set pressure inside the autoclave before and after the start of polymerization was changed to 0.928 MPa. Copolymer pellets were obtained in the same manner as in Comparative Example 1. Various physical properties were measured using the pellets obtained by the above-mentioned methods. The results are shown in Table 3.
[0140] Comparative Example 3
[0141] 40.25 kg of deionized water and 0.317 kg of methanol were added to an autoclave with a stirrer of a volume of 174 L, and the autoclave was fully replaced with vacuum nitrogen. Then, the autoclave was vacuum degassed, 40.25 kg of HFP was added to the autoclave in a vacuum state, and the autoclave was heated to 25.5 ° C. Next, TFE was added until the internal pressure of the autoclave reached 0.837 MPa, and then 1.25 kg of 8% by mass di(ω-hydroperfluorohexanoyl) peroxide solution (hereinafter referred to as DHP) was added to the autoclave to start polymerization. The internal pressure of the autoclave at the start of polymerization was set to 0.837 MPa, and the set pressure was maintained by continuously adding TFE. 0.317 kg of methanol was added 1.5 hours after the start of polymerization. 1.25 kg of DHP was added 2 hours and 4 hours after the start of polymerization, and the internal pressure was reduced by 0.002 MPa. 0.96 kg was added 6 hours later, and the internal pressure was reduced by 0.002 MPa. Thereafter, 0.25 kg of DHP was added every 2 hours until the reaction was completed, and the internal pressure was reduced by 0.002 MPa each time.
[0142] In addition, when the additional amount of TFE reached 6.0 kg and 18.1 kg, 0.317 kg of methanol was added to the autoclave, respectively. Then, when the additional amount of TFE reached 40.25 kg, the polymerization was terminated. After the polymerization was completed, unreacted TFE and HFP were released to obtain a wet powder. Thereafter, the wet powder was washed with pure water and dried at 150° C. for 10 hours to obtain 44.8 kg of dry powder.
[0143] The obtained powder was melt-extruded at 370°C using a screw extruder (trade name: PCM46, manufactured by Ikegai Co., Ltd.) to obtain pellets of the copolymer. The HFP content and PPVE content of the obtained pellets were measured by the above-mentioned method. The results are shown in Table 3.
[0144] Comparative Example 4
[0145] The amount of methanol added before the start of polymerization was changed to 0.361 kg, the amount of methanol added in batches after the start of polymerization was changed to 0.361 kg, and the set pressure inside the autoclave before and after the start of polymerization was changed to 0.918 MPa. Copolymer pellets were obtained in the same manner as in Comparative Example 1. Various physical properties were measured using the pellets obtained by the above-mentioned methods. The results are shown in Table 3.
[0146] Comparative Example 5
[0147] 40.25 kg of deionized water and 0.232 kg of methanol were added to an autoclave with a stirrer of a volume of 174 L, and the autoclave was fully replaced with vacuum nitrogen. Then, the autoclave was vacuum degassed, 40.25 kg of HFP and 0.38 kg of PPVE were added to the autoclave in a vacuum state, and the autoclave was heated to 30.0 ° C. Next, TFE was added until the internal pressure of the autoclave reached 0.918 MPa, and then 0.63 kg of 8% by mass di(ω-hydroperfluorohexanoyl) peroxide solution (hereinafter referred to as DHP) was added to the autoclave to start polymerization. The internal pressure of the autoclave at the start of polymerization was set to 0.918 MPa, and the set pressure was maintained by continuously adding TFE. 0.232 kg of methanol was added 1.5 hours after the start of polymerization. 2 hours and 4 hours after the start of polymerization, 0.63 kg of DHP was added and the internal pressure was reduced by 0.001 MPa. 6 hours later, 0.48 kg was added and the internal pressure was reduced by 0.001 MPa. Thereafter, 0.13 kg of DHP was added every 2 hours until the reaction was completed, and the internal pressure was reduced by 0.001 MPa each time.
[0148] It should be noted that 0.11 kg of PPVE was added when the continuous additional input amount of TFE reached 8.1 kg, 16.2 kg, and 24.3 kg, respectively. In addition, 0.232 kg of methanol was added to the autoclave when the additional input amount of TFE reached 6.0 kg and 18.1 kg, respectively. Then, the polymerization was terminated when the additional input amount of TFE reached 40.25 kg. After the polymerization was completed, the unreacted TFE and HFP were released to obtain a wet powder. After that, the wet powder was washed with pure water and dried at 150°C for 10 hours to obtain 45.9 kg of dry powder.
[0149] The obtained powder was melt-extruded at 370°C using a screw extruder (trade name: PCM46, manufactured by Ikegai Co., Ltd.) to obtain pellets of the copolymer. Various physical properties were measured using the obtained pellets by the above-mentioned methods. The results are shown in Table 3.
[0150] Example 1
[0151] The amount of methanol added before the start of polymerization was changed to 0.315 kg, the amount of methanol added in batches after the start of polymerization was changed to 0.315 kg, and the set pressure inside the autoclave before and after the start of polymerization was changed to 0.937 MPa. Copolymer pellets were obtained in the same manner as in Comparative Example 1. Various physical properties were measured using the pellets obtained by the above-mentioned methods. The results are shown in Table 3.
[0152] Example 2
[0153] The amount of methanol added before the start of polymerization was changed to 0.265 kg, the amount of methanol added in batches after the start of polymerization was changed to 0.265 kg, and the set pressure inside the autoclave before and after the start of polymerization was changed to 0.928 MPa. Copolymer pellets were obtained in the same manner as in Comparative Example 1. The obtained pellets were used to measure the HFP content and PPVE content by the above method. The results are shown in Table 3.
[0154] The obtained pellets were degassed in an electric furnace at 200°C for 8 hours, and then placed in a vacuum vibration reactor VVD-30 (manufactured by Ohkawara Manufacturing Co., Ltd.) and heated to 200°C. After evacuation, the pellets were heated with N 2 The gas was diluted to 20% by volume of F 2 The gas is introduced to atmospheric pressure. 2 After 0.5 hours from the gas time, temporarily evacuate the air and re-introduce F 2 After a further 0.5 hour, the vacuum was drawn again and F 2 Gas. Then, the above F 2 The gas introduction and vacuuming were performed once every hour, and the reaction was carried out at 200°C for 8 hours. After the reaction was completed, the reactor was fully replaced with N 2 The fluorination reaction was terminated by removing the gas and obtaining pellets. The obtained pellets were used to measure various physical properties by the above methods. The results are shown in Table 3.
[0155] Example 3
[0156] 40.25 kg of deionized water and 0.307 kg of methanol were added to an autoclave with a stirrer of a volume of 174 L, and the autoclave was fully replaced with vacuum nitrogen. Then, the autoclave was vacuum degassed, 40.25 kg of HFP and 0.04 kg of PPVE were added to the autoclave in a vacuum state, and the autoclave was heated to 30.0 ° C. Next, TFE was added until the internal pressure of the autoclave reached 0.926 MPa, and then 0.63 kg of 8% by mass di(ω-hydroperfluorohexanoyl) peroxide solution (hereinafter referred to as DHP) was added to the autoclave to start polymerization. The internal pressure of the autoclave at the start of polymerization was set to 0.926 MPa, and the set pressure was maintained by continuously adding TFE. 0.307 kg of methanol was added 1.5 hours after the start of polymerization. 2 hours and 4 hours after the start of polymerization, 0.63 kg of DHP was added and the internal pressure was reduced by 0.001 MPa. 6 hours later, 0.48 kg was added and the internal pressure was reduced by 0.001 MPa. Thereafter, 0.13 kg of DHP was added every 2 hours until the reaction was completed, and the internal pressure was reduced by 0.001 MPa each time.
[0157] It should be noted that PPVE was added with 0.01 kg of TFE when the continuous additional input amount reached 8.1 kg, 16.2 kg, and 24.3 kg. In addition, 0.307 kg of methanol was added to the autoclave when the additional input amount of TFE reached 6.0 kg and 18.1 kg. Then, the polymerization was terminated when the additional input amount of TFE reached 40.25 kg. After the polymerization was completed, the unreacted TFE and HFP were released to obtain a wet powder. After that, the wet powder was washed with pure water and dried at 150°C for 10 hours to obtain 45.3 kg of dry powder.
[0158] The obtained powder was melt-extruded at 370°C using a screw extruder (trade name: PCM46, manufactured by Ikegai Co., Ltd.) to obtain pellets of the copolymer. Various physical properties were measured using the obtained pellets by the above-mentioned methods. The results are shown in Table 3.
[0159] Example 4
[0160] The amount of methanol added before the start of polymerization was changed to 0.288 kg, the amount of methanol added in batches after the start of polymerization was changed to 0.288 kg, and the set pressure inside the autoclave before and after the start of polymerization was changed to 0.918 MPa. Copolymer pellets were obtained in the same manner as in Comparative Example 1. Various physical properties of the obtained pellets were measured by the above-mentioned methods. The results are shown in Table 3.
[0161] [Table 3]
[0162] Table 3
[0163]
[0164] "Others (pcs / C10)" in Table 3 6 )" means -COOCH 3 , -CF=CF 2 and-CONH 2 The total number of "<9" in Table 3 refers to -CF 2 The number of H groups (total number) is less than 9. The description "<6" in Table 3 means that the number of target functional groups (total number) is less than 6. The description "ND" in Table 3 means that the peak for the target functional group cannot be confirmed to a quantitative degree.
[0165] Next, the following properties were evaluated using the obtained pellets. The results are shown in Table 4.
[0166] (Molding conditions)
[0167] use A wire coating molding machine (manufactured by TANABE PLASTIC MACHINERY CO., LTD.) was used to extrusion coat a copper conductor having a conductor diameter of 0.70 mm with the following coating thickness to obtain a coated wire. The wire coating extrusion molding conditions were as follows.
[0168] a) Core conductor: soft steel wire conductor diameter 0.70mm
[0169] b) Coating thickness: 0.30mm
[0170] c) Diameter of coated wire: 1.30mm
[0171] d) Wire pulling speed: 20m / min
[0172] e) Extrusion conditions:
[0173] · Single screw extruder with barrel diameter = 30mm, L / D = 22
[0174] Die head (inner diameter) / sheet (outer diameter) = 13.0mm / 7.0mm
[0175] The set temperatures of the extruder were: barrel C-1 (330°C), barrel C-2 (360°C), barrel C-3 (370°C), head H (380°C), die head D-1 (385°C), die head D-2 (380°C). The core wire preheating was set to 80°C.
[0176] (Evaluation of outer diameter jitter)
[0177] The outer diameter measuring instrument (ODAC18XY manufactured by Zumbach) was used to measure continuously for 1 hour. The detection values of the maximum and minimum values of the outer diameter were rounded to the third decimal place relative to the target outer diameter of 1.30 mm. A value less than ±1% was recorded as acceptable (0), and a value greater than 1% was recorded as unacceptable (×).
[0178] (Tensile creep test)
[0179] Use TMA-7100 manufactured by Hitachi High-Technologies Corporation to measure tensile creep strain. Cut a 20cm long wire from the obtained coated wire, put water and the cut wire into a portable reactor (TVS1 type, manufactured by Pressure Glass Industry Co., Ltd.), heat it in an electric furnace at 150°C for 7 hours, take it out, cool it to room temperature and take out the wire, and peel off the coating. A sample with a width of 2mm and a length of 22mm is made from the obtained coating. The sample is mounted on the measuring fixture with a distance of 10mm between the fixtures. For the sample, the cross-sectional load becomes 2.93N / mm 2 The load is applied in a manner, placed at 150°C, and the displacement (mm) of the length of the sample from 70 minutes after the start of the test to 300 minutes after the start of the test is measured, and the ratio of the displacement (mm) of the length to the initial sample length (10 mm) is calculated (tensile creep strain (%)). The coating layer with a small tensile creep strain (%) measured at 150°C and 300 minutes is not easy to elongate even if the tensile load is applied for a long time in a high temperature environment, and has excellent tensile creep resistance at 150°C.
[0180] (Coiling crack test)
[0181] Ten wires of 20 cm in length were cut from the obtained covered wires to serve as wires (test pieces) for the winding crack test. The test piece was placed in a portable reactor (TVS1 type, manufactured by Pressure Glass Industry Co., Ltd.) filled with water in a straight state, heated at 150°C for 7 hours in an electric furnace, and then the test piece was taken out after cooling to room temperature. The test piece was wound around a wire of the same diameter as the test piece and placed in a portable reactor (TVS1 type, manufactured by Pressure Glass Industry Co., Ltd.) filled with water again. After heating at 150°C for 1 hour in an electric furnace, the sample was taken out after cooling to room temperature, and the wire was unwound. The number of cracked wires was counted visually and with a magnifying glass. As long as there is one crack in a wire, it is considered to have a crack. If there are less than 1 wire with cracks among 10 wires, it is marked as ○, and if there are more than 2 wires, it is marked as ×.
[0182] (150℃ tensile elastic modulus, 150℃ tensile elongation)
[0183] Cut a 20 cm long wire from the obtained covered wire, put water and the cut wire into a portable reactor (TVS1 type, manufactured by Pressure Glass Industry Co., Ltd.), take it out after heating it at 150°C in an electric furnace for 7 hours, take out the wire after cooling to room temperature, take out the core wire, and use the remaining coating as a test piece. Use Autograph (AG-I300kN manufactured by Shimadzu Corporation) to measure the tensile modulus and tensile elongation at 150°C under the conditions of a gauge length of 20mm and a tensile speed of 50mm / min in accordance with ASTM D638. The coating with a high tensile modulus at 150°C has excellent deformation resistance to the tensile load applied at 150°C. In addition, the coating with a large tensile elongation at 150°C has excellent ductility to the tensile force applied at 150°C.
[0184] [Table 4]
[0185] Table 4
[0186]
[0187] (Reference example: Film forming)
[0188] use Films of the copolymers described in Comparative Examples 1 to 5 and Examples 1 to 4 were produced using a T-die using an extruder (manufactured by Imoto Seisakusho), and visual inspection confirmed that the films were produced without any problems. The extrusion molding conditions were as follows.
[0189] a) Winding speed: 1m / min
[0190] b) Roller temperature: 120°C
[0191] c) Film width: 70mm
[0192] d)Thickness: 0.10mm
[0193] e) Extrusion conditions:
[0194] · Single screw extruder with barrel diameter = 14mm, L / D = 20
[0195] Extruder set temperature: barrel C-1 (330°C), barrel C-2 (350°C), barrel C-3 (365°C), T-die head (370°C)
[0196] (Reference example: Tube forming)
[0197] use An extruder (manufactured by Tanabe Plastic Machinery) was used to extrusion-mold a tube having an outer diameter of 10.0 mm and a wall thickness of 1.0 mm using the copolymers described in Comparative Examples 1, 2, 5, and Examples 1 to 4, and visually confirmed that the tube was produced without any problem. The extrusion molding conditions were as follows.
[0198] a) Die head inner diameter: 25mm
[0199] b) Shaft outer diameter: 13mm
[0200] c) Inner diameter of shaping die: 10.5mm
[0201] d) Traction speed: 0.4m / min
[0202] e) Outer diameter: 10.0mm
[0203] f) Wall thickness: 1.0mm
[0204] g) Extrusion conditions:
[0205] · Single screw extruder with barrel diameter = 30mm, L / D = 22
[0206] The set temperatures of the extruder are: barrel C-1 (350°C), barrel C-2 (370°C), barrel C-3 (380°C), head H-1 (390°C), die head D-1 (390°C), die head D-2 (390°C).
Claims
1. A covered electric wire comprising a core wire and a covering layer provided around the core wire, wherein: The coating layer contains a fluorine-containing copolymer, wherein the fluorine-containing copolymer contains a tetrafluoroethylene unit, a hexafluoropropylene unit, and a fluoro(alkyl vinyl ether) unit. The content of the hexafluoropropylene unit in the fluorinated copolymer is 9.5 to 10.5% by mass based on the total monomer units. The content of the fluorinated (alkyl vinyl ether) unit in the fluorinated copolymer is 0% by mass to 0.3% by mass based on the total monomer units. The melt flow rate of the fluorine-containing copolymer at 372° C. is 5.6 g / 10 min to 8.9 g / 10 min.
2. The covered electric wire according to claim 1, wherein The content of the hexafluoropropylene unit in the fluorinated copolymer is 9.6% by mass to 10.4% by mass based on the total monomer units.
3. The covered electric wire according to claim 1 or 2, wherein: The content of the fluorinated (alkyl vinyl ether) unit in the fluorinated copolymer is 0% by mass to 0.1% by mass based on all monomer units.
4. The covered electric wire according to any one of claims 1 to 3, wherein The fluoro(alkyl vinyl ether) unit is a perfluoro(propyl vinyl ether) unit.
5. The covered electric wire according to any one of claims 1 to 4, wherein The melt flow rate of the fluorine-containing copolymer at 372° C. is 6.1 g / 10 min to 8.1 g / 10 min.
6. The covered electric wire according to any one of claims 1 to 5, wherein The total number of the carbonyl-containing terminal groups, -CF=CF2 and -CH2OH of the fluorinated copolymer is relative to every 10 6 The number of carbon atoms in the main chain is 70 or less.
7. The covered electric wire according to any one of claims 1 to 6, wherein The amount of -CF2H in the fluorinated copolymer is relative to every 10 6 The number of carbon atoms in the main chain is 50 or more.