Substrate processing method

By coating a drying aid liquid of thermosetting material and solvent onto a substrate and heating it to form a cured film, the problem of pattern breakage in patterned substrate processing in the prior art is solved, and proper substrate drying and protection are achieved.

CN118946953APending Publication Date: 2024-11-12SCREEN HOLDINGS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029427.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-22
Filing Date
2023-03-17
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing substrate processing methods are not suitable for processing patterned substrates, especially fine patterns, which can easily lead to pattern damage.

Method used

A drying aid liquid containing thermosetting materials and solvents is applied to the substrate, and a curing film is formed by heating. During the thermal decomposition of the curing film, the curing film is kept above the pattern to protect the protrusions and avoid the influence of volume changes.

Benefits of technology

It effectively protects the raised parts of the substrate pattern from the effects of changes in the volume of the cured film, preventing damage, while also achieving substrate drying. It is suitable for substrate processing of various pattern sizes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946953A_ABST
    Figure CN118946953A_ABST
Patent Text Reader

Abstract

The substrate processing method is used for processing a substrate (W) on which a pattern (P) is formed. The pattern (P) includes a plurality of convex portions (A) and a plurality of concave portions (B). The substrate processing method includes a first coating step, a first hardening step, and a first thermal decomposition step. In the first coating step, the substrate (W) is coated with a first drying auxiliary liquid (F1). The first drying auxiliary liquid (F1) contains a thermosetting material and a solvent. In the first hardening step, the first drying auxiliary liquid (F1) on the substrate (W) is heated. In the first curing step, a first cured film (H1) is formed on a substrate (W). In the first thermal decomposition step, the first cured film (H1) is thermally decomposed by heating the first cured film (H1). In the first thermal decomposition step, the substrate (W) is dried.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a substrate processing method. The substrate is, for example, a semiconductor wafer, a substrate for a liquid crystal display, a substrate for an organic EL (Electroluminescence), a substrate for an FPD (Flat Panel Display), a substrate for an optical display, a substrate for a magnetic disk, a substrate for an optical disk, a substrate for an optical magneto-magnetic disk, a substrate for a photomask, or a substrate for a solar cell. Background Art

[0002] Patent document 1 discloses a substrate processing method for processing a substrate. The substrate processing method of Patent document 1 includes a processing step, a replacement step, and a removal step. In the processing step, a rinse liquid is supplied to the substrate. In the replacement step, the rinse liquid on the substrate is replaced with an organic solvent. In the removal step, the organic solvent is removed from the substrate. Through the removal step, the substrate is dried.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1

[0006] Japanese Patent Laid-Open No. 2012-156561 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] There are also cases where the previous substrate processing method cannot properly process the substrate. For example, when the substrate has a pattern, the previous substrate processing method may also cause the pattern to collapse. For example, when the pattern is fine, there are also cases where the previous substrate processing method cannot fully suppress the collapse of the pattern.

[0009] The present invention has been made in view of the above situation, and an object of the present invention is to provide a substrate processing method capable of appropriately processing a substrate.

[0010] Means used to solve problems

[0011] In order to achieve this object, the present invention adopts the following structure. That is, the present invention is a substrate processing method, which processes a substrate formed with a pattern including a plurality of protrusions and a plurality of recesses, and includes: a first coating step, coating the substrate with a first drying auxiliary liquid including a thermosetting material and a solvent; a first curing step, heating the first drying auxiliary liquid on the substrate to form a first cured film on the substrate; and a first thermal decomposition step, heating the first cured film to thermally decompose the first cured film to dry the substrate; in the first curing step, at least a portion of the first cured film is formed above the pattern, the first cured film is in contact with the upper end of the protrusion, and the first cured film is entirely located above the bottom of the recess.

[0012] The substrate processing method is used to process a substrate formed with a pattern. The pattern includes a plurality of protrusions and a plurality of recesses. The substrate processing method includes a first coating step and a first curing step. In the first coating step, a first drying auxiliary liquid is coated on the substrate. The first drying auxiliary liquid includes a thermosetting material and a solvent. In the first curing step, the first drying auxiliary liquid on the substrate is heated. In the first curing step, a first cured film is formed on the substrate. Therefore, the first cured film can be appropriately formed on the substrate.

[0013] In the first curing step, at least a portion of the first cured film is formed above the pattern. In the first curing step, the first cured film is in contact with the upper end of the protrusion. Therefore, the first cured film can appropriately support the protrusion.

[0014] In the first curing step, the first cured film is entirely located above the bottom of the concave portion. Therefore, a portion of the convex portion does not contact the first cured film. Therefore, in the first curing step, the convex portion is not easily affected by the volume change of the first cured film.

[0015] The substrate processing method includes a first thermal decomposition step. In the first thermal decomposition step, the first cured film is thermally decomposed by heating the first cured film. In the first thermal decomposition step, the substrate is dried. Therefore, the first cured film can be appropriately thermally decomposed. Furthermore, in the first thermal decomposition step, the convex portion is not easily affected by the volume change of the first cured film. Therefore, the first cured film can be appropriately removed from the substrate. Therefore, the collapse of the convex portion can be suppressed, and the substrate can be dried. That is, the substrate can be dried in a state where the pattern is protected.

[0016] As described above, according to the substrate processing method, the substrate can be appropriately processed.

[0017] In the substrate processing method, it is preferred that the width of the concave portion is 10 nm or less. In the first curing step, it is very easy to make the entire first cured film located above the bottom of the concave portion. Therefore, it is easier to properly process the substrate.

[0018] In the substrate processing method, preferably, in the first curing step, the first cured film bridges the upper ends of the protrusions. The first cured film can more appropriately support the protrusions.

[0019] In the above-mentioned substrate processing method, it is preferred that: in the above-mentioned first curing step, the above-mentioned first cured film is entirely located at a position equal to or higher than the above-mentioned upper end of the above-mentioned convex portion. The first cured film is entirely located above the concave portion. The first cured film substantially does not have a portion located in the concave portion. Therefore, the convex portion is substantially not affected by the volume change of the first cured film.

[0020] In the above-mentioned substrate processing method, it is preferred that: in the above-mentioned first curing step, the above-mentioned first cured film has a lower surface, the above-mentioned lower surface of the above-mentioned first cured film is in contact with the above-mentioned upper end of the above-mentioned convex part, and is convexly curved upward between the above-mentioned convex parts adjacent to each other. The shape of the lower surface of the first cured film can appropriately prevent the first cured film from entering the concave part. Therefore, the convex part can be appropriately protected from the influence of the volume change of the first cured film. The convex part is substantially not affected by the volume change of the first cured film.

[0021] In the above-mentioned substrate processing method, it is preferred that: in the above-mentioned first curing step, the above-mentioned thermosetting material becomes a polymer, the above-mentioned first cured film contains the above-mentioned polymer, and the above-mentioned polymer has a length greater than the width of the above-mentioned recess. The recess is too narrow for the polymer of the thermosetting material. Therefore, it is difficult for the thermosetting material to become a polymer in the recess. Therefore, it is difficult to form the first cured film in the recess. Therefore, in the first curing step, it is easier to make the first cured film all located above the bottom of the recess. It is preferred that the first cured film is all located above the bottom of the recess.

[0022] In the substrate processing method, it is preferred that: in the first curing step, the heating temperature of the first drying auxiliary liquid is adjusted based on the width of the concave portion. In this way, regardless of the width of the concave portion, it is easier to make the first cured film all located above the bottom of the concave portion in the first curing step. Regardless of the width of the concave portion, it is preferred that the first cured film all located above the bottom of the concave portion.

[0023] In the above-mentioned substrate processing method, it is preferred that: in the above-mentioned first curing step, the above-mentioned first drying auxiliary liquid is heated at a first low temperature, and in the above-mentioned first thermal decomposition step, the above-mentioned first cured film is heated at a first high temperature higher than the above-mentioned first low temperature. The first low temperature is lower than the first high temperature. Therefore, in the first curing step, thermal decomposition of the first cured film can be appropriately prevented. Therefore, in the first curing step, the first cured film can be appropriately formed. Therefore, in the first curing step, the first cured film can appropriately support the protrusion. The first high temperature is higher than the first low temperature. Therefore, in the first thermal decomposition step, the first cured film can be appropriately thermally decomposed.

[0024] In the above substrate processing method, it is preferred that: in the above first hardening step, the above solvent in the above first drying auxiliary liquid is also evaporated. Therefore, when the first hardening step is completed, no solvent exists on the substrate. That is, in the first thermal decomposition step, no solvent exists on the substrate. Therefore, in the first thermal decomposition step, it is easier to protect the convex portion.

[0025] In the above-mentioned substrate processing method, it is preferred that: in the above-mentioned first curing step, the above-mentioned first drying auxiliary liquid includes a non-reactive portion that does not become the above-mentioned first cured film, and in the above-mentioned first curing step, the above-mentioned non-reactive portion of the above-mentioned first drying auxiliary liquid is removed from the above-mentioned substrate. Therefore, when the first curing step is completed, the first drying auxiliary liquid does not exist on the substrate. That is, in the first thermal decomposition step, the first drying auxiliary liquid does not exist on the substrate. Therefore, in the first thermal decomposition step, it is further easier to protect the convex portion.

[0026] The substrate processing method is preferably configured such that: the substrate processing method further comprises a first processing liquid supplying step of supplying a processing liquid to the substrate before the first coating step. In this way, the substrate can be processed more appropriately.

[0027] In the substrate processing method, it is preferred that: in the first coating step, the processing liquid is removed from the substrate. Therefore, in the first hardening step and the first thermal decomposition step, the processing liquid is not present on the substrate. Therefore, in the first hardening step and the first thermal decomposition step, it is easier to protect the convex portion.

[0028] The present invention is a substrate processing method, which processes a substrate formed with a pattern including a plurality of protrusions and a plurality of recesses, comprising a second coating step of coating the substrate with a second drying auxiliary liquid including an ultraviolet curable material; a second curing step of irradiating the second drying auxiliary liquid on the substrate with ultraviolet rays, thereby forming a second cured film on the substrate; and a second thermal decomposition step of heating the second cured film to thermally decompose the second cured film to dry the substrate; in the second curing step, at least a portion of the second cured film is formed above the pattern, the second cured film is in contact with the upper end of the protrusion, and the entire second cured film is located above the bottom of the recess.

[0029] The substrate processing method is used to process a substrate formed with a pattern. The pattern includes a plurality of protrusions and a plurality of recesses. The substrate processing method includes a second coating step and a second curing step. In the second coating step, a second drying auxiliary liquid is coated on the substrate. The second drying auxiliary liquid includes an ultraviolet curable material. In the second curing step, ultraviolet rays are irradiated on the second drying auxiliary liquid on the substrate. In the second curing step, a second cured film is formed on the substrate. Therefore, the second cured film can be appropriately formed on the substrate.

[0030] In the second curing step, at least a portion of the second cured film is formed above the pattern. In the second curing step, the second cured film is in contact with the upper end of the protrusion. Therefore, the second cured film can appropriately support the protrusion.

[0031] In the second curing step, the second cured film is entirely located above the bottom of the concave portion. Therefore, at least a portion of the convex portion does not contact the second cured film. Therefore, in the second curing step, the convex portion is not easily affected by the volume change of the second cured film.

[0032] The substrate processing method includes a second thermal decomposition step. In the second thermal decomposition step, the second cured film is thermally decomposed by heating the second cured film. In the second thermal decomposition step, the substrate is dried. Therefore, the second cured film can be thermally decomposed appropriately. Furthermore, in the second thermal decomposition step, the convex portion is not easily affected by the volume change of the second cured film. Therefore, the second cured film can be appropriately removed from the substrate. Therefore, the collapse of the convex portion can be suppressed, and the substrate can be dried. That is, the substrate can be dried in a state where the pattern is protected.

[0033] As described above, according to the substrate processing method, the substrate can be appropriately processed.

[0034] In the above substrate processing method, it is preferred that the width of the concave portion is 10 nm or less. In the second curing step, it is very easy to make the entire second cured film located above the bottom of the concave portion. Therefore, it is easier to properly process the substrate.

[0035] In the substrate processing method, it is preferable that in the second curing step, the second cured film bridges the upper ends of the protrusions. The second cured film can more appropriately support the protrusions.

[0036] In the above-mentioned substrate processing method, it is preferred that: in the above-mentioned second curing step, the above-mentioned second cured film is entirely located at a position equal to or higher than the above-mentioned upper end of the above-mentioned convex portion. The second cured film is entirely located above the concave portion. The second cured film substantially does not have a portion located in the concave portion. Therefore, the convex portion is substantially not affected by the volume change of the second cured film.

[0037] In the above-mentioned substrate processing method, it is preferred that: in the above-mentioned second curing step, the above-mentioned second cured film has a lower surface, the above-mentioned lower surface of the above-mentioned second cured film is in contact with the above-mentioned upper end of the above-mentioned convex portion, and is convexly curved upward between the above-mentioned convex portions adjacent to each other. The shape of the lower surface of the second cured film can appropriately prevent the second cured film from entering the concave portion. Therefore, the convex portion can be appropriately protected from the volume change of the second cured film. The convex portion is substantially not affected by the volume change of the second cured film.

[0038] In the above-mentioned substrate processing method, it is preferred that: in the above-mentioned second curing step, the above-mentioned ultraviolet curable material becomes a polymer, the above-mentioned second cured film contains the above-mentioned polymer, and the above-mentioned polymer has a length greater than the width of the above-mentioned recess. The recess is too narrow for the polymer of the ultraviolet curable material. Therefore, it is difficult for the ultraviolet curable material to become a polymer in the recess. Therefore, it is difficult to form a second cured film in the recess. Therefore, in the second curing step, it is easier to make the second cured film all located at a position higher than the bottom of the recess. It is preferred that the second cured film is all located at a position higher than the bottom of the recess.

[0039] In the substrate processing method, it is preferred that: when the second curing step is completed, a portion of the second drying auxiliary liquid remains on the substrate, and in the second thermal decomposition step, the second drying auxiliary liquid remaining on the substrate is also evaporated. In the second thermal decomposition step, the second drying auxiliary liquid remaining on the substrate can be appropriately removed from the substrate. Therefore, the substrate can be appropriately dried.

[0040] In the above-mentioned substrate processing method, it is preferred that: in the above-mentioned second thermal decomposition step, before the above-mentioned second cured film is thermally decomposed, the above-mentioned second drying auxiliary liquid remaining on the above-mentioned substrate evaporates. In the second thermal decomposition step, the second drying auxiliary liquid remaining on the substrate evaporates, and thereafter, the second cured film is thermally decomposed. In the second thermal decomposition step, the second cured film is not substantially thermally decomposed until the second drying auxiliary liquid remaining on the substrate evaporates. Therefore, in the second thermal decomposition step, the second cured film always supports the protrusion until the second drying auxiliary liquid remaining on the substrate evaporates. That is, in the second thermal decomposition step, the second cured film can appropriately protect the protrusion from the influence of the second drying auxiliary liquid. Furthermore, when the second cured film is thermally decomposed, the second drying auxiliary liquid does not exist on the substrate. Therefore, when the second cured film is thermally decomposed, it is easier to protect the protrusion. Therefore, the substrate can be appropriately dried.

[0041] In the substrate processing method, it is preferred that: in the second curing step, the second drying auxiliary liquid includes a non-reactive portion that does not become the second cured film, and in the second thermal decomposition step, the non-reactive portion of the second drying auxiliary liquid is removed from the substrate. In the second thermal decomposition step, the non-reactive portion of the second drying auxiliary liquid can be appropriately removed from the substrate. Therefore, the substrate can be appropriately dried.

[0042] In the above-mentioned substrate processing method, it is preferred that: in the above-mentioned second thermal decomposition step, before the above-mentioned second cured film is thermally decomposed, the above-mentioned non-reactive portion of the second drying auxiliary liquid is removed from the substrate. In the second thermal decomposition step, until the non-reactive portion of the second drying auxiliary liquid is removed from the substrate, the second cured film is not substantially thermally decomposed. Therefore, in the second thermal decomposition step, until the non-reactive portion of the second drying auxiliary liquid is removed from the substrate, the second cured film always supports the protrusion. That is, in the second thermal decomposition step, the second cured film can appropriately protect the protrusion from the influence of the second drying auxiliary liquid. Furthermore, when the second cured film is thermally decomposed, the second drying auxiliary liquid is not present on the substrate. Therefore, when the second cured film is thermally decomposed, it is easier to protect the protrusion.

[0043] In the substrate processing method, the second thermal decomposition step preferably includes: a low temperature heating step of heating the non-reactive portion of the second drying auxiliary liquid at a second low temperature to evaporate the non-reactive portion of the second drying auxiliary liquid; and a high temperature heating step of thermally decomposing the second cured film by heating the second cured film at a second high temperature higher than the second low temperature after the low temperature heating step. In the low temperature heating step, the non-reactive portion of the second drying auxiliary liquid can be appropriately removed from the substrate. As a result, the second drying auxiliary liquid does not exist on the substrate when the low temperature heating step is completed. After the low temperature heating step, the high temperature heating step is performed. In the high temperature heating step, the second drying auxiliary liquid does not exist on the substrate. Therefore, in the high temperature heating step, it is easier to protect the convex portion. The second low temperature is lower than the second high temperature. Therefore, in the low temperature heating step, the thermal decomposition of the second cured film can be appropriately prevented. Therefore, in the low temperature heating step, the convex portion can be appropriately supported by the second cured film. Therefore, in the low temperature heating step, the convex portion can be appropriately protected by the second cured film. On the other hand, in the second high-temperature heating step, the second cured film is thermally decomposed. The second high temperature is higher than the second low temperature. Therefore, in the high-temperature heating step, the second cured film can be thermally decomposed appropriately.

[0044] The substrate processing method preferably further comprises a second processing liquid supplying step of supplying a processing liquid to the substrate before the second coating step, so that the substrate can be processed more appropriately.

[0045] In the substrate processing method, it is preferred that: in the second coating step, the processing liquid is removed from the substrate. Therefore, in the second hardening step and the second thermal decomposition step, the processing liquid is not present on the substrate. Therefore, in the second hardening step and the second thermal decomposition step, it is easier to protect the convex portion.

[0046] Effects of the Invention

[0047] According to the substrate processing method of the present invention, a substrate can be processed appropriately. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 This is a diagram schematically showing a part of a substrate.

[0049] Figure 2 It is a plan view showing the interior of the substrate processing apparatus according to the first embodiment.

[0050] Figure 3 It is a control block diagram of a substrate processing apparatus.

[0051] Figure 4 It is a diagram showing the configuration of a processing unit according to the first embodiment.

[0052] Figure 5 This is a flowchart showing the procedure of the substrate processing method according to the first embodiment.

[0053] Figure 6 It is a figure which shows schematically the board|substrate in the 1st coating process.

[0054] Figure 7 It is a figure which shows schematically the board|substrate in the 1st hardening process.

[0055] Figure 8 This is an enlarged view schematically showing the substrate in the first curing step.

[0056] Fig. 9 This is an enlarged view schematically showing the substrate in the first curing step.

[0057] Fig.10 This is an enlarged view schematically showing the substrate in the first curing step.

[0058] Fig.11 This is an enlarged view schematically showing the substrate in the first thermal decomposition step.

[0059] Fig.12 This is an enlarged view schematically showing the substrate in the first thermal decomposition step.

[0060] Fig.13 It is a diagram showing the configuration of a processing unit according to the second embodiment.

[0061] Fig.14 This is a flowchart showing the procedure of the substrate processing method according to the second embodiment.

[0062] Fig.15 It is a figure which shows schematically the board|substrate in the 2nd coating process.

[0063] Fig.16 It is a figure which shows typically the board|substrate in the 2nd hardening process.

[0064] Fig.17 It is an enlarged view schematically showing the substrate in the second curing step.

[0065] Fig.18 This is an enlarged view schematically showing the substrate in the second thermal decomposition step.

[0066] Fig.19 This is an enlarged view schematically showing the substrate in the second thermal decomposition step.

[0067] Fig. 20 This is an enlarged view schematically showing the substrate in the second thermal decomposition step.

[0068] Fig.21 This is an enlarged view schematically showing the substrate in the second thermal decomposition step.

[0069] Fig. 22 This is a flowchart showing the procedure of the second thermal decomposition step according to the modified embodiment.

[0070] Fig.23 It is a diagram showing the structure of a processing unit according to a modified embodiment.

[0071] Fig.24 It is a left side view showing the structure of the left portion of the substrate processing apparatus according to the modified embodiment. DETAILED DESCRIPTION

[0072] Hereinafter, the substrate processing method of the present invention will be described with reference to the accompanying drawings.

[0073] <First embodiment>

[0074] <1-1.Substrate>

[0075] The substrate W is, for example, a semiconductor wafer, a substrate for a liquid crystal display, a substrate for an organic EL (Electroluminescence), a substrate for an FPD (Flat Panel Display), a substrate for an optical display, a substrate for a magnetic disk, a substrate for an optical disk, a substrate for an optical magnetic disk, a substrate for a photomask, or a substrate for a solar cell. The substrate W has a thin flat plate shape. The substrate W has a roughly circular shape when viewed from above.

[0076] Figure 1 2 is a diagram schematically showing a part of a substrate W. The substrate W has a pattern P. The pattern P is formed on the surface WS of the substrate W. The pattern P has, for example, a concavo-convex shape.

[0077] The pattern P, for example, has a plurality of convex portions A. Each convex portion A is a part of the substrate W. Each convex portion A is a structure. Each convex portion A, for example, is composed of at least one of a single crystal silicon film, a silicon oxide film (SiO2), a silicon nitride film (SiN), and a polycrystalline silicon film. Each convex portion A rises from the surface WS. The plurality of convex portions A are separated from each other.

[0078] Each convex portion A has a base end A1, a top end A2, and a side A3. The base end A1 is connected to the surface WS. The side A3 extends from the base end A1 to the top end A2.

[0079] The convex portion A has a height AH. The height AH corresponds to the length of the side A3. The height AH corresponds to the length between the base end A1 and the top end A2.

[0080] The pattern P has a plurality of recesses B. Each recess B is a space. The plurality of recesses B may be interconnected, for example. Alternatively, the plurality of recesses B may be isolated from each other. The recesses B are located on the side of the convex portion A. The recesses B are located around the convex portion A. The recesses B are located between two or more adjacent convex portions A. The recesses B are connected to two or more side edges A3.

[0081] The recess B has a bottom B1. The bottom B1 is located between adjacent base ends A1. The bottom B1 corresponds to the portion of the surface WS located between adjacent base ends A1. The bottom B1 extends between adjacent side edges A3. The recess B is surrounded by the side edges A3 and the bottom B1.

[0082] The concave portion B has a width BW. The width BW corresponds to the distance between two adjacent convex portions A. The width BW corresponds to the distance between two adjacent side edges A3.

[0083] <1-2. Overview of substrate processing apparatus 1>

[0084] Figure 2 1 is a plan view showing the inside of the substrate processing apparatus 1 according to the first embodiment. The substrate processing apparatus 1 processes a substrate W. The processing in the substrate processing apparatus 1 includes a drying process.

[0085] The substrate processing apparatus 1 includes an indexer unit 3 and a processing block 7. The processing block 7 is connected to the indexer unit 3. The indexer unit 3 supplies substrates W to the processing block 7. The processing block 7 processes the substrates W. The indexer unit 3 recovers the substrates W from the processing block 7.

[0086] In this specification, for the sake of convenience, the direction in which the divider portion 3 and the processing block 7 are arranged is referred to as the "front-to-back direction X". The front-to-back direction X is horizontal. The direction from the processing block 7 to the divider portion 3 in the front-to-back direction X is referred to as the "front". The direction opposite to the front is referred to as the "rear". The direction orthogonal to the front-to-back direction X is referred to as the "width direction Y". The width direction Y is horizontal. One direction in the "width direction Y" is appropriately referred to as the "right". The direction opposite to the right is referred to as the "left". When there is no need to distinguish between the front-to-back direction X and the width direction Y, they are collectively referred to as the "horizontal direction". The direction perpendicular to the horizontal direction is referred to as the "vertical direction Z". Front, rear, right, left, top, and bottom are appropriately indicated in each figure for reference.

[0087] The indexer unit 3 includes a plurality of (for example, four) carrier mounting units 4. Each carrier mounting unit 4 mounts one carrier C. The carrier C accommodates a plurality of substrates W. The carrier C is, for example, a FOUP (Front Opening Unified Pod), a SMIF (Standard Mechanical Interface), or an OC (Open Cassette).

[0088] The indexer unit 3 includes a transport mechanism 5 . The transport mechanism 5 is disposed behind the carrier placement unit 4 . The transport mechanism 5 transports the substrate W. The transport mechanism 5 is configured to be accessible to the carrier C placed on the carrier placement unit 4 .

[0089] The transport mechanism 5 includes a hand 5a and a hand driving unit 5b. The hand 5a supports the substrate W. The hand driving unit 5b is connected to the hand 5a. The hand driving unit 5b moves the hand 5a. The hand driving unit 5b moves the hand 5a in, for example, the front-back direction X, the width direction Y, and the vertical direction Z. The hand driving unit 5b rotates the hand 5a in a horizontal plane, for example.

[0090] The processing block 7 includes a transport mechanism 8 . The transport mechanism 8 transports the substrate W. The transport mechanism 8 is configured to be able to receive the substrate W from the transport mechanism 5 and to deliver the substrate W to the transport mechanism 5 .

[0091] The transport mechanism 8 includes a hand 8a and a hand driving unit 8b. The hand 8a supports the substrate W. The hand driving unit 8b is connected to the hand 8a. The hand driving unit 8b moves the hand 8a. The hand driving unit 8b moves the hand 8a in, for example, the front-rear direction X, the width direction Y, and the vertical direction Z. The hand driving unit 8b rotates the hand 8a in a horizontal plane, for example.

[0092] The processing block 7 includes a plurality of processing units 11. The processing units 11 are disposed on the side of the conveying mechanism 8. Each processing unit 11 processes a substrate W.

[0093] Each processing unit 11 includes a substrate holding portion 13. The substrate holding portion 13 holds a substrate W.

[0094] The transport mechanism 8 is configured to be accessible to each processing unit 11. The transport mechanism 8 is configured to be able to deliver the substrate W to the substrate holding portion 13 and to be able to pick up the substrate W from the substrate holding portion 13.

[0095] Figure 3 1 is a control block diagram of the substrate processing apparatus 1. The substrate processing apparatus 1 includes a control unit 10. The control unit 10 is connected to the conveying mechanisms 5 and 8 and the processing unit 11 so as to be able to communicate with each other. The control unit 10 controls the conveying mechanisms 5 and 8 and the processing unit 11.

[0096] The control unit 10 is implemented by a central processing unit (CPU) that performs various processing, a RAM (Random-Access Memory) that serves as a processing operation area, and a storage medium such as a fixed disk. The control unit 10 has various information pre-stored in the storage medium. The information possessed by the control unit 10 includes, for example, transport condition information and processing condition information. The transport condition information specifies conditions related to the operation of the transport mechanism 5, 8. The processing condition information specifies conditions related to the operation of the processing unit 11. The processing condition information is also called a processing recipe.

[0097] An operation example of the substrate processing apparatus 1 will be briefly described.

[0098] The indexer unit 3 supplies the substrate W to the processing block 7 . Specifically, the transport mechanism 5 delivers the substrate W from the carrier C to the transport mechanism 8 of the processing block 7 .

[0099] The transport mechanism 8 distributes the substrate W to the processing unit 11 . Specifically, the transport mechanism 8 transports the substrate W from the transport mechanism 5 to the substrate holding portion 13 of each processing unit 11 .

[0100] The processing unit 11 processes the substrate W held by the substrate holding portion 13. The processing unit 11 performs a drying process on the substrate W, for example.

[0101] After the processing units 11 have processed the substrate W, the transport mechanism 8 collects the substrate W from each processing unit 11 . Specifically, the transport mechanism 8 picks up the substrate W from each substrate holding portion 13 . Then, the transport mechanism 8 delivers the substrate W to the transport mechanism 5 .

[0102] The indexer unit 3 collects the substrate W from the processing block 7. Specifically, the transport mechanism 5 transports the substrate W from the transport mechanism 8 to the carrier C.

[0103] <1-3. Configuration of Processing Unit 11>

[0104] Figure 4 1 is a diagram showing the configuration of the processing unit 11 according to the first embodiment. Each processing unit 11 has the same structure. The processing unit 11 is a single-wafer type. That is, each processing unit 11 processes only one substrate W at a time.

[0105] The processing unit 11 includes a housing 12 . The housing 12 has a substantially box-like shape. The substrate W is processed inside the housing 12 .

[0106] The interior of the housing 12 is maintained at normal pressure, for example. Therefore, the substrate W is processed, for example, under normal pressure. Here, normal pressure includes standard atmospheric pressure (1 atmosphere, 101325 Pa). Normal pressure is, for example, a pressure in the range of 0.7 atmospheres to 1.3 atmospheres. In this specification, pressure is expressed as absolute pressure based on absolute vacuum.

[0107] The substrate holding portion 13 is provided inside the housing 12. The substrate holding portion 13 holds one substrate W. The substrate holding portion 13 holds the substrate W in a substantially horizontal posture.

[0108] The substrate holding portion 13 is located below the substrate W held by the substrate holding portion 13. The substrate holding portion 13 contacts at least one of the lower surface WS2 of the substrate W and the peripheral edge of the substrate W. The substrate holding portion 13 does not contact the upper surface WS1 of the substrate W. Here, the upper surface WS1 faces upward. The lower surface WS2 faces downward. The upper surface WS1 is a part of the surface WS. The lower surface WS2 is another part of the surface WS. The lower surface WS2 is also called the back side of the substrate W.

[0109] An example of the structure of the substrate holding portion 13 is described. The substrate holding portion 13 includes a support member 14. The support member 14 has a plate-like shape. The support member 14 extends in the horizontal direction. The support member 14 has a size substantially the same as the substrate W when viewed from above, but the relevant illustration is omitted. The support member 14 has a circular ring shape when viewed from above. The support member 14 forms an opening. The opening is located at the center of the support member 14 when viewed from above.

[0110] The substrate holding portion 13 includes a plurality of holding pins 15. Each holding pin 15 is supported by a support member 14. Each holding pin 15 is disposed at a peripheral portion of the support member 14. Each holding pin 15 extends upward from the support member 14. Each holding pin 15 holds a substrate W. When the substrate W is held by the holding pins 15, the substrate W is located above the support member 14.

[0111] The processing unit 11 includes a rotation drive unit 17. At least a part of the rotation drive unit 17 is disposed inside the housing 12. The rotation drive unit 17 is connected to the substrate holding unit 13. The rotation drive unit 17 rotates the substrate holding unit 13. The substrate W held by the substrate holding unit 13 rotates integrally with the substrate holding unit 13. The substrate W held by the substrate holding unit 13 rotates, for example, around a rotation axis D. The rotation axis D passes through the center of the substrate W, for example. The rotation axis D extends along the vertical direction Z, for example.

[0112] An example of the configuration of the rotation drive unit 17 is described. The rotation drive unit 17 includes a shaft 18 and a motor 19. The shaft 18 is connected to the support member 14. The shaft 18 extends downward from the support member 14. The shaft 18 extends on the rotation axis D. The shaft 18 is a so-called hollow shaft. The shaft 18 has a cylindrical shape. The shaft 18 forms a hollow portion. The hollow portion is located inside the shaft 18. The motor 19 is connected to the shaft 18. The motor 19 rotates the shaft 18 around the rotation axis D.

[0113] The processing unit 11 includes supply parts 21a and 21b. The supply parts 21a and 21b supply liquid to the substrate W held by the substrate holding part 13. The supply parts 21a and 21b supply liquid to the upper surface WS1 of the substrate W held by the substrate holding part 13.

[0114] The supply unit 21a supplies the processing liquid L. The processing liquid L is used to process the substrate W. The processing liquid L is used, for example, to clean the substrate W. The processing liquid L is, for example, a cleaning liquid. The processing liquid L is, for example, a rinse liquid.

[0115] The processing liquid L is, for example, an organic solvent, an alcohol, or isopropyl alcohol (IPA).

[0116] The treatment liquid L is, for example, deionized water. The treatment liquid L is, for example, SC1. SC1 is a mixture of ammonia water, hydrogen peroxide, and deionized water.

[0117] The supply unit 21b supplies the first drying auxiliary liquid F1. The first drying auxiliary liquid F1 is used to dry the substrate W. The first drying auxiliary liquid F1 has a function of assisting the drying of the substrate W. The first drying auxiliary liquid F1 is a liquid. The first drying auxiliary liquid F1 is a liquid at room temperature.

[0118] The first drying auxiliary liquid F1 contains a thermosetting material. The thermosetting material has thermosetting properties. The thermosetting material has not yet been cured by heat. The thermosetting material has the property of polymerizing by heat. The thermosetting material has the property of becoming a polymer by heat. The thermosetting material has the property of curing by heat.

[0119] The thermosetting material contains at least one of a monomer and an oligomer. At least one of the monomer and the oligomer in the thermosetting material has the property of being polymerized by heat. The thermosetting material does not contain a polymer. The thermosetting material does not contain a macromolecular compound.

[0120] The thermosetting material includes, for example, phenol. The thermosetting material includes, for example, a phenol monomer. The thermosetting material includes, for example, an oligomer derived from phenol. The thermosetting material includes, for example, novolac. The thermosetting material includes, for example, a novolac-type phenolic resin. Novolac is an example of an oligomer derived from phenol. Novolac-type phenolic resin is an example of an oligomer derived from phenol.

[0121] The first drying auxiliary liquid F1 contains a solvent. The solvent is a liquid. The solvent is a liquid at room temperature. The solvent is volatile. The solvent is easily vaporized. The solvent can dissolve the thermosetting material. Therefore, the thermosetting material in the first drying auxiliary liquid F1 is dissolved in the solvent. That is, the first drying auxiliary liquid F1 contains a solvent and a thermosetting material dissolved in the solvent. The thermosetting material is equivalent to the solute of the first drying auxiliary liquid F1.

[0122] The solvent is, for example, an organic solvent. The solvent is, for example, an alcohol. The solvent includes, for example, at least one of isopropyl alcohol (IPA), methanol, ethanol, 1-propanol, isobutyl alcohol, propylene glycol monomethyl ether acetate (PGMEA), 1-ethoxy-2-propanol (PGEE), acetone, and 1-butanol.

[0123] For example, the first drying auxiliary liquid F1 contains only a thermosetting material and a solvent.

[0124] The supply unit 21a includes a nozzle 22a. The nozzle 22a discharges the processing liquid L. The supply unit 21b includes a nozzle 22b. The nozzle 22b discharges the first drying auxiliary liquid F1.

[0125] The nozzles 22a and 22b are respectively disposed inside the housing 12. The nozzles 22a and 22b are respectively movable between a standby position and a processing position. Figure 4 The nozzles 22a and 22b at the standby position are indicated by solid lines. Figure 4 The nozzles 22a and 22b at the processing position are indicated by dotted lines. The standby position is, for example, a position offset from above the substrate W held by the substrate holding portion 13. The processing position is, for example, a position above the substrate W held by the substrate holding portion 13.

[0126] The first drying auxiliary liquid F1 is used inside the housing 12. As described above, the inside of the housing 12 is maintained at, for example, normal pressure. Therefore, the first drying auxiliary liquid F1 is used, for example, under normal pressure. The processing liquid L is used inside the housing 12. Therefore, the processing liquid L is also used, for example, under normal pressure.

[0127] The supply unit 21a includes a pipe 23a and a valve 24a. The pipe 23a is connected to the nozzle 22a. The valve 24a is provided on the pipe 23a. When the valve 24a is opened, the nozzle 22a ejects the processing liquid L. When the valve 24a is closed, the nozzle 22a does not eject the processing liquid L. Similarly, the supply unit 21b includes a pipe 23b and a valve 24b. The pipe 23b is connected to the nozzle 22b. The valve 24b is provided on the pipe 23b. The valve 24b controls the ejection of the first drying auxiliary liquid F1.

[0128] The supply unit 21a is connected to a supply source 25a. The supply source 25a is connected to, for example, the pipe 23a. The supply source 25a delivers the processing liquid L to the supply unit 21a. Similarly, the supply unit 21b is connected to a supply source 25b. The supply source 25b is connected to, for example, the pipe 23b. The supply source 25b delivers the first drying auxiliary liquid F1 to the supply unit 21b.

[0129] At least a portion of the piping 23a may be provided outside the housing 12. The piping 23b may be configured in the same manner as the piping 23a. The valve 24a may be provided outside the housing 12. The valve 24b may be configured in the same manner as the valve 24a. The supply source 25a may be provided outside the housing 12. The supply source 25b may be configured in the same manner as the supply source 25a.

[0130] The supply source 25a may supply the processing liquid L to a plurality of processing units 11. Alternatively, the supply source 25a may supply the processing liquid L to only one processing unit 11. The same applies to the supply source 25b.

[0131] The supply source 25a may be an element of the substrate processing apparatus 1. For example, the supply source 25a may be disposed inside the substrate processing apparatus 1. Alternatively, the supply source 25a may not be an element of the substrate processing apparatus 1. For example, the supply source 25a may also be disposed outside the substrate processing apparatus 1. Similarly, the supply source 25b may be an element of the substrate processing apparatus 1. Alternatively, the supply source 25b may not be an element of the substrate processing apparatus 1.

[0132] The supply unit 21a may also be referred to as a “processing liquid supply unit”. The supply unit 21b may also be referred to as a “drying auxiliary liquid supply unit”.

[0133] The processing unit 11 includes a heating unit 31 . The heating unit 31 heats the substrate W held by the substrate holding unit 13 .

[0134] An example of the configuration of the heating unit 31 is described. The heating unit 31 includes a heater 32. The heater 32 generates heat. The heater 32 is, for example, a resistance heater. The heater 32 is, for example, an electric heater. The heater 32 includes, for example, an electric heating wire. The heater 32 is arranged below the substrate W held by the substrate holding unit 13. The heater 32 is opposite to the lower surface WS2 of the substrate W held by the substrate holding unit 13. The heater 32 extends in the horizontal direction. The heating range heated by the heater 32 covers the entire substrate W. The heater 32 heats the entire substrate W uniformly.

[0135] The heating section 31 includes a supporting member 33 and a shaft 34. The supporting member 33 supports the heater 32. The supporting member 33 has a plate-like shape. The supporting member 33 extends in the horizontal direction. The supporting member 33 is located below the substrate W held by the substrate holding section 13. The supporting member 33 is located above the supporting member 14. The supporting member 14 has approximately the same size as the substrate W when viewed from above, but the relevant illustration is omitted. The shaft 34 is connected to the supporting member 33. The shaft 34 extends downward from the supporting member 33. The shaft 34 extends on the rotation axis D. The shaft 34 passes through the opening of the supporting member 14. The shaft 34 is inserted into the hollow portion of the shaft 18. Even when the shaft 18 rotates, the shaft 34 does not rotate. Therefore, the heater 32 and the supporting member 33 do not rotate. The shaft 34 is fixed to the housing 12, for example.

[0136] The heating unit 31 includes a power supply 35. The power supply 35 is electrically connected to the heater 32. The power supply 35 supplies power to the heater 32. The power supply 35 controls the heater 32. The power supply 35, for example, switches the heater 32 between heating and non-heating. The power supply 35, for example, adjusts the output of the heater 32. The power supply 35, for example, adjusts the heating temperature of the heater 32. The power supply 35, for example, adjusts the heating time of the heater 32.

[0137] The processing unit 11 may further include a cup (not shown). The cup is provided inside the housing 12. The cup is arranged on the side of the substrate holding portion 13. The cup surrounds the outside of the substrate holding portion 13. The cup receives liquid scattered from the substrate W held on the substrate holding portion 13.

[0138] Reference Figure 3 The control unit 10 controls the rotation drive unit 17 . The control unit 10 controls the supply units 21 a and 21 b . The control unit 10 controls the valves 24 a and 24 b . The control unit 10 controls the heating unit 31 . The control unit 10 controls the power supply 35 .

[0139] <1-4. Example of operation of the processing unit 11>

[0140] Reference Figure 4 , 5 . Figure 51 is a flowchart showing the sequence of the substrate processing method of the first embodiment. The substrate processing method is used to process a substrate W having a pattern P formed thereon. The substrate processing method includes steps S1 to S4. Steps S1 to S4 are performed in sequence. Steps S1 to S4 are performed by the processing unit 11. The processing unit 11 operates under the control of the control unit 10.

[0141] Step S1: First treatment liquid supply step

[0142] The processing liquid L is supplied to the substrate W.

[0143] The substrate holding part 13 holds the substrate W. The rotation drive part 17 rotates the substrate holding part 13. The supply part 21a supplies the processing liquid L to the substrate W held by the substrate holding part 13. The heating part 31 does not heat the substrate W.

[0144] The substrate W is held in a substantially horizontal posture. The substrate W rotates integrally with the substrate holding portion 13. The processing liquid L is supplied to the upper surface WS1 of the substrate W. Since the substrate W is rotating, the processing liquid L smoothly spreads over the entire upper surface WS1. For example, the processing liquid L cleans the substrate W.

[0145] Then, the supply unit 21 a stops supplying the processing liquid L to the substrate W.

[0146] In the first process liquid supplying step, the interior of the housing 12 is maintained at room temperature, for example. Therefore, in the first process liquid supplying step, the substrate W is processed, for example, in a room temperature environment. The process liquid L is used in a room temperature environment. Here, room temperature includes room temperature. Room temperature is, for example, a temperature in the range of 5°C to 35°C. Room temperature is, for example, a temperature in the range of 10°C to 30°C. Room temperature is, for example, a temperature in the range of 15°C to 25°C.

[0147] When the first processing liquid supplying step is completed, the processing liquid L is present on the substrate W. The substrate W is in a wet state. The substrate W is in a non-dry state.

[0148] Step S2: First coating step

[0149] The substrate W is coated with the first drying auxiliary liquid F1.

[0150] The substrate holding part 13 holds the substrate W. The rotation driving part 17 rotates the substrate holding part 13 and the substrate W. The supply part 21 b supplies the first drying auxiliary liquid F1 to the substrate W held by the substrate holding part 13. The heating part 31 does not heat the substrate W.

[0151] The first drying auxiliary liquid F1 is supplied to the upper surface WS1 of the substrate W. Since the substrate W is rotating, the first drying auxiliary liquid F1 is smoothly spread over the entire upper surface WS1. The first drying auxiliary liquid F1 is applied to the upper surface WS1. The upper surface WS1 is covered with the first drying auxiliary liquid F1. The first drying auxiliary liquid F1 removes the processing liquid L from the substrate W. The processing liquid L on the substrate W is replaced with the first drying auxiliary liquid F1.

[0152] Then, the supply unit 21 b stops supplying the first drying auxiliary liquid F1 to the substrate W. The rotation drive unit 17 stops rotating the substrate holding unit 13 and the substrate W. The substrate W stops.

[0153] In the first coating step, the interior of the housing 12 is maintained at room temperature, for example. Therefore, in the first coating step, the substrate W is processed at room temperature, for example. The first drying auxiliary liquid F1 is coated on the substrate W at room temperature, for example.

[0154] Figure 6 Schematically showing a substrate W in the first coating step. The substrate W is in a posture with the pattern P facing upward. The pattern P is located on the upper surface WS1 of the substrate W. The pattern P faces upward. The substrate W is held by the substrate holding portion 13. When the substrate W is held by the substrate holding portion 13, the pattern P is located on the upper surface WS1 of the substrate W. When the substrate W is held by the substrate holding portion 13, the pattern P faces upward.

[0155] The positions and shapes of the convex parts A and the concave parts B when the pattern P is facing upward are described. Each convex part A protrudes upward. A plurality of convex parts A are arranged horizontally. The concave part B is recessed downward. The concave part B is open upward. The base end A1 is equivalent to the lower end of the convex part A. The top end A2 is equivalent to the upper end of the convex part A. The bottom part B1 is equivalent to the lower end of the concave part B. The bottom part B1 is located at approximately the same height as the base end A1. The bottom part B1 is located at a position lower than the top end A2.

[0156] Hereinafter, the top end A2 when the pattern P faces upward is appropriately referred to as “upper end A2 ”.

[0157] The first drying auxiliary liquid F1 exists on the substrate W. The first drying auxiliary liquid F1 exists on the upper surface WS1.

[0158] The first drying auxiliary liquid F1 is applied to the pattern P. The pattern P is covered with the first drying auxiliary liquid F1. The pattern P is in contact with the first drying auxiliary liquid F1. The convex portion A is in contact with the first drying auxiliary liquid F1.

[0159] Furthermore, the processing liquid L has been removed from the substrate W by the first drying auxiliary liquid F1. Therefore, the processing liquid L does not exist on the substrate W. In the recess B, no processing liquid L remains.

[0160] The first drying auxiliary liquid F1 on the substrate W forms a first liquid film G1. The first liquid film G1 is located on the substrate W. The first liquid film G1 is located on the upper surface WS1. The first liquid film G1 covers the upper surface WS1. The first liquid film G1 covers the pattern P.

[0161] In the first coating step, the thickness of the first liquid film G1 may be further adjusted. For example, the thickness of the first liquid film G1 may be adjusted while the supply unit 21b supplies the first drying auxiliary liquid F1 to the substrate W. For example, the thickness of the first liquid film G1 may be adjusted after the supply unit 21b stops supplying the first drying auxiliary liquid F1. For example, the thickness of the first liquid film G1 may be adjusted by adjusting the rotation speed of the substrate W. For example, the thickness of the first liquid film G1 may be adjusted by adjusting the rotation time of the substrate W.

[0162] The thickness of the first liquid film G1 is, for example, much greater than the height AH of the convex portion A. The thickness of the first liquid film G1 is, for example, twice or more the height AH. The thickness of the first liquid film G1 is, for example, several dozen times or more the height AH. The thickness of the first liquid film G1 is, for example, several dozen μm or more.

[0163] The thickness of the first liquid film G1 is not too large and is, for example, several hundred μm or less.

[0164] The pattern P is entirely immersed in the first liquid film G1. The convex portion A is entirely immersed in the first liquid film G1.

[0165] The convex portion A does not contact the gas. The convex portion A does not contact the gas-liquid interface. Therefore, the capillary force does not act on the convex portion A. The capillary force is, for example, the surface tension of the first drying auxiliary liquid F1.

[0166] The concave portion B is filled with the first liquid film G1. The entire concave portion B is filled only with the first liquid film G1.

[0167] Step S3: First Hardening Step

[0168] The first drying auxiliary liquid F1 on the substrate W is heated. A first cured film H1 is formed on the substrate W.

[0169] The substrate holding portion 13 holds the substrate W. The heating portion 31 heats the substrate W held by the substrate holding portion 13. The rotation drive portion 17 does not rotate the substrate holding portion 13 and the substrate W.

[0170] Figure 7 Schematically shows the substrate W in the first curing step. The substrate W is in a posture where the pattern P faces upward. The pattern P is located on the upper surface WS1 of the substrate W. The pattern P faces upward.

[0171] The first drying auxiliary liquid F1 is heated via the substrate W held by the substrate holding portion 13 .

[0172] In the first curing step, the first drying auxiliary liquid F1 on the substrate W is heated at the first low temperature T1L. The first low temperature T1L is higher than room temperature. For example, the temperature of the first drying auxiliary liquid F1 rises from room temperature. The temperature of the first drying auxiliary liquid F1 rises to the first low temperature T1L. The first low temperature T1L corresponds to the heating temperature of the first drying auxiliary liquid F1.

[0173] The thermosetting material in the first drying auxiliary liquid F1 on the substrate W begins to polymerize. As the polymerization reaction of the thermosetting material proceeds, the degree of polymerization of the thermosetting material increases. The fluidity of the first drying auxiliary liquid F1 on the substrate W decreases. The first drying auxiliary liquid F1 on the substrate W hardens. The first drying auxiliary liquid F1 on the substrate W hardens.

[0174] Soon, the thermosetting material became a polymer. The polymer of the thermosetting material is equivalent to the cured product of the thermosetting material. The polymer of the thermosetting material is equivalent to a macromolecule. The polymer of the thermosetting material is equivalent to a macromolecular compound.

[0175] The polymer of the thermosetting material constitutes the first cured film H1. The first cured film H1 contains the polymer of the thermosetting material.

[0176] In other words, due to the polymerization reaction of the thermosetting material, part of the first drying auxiliary liquid F1 becomes the first cured film H1. Part of the first liquid film G1 becomes the first cured film H1. Therefore, the first drying auxiliary liquid F1 decreases. The first liquid film G1 becomes thinner.

[0177] The first cured film H1 is formed on the substrate W. The first cured film H1 is formed on the upper surface WS1. The first cured film H1 is formed on the pattern P.

[0178] The first cured film H1 covers the upper surface WS1. The first cured film H1 covers the pattern P.

[0179] Here, the polymer of the thermosetting material has a length greater than the width BW of the recess B. The polymer of the thermosetting material has a size greater than the size of the recess B. Therefore, the thermosetting material cannot be polymerized in the recess B. However, the thermosetting material can be polymerized at a position above the recess B. Therefore, the thermosetting material located above the recess B becomes a polymer. After the thermosetting material located in the recess B moves to a position above the recess B, it becomes a polymer at a position above the recess B.

[0180] Therefore, at least a portion of the first cured film H1 is located above the recess B. In other words, at least a portion of the first cured film H1 is located above the pattern P. At least a portion of the first cured film H1 is located at a position equal to or higher than the upper end A2 of the convex portion A.

[0181] The first cured film H1 is entirely located above the bottom B1 of the recess B. The first cured film H1 is entirely located above the bottom B1. The first cured film H1 is separated from the bottom B1. The first cured film H1 is not in contact with the bottom B1. The first cured film H1 does not have a portion in contact with the bottom B1. At least a portion of the recess B is not filled with the first cured film H1. At least a portion of the recess B is a gap formed between the first cured film H1 and the bottom B1. The gap is located below the first cured film H1 and above the bottom B1.

[0182] The first cured film H1 does not contact at least a portion of each convex portion A. Specifically, the first cured film H1 does not contact at least a portion of each side A3. The first cured film H1 and at least a portion of the side A3 are separated from each other. Therefore, even if the volume of the first cured film H1 changes, it is not easy for the first cured film H1 to apply a significant force to the side A3. "Volume change of the first cured film H1" refers to, for example, expansion of the first cured film H1. "Volume change of the first cured film H1" refers to, for example, contraction of the first cured film H1. The force applied to the side A3 refers to, for example, a force that squeezes the side A3 laterally. The force applied to the side A3 refers to, for example, a force that pulls the side A3 laterally. "Significant force" refers to a force large enough to collapse the convex portion A.

[0183] For example, the first cured film H1 is entirely located above the recessed portion B. For example, the first cured film H1 does not have a portion located at the recessed portion B. For example, the first cured film H1 is entirely located at a position equal to or higher than the upper end A2 of the convex portion A. For example, the first cured film H1 is entirely located above the pattern P. For example, the first cured film H1 is entirely separated from the side A3. For example, the first cured film H1 does not have a portion in contact with the side A3. In this case, even if the volume of the first cured film H1 changes, the first cured film H1 does not apply a force to the side A3.

[0184] The first drying auxiliary liquid F1 includes a non-reactive portion in addition to the portion to be converted into the first cured film H1. The non-reactive portion of the first drying auxiliary liquid F1 remains on the substrate W and does not become the first cured film H1. The non-reactive portion of the first drying auxiliary liquid F1 is located in the concave portion B. The first drying auxiliary liquid F1 in the concave portion B corresponds to the non-reactive portion of the first drying auxiliary liquid F1.

[0185] The first drying auxiliary liquid F1 of the concave portion B contacts a portion of the convex portion A. The first drying auxiliary liquid F1 of the concave portion B contacts at least a portion of the side A3 of the convex portion A.

[0186] As described above, the thermosetting material in the recess B moves upward in the recess B. Therefore, the first drying auxiliary liquid F1 in the recess B does not substantially contain the thermosetting material. The first drying auxiliary liquid F1 in the recess B is substantially composed of the solvent. The non-reactive portion of the first drying auxiliary liquid F1 is substantially composed of the solvent.

[0187] Furthermore, the first cured film H1 is in contact with the upper end A2 of the convex portion A. The first cured film H1 is connected to the upper end A2. The first cured film H1 is connected to the upper end A2. For example, the first cured film H1 is in contact with the upper end A2. Therefore, the first cured film H1 appropriately supports the convex portion A. The first cured film H1 can appropriately prevent the collapse of the convex portion A. For example, the first cured film H1 can prevent the upper end A2 from moving sideways. For example, the first cured film H1 can prevent the convex portion A from falling sideways.

[0188] The first cured film H1 bridges the upper ends A2. The first cured film H1 is equivalent to a bridge connecting the upper ends A2. Two or more upper ends A2 are connected to each other through the first cured film H1. Therefore, the first cured film H1 more appropriately supports the convex portion A. The first cured film H1 can more appropriately prevent the collapse of the convex portion A.

[0189] The first cured film H1 has a thickness. The thickness of the first cured film H1 is much larger than the height AH of the convex portion A. The thickness of the first cured film H1 is, for example, at least twice the height AH. The thickness of the first cured film H1 is, for example, at least several dozen times the height AH.

[0190] The thickness of the first cured film H1 is not too large and is, for example, several hundred μm or less.

[0191] Figure 8 1 is an enlarged view schematically showing the substrate W in the first curing step. The first cured film H1 will be described in more detail. The first cured film H1 has a lower surface H1b. The lower surface H1b is in contact with the upper end A2 of the convex portion A. The first cured film H1 is formed above the pattern P in a state where the lower surface H1b is in contact with the upper end A2.

[0192] The entire lower surface H1b is located at a position higher than the bottom B1 of the recessed portion B. The lower surface H1b is separated from the bottom B1. The lower surface H1b is not in contact with the bottom B1.

[0193] For example, the lower surface H1b is convexly curved upward between adjacent convex portions A. For example, the lower surface H1b is convexly curved upward above the concave portion B. For example, a portion of the lower surface H1b between adjacent convex portions A is located at a position higher than the upper end A2. For example, a portion of the lower surface H1b above the concave portion B is located at a position higher than the upper end A2.

[0194] The first cured film H1 is solid. The first cured film H1 may also be called a “cured film.” The first cured film H1 may also be called a “polymer film.”

[0195] For example, the first cured film H1 does not substantially have elasticity. For example, the first cured film H1 does not substantially deform. Alternatively, the first cured film H1 may have elasticity.

[0196] The first cured film H1 has thermal decomposition properties.

[0197] The first cured film H1 has a thermal decomposition temperature Tp1. The thermal decomposition temperature Tp1 is higher than room temperature. The thermal decomposition temperature Tp1 is, for example, 100 degrees or higher. The thermal decomposition temperature Tp1 is, for example, 200 degrees or higher. The thermal decomposition temperature Tp1 is, for example, 400 degrees or higher. The thermal decomposition temperature Tp1 is, for example, 700 degrees or higher.

[0198] The first low temperature T1L is lower than the thermal decomposition temperature Tp1. That is, in the first curing step, the first drying auxiliary liquid F1 is heated at a temperature lower than the thermal decomposition temperature Tp1. Therefore, in the first curing step, the first cured film H1 is not thermally decomposed.

[0199] The heating temperature of the first drying auxiliary liquid F1 is one of the factors that determine the length of the polymer of the thermosetting material. As described above, the first low temperature T1L corresponds to the heating temperature of the first drying auxiliary liquid F1. Therefore, it is preferable to adjust the first low temperature T1L based on the width BW of the recess B. It is preferable that the first low temperature T1L changes based on the width BW of the recess B.

[0200] For example, the first low temperature T1L is adjusted so that the length of the polymer of the thermosetting material is larger than the width BW. For example, when the width BW is larger, the first low temperature T1L is adjusted so that the length of the polymer of the thermosetting material is larger.

[0201] Fig. 9 2 is an enlarged view schematically showing the substrate W in the first curing step. The solvent in the first drying auxiliary liquid F1 evaporates. The solvent evaporates from the first drying auxiliary liquid F1 on the substrate W.

[0202] The solvent evaporates easily. For example, the solvent evaporates at a temperature lower than the thermal decomposition temperature Tp1. For example, the solvent evaporates at the first low temperature T1L. For example, the solvent evaporates at room temperature. For example, the solvent may start evaporating after the first hardening step starts. Alternatively, the solvent may start evaporating before the first hardening step starts.

[0203] For example, the first low temperature T1L may be above the boiling point of the solvent. In this case, the solvent evaporates quickly. Alternatively, the first low temperature T1L may be below the boiling point of the solvent. In this case, the solvent also evaporates smoothly.

[0204] The boiling point of the solvent is, for example, higher than room temperature and lower than the thermal decomposition temperature Tp1.

[0205] As described above, the first drying auxiliary liquid F1 remaining in the recess B is substantially composed of a solvent. Therefore, as the solvent evaporates, the first drying auxiliary liquid F1 in the recess B decreases. The first drying auxiliary liquid F1 in the recess B is removed from the substrate W without becoming the first cured film H1. In other words, the unreacted portion of the first drying auxiliary liquid F1 is removed from the substrate W without becoming the first cured film H1.

[0206] The gas J in the housing 12 enters the recess B. The first drying auxiliary liquid F1 contacts the gas J in the recess B. The first drying auxiliary liquid F1 and the gas J form a gas-liquid interface K1. The gas-liquid interface K1 is located in the recess B. The gas-liquid interface K1 contacts the convex portion A. The gas-liquid interface K1 contacts the side A3 of the convex portion A. The capillary force of the first drying auxiliary liquid F1 acts on the convex portion A. However, the convex portion A is supported by the first cured film H1. Therefore, even if the capillary force acts on the convex portion A, the convex portion A will not collapse.

[0207] Fig.10 2 is an enlarged view schematically showing the substrate W in the first curing step. Finally, the solvent on the substrate W is completely evaporated. The solvent on the substrate W is completely removed from the substrate W.

[0208] Therefore, the first drying auxiliary liquid F1 in the recess B is completely removed from the substrate W. The unreacted portion of the first drying auxiliary liquid F1 is completely removed from the substrate W. As described above, the first drying auxiliary liquid F1 other than the unreacted portion becomes the first cured film H1. Therefore, the first drying auxiliary liquid F1 completely disappears from the substrate W.

[0209] The convex portion A is still supported by the first cured film H1. The first cured film H1 supports the convex portion A until all the unreacted portions of the first drying auxiliary liquid F1 are removed from the substrate W.

[0210] After all the unreacted portions of the first drying auxiliary liquid F1 are removed from the substrate W, no liquid exists on the substrate W. No liquid exists in the concave portion B. The convex portion A does not come into contact with the liquid.

[0211] Step S4: First thermal decomposition step

[0212] The first cured film H1 on the substrate W is heated to thermally decompose the first cured film H1 and the substrate W is dried.

[0213] The substrate holding portion 13 holds the substrate W. The heating portion 31 heats the substrate W held by the substrate holding portion 13. The rotation drive portion 17 does not rotate the substrate holding portion 13 and the substrate W.

[0214] Fig.111 is an enlarged view schematically showing the substrate W in the first thermal decomposition step. The substrate W is in a posture where the pattern P faces upward. The pattern P is located on the upper surface WS1 of the substrate W. The pattern P faces upward.

[0215] The first cured film H1 is heated via the substrate W held by the substrate holding unit 13 .

[0216] In the first thermal decomposition step, the first cured film H1 is heated at the first high temperature T1H. The first high temperature T1H is higher than the first low temperature T1L. The first high temperature T1H is higher than room temperature. The first high temperature T1H is higher than the boiling point of the solvent. The temperature of the first cured film H1 rises from the first low temperature T1L. The temperature of the first cured film H1 rises to the first high temperature T1H. The first high temperature T1H corresponds to the heating temperature of the first cured film H1.

[0217] The first high temperature T1H is higher than the thermal decomposition temperature Tp1. That is, the first cured film H1 is heated at a temperature higher than the thermal decomposition temperature Tp1. For example, the first high temperature T1H is higher than 100 degrees. For example, the first high temperature T1H is higher than 200 degrees. For example, the first high temperature T1H is higher than 400 degrees. For example, the first high temperature T1H is higher than 700 degrees.

[0218] The first cured film H1 is removed by thermally decomposing the first cured film H1. Specifically, the first cured film H1 is reduced and thinned.

[0219] The polymer of the thermosetting material in the first cured film H1 is thermally decomposed. The polymer of the thermosetting material is depolymerized. The molecular weight of the polymer of the thermosetting material is reduced.

[0220] For example, the first cured film H1 is vaporized. For example, a polymer of a thermosetting material is vaporized.

[0221] For example, the first cured film H1 is decomposed into a plurality of particles. For example, a polymer of a thermosetting material is decomposed into a plurality of particles. The plurality of particles are suspended from the substrate W. The suspended particles form smoke, for example.

[0222] For example, the first cured film H1 is removed from the substrate W without melting. For example, a polymer of a thermosetting material is removed from the substrate W without melting.

[0223] When the first cured film H1 is thermally decomposed, the first cured film H1 does not apply a significant force to the convex portion A. When the first cured film H1 is thermally decomposed, the force acting on the convex portion A is small.

[0224] Fig.12Schematically showing an enlarged view of the substrate W in the first thermal decomposition step. Finally, the first cured film H1 is completely removed from the substrate W. The upper surface WS1 of the substrate W is exposed to the gas J. The pattern P is completely exposed to the gas J. The convex portions A are completely exposed to the gas J. The concave portions B are completely filled with only the gas J. No liquid exists on the substrate W. The substrate W is dried.

[0225] <1-5. Technical significance of the substrate processing method according to the first embodiment>

[0226] The technical significance of the substrate processing method according to the first embodiment will be described through Example 1.

[0227] The conditions of Example 1 are described.

[0228] A substrate W having a pattern P formed thereon is prepared. The pattern P includes a plurality of convex portions A and a plurality of concave portions B. The width BW of the concave portion B is 10 nm.

[0229] In Example 1, a series of processes including the first processing liquid supplying step, the first coating step, the first curing step, and the first thermal decomposition step are performed on the substrate W.

[0230] In the first process liquid supplying step, the process liquid L is isopropyl alcohol.

[0231] In the first coating step, the first drying auxiliary liquid F1 is composed of THMR-ip5720 (manufactured by Tokyo Ohka Kogyo Co., Ltd.) and isopropyl alcohol. THMR-ip5720 corresponds to the thermosetting material, and isopropyl alcohol corresponds to the solvent.

[0232] In the first curing step, the substrate W and the first cured film H1 are heated at 100 degrees.

[0233] In the first thermal decomposition step, the substrate W and the first cured film H1 are heated at 700 degrees.

[0234] The substrate W processed in Example 1 was evaluated by the local collapse rates E1, E2, E3 and the average collapse rate EA.

[0235] The local collapse rates E1 to E3 and the average collapse rate EA are solved as follows. The local collapse rates Ei are collapse rates of local areas Mi. Here, i is any one of 1, 2, and 3. Each local area Mi is a tiny area of ​​the substrate W. For example, each local area Mi is magnified to 50,000 times using a scanning electron microscope. The observer observes the convex portions A of each local area Mi one by one. The observer divides each convex portion A into collapsed convex portions A and uncollapsed convex portions A. Here, the number of convex portions A observed in the local area Mi is recorded as NAi. The number of collapsed convex portions A in the local area Mi is recorded as NBi. The number NBi is less than the number NAi. The local collapse rate Ei is the ratio of the number NBi to the number NAi. The local collapse rate Ei is defined, for example, by the following formula.

[0236] Ei=NBi / NAi×100(%)

[0237] The average collapse rate EA is the average value of the local collapse rates E1 to E3.

[0238] The local collapse rate E1 of Example 1 is 0%. Similarly, the local collapse rates E2 and E3 of Example 1 are also 0%. The average collapse rate EA of Example 1 is 0%.

[0239] The following conclusions can be drawn from Example 1. In Example 1, each convex portion A was not collapsed. No collapsed convex portion A was generated. In Example 1, the collapse of the convex portion A was completely prevented. In Example 1, the substrate W was dried in a state where the pattern P was appropriately protected.

[0240] <1-6. Effects of the first embodiment>

[0241] The substrate processing method of the first embodiment is used to process a substrate W having a pattern P formed thereon. The pattern P includes a plurality of convex portions A and a plurality of concave portions B. The substrate processing method includes a first coating step and a first curing step. In the first coating step, a first drying auxiliary liquid F1 is coated on the substrate W. The first drying auxiliary liquid F1 includes a thermosetting material and a solvent. In the first curing step, the first drying auxiliary liquid F1 on the substrate W is heated. In the first curing step, a first cured film H1 is formed on the substrate W. Therefore, the first cured film H1 is appropriately formed on the substrate W.

[0242] In the first curing step, at least a portion of the first cured film H1 is formed above the pattern P. In the first curing step, the first cured film H1 is in contact with the upper end A2 of the convex portion A. Therefore, the first cured film H1 supports the convex portion A appropriately.

[0243] In the first curing step, the entire first cured film H1 is located above the bottom B1 of the recessed portion B. Therefore, a portion of the convex portion A does not contact the first cured film H1. Specifically, at least a portion of the side A3 of the convex portion A does not contact the first cured film H1. Therefore, in the first curing step, the convex portion A is not easily affected by the volume change of the first cured film H1. That is, in the first curing step, the volume change of the first cured film H1 has little effect on the convex portion A.

[0244] Specifically, even if the volume of the first cured film H1 changes, the force applied by the first cured film H1 to the side A3 is small. For example, even if the first cured film H1 expands, the first cured film H1 is not likely to press the side A3 with a significant force. Therefore, even if the first cured film H1 expands, the convex portion A is not likely to collapse. For example, even if the first cured film H1 shrinks, the first cured film H1 is not likely to pull the side A3 with a significant force. Therefore, even if the first cured film H1 shrinks, the convex portion A is not likely to collapse.

[0245] The substrate processing method includes a first thermal decomposition step. In the first thermal decomposition step, the first cured film H1 is thermally decomposed by heating the first cured film H1. In the first thermal decomposition step, the substrate W is dried. Therefore, the first cured film H1 is thermally decomposed appropriately. Furthermore, in the first thermal decomposition step, the convex portion A is not easily affected by the volume change of the first cured film H1. Therefore, the first cured film H1 can be appropriately removed from the substrate W. Therefore, when the substrate W is dried, the collapse of the convex portion A can be suppressed. That is, the substrate W can be dried in a state where the pattern P is protected.

[0246] As described above, according to the substrate processing method of the first embodiment, the substrate W can be processed appropriately.

[0247] The finer the pattern P of the substrate W, the smaller the width BW of the recess B. Even if the width BW is small, it is easy to make the first cured film H1 all located above the bottom B1 of the recess B in the first curing step. It can even be said that the smaller the width BW of the recess B, the easier it is to make the first cured film H1 all located above the bottom B1 of the recess B in the first curing step. Therefore, the finer the pattern P of the substrate W, the smaller the influence of the volume change of the first cured film H1 on the convex portion A. Therefore, the finer the pattern P of the substrate W, the easier it is to properly process the substrate W.

[0248] The width BW of the concave portion B is less than 10 nm. Therefore, in the first curing step, it is very easy to make the entire first cured film H1 located above the bottom B1 of the concave portion B. Therefore, the volume change of the first cured film H1 has very little effect on the convex portion A. Therefore, it is easier to properly process the substrate W.

[0249] In the first curing step, the first cured film H1 bridges the upper ends A2 of the projections A. Therefore, the first cured film H1 supports the projections A more appropriately.

[0250] In the first curing step, the first cured film H1 is entirely located at a position equal to or higher than the upper end A2 of the convex portion A. Therefore, the first cured film H1 is entirely located above the concave portion B. The first cured film H1 is entirely located at a position higher than the concave portion B. The first cured film H1 does not substantially have a portion located at the concave portion B. Therefore, the side edge A3 of the convex portion A is entirely separated from the first cured film H1. Therefore, the first cured film H1 does not substantially apply a force to the side edge A3. The convex portion A is substantially not affected by the volume change of the first cured film H1.

[0251] Even if the width BW of the recessed portion B is small, it is easy to make the first cured film H1 all located at the same position as or higher than the upper end A2 of the convex portion A in the first curing step. It can even be said that the smaller the width BW of the recessed portion B, the easier it is to make the first cured film H1 all located at the same position as or higher than the upper end A2 of the convex portion A in the first curing step. Therefore, the finer the pattern P of the substrate W is, the easier it is to properly process the substrate W.

[0252] In the first curing step, for example, the entire first cured film H1 is located above the recess B. Therefore, when the first thermal decomposition step is completed, no residue of the first cured film H1 remains in the recess B. Therefore, a clean substrate W can be obtained in the first thermal decomposition step.

[0253] In the first curing step, the first cured film H1 has a lower surface H1b. In the first curing step, the lower surface H1b contacts the upper end A2 of the convex portion A. In the first curing step, the lower surface H1b is convexly curved upward between adjacent convex portions A. Therefore, the shape of the lower surface H1b can appropriately block the first cured film H1 from entering the concave portion B. Therefore, the lower surface H1b appropriately separates the first cured film H1 from the side A3. Thus, the convex portion A is appropriately protected from the volume change of the first cured film H1. The convex portion A is substantially not affected by the volume change of the first cured film H1.

[0254] In the first curing step, the thermosetting material becomes a polymer. The first cured film H1 contains a polymer of the thermosetting material. The polymer of the thermosetting material has a length greater than the width BW of the recess B. The recess B is too narrow for the polymer of the thermosetting material. Therefore, it is not easy for the thermosetting material to become a polymer in the recess B. In this way, it is difficult to form the first cured film H1 in the recess B. Therefore, in the first curing step, it is easier to make the first cured film H1 all located above the bottom B1 of the recess B. The first cured film H1 is all appropriately located above the bottom BW of the recess B.

[0255] In the first curing step, the heating temperature of the first drying auxiliary liquid F1 is adjusted based on the width BW of the recess B. Therefore, in the first curing step, it is easier to position the entire first cured film H1 above the bottom B1 of the recess B regardless of the width BW of the recess B. Regardless of the width BW of the recess B, the entire first cured film H1 is appropriately positioned above the bottom B1 of the recess B.

[0256] In the first curing step, the first drying auxiliary liquid F1 is heated at the first low temperature T1L. The first low temperature T1L is lower than the first high temperature T1H. Therefore, in the first curing step, thermal decomposition of the first cured film H1 can be appropriately prevented. Therefore, in the first curing step, the first cured film H1 is appropriately formed. Therefore, in the first curing step, the first cured film H1 appropriately supports the protrusion A.

[0257] The first low temperature T1L is lower than the thermal decomposition temperature Tp1. Therefore, in the first curing step, the first cured film H1 is not thermally decomposed. Therefore, in the first curing step, the first cured film H1 appropriately supports the convex portion A. Therefore, in the first curing step, collapse of the convex portion A can be appropriately prevented.

[0258] In the first curing step, the solvent in the first drying auxiliary liquid F1 further evaporates. Therefore, when the first curing step is completed, no solvent exists on the substrate W. That is, in the first thermal decomposition step, no solvent exists on the substrate W. Therefore, in the first thermal decomposition step, the capillary force of the solvent does not act on the convex portion A. Therefore, in the first thermal decomposition step, it is easier to protect the convex portion A.

[0259] The solvent evaporates at a temperature lower than the thermal decomposition temperature Tp1. Therefore, before the first cured film H1 is thermally decomposed, the solvent on the substrate W is completely evaporated. Therefore, until the solvent on the substrate W is completely evaporated, the first cured film H1 always supports the protrusion A. Therefore, until the solvent on the substrate W is completely evaporated, the collapse of the protrusion A can be properly prevented.

[0260] The boiling point of the solvent is lower than the thermal decomposition temperature Tp1. Therefore, the solvent is appropriately evaporated at a temperature lower than the thermal decomposition temperature Tp1.

[0261] The first low temperature T1L is higher than the boiling point of the solvent. Therefore, in the first curing step, the solvent evaporates rapidly.

[0262] In the first curing step, the first drying auxiliary liquid F1 includes a non-reactive portion that does not become the first cured film H1. In the first curing step, the non-reactive portion of the first drying auxiliary liquid F1 is removed from the substrate W. Therefore, when the first curing step is completed, the first drying auxiliary liquid F1 does not exist on the substrate W. That is, in the first thermal decomposition step, the first drying auxiliary liquid F1 does not exist on the substrate W. Therefore, in the first thermal decomposition step, the capillary force of the first drying auxiliary liquid F1 does not act on the convex portion A. Therefore, in the first thermal decomposition step, it is easier to protect the convex portion A.

[0263] In the first thermal decomposition step, the first cured film H1 is heated at the first high temperature T1H. The first high temperature T1H is higher than the first low temperature T1L. Therefore, in the first thermal decomposition step, the first cured film H1 is appropriately thermally decomposed.

[0264] The first cured film H1 has thermal decomposition properties. Therefore, in the first thermal decomposition step, the first cured film H1 is thermally decomposed appropriately.

[0265] In the first thermal decomposition step, the first cured film H1 is heated at a temperature equal to or higher than the thermal decomposition temperature Tp1. Therefore, in the first thermal decomposition step, the first cured film H1 is thermally decomposed more appropriately.

[0266] In the first thermal decomposition step, the first cured film H1 is heated at a temperature of 700 degrees or higher. Therefore, it is easy to make the heating temperature of the first cured film H1 equal to or higher than the thermal decomposition temperature Tp1.

[0267] In the first thermal decomposition step, the first cured film H1 is thermally decomposed to remove the first cured film H1 from the substrate W. Therefore, after the first thermal decomposition step, no first cured film H1 remains on the substrate W. After the first thermal decomposition step, no residue of the first cured film H1 remains on the substrate W. Therefore, after the first thermal decomposition step, a clean substrate W can be obtained.

[0268] The first cured film H1 is vaporized in the first thermal decomposition step. Therefore, the first cured film H1 is appropriately removed from the substrate W in the first thermal decomposition step.

[0269] In the first thermal decomposition step, the first cured film H1 is decomposed into a plurality of particles. In the first thermal decomposition step, the particles are suspended from the substrate W. Therefore, the first cured film H1 is appropriately removed from the substrate W in the first thermal decomposition step.

[0270] In the first thermal decomposition step, the first cured film H1 is removed from the substrate W without melting. Therefore, when the first cured film H1 is thermally decomposed, the force acting on the protrusion A is smaller. Therefore, when the first cured film H1 is thermally decomposed, the protrusion A is also appropriately protected.

[0271] In the first curing step, the thermosetting material becomes a polymer. The first cured film H1 includes a polymer of the thermosetting material. Therefore, in the first curing step, the first cured film H1 is appropriately formed.

[0272] In the first thermal decomposition step, the polymer of the thermosetting material is thermally decomposed. In other words, in the first thermal decomposition step, the polymer of the thermosetting material is depolymerized. In the first thermal decomposition step, the molecular weight of the polymer of the thermosetting material is reduced. Therefore, in the first thermal decomposition step, the first cured film H1 is appropriately thermally decomposed.

[0273] The thickness of the first cured film H1 is not too large. For example, the thickness of the first cured film H1 is several hundred μm or less. Therefore, in the first thermal decomposition step, the first cured film H1 is rapidly thermally decomposed. The time of the first thermal decomposition step is appropriately shortened.

[0274] In the first coating step, the thickness of the first liquid film G1 is adjusted. In the first curing step, a part of the first liquid film G1 becomes the first cured film H1. Therefore, the thickness of the first cured film H1 is appropriately adjusted.

[0275] In the first coating step, the first drying auxiliary liquid F1 on the substrate W forms a first liquid film G1. The first liquid film G1 has a thickness much greater than the height AH of the convex portion A. The convex portion A is completely immersed in the first liquid film G1. Therefore, in the first coating step, the convex portion A does not contact the air-liquid interface. Therefore, in the first coating step, the capillary force of the first drying auxiliary liquid F1 does not act on the convex portion A. Therefore, in the first coating step, the convex portion A is also properly protected. In the first coating step, the collapse of the convex portion A can also be properly prevented.

[0276] The substrate processing method of the first embodiment further includes a first processing liquid supplying step. The first processing liquid supplying step is performed before the first coating step. In the first processing liquid supplying step, the processing liquid L is supplied to the substrate W. Therefore, the substrate W is processed more appropriately.

[0277] In the first coating step, the processing liquid L is removed from the substrate W. Therefore, in the first curing step and the first thermal decomposition step, the processing liquid L does not exist on the substrate W. Therefore, in the first curing step and the first thermal decomposition step, the convex portion A is more easily protected.

[0278] <Second embodiment>

[0279] The second embodiment will be described with reference to the drawings. Note that the same components as those of the first embodiment are denoted by the same reference numerals and detailed descriptions thereof will be omitted.

[0280] The second embodiment is substantially the same as the first embodiment in outline with respect to the substrate W and the substrate processing apparatus 1 .

[0281] <2-1. Configuration of the processing unit 11>

[0282] Fig.13 1 is a diagram showing the configuration of the processing unit 11 according to the second embodiment. In the second embodiment, the supply unit 21b supplies the second drying auxiliary liquid F2. In the second embodiment, the supply unit 21b does not supply the first drying auxiliary liquid F1. The second drying auxiliary liquid F2 is used to dry the substrate W. The second drying auxiliary liquid F2 has a function of assisting the drying of the substrate W. The second drying auxiliary liquid F2 is a liquid. The second drying auxiliary liquid F2 is a liquid at room temperature.

[0283] The second drying auxiliary liquid F2 contains an ultraviolet curable material. The ultraviolet curable material has ultraviolet curability. The ultraviolet curable material has not yet been cured by ultraviolet rays. The ultraviolet curable material has the property of polymerizing by ultraviolet rays. The ultraviolet curable material has the property of becoming a polymer by ultraviolet rays. The ultraviolet curable material has the property of curing by ultraviolet rays.

[0284] The ultraviolet curable material contains at least one of a monomer and an oligomer. At least one of the monomer and the oligomer in the ultraviolet curable material has the property of being polymerized by ultraviolet rays. The ultraviolet curable material does not contain a polymer. The ultraviolet curable material does not contain a high molecule. The ultraviolet curable material does not contain a high molecular compound.

[0285] The UV curable material is a liquid. The UV curable material is a liquid at room temperature.

[0286] The ultraviolet curable material is, for example, isobornyl acrylate. The ultraviolet curable material is, for example, isobornyl acrylate monomer.

[0287] The second drying auxiliary liquid F2 contains a polymerization initiator. The polymerization initiator may also be called a “photopolymerization initiator.” The polymerization initiator starts polymerization of the ultraviolet curable material.

[0288] The polymerization initiator is, for example, a solid. The polymerization initiator is, for example, a solid at room temperature. The polymerization initiator is, for example, a powder. The polymerization initiator in the second drying auxiliary liquid F2 is, for example, soluble in the ultraviolet curable material. The concentration of the polymerization initiator in the second drying auxiliary liquid F2 is, for example, 1 wt% or more. The concentration of the polymerization initiator in the second drying auxiliary liquid F2 is, for example, 10 wt% or less.

[0289] The polymerization initiator is, for example, 1-hydroxycyclohexyl phenyl ketone.

[0290] The second drying auxiliary liquid F2 does not contain a solvent. The solvent is, for example, at least one of an organic solvent and deionized water. As described above, the ultraviolet curable material is a liquid. Therefore, it is not necessary to dissolve the ultraviolet curable material in a solvent in order to generate the second drying auxiliary liquid F2. As described above, the polymerization initiator is soluble in the ultraviolet curable material. Therefore, it is not necessary to dissolve the polymerization initiator in a solvent in order to generate the second drying auxiliary liquid F2.

[0291] For example, the second drying auxiliary liquid F2 contains only the ultraviolet curable material and the polymerization initiator.

[0292] The nozzle 22b ejects the second drying auxiliary liquid F2. The valve 24b controls the ejection of the second drying auxiliary liquid F2. The supply source 25b delivers the second drying auxiliary liquid F2 to the supply portion 21b.

[0293] The second drying auxiliary liquid F2 is used inside the housing 12. Therefore, the second drying auxiliary liquid F2 is used under, for example, a normal pressure environment.

[0294] The processing unit 11 includes an irradiation unit 41. The irradiation unit 41 irradiates ultraviolet rays to the substrate W held by the substrate holding unit 13. Specifically, the irradiation unit 41 irradiates the upper surface WS1 of the substrate W held by the substrate holding unit 13 with ultraviolet rays.

[0295] Fig.13 The ultraviolet rays are schematically represented by a two-dot chain line. The irradiation unit 41 irradiates the ultraviolet rays downward. The irradiation area of ​​the irradiation unit 41 irradiates the ultraviolet rays is equal to or larger than the upper surface WS1 of the substrate W. The irradiation area of ​​the irradiation unit 41 irradiates the ultraviolet rays covers the entire upper surface WS1 of the substrate W. The entire upper surface WS1 of the substrate W receives the ultraviolet rays from the irradiation unit 41 at the same time.

[0296] The configuration example of the irradiation unit 41 will be described. The irradiation unit 41 includes a light emitting unit 42. The light emitting unit 42 is provided above the substrate holding unit 13. The light emitting unit 42 is provided above the substrate W held by the substrate holding unit 13. The light emitting unit 42 is provided inside the housing 12, for example.

[0297] For example, the light emitting unit 42 does not move in the horizontal direction relative to the substrate W held by the substrate holding unit 13 . For example, the light emitting unit 42 does not move in the vertical direction Z relative to the substrate W held by the substrate holding unit 13 . For example, the light emitting unit 42 is fixed to the housing 12 .

[0298] The light emitting unit 42 includes one or more light sources 43. The light source 43 generates ultraviolet rays. The light source 43 is, for example, a lamp. The lamp is, for example, a xenon lamp. The light source 43 is, for example, a light emitting diode (LED).

[0299] The light emitting unit 42 includes a cover 44. The cover 44 supports the light source 43. The cover 44 has a substantially box-like shape. The cover 44 accommodates the light source 43.

[0300] The light emitting portion 42 includes an exit surface 45. The exit surface 45 emits ultraviolet rays from the light source 43. The exit surface 45 emits ultraviolet rays downward. The exit surface 45 allows ultraviolet rays to pass through. The exit surface 45 is made of, for example, quartz glass. The exit surface 45 is, for example, arranged at the bottom of the cover portion 44. The exit surface 45 is arranged above the substrate W held by the substrate holding portion 13. The exit surface 45 extends in the horizontal direction. The exit surface 45 completely overlaps with the substrate W held by the substrate holding portion 13 when viewed from above.

[0301] The irradiation unit 41 includes a power supply 46. The power supply 46 is electrically connected to the light emitting unit 42 (specifically, the light source 43). The power supply 46 supplies power to the light emitting unit 42. The power supply 46 controls the light emitting unit 42. The power supply 46, for example, switches the light emitting unit 42 between irradiation and non-irradiation of ultraviolet rays. The power supply 46, for example, adjusts the intensity of ultraviolet rays. The power supply 46, for example, adjusts the irradiation time of ultraviolet rays.

[0302] The control unit 10 further controls the irradiation unit 41 , but the related illustration is omitted. The control unit 10 controls the power supply 46 .

[0303] <2-2. Example of operation of the processing unit 11>

[0304] Reference Fig.13 , 14 . Fig.14 1 is a flowchart showing the sequence of the substrate processing method of the second embodiment. The substrate processing method is used to process a substrate W having a pattern P formed thereon. The pattern P includes a plurality of convex portions A and a plurality of concave portions B. The substrate processing method includes steps S11 to S14. Steps S11 to S14 are performed in sequence. Steps S11 to S14 are performed by the processing unit 11.

[0305] Step S11: Second processing liquid supply step

[0306] The processing liquid L is supplied to the substrate W.

[0307] The operation of the second process liquid supplying step is substantially the same as the operation of the first process liquid supplying step of the first embodiment. The first process liquid supplying step is performed before the first coating step, and the second process liquid supplying step is performed before the second coating step.

[0308] Step S12: Second coating step

[0309] The substrate W is coated with the second drying auxiliary liquid F2.

[0310] The operation of the second coating step is similar to that of the first coating step. The second coating step is equivalent to the first coating step in which the first drying auxiliary liquid F1 is replaced with the second drying auxiliary liquid F2. For the sake of caution, the second coating step will be briefly described.

[0311] The substrate holding portion 13 holds the substrate W. The rotation driving portion 17 rotates the substrate holding portion 13 and the substrate W. The supply portion 21b supplies the second drying auxiliary liquid F2 to the substrate W held by the substrate holding portion 13. The heating portion 31 does not heat the substrate W. The irradiation portion 41 does not irradiate ultraviolet rays.

[0312] The second drying auxiliary liquid F2 is supplied to the upper surface WS1 of the substrate W. Since the substrate W is rotating, the second drying auxiliary liquid F2 is smoothly spread to the entire upper surface WS1. The second drying auxiliary liquid F2 is applied to the upper surface WS1. The upper surface WS1 is covered with the second drying auxiliary liquid F2. The second drying auxiliary liquid F2 removes the processing liquid L from the substrate W. The processing liquid L on the substrate W is replaced by the second drying auxiliary liquid F2.

[0313] In the second coating step, the interior of the housing 12 is maintained at room temperature, for example. In the second coating step, the substrate W is processed at room temperature, for example. The second drying auxiliary liquid F2 is coated on the substrate W at room temperature, for example.

[0314] Fig.15 Schematically showing a substrate W in the second coating step. The substrate W is in a posture with the pattern P facing upward. The pattern P is located on the upper surface WS1 of the substrate W. The pattern P faces upward. The substrate W is held by the substrate holding portion 13. When the substrate W is held by the substrate holding portion 13, the pattern P is located on the upper surface WS1 of the substrate W. When the substrate W is held by the substrate holding portion 13, the pattern P faces upward.

[0315] The second drying auxiliary liquid F2 is applied to the pattern P. The pattern P is covered with the second drying auxiliary liquid F2. The pattern P is in contact with the second drying auxiliary liquid F2. The convex portion A is in contact with the second drying auxiliary liquid F2.

[0316] The second drying auxiliary liquid F2 on the substrate W forms a second liquid film G2. The second liquid film G2 is located on the substrate W. The second liquid film G2 is located on the upper surface WS1. The second liquid film G2 covers the upper surface WS1. The second liquid film G2 covers the pattern P.

[0317] In the second coating step, the thickness of the second liquid film G2 may be further adjusted.

[0318] The thickness of the second liquid film G2 is, for example, much greater than the height AH of the convex portion A. The thickness of the second liquid film G2 is, for example, more than twice the height AH. The thickness of the second liquid film G2 is, for example, more than several dozen times the height AH. The thickness of the second liquid film G2 is, for example, more than several dozen μm.

[0319] The thickness of the second liquid film G2 is not too large. The thickness of the second liquid film G2 is, for example, several hundred μm or less.

[0320] The pattern P is entirely immersed in the second liquid film G2. The convex portion A is entirely immersed in the second liquid film G2.

[0321] The convex portion A does not contact the gas. The convex portion A does not contact the gas-liquid interface. Therefore, the capillary force does not act on the convex portion A. The capillary force is, for example, the surface tension of the first drying auxiliary liquid F1.

[0322] The concave portion B is filled with the second liquid film G2. The entire concave portion B is filled only with the second liquid film G2.

[0323] Step S13: Second hardening step

[0324] The second drying auxiliary liquid F2 on the substrate W is irradiated with ultraviolet rays, so that a second cured film is formed on the substrate W.

[0325] The substrate holding part 13 holds the substrate W. The irradiation part 41 irradiates the substrate W held by the substrate holding part 13 with ultraviolet rays. The rotation drive part 17 does not rotate the substrate holding part 13 and the substrate W. The heating part 31 does not heat the substrate W.

[0326] In the second curing step, the interior of the housing 12 is maintained at, for example, room temperature. Therefore, in the second curing step, the substrate W is processed at, for example, room temperature. The second cured film is formed at, for example, room temperature.

[0327] Fig.16 2 is a diagram schematically showing a substrate W in the second curing step. The substrate W is in a posture where the pattern P faces upward. The pattern P is located on the upper surface WS1 of the substrate W. The pattern P faces upward.

[0328] The upper surface WS1 of the substrate W is exposed to ultraviolet rays. The second drying auxiliary liquid F2 on the substrate W is exposed to ultraviolet rays. The polymerization initiator of the second drying auxiliary liquid F2 produces active species. The active species are, for example, free radicals. The active species cause the ultraviolet curing material of the second drying auxiliary liquid F2 to start a polymerization reaction. As the polymerization reaction of the ultraviolet curing material proceeds, the degree of polymerization of the ultraviolet curing material increases. The fluidity of the second drying auxiliary liquid F2 on the substrate W decreases. The second drying auxiliary liquid F2 on the substrate W hardens. The second drying auxiliary liquid F2 on the substrate W hardens.

[0329] After a while, the UV curable material becomes a polymer. The polymer of the UV curable material is equivalent to the cured product of the UV curable material. The polymer of the UV curable material is equivalent to a macromolecule. The polymer of the UV curable material is equivalent to a macromolecular compound.

[0330] The polymer of the ultraviolet curable material constitutes the second cured film H2. The second cured film H2 contains the polymer of the ultraviolet curable material.

[0331] In other words, due to the polymerization reaction of the ultraviolet curable material, part of the second drying auxiliary liquid F2 becomes the second cured film H2. Part of the second liquid film G2 becomes the second cured film H2. Therefore, the second drying auxiliary liquid F2 decreases. The second liquid film G2 becomes thinner.

[0332] The second cured film H2 is formed on the substrate W. The second cured film H2 is formed on the upper surface WS1. The second cured film H2 is formed on the pattern P.

[0333] The second cured film H2 covers the upper surface WS1. The second cured film H2 covers the pattern P.

[0334] Here, the polymer of the ultraviolet curable material has a length greater than the width BW of the recess B. The polymer of the ultraviolet curable material has a size greater than the size of the recess B. Therefore, the ultraviolet curable material cannot be polymerized in the recess B. However, the ultraviolet curable material can be polymerized at a position above the recess B. Therefore, the ultraviolet curable material located above the recess B becomes a polymer. The ultraviolet curable material located in the recess B does not become a polymer.

[0335] Therefore, at least a portion of the second cured film H2 is located above the recess B. In other words, at least a portion of the second cured film H2 is located above the pattern P. At least a portion of the second cured film H2 is located at a position equal to or higher than the upper end A2 of the convex portion A.

[0336] The entire second cured film H2 is located above the bottom B1 of the recess B. The entire second cured film H2 is located higher than the bottom B1. The second cured film H2 is separated from the bottom B1. The second cured film H2 is not in contact with the bottom B1. The second cured film H2 does not have a portion in contact with the bottom B1. At least a portion of the recess B is not filled with the second cured film H2. At least a portion of the recess B is a gap formed between the second cured film H2 and the bottom B2. The gap is located below the second cured film H2 and above the bottom B2.

[0337] The second cured film H2 does not contact at least a portion of each convex portion A. Specifically, the second cured film H2 does not contact at least a portion of each side A3. The second cured film H2 is separated from at least a portion of the side A3. Therefore, even if the volume of the second cured film H2 changes, it is difficult for the second cured film H2 to apply a significant force to the side A3.

[0338] For example, the second cured film H2 is entirely located above the recessed portion B. For example, the second cured film H2 does not have a portion located at the recessed portion B. For example, the second cured film H2 is entirely located at a position equal to or higher than the upper end A2 of the convex portion A. For example, the second cured film H2 is entirely located above the pattern P. For example, the second cured film H2 is entirely separated from the side A3 of the convex portion A. For example, the second cured film H2 does not have a portion in contact with the side A3. In this case, even if the volume of the second cured film H2 changes, the second cured film H2 does not apply a force to the side A3.

[0339] The second drying auxiliary liquid F2 includes a non-reactive portion in addition to the portion that will become the second cured film H2. The non-reactive portion of the second drying auxiliary liquid F2 remains on the substrate W and does not become the second cured film H2. The non-reactive portion of the second drying auxiliary liquid F2 is located in the concave portion B. The second drying auxiliary liquid F2 in the concave portion B corresponds to the non-reactive portion of the second drying auxiliary liquid F2.

[0340] The second drying auxiliary liquid F2 of the concave portion B contacts a part of the convex portion A. The second drying auxiliary liquid F2 of the concave portion B contacts at least a part of the side A3 of the convex portion A.

[0341] The second drying auxiliary liquid F2 in the recessed portion B contains an ultraviolet curable material. The non-reactive portion of the second drying auxiliary liquid F2 contains an ultraviolet curable material.

[0342] Furthermore, the second solidified film H2 is in contact with the upper end A2 of the convex portion A. The second solidified film H2 is connected to the upper end A2. The second solidified film H2 is connected to the upper end A2. The second solidified film H2 is, for example, in contact with the upper end A2. Therefore, the second solidified film H2 appropriately supports the convex portion A. The second solidified film H2 can appropriately prevent the collapse of the convex portion A. For example, the second solidified film H2 can prevent the upper end A2 from moving sideways. For example, the second solidified film H2 can prevent the convex portion A from tipping sideways.

[0343] The second cured film H2 bridges the upper ends A2. The second cured film H2 is equivalent to a bridge connecting the upper ends A2. Two or more upper ends A2 are connected to each other through the second cured film H2. Therefore, the second cured film H2 more appropriately supports the convex portion A. The second cured film H2 can more appropriately prevent the collapse of the convex portion A.

[0344] The second cured film H2 has a thickness. The thickness of the second cured film H2 is much greater than the height AH of the convex portion A. The thickness of the second cured film H2 is, for example, more than twice the height AH. The thickness of the second cured film H2 is, for example, more than several dozen times the height AH.

[0345] The thickness of the second cured film H2 is not too large and is, for example, several hundred μm or less.

[0346] Fig.17 2 is an enlarged view schematically showing the substrate W in the second curing step. The second cured film H2 will be described in more detail. The second cured film H2 has a lower surface H2b. The lower surface H2b is in contact with the upper end A2 of the convex portion A. The second cured film H2 is formed above the pattern P in a state where the lower surface H2b is in contact with the upper end A2.

[0347] The entire lower surface H2b is located at a position higher than the bottom B1 of the recessed portion B. The lower surface H2b is separated from the bottom B1. The lower surface H2b is not in contact with the bottom B1.

[0348] For example, the lower surface H2b is convexly curved upward between adjacent convex portions A. For example, the lower surface H2b is convexly curved upward above the concave portion B. For example, a portion of the lower surface H2b between adjacent convex portions A is located at a position higher than the upper end A2. For example, a portion of the lower surface H2b above the concave portion B is located at a position higher than the upper end A2.

[0349] The second cured film H2 is solid. The second cured film H2 is solid at room temperature. The second cured film H2 may also be referred to as a "cured film". The second cured film H2 may also be referred to as a "polymer film".

[0350] For example, the second cured film H2 does not substantially have elasticity. For example, the second cured film H2 does not substantially deform. Alternatively, the second cured film H2 may have elasticity.

[0351] The second cured film H2 has thermal decomposition properties.

[0352] The second cured film H2 has a thermal decomposition temperature Tp2. The thermal decomposition temperature Tp2 is higher than room temperature. The thermal decomposition temperature Tp2 is, for example, 100 degrees or higher. The thermal decomposition temperature Tp2 is, for example, 200 degrees or higher. The thermal decomposition temperature Tp2 is, for example, 400 degrees or higher. The thermal decomposition temperature Tp2 is, for example, 700 degrees or higher.

[0353] Furthermore, the second drying auxiliary liquid F2 does not substantially evaporate at room temperature. The ultraviolet curable material does not substantially evaporate at room temperature. The boiling point of the second drying auxiliary liquid F2 is, for example, higher than room temperature. The boiling point of the ultraviolet curable material is, for example, higher than room temperature.

[0354] Therefore, in the second curing step, the unreacted portion of the second drying auxiliary liquid F2 is not removed from the substrate W. When the second curing step is completed, the unreacted portion of the second drying auxiliary liquid F2 still remains on the substrate W. When the second curing step is completed, the unreacted portion of the second drying auxiliary liquid F2 still remains in the recess B.

[0355] Step S14: Second thermal decomposition step

[0356] The second cured film H2 on the substrate W is heated to thermally decompose the second cured film H2 and the substrate W is dried.

[0357] The substrate holding portion 13 holds the substrate W. The heating portion 31 heats the substrate W held by the substrate holding portion 13. The rotation drive portion 17 does not rotate the substrate holding portion 13 and the substrate W. The irradiation portion 41 does not irradiate ultraviolet rays.

[0358] Fig.18 1 is an enlarged view schematically showing the substrate W in the second thermal decomposition step. The substrate W is in a posture where the pattern P faces upward. The pattern P is located on the upper surface WS1 of the substrate W. The pattern P faces upward.

[0359] The second cured film H2 is heated via the substrate W held by the substrate holding unit 13 .

[0360] In the second thermal decomposition step, the second cured film H2 is heated at a second temperature T2. The second temperature T2 is higher than room temperature. For example, the temperature of the second cured film H2 rises from room temperature. The temperature of the second cured film H2 rises to the second temperature T2. The second temperature T2 corresponds to the heating temperature of the second cured film H2.

[0361] The second temperature T2 is higher than the thermal decomposition temperature Tp2. That is, the second cured film H2 is heated at a temperature higher than the thermal decomposition temperature Tp2. For example, the second temperature T2 is higher than 100 degrees. For example, the second temperature T2 is higher than 200 degrees. For example, the second temperature T2 is higher than 400 degrees. For example, the second temperature T2 is higher than 700 degrees.

[0362] The second temperature T2 is higher than the boiling point of the second drying auxiliary liquid F2. The second temperature T2 is higher than the boiling point of the ultraviolet curable material.

[0363] As described above, at the end of the second curing step, a portion of the second drying auxiliary liquid F2 remains on the substrate W. In the second thermal decomposition step, the second drying auxiliary liquid F2 remaining on the substrate W is also heated via the substrate W held by the substrate holding portion 13. In the second thermal decomposition step, the second drying auxiliary liquid F2 remaining on the substrate W evaporates. In other words, in the second thermal decomposition step, the non-reactive portion of the second drying auxiliary liquid F2 is heated. In the second thermal decomposition step, the non-reactive portion of the second drying auxiliary liquid F2 evaporates. Specifically, in the second thermal decomposition step, the second drying auxiliary liquid F2 in the recess B evaporates.

[0364] The second drying auxiliary liquid F2 evaporates at a temperature lower than the thermal decomposition temperature Tp2. The ultraviolet curable material evaporates at a temperature lower than the thermal decomposition temperature Tp2. For example, the boiling point of the second drying auxiliary liquid F2 is lower than the thermal decomposition temperature Tp2. For example, the boiling point of the ultraviolet curable material is lower than the thermal decomposition temperature Tp2.

[0365] Therefore, in the second thermal decomposition step, before the second cured film H2 is thermally decomposed, the second drying auxiliary liquid F2 remaining on the substrate W evaporates. In the second thermal decomposition step, before the second cured film H2 is thermally decomposed, the unreacted portion of the second drying auxiliary liquid F2 evaporates.

[0366] When the second drying auxiliary liquid F2 evaporates, the second cured film H2 does not substantially thermally decompose. When the second drying auxiliary liquid F2 evaporates, the second cured film H2 supports the protrusions A.

[0367] As the second drying auxiliary liquid F2 evaporates, the second drying auxiliary liquid F2 in the recess B decreases. The second drying auxiliary liquid F2 in the recess B is removed from the substrate W without becoming the second cured film H2. The unreacted portion of the second drying auxiliary liquid F2 is removed from the substrate W without becoming the second cured film H2.

[0368] The gas J in the housing 12 enters the recess B. The second drying auxiliary liquid F2 contacts the gas J in the recess B. The second drying auxiliary liquid F2 and the gas J form a gas-liquid interface K2. The gas-liquid interface K2 is located in the recess B. The gas-liquid interface K2 contacts the convex portion A. The gas-liquid interface K2 contacts the side A3 of the convex portion A. The capillary force of the second drying auxiliary liquid F2 acts on the convex portion A. However, the convex portion A is supported by the second cured film H2. Therefore, even if the capillary force acts on the convex portion A, the convex portion A will not collapse.

[0369] Fig.19 : is an enlarged view schematically showing the substrate W in the second thermal decomposition step. Finally, the second drying auxiliary liquid F2 in the recess B is completely evaporated. The second drying auxiliary liquid F2 in the recess B is completely removed from the substrate W. The unreacted portion of the second drying auxiliary liquid F2 is completely removed from the substrate W. As described above, the second drying auxiliary liquid F2 other than the unreacted portion becomes the second cured film H2. Therefore, the second drying auxiliary liquid F2 on the substrate W completely disappears from the substrate W.

[0370] The convex portion A is still supported by the second cured film H2. The second cured film H2 supports the convex portion A until all the unreacted portions of the second drying auxiliary liquid F2 are removed from the substrate W.

[0371] After all the unreacted portions of the second drying auxiliary liquid F2 are removed from the substrate W, no liquid exists on the substrate W. No liquid exists in the concave portion B. The convex portion A does not come into contact with the liquid.

[0372] Fig. 20 Schematically shows the substrate W in the second thermal decomposition step. After the unreacted portion of the second drying auxiliary liquid F2 is removed from the substrate W, the second cured film H2 is thermally decomposed. The second cured film H2 is removed by thermally decomposing the second cured film H2. Specifically, the second cured film H2 is reduced. The second cured film H2 becomes thinner.

[0373] The polymer of the ultraviolet curable material in the second cured film H2 is thermally decomposed. The polymer of the ultraviolet curable material is depolymerized. The molecular weight of the polymer of the ultraviolet curable material is reduced.

[0374] For example, the second cured film H2 is vaporized. For example, the polymer of the ultraviolet curable material is vaporized.

[0375] For example, the second cured film H2 is decomposed into a plurality of particles. For example, a polymer of an ultraviolet curable material is decomposed into a plurality of particles. The plurality of particles are suspended from the substrate W. The suspended particles form smoke, for example.

[0376] For example, the second cured film H2 is removed from the substrate W without melting. For example, a polymer of an ultraviolet curable material is removed from the substrate W without melting.

[0377] When the second cured film H2 is thermally decomposed, the second cured film H2 does not apply a significant force to the convex portion A. When the second cured film H2 is thermally decomposed, the force acting on the convex portion A is small.

[0378] Fig.21 Schematically shows the substrate W in the second thermal decomposition step. Finally, the second cured film H2 is completely removed from the substrate W. The upper surface WS1 of the substrate W is exposed to the gas J. The pattern P is completely exposed to the gas J. The convex portions A are completely exposed to the gas J. The concave portions B are completely filled with only the gas J. No liquid exists on the substrate W. The substrate W is dried.

[0379] <2-3. Technical significance of the substrate processing method according to the second embodiment>

[0380] The technical significance of the drying method according to the second embodiment will be described with reference to Example 2.

[0381] The conditions of Example 2 are described.

[0382] A substrate W having a pattern P formed thereon is prepared. The pattern P includes a plurality of convex portions A and a plurality of concave portions B. The width BW of the concave portion B is 10 nm.

[0383] In Example 2, a series of processes including a second processing liquid supplying step, a second coating step, a second curing step, and a second thermal decomposition step are performed on the substrate W.

[0384] In the second process liquid supplying step, the process liquid L is isopropyl alcohol.

[0385] In the second coating step, the second drying auxiliary liquid F2 contains only isobornyl acrylate monomer and 1-hydroxycyclohexyl phenyl ketone. The isobornyl acrylate monomer corresponds to the ultraviolet curable material. The 1-hydroxycyclohexyl phenyl ketone corresponds to the polymerization initiator.

[0386] In the second curing step, the ultraviolet light has a wavelength of 365 nm and a power of 342 mW / cm 2 The second drying auxiliary liquid F2 on the substrate W is irradiated with ultraviolet rays for 10 minutes.

[0387] In the second thermal decomposition step, the substrate W and the second cured film H2 are heated at 700 degrees C. The substrate W and the second cured film H2 are heated for 1 hour.

[0388] The substrate W processed in Example 2 was evaluated by the local collapse rates E1, E2, E3 and the average collapse rate EA.

[0389] The local collapse rates E1, E2, and E3 of Example 2 are 0%, 0%, and 12%, respectively. The average collapse rate EA of Example 2 is 4%.

[0390] The following conclusions were obtained from Example 2. In Example 2, almost all the convex portions A were not collapsed. In Example 2, the collapse of the convex portions A was sufficiently prevented. In Example 2, the substrate W was dried in a state where the pattern P was appropriately protected.

[0391] <2-4. Effects of the Second Embodiment>

[0392] The substrate processing method of the second embodiment is used to process a substrate W having a pattern P formed thereon. The pattern P includes a plurality of convex portions A and a plurality of concave portions B. The substrate processing method includes a second coating step and a second curing step. In the second coating step, a second drying auxiliary liquid F2 is coated on the substrate W. The second drying auxiliary liquid F2 includes an ultraviolet curable material. In the second curing step, ultraviolet rays are irradiated on the second drying auxiliary liquid F2 on the substrate W. In the second curing step, a second cured film H2 is formed on the substrate W. Therefore, the second cured film H2 is appropriately formed on the substrate W.

[0393] In the second curing step, at least a portion of the second cured film H2 is formed above the pattern P. In the second curing step, the second cured film H2 is in contact with the upper end A2 of the convex portion A. Therefore, the second cured film H2 supports the convex portion A appropriately.

[0394] In the second curing step, the entire second cured film H2 is located above the bottom B1 of the recessed portion B. Therefore, at least a portion of the convex portion A does not contact the second cured film H2. Specifically, at least a portion of the side A3 of the convex portion A does not contact the second cured film H2. Therefore, in the second curing step, the convex portion A is not easily affected by the volume change of the second cured film H2. That is, in the second curing step, the volume change of the second cured film H2 has little effect on the convex portion A.

[0395] Specifically, even if the volume of the second cured film H2 changes, the force applied by the second cured film H2 to the side A3 is small. For example, even if the second cured film H2 expands, the second cured film H2 is not likely to squeeze the side A3 with a significant force. Therefore, even if the second cured film H2 expands, the convex portion A is not likely to collapse. For example, even if the second cured film H2 shrinks, the second cured film H2 is not likely to pull the side A3 with a significant force. Therefore, even if the second cured film H2 shrinks, the convex portion A is not likely to collapse.

[0396] The substrate processing method includes a second thermal decomposition step. In the second thermal decomposition step, the second cured film H2 is thermally decomposed by heating the second cured film H2. In the second thermal decomposition step, the substrate W is dried. Therefore, the second cured film H2 is thermally decomposed appropriately. Furthermore, in the second thermal decomposition step, the convex portion A is not easily affected by the volume change of the second cured film H2. Therefore, the second cured film H2 is appropriately removed from the substrate W. Therefore, the collapse of the convex portion A can be suppressed, and the substrate W can be dried. That is, the substrate W is dried in a state where the pattern P is protected.

[0397] As described above, according to the substrate processing method of the second embodiment, the substrate W can be processed appropriately.

[0398] The finer the pattern P of the substrate W, the smaller the width BW of the recess B. Even if the width BW is small, it is easy to make the second cured film H2 all located above the bottom B1 of the recess B in the second curing step. It can even be said that the smaller the width BW of the recess B, the easier it is to make the second cured film H2 all located above the bottom B1 of the recess B in the second curing step. Therefore, the finer the pattern P of the substrate W, the smaller the influence of the volume change of the second cured film H2 on the convex part A. Therefore, the finer the pattern P of the substrate W, the easier it is to properly process the substrate W.

[0399] The width BW of the concave portion B is less than 10 nm. Therefore, in the second curing step, it is very easy to make the entire second cured film H2 located above the bottom B1 of the concave portion B. Therefore, the volume change of the second cured film H2 has very little effect on the convex portion A. Therefore, it is easier to properly process the substrate W.

[0400] In the second curing step, the second cured film H2 bridges the upper ends A2 of the projections A. Therefore, the second cured film H2 supports the projections A more appropriately.

[0401] In the second curing step, for example, the entire second cured film H2 is located at the same position as the upper end A2 of the convex portion A or at a position higher than the upper end A2 of the convex portion A. Therefore, the entire second cured film H2 is located above the concave portion B. The entire second cured film H2 is located at a position higher than the concave portion B. The second cured film H2 does not substantially have a portion located at the concave portion B. Therefore, the entire side A3 of the convex portion A is separated from the second cured film H2. Therefore, the second cured film H2 does not substantially apply a force to the side A3. The convex portion A is substantially not affected by the volume change of the second cured film H2.

[0402] Even if the width BW of the recessed portion B is small, it is easy to make the entire second cured film H2 be located at the same position as or higher than the upper end A2 of the convex portion A in the second curing step. It can even be said that the smaller the width BW of the recessed portion B is, the easier it is to make the entire second cured film H2 be located at the same position as or higher than the upper end A2 of the convex portion A in the second curing step. Therefore, the finer the pattern P of the substrate W is, the easier it is to properly process the substrate W.

[0403] In the second curing step, for example, the entire second cured film H2 is located above the recess B. Therefore, when the second thermal decomposition step is completed, no residue of the second cured film H2 remains in the recess B. Therefore, a clean substrate W can be obtained in the second thermal decomposition step.

[0404] In the second curing step, the second cured film H2 has a lower surface H2b. In the second curing step, the lower surface H2b contacts the upper end A2 of the convex portion A. In the second curing step, the lower surface H2b is convexly curved upward between adjacent convex portions A. Therefore, the shape of the lower surface H2b can appropriately prevent the second cured film H2 from entering the concave portion B. Therefore, the lower surface H2b appropriately separates the second cured film H2 from the side A3. Therefore, the convex portion A is appropriately protected from the volume change of the second cured film H2. The convex portion A is substantially not affected by the volume change of the second cured film H2.

[0405] In the second curing step, the ultraviolet curable material becomes a polymer. The second cured film H2 contains a polymer of the ultraviolet curable material. The polymer of the ultraviolet curable material has a length greater than the width BW of the recess B. The recess B is too narrow for the polymer of the ultraviolet curable material. Therefore, it is difficult for the ultraviolet curable material to become a polymer in the recess B. Therefore, it is difficult to form the second cured film H2 in the recess B. Therefore, in the second curing step, it is easier to make the second cured film H2 all located above the bottom B1 of the recess B. It is better that the second cured film H2 is all located above the bottom B1 of the recess B.

[0406] When the second curing step is finished, a part of the second drying auxiliary liquid F2 remains on the substrate W. In the second thermal decomposition step, the second drying auxiliary liquid F2 remaining on the substrate W is further evaporated. Therefore, in the second thermal decomposition step, the second drying auxiliary liquid F2 remaining on the substrate W is appropriately removed from the substrate W. Therefore, the substrate W is appropriately dried.

[0407] In the second thermal decomposition step, before the second cured film H2 is thermally decomposed, the second drying auxiliary liquid F2 remaining on the substrate W evaporates. In the second thermal decomposition step, the second drying auxiliary liquid F2 remaining on the substrate W evaporates, and then the second cured film H2 is thermally decomposed. In the second thermal decomposition step, the second cured film H2 is not substantially thermally decomposed until the second drying auxiliary liquid F2 remaining on the substrate W evaporates. Therefore, in the second thermal decomposition step, until the second drying auxiliary liquid F2 remaining on the substrate W evaporates, the second cured film H2 always supports the protrusion A. That is, in the second thermal decomposition step, the second cured film H2 appropriately protects the protrusion A from the second drying auxiliary liquid F2. Furthermore, when the second cured film H2 is thermally decomposed, the second drying auxiliary liquid F2 does not exist on the substrate W. Therefore, when the second cured film H2 is thermally decomposed, it is easier to protect the protrusion A. Therefore, the substrate W can be properly dried.

[0408] In the second curing step, the second drying auxiliary liquid F2 includes a non-reactive portion that does not become the second cured film H2. In the second thermal decomposition step, the non-reactive portion of the second drying auxiliary liquid F2 is removed from the substrate W. Therefore, in the second thermal decomposition step, the non-reactive portion of the second drying auxiliary liquid F2 can be appropriately removed from the substrate W. Therefore, the substrate W can be appropriately dried.

[0409] In the second thermal decomposition step, before the second cured film H2 is thermally decomposed, the non-reactive portion of the second drying auxiliary liquid F2 is removed from the substrate W. Therefore, in the second thermal decomposition step, until the non-reactive portion of the second drying auxiliary liquid F2 is removed from the substrate W, the second cured film H2 is not substantially thermally decomposed. Therefore, in the second thermal decomposition step, until the non-reactive portion of the second drying auxiliary liquid F2 is removed from the substrate W, the second cured film H2 always supports the protrusion A. That is, in the second thermal decomposition step, the second cured film H2 appropriately protects the protrusion A so that it does not contact the second drying auxiliary liquid F2. Furthermore, when the second cured film H2 is thermally decomposed, the second drying auxiliary liquid F2 does not exist on the substrate W. Therefore, when the second cured film H2 is thermally decomposed, it is easier to protect the protrusion A.

[0410] The second drying auxiliary liquid F2 evaporates at a temperature lower than the thermal decomposition temperature Tp2. Therefore, in the second thermal decomposition step, before the second cured film H2 is thermally decomposed, the second drying auxiliary liquid F2 remaining on the substrate W is appropriately evaporated. In the second thermal decomposition step, before the second cured film H2 is thermally decomposed, the unreacted portion of the second drying auxiliary liquid F2 is appropriately removed from the substrate W.

[0411] The boiling point of the second drying auxiliary liquid F2 is lower than the thermal decomposition temperature Tp2. Therefore, the second drying auxiliary liquid F2 is appropriately evaporated at a temperature lower than the thermal decomposition temperature Tp2.

[0412] The ultraviolet curable material evaporates at a temperature lower than the thermal decomposition temperature Tp2. Therefore, the second drying auxiliary liquid F2 evaporates appropriately at a temperature lower than the thermal decomposition temperature Tp2.

[0413] The boiling point of the ultraviolet curable material is lower than the thermal decomposition temperature Tp2. Therefore, the ultraviolet curable material is appropriately evaporated at a temperature lower than the thermal decomposition temperature Tp2.

[0414] The second cured film H2 has thermal decomposition properties. Therefore, in the second thermal decomposition step, the second cured film H2 is appropriately thermally decomposed.

[0415] In the second thermal decomposition step, the second cured film H2 is heated at a temperature equal to or higher than the thermal decomposition temperature Tp2. Therefore, in the second thermal decomposition step, the second cured film H2 is thermally decomposed more appropriately.

[0416] In the second thermal decomposition step, the second cured film H2 is heated at a temperature of 700 degrees or higher. Therefore, it is easy to make the heating temperature of the second cured film H2 equal to or higher than the thermal decomposition temperature Tp2.

[0417] In the second thermal decomposition step, the second cured film H2 is thermally decomposed to remove the second cured film H2 from the substrate W. Therefore, after the second thermal decomposition step, no second cured film H2 remains on the substrate W. After the second thermal decomposition step, no residue of the second cured film H2 remains on the substrate W. Therefore, after the second thermal decomposition step, a clean substrate W can be obtained.

[0418] In the second thermal decomposition step, the second cured film H2 is vaporized. Therefore, in the second thermal decomposition step, the second cured film H2 is appropriately removed from the substrate W.

[0419] In the second thermal decomposition step, the second cured film H2 is decomposed into a plurality of particles. In the second thermal decomposition step, the particles are suspended from the substrate W. Therefore, in the second thermal decomposition step, the second cured film H2 is removed from the substrate W appropriately.

[0420] In the second thermal decomposition step, the second cured film H2 is removed from the substrate W without melting. Therefore, when the second cured film H2 is thermally decomposed, the force acting on the protrusion A is smaller. Therefore, even when the second cured film H2 is thermally decomposed, the protrusion A is appropriately protected.

[0421] In the second curing step, the ultraviolet curable material becomes a polymer. The second cured film H2 contains the polymer of the ultraviolet curable material. Therefore, in the second curing step, the second cured film H2 is appropriately formed.

[0422] In the second thermal decomposition step, the polymer of the ultraviolet curable material is thermally decomposed. In other words, in the second thermal decomposition step, the polymer of the ultraviolet curable material is depolymerized. In the second thermal decomposition step, the molecular weight of the polymer of the ultraviolet curable material is reduced. Therefore, in the second thermal decomposition step, the second cured film H2 is appropriately thermally decomposed.

[0423] The ultraviolet curable material is a liquid. Therefore, the second drying auxiliary liquid F2 can be easily obtained from the ultraviolet curable material. For example, the second drying auxiliary liquid F2 can be obtained without using a solvent. For example, the second drying auxiliary liquid F2 can be obtained without using a solvent.

[0424] The ultraviolet curable material does not contain a polymer, so it is easy to obtain a liquid of the ultraviolet curable material.

[0425] The ultraviolet curable material is isobornyl acrylate. As described in Example 2, when the ultraviolet curable material is isobornyl acrylate, the pattern P is more appropriately protected. Therefore, the substrate W is more appropriately dried.

[0426] The ultraviolet curable material is isobornyl acrylate monomer, so the substrate W is dried more appropriately, and further, the liquid of the ultraviolet curable material is more easily obtained.

[0427] The second drying auxiliary liquid F2 does not contain a solvent. Therefore, in the second coating step, no solvent is applied to the substrate W. In the second hardening step and the second thermal decomposition step, no solvent exists on the substrate W. Therefore, in the second hardening step and the second thermal decomposition step, the capillary force of the solvent does not act on the convex portion A. That is, in the second hardening step and the second thermal decomposition step, the force acting on the convex portion A is further reduced. Therefore, in the second hardening step and the second thermal decomposition step, it is easier to protect the convex portion A.

[0428] The second drying auxiliary liquid F2 further contains a polymerization initiator. The polymerization initiator promotes the polymerization of the ultraviolet curable material. Therefore, in the second curing step, the second cured film H2 is quickly formed.

[0429] The thickness of the second cured film H2 is not too large. For example, the thickness of the second cured film H2 is less than several hundred μm. Therefore, in the second thermal decomposition step, the second cured film H2 can be thermally decomposed quickly, and the time of the second thermal decomposition step can be appropriately shortened.

[0430] In the second coating step, the thickness of the second liquid film G2 is adjusted. In the second curing step, a part of the second liquid film G2 becomes the second cured film H2. Therefore, the thickness of the second cured film H2 can be appropriately adjusted.

[0431] The irradiation area of ​​the irradiation unit 41 covers the entire substrate W. Therefore, the ultraviolet rays can be uniformly irradiated over the entire second drying auxiliary liquid F2 on the substrate W. Therefore, the second cured film H2 is uniformly formed over the entire substrate W. The second cured film H2 is uniformly formed over the entire upper surface WS1. Furthermore, the entire second drying auxiliary liquid F2 on the substrate W is simultaneously exposed to the ultraviolet rays. Therefore, in the second curing step, the second cured film H2 can be quickly formed. Therefore, the time of the second curing step can be appropriately shortened.

[0432] In the second coating step, the second drying auxiliary liquid F2 on the substrate W forms a second liquid film G2. The second liquid film G2 has a thickness much greater than the height AH of the convex portion A. The convex portion A is completely immersed in the second liquid film G2. Therefore, in the second coating step, the convex portion A does not contact the air-liquid interface. Therefore, in the second coating step, the capillary force of the second drying auxiliary liquid F2 does not act on the convex portion A. Therefore, in the second coating step, the convex portion A can also be properly protected. In the second coating step, the collapse of the convex portion A can also be properly prevented.

[0433] The substrate processing method of the second embodiment further includes a second processing liquid supplying step. The second processing liquid supplying step is performed before the second coating step. In the second processing liquid supplying step, the processing liquid L is supplied to the substrate W. Therefore, the substrate is processed more appropriately.

[0434] In the second coating step, the processing liquid L is removed from the substrate W. Therefore, in the second curing step and the second thermal decomposition step, the processing liquid L does not exist on the substrate W. Therefore, in the second curing step and the second thermal decomposition step, the protrusions A are more easily protected.

[0435] <3. Modified Embodiment>

[0436] The present invention is not limited to the first and second embodiments, and can be implemented in various modified forms as described below.

[0437] (1) In the first curing step of the first embodiment described above, the first cured film H1 is entirely located at a position equal to or higher than the upper end A2 of the convex portion A. In the first curing step, the first cured film H1 does not have a portion in contact with the side edge A3. However, the present invention is not limited thereto. For example, in the first curing step, the first cured film H1 may include a portion located lower than the upper end A2 of the convex portion A. In the first curing step, the first cured film H1 may also have a portion in contact with the side edge A3.

[0438] Similarly, in the second curing step of the second embodiment, the second cured film H2 is entirely located at the same position as the upper end A2 of the convex portion A or at a position higher than the upper end A2 of the convex portion A. In the second curing step, the second cured film H2 does not have a portion in contact with the side A3. However, this is not limited to this. For example, in the second curing step, the second cured film H2 may also include a portion located at a position lower than the upper end A2 of the convex portion A. In the second curing step, the second cured film H2 may also have a portion in contact with the side A3.

[0439] (2) In the first embodiment described above, the thermosetting material contained in the first drying auxiliary liquid F1 may be appropriately selected and changed according to the width BW of the recess B. For example, the substrate processing method may also include a first selection step of selecting a thermosetting material that will become a polymer having a length greater than the width BW of the recess B from among a plurality of thermosetting materials. In the first coating step, the first drying auxiliary liquid F1 includes the thermosetting material selected in the first selection step.

[0440] Similarly, in the second embodiment described above, the ultraviolet curable material contained in the second drying auxiliary liquid F2 may be appropriately selected and changed according to the width BW of the recess B. For example, the substrate processing method may also include a second selection step of selecting, from among a plurality of ultraviolet curable materials, an ultraviolet curable material that will become a polymer having a length greater than the width BW of the recess B. In the second coating step, the second drying auxiliary liquid F2 includes the ultraviolet curable material selected in the second selection step.

[0441] (3) In the first curing step of the first embodiment, the temperature rise curve of the first drying auxiliary liquid F1 may be appropriately selected and changed. For example, in the first curing step, the temperature of the first drying auxiliary liquid F1 rises continuously from room temperature to the first low temperature T1L. Alternatively, in the first curing step, the temperature of the first drying auxiliary liquid F1 rises stepwise from room temperature to the first low temperature T1L.

[0442] (4) In the first thermal decomposition step of the first embodiment, the temperature rise curve of the first cured film H1 may be appropriately selected and changed. For example, in the first thermal decomposition step, the temperature of the first cured film H1 rises continuously from the first low temperature T1L to the first high temperature T1H. Alternatively, in the first thermal decomposition step, the temperature of the first cured film H1 rises stepwise from the first low temperature T1L to the first high temperature T1H.

[0443] (5) In the second thermal decomposition step of the second embodiment described above, the temperature rise curve of the second cured film H2 may be appropriately selected and changed. Two modified embodiments will be described below.

[0444] (5-1) In the second thermal decomposition step, the temperature of the second cured film H2 is continuously increased from room temperature to the second temperature T2. According to this modified embodiment, it is easy to rapidly increase the temperature of the second cured film H2. Therefore, the second cured film H2 can be rapidly thermally decomposed. Therefore, the time of the second thermal decomposition step can be effectively shortened. Therefore, the substrate W can be processed efficiently.

[0445] (5-2) In the second thermal decomposition step, the temperature of the second cured film H2 is increased in stages.

[0446] Fig. 22 1 is a flowchart showing the sequence of the second thermal decomposition step of the modified embodiment. Specifically, the second thermal decomposition step includes a low-temperature heating step (step S21) and a high-temperature heating step (step S22). The low-temperature heating step is performed after the second curing step. As described above, at the end of the second curing step, a portion of the second drying auxiliary liquid F2 remains on the substrate W. The second drying auxiliary liquid F2 remaining on the substrate W corresponds to the unreacted portion of the second drying auxiliary liquid F2. The low-temperature heating step and the high-temperature heating step are described.

[0447] Step S21: Low temperature heating step

[0448] The unreacted portion of the second drying auxiliary liquid F2 on the substrate W is evaporated.

[0449] The heating unit 31 heats the substrate W held by the substrate holding unit 13. The non-reactive portion of the second drying auxiliary liquid F2 is heated via the substrate W. The non-reactive portion of the second drying auxiliary liquid F2 evaporates. The non-reactive portion of the second drying auxiliary liquid F2 is removed from the substrate W without becoming the second cured film H2.

[0450] In the low-temperature heating step, the non-reactive portion of the second drying auxiliary liquid F2 is heated at the second low temperature T2L. The second low temperature T2L is higher than room temperature. For example, the temperature of the non-reactive portion of the second drying auxiliary liquid F2 rises from room temperature. The temperature of the non-reactive portion of the second drying auxiliary liquid F2 rises to the second low temperature T2L. The second low temperature T2L corresponds to the heating temperature of the non-reactive portion of the second drying auxiliary liquid F2.

[0451] The second low temperature T2L is equal to or higher than the boiling point of the second drying auxiliary liquid F2. Therefore, in the low-temperature heating step, the unreacted portion of the second drying auxiliary liquid F2 can be appropriately removed from the substrate W.

[0452] The second low temperature T2L is equal to or higher than the boiling point of the ultraviolet curable material. Therefore, in the low temperature heating step, the unreacted portion of the second drying auxiliary liquid F2 can be removed from the substrate W more appropriately.

[0453] The second low temperature T2L is lower than the thermal decomposition temperature Tp2. Therefore, in the low temperature heating step, the thermal decomposition of the second cured film H2 can be appropriately prevented. Therefore, in the low temperature heating step, the second cured film H2 supports the convex portion A. Therefore, even if the capillary force acts on the convex portion A, the convex portion A will not collapse. That is, the convex portion A can be appropriately protected by the second cured film H2.

[0454] When the low temperature heating step is completed, all the unreacted parts of the second drying auxiliary liquid F2 are removed from the substrate W. When the low temperature heating step is completed, the second drying auxiliary liquid F2 disappears from the substrate W. When the low temperature heating step is completed, the second drying auxiliary liquid F2 does not exist on the substrate W.

[0455] In the low-temperature heating step, for example, the temperature of the second cured film H2 also rises from room temperature to the second low temperature T2L.

[0456] Step S22: High temperature heating step

[0457] The high temperature heating step is performed after the low temperature heating step. In the high temperature heating step, the second drying auxiliary liquid F2 does not exist on the substrate W. Therefore, it is easier to protect the protrusion A in the high temperature heating step.

[0458] In the high-temperature heating step, the second cured film H2 is thermally decomposed.

[0459] The heating unit 31 heats the substrate W held by the substrate holding unit 13. The second cured film H2 is heated via the substrate W. Therefore, the second cured film H2 is thermally decomposed.

[0460] In the high temperature heating step, the second cured film H2 is heated at the second high temperature T2H. The second high temperature T2H is higher than the second low temperature T2L. For example, the temperature of the second cured film H2 rises from the second low temperature T2L. The temperature of the second cured film H2 rises to the second high temperature T2H. The second high temperature T2H corresponds to the heating temperature of the second cured film H2.

[0461] The second high temperature T2H is higher than the thermal decomposition temperature Tp2. Therefore, in the high-temperature heating step, the second cured film H2 can be appropriately thermally decomposed.

[0462] (6) In the second embodiment, the irradiation area of ​​the irradiation unit 41 is larger than the upper surface WS1 of the substrate W. The irradiation unit 41 of the second embodiment does not move in the horizontal direction relative to the substrate W held by the substrate holding unit 13. The irradiation unit 41 of the second embodiment does not move in the vertical direction Z relative to the substrate W held by the substrate holding unit 13. However, this is not limited to this. For example, the irradiation area of ​​the irradiation unit 41 may be smaller than the upper surface WS1 of the substrate W. For example, the irradiation unit 41 may also move in the horizontal direction relative to the substrate W held by the substrate holding unit 13. For example, the irradiation unit 41 may also move in the vertical direction Z relative to the substrate W held by the substrate holding unit 13.

[0463] Fig.23 1 is a diagram showing the structure of the processing unit of the modified embodiment. In addition, the same symbols are marked for the same structures as the first and second embodiments, and detailed description is omitted. The irradiation unit 41 includes a light-emitting unit 52. The light-emitting unit 52 irradiates ultraviolet rays. The irradiation area of ​​the light-emitting unit 52 irradiating ultraviolet rays is smaller than the upper surface WS1 of the substrate W. The light-emitting unit 52 is smaller than the light-emitting unit 42 of the second embodiment. The light-emitting unit 52 is electrically connected to a power supply 46 not shown.

[0464] The irradiation unit 41 includes a moving mechanism 53. The moving mechanism 53 moves the light emitting unit 52. The moving mechanism 53 moves the light emitting unit 52 to, for example, a first position Q1, a second position Q2, and a third position Q3. The first position Q1 is located above the first side portion of the substrate W held by the substrate holding unit 13 in a side view. The second position Q2 is located above the second side portion of the substrate W held by the substrate holding unit 13 in a side view. The second position Q2 is at the same height as the first position Q1. The third position Q3 is higher than the first position Q1 and the second position Q2.

[0465] The moving mechanism 53 includes, for example, a horizontal moving mechanism 54 and a vertical moving mechanism 55. The horizontal moving mechanism 54 supports the light emitting unit 52. The horizontal moving mechanism 54 moves the light emitting unit 52 in the horizontal direction. The vertical moving mechanism 55 supports the horizontal moving mechanism 54. The vertical moving mechanism 55 moves the horizontal moving mechanism 54 in the vertical direction Z.

[0466] An example of the movement of the light emitting unit 52 is described. In the second processing liquid supply step and the second coating step, the light emitting unit 52 is located at the third position Q3. Therefore, when the nozzles 22a and 22b move to the processing position, the nozzles 22a and 22b do not interfere with the light emitting unit 52. In the second curing step, the light emitting unit 52 moves from the third position Q3 to the first position Q1. Then, the light emitting unit 52 irradiates ultraviolet rays while the light emitting unit 52 moves from the first position Q1 to the second position Q2. The irradiation area of ​​the ultraviolet rays moves on the substrate W. As a result, the ultraviolet rays are irradiated to the entire upper surface WS1 of the substrate W. The ultraviolet rays are irradiated to the entire second drying auxiliary liquid F2 on the substrate W.

[0467] According to the present modified embodiment, the light emitting unit 52 is relatively small, so it is easy to miniaturize the processing unit 11.

[0468] (7) In the first embodiment, the heating unit 31 heats the first drying auxiliary liquid F1 via the substrate W. However, the present invention is not limited thereto. For example, the heating unit 31 may directly heat the first drying auxiliary liquid F1. For example, the heating unit 31 may transfer heat to the first drying auxiliary liquid F1 without passing through the substrate W.

[0469] In the first embodiment, the heating unit 31 heats the first cured film H1 via the substrate W. However, the present invention is not limited thereto. For example, the heating unit 31 may directly heat the first cured film H1. For example, the heating unit 31 may transfer heat to the first cured film H1 without passing through the substrate W.

[0470] In the second embodiment, the heating unit 31 heats the second cured film H2 via the substrate W. However, the present invention is not limited thereto. For example, the heating unit 31 may directly heat the second cured film H2. For example, the heating unit 31 may transfer heat to the second cured film H2 without passing through the substrate W.

[0471] (8) In the first and second embodiments, the heating unit 31 is opposite to the lower surface WS2 of the substrate W. However, the present invention is not limited thereto. The heating unit 31 may be opposite to the upper surface WS1 of the substrate W. According to this modified embodiment, the heating unit 31 directly heats at least one of the first drying auxiliary liquid F1, the second drying auxiliary liquid F2, the first cured film H1, and the second cured film H2. The heating unit 31 transfers heat to at least one of the first drying auxiliary liquid F1, the second drying auxiliary liquid F2, the first cured film H1, and the second cured film H2 without passing through the substrate W.

[0472] (9) In the first embodiment, the first coating step, the first hardening step, and the first thermal decomposition step are performed by the same processing unit 11. However, this is not limiting. For example, the processing unit that performs the first coating step may be different from the processing unit that performs the first hardening step. For example, the processing unit that performs the first coating step may be different from the processing unit that performs the first thermal decomposition step. For example, the processing unit that performs the first hardening step may be different from the processing unit that performs the first thermal decomposition step. For example, two processing units may be used to perform one first thermal decomposition step.

[0473] The second embodiment can also be modified in the same manner.

[0474] Fig.24 It is a left side view showing the structure of the left part of the substrate processing apparatus 1 according to the modified embodiment. Note that the same reference numerals are given to the same structures as those in the first and second embodiments, and detailed description thereof will be omitted.

[0475] The processing block 7 includes processing units 11 a , 11 b , 11 c , and 11 d .

[0476] The processing unit 11 a includes a substrate holding portion 13 , a rotation driving portion 17 , and supply portions 21 a and 21 b .

[0477] The processing unit 11 b includes a substrate holding portion 13 and an irradiation portion 41 .

[0478] The processing unit 11c includes a heating section 61. The heating section 61 heats the substrate W. The heating section 61 includes a heating plate 62 and a heater 63. The heating plate 62 extends in the horizontal direction. The heating plate 62 has a size substantially the same as that of the substrate W in a plan view. The substrate W is placed on the heating plate 62. The heating plate 62 supports the substrate W so that it is in a horizontal position. The heater 63 is mounted on the heating plate 62. The heater 63 heats the substrate W on the heating plate 62.

[0479] The processing unit 11d includes a substrate container 71, a substrate support portion 72, and a heating portion 73. The substrate W is stored in the substrate container 71. The substrate container 71 has, for example, a cylindrical shape. The substrate container 71 has, for example, a tubular shape. The substrate container 71 allows infrared rays to pass through. The substrate container 71 is made of, for example, quartz glass. The substrate support portion 72 is provided in the substrate container 71. The substrate support portion 72 is supported by, for example, the substrate container 71. The substrate support portion 72 supports the substrate W so that it is in a horizontal position. The heating portion 73 is provided outside the substrate container 71. The heating portion 73 is arranged around the substrate container 71. The heating portion 73 irradiates, for example, infrared rays. The infrared rays pass through the substrate container 71. The heating portion 73 irradiates, for example, the entire substrate W with infrared rays. The heating portion 73 irradiates, for example, infrared rays to at least one of the first drying liquid F1 and the second drying auxiliary liquid F2 on the substrate W. The heating unit 73 irradiates, for example, infrared rays to at least one of the first cured film H1 and the second cured film H2 on the substrate W. The heating unit 73 is, for example, a lamp heater.

[0480] The conveying mechanism 8 is configured to be accessible to the processing units 11a, 11b, 11c, and 11d, but is not shown in the drawings.

[0481] When the substrate processing method according to the first embodiment is performed, the substrate processing apparatus 1 operates as follows.

[0482] First, the transport mechanism 8 transports the substrate W to the processing unit 11a. The transport mechanism 8 delivers the substrate W to the substrate holding portion 13 of the processing unit 11a. The processing unit 11a performs the first processing liquid supply step and the second coating step on the substrate W. The supply unit 21a supplies the processing liquid L to the substrate W. Thereafter, the supply unit 21b coats the substrate W with the first drying auxiliary liquid F1.

[0483] Next, the transport mechanism 8 transports the substrate W from the processing unit 11a to the processing unit 11c. The transport mechanism 8 picks up the substrate W from the substrate holding portion 13 of the processing unit 11a. The transport mechanism 8 places the substrate W on the heating plate 62 of the processing unit 11c. The processing unit 11b performs the first curing step on the substrate W. The heating unit 61 (specifically, the heater 63) heats the first drying auxiliary liquid F1 on the substrate W. A first cured film H1 is formed on the substrate W.

[0484] Next, the transport mechanism 8 transports the substrate W from the processing unit 11c to the processing unit 11d. The transport mechanism 8 picks up the substrate W from the heating plate 62 of the processing unit 11c. The transport mechanism 8 delivers the substrate W to the substrate support portion 72 of the processing unit 11d. The processing unit 11d performs the first thermal decomposition step on the substrate W. The heating portion 73 heats the first cured film H1 on the substrate W. The first cured film H1 is thermally decomposed. The substrate W is dried.

[0485] When the substrate processing method according to the second embodiment is performed, the substrate processing apparatus 1 operates as follows.

[0486] First, the transport mechanism 8 transports the substrate W to the processing unit 11a. The processing unit 11a performs the second processing liquid supply step and the second coating step on the substrate W. The supply unit 21a supplies the processing liquid L to the substrate W. Thereafter, the supply unit 21b coats the substrate W with the second drying auxiliary liquid F2.

[0487] Next, the transport mechanism 8 transports the substrate W from the processing unit 11a to the processing unit 11b. The transport mechanism 8 picks up the substrate W from the substrate holding portion 13 of the processing unit 11a. The transport mechanism 8 delivers the substrate W to the substrate holding portion 13 of the processing unit 11b. The processing unit 11b performs a second curing step on the substrate W. The irradiation unit 41 irradiates the second drying auxiliary liquid F2 on the substrate W with ultraviolet rays. A second cured film H2 is formed on the substrate W.

[0488] Next, the transport mechanism 8 transports the substrate W from the processing unit 11b to the processing unit 11c. The transport mechanism 8 picks up the substrate W from the substrate holding portion 13 of the processing unit 11b. The transport mechanism 8 places the substrate W on the heating plate 62 of the processing unit 11c. The processing unit 11c performs a second thermal decomposition step on the substrate W. For example, the processing unit 11c performs a low-temperature heating step. The heating unit 61 (specifically, the heater 63) heats the substrate W at the second low temperature T2L. The unreacted portion of the second drying auxiliary liquid F2 is removed from the substrate W.

[0489] Next, the transport mechanism 8 transports the substrate W from the processing unit 11c to the processing unit 11d. The transport mechanism 8 picks up the substrate W from the heating plate 62 of the processing unit 11c. The transport mechanism 8 delivers the substrate W to the substrate support portion 72 of the processing unit 11d. The processing unit 11d performs a second thermal decomposition step on the substrate W. For example, the processing unit 11d performs a high-temperature heating step on the substrate W. The heating portion 73 heats the second cured film H2 on the substrate W at the second high temperature T2H. The second cured film H2 is thermally decomposed. The substrate W is dried.

[0490] (10) In the first curing step of the first embodiment, the substrate W is not rotated. However, the present invention is not limited thereto. The substrate W may be rotated in the first curing step. In the first curing step, the first drying auxiliary liquid F1 on the substrate W may be heated while the substrate W is rotated.

[0491] In the second curing step of the second embodiment, the substrate W is not rotated. However, the present invention is not limited thereto. In the second curing step, the substrate W may be rotated. In the second curing step, the second drying auxiliary liquid F2 on the substrate W may be irradiated with ultraviolet rays while the substrate W is rotated.

[0492] (11) In the first thermal decomposition step of the first embodiment, the substrate W is not rotated. However, the present invention is not limited thereto. The substrate W may be rotated in the first thermal decomposition step. In the first thermal decomposition step, the first cured film H1 on the substrate W may be thermally decomposed while the substrate W is rotated.

[0493] In the second thermal decomposition step of the second embodiment, the substrate W is not rotated. However, the present invention is not limited thereto. In the second thermal decomposition step, the substrate W may be rotated. In the second thermal decomposition step, the second cured film H2 on the substrate W may be thermally decomposed while the substrate W is rotated.

[0494] (12) In the first and second embodiments, the example of the processing liquid L is described. However, the present invention is not limited to this. For example, the processing liquid L may be a chemical liquid. For example, the processing liquid L may be an etching liquid.

[0495] (13) In the first processing liquid supplying step of the first embodiment, one processing liquid L is supplied to the substrate W. However, the present invention is not limited thereto. In the first processing liquid supplying step, a plurality of processing liquids may be supplied to the substrate W. For example, in the first processing liquid supplying step, the first processing liquid may be supplied to the substrate W, and then the second processing liquid may be supplied to the substrate W. Here, the composition of the second processing liquid is different from that of the first processing liquid.

[0496] The second processing liquid supplying step in the second embodiment can also be changed in the same manner.

[0497] (14) The substrate processing method of the first embodiment includes the first processing liquid supplying step. However, the present invention is not limited thereto. For example, the first processing liquid supplying step may be omitted. For example, the first processing liquid supplying step may not be performed before the first coating step.

[0498] The substrate processing method of the second embodiment includes a second processing liquid supplying step. However, the present invention is not limited thereto. For example, the second processing liquid supplying step may be omitted. For example, the second processing liquid supplying step may not be performed before the second coating step.

[0499] (15) In the first embodiment, when the first coating step is performed, liquid (e.g., processing liquid L) is present on the substrate W. That is, in the first coating step, the first drying auxiliary liquid F1 is coated on the substrate W in a wet state. However, the present invention is not limited thereto. For example, when the first coating step is performed, liquid (e.g., processing liquid L) is not present on the substrate W. For example, in the first coating step, the first drying auxiliary liquid F1 is coated on the substrate W in a dry state.

[0500] The second coating step in the second embodiment can also be changed in the same manner.

[0501] (16) In the first and second embodiments, the pattern P on the substrate W may be formed on the substrate W before executing the substrate processing method. Alternatively, the pattern P may be formed on the substrate W in at least one of the first processing liquid supplying step and the second processing liquid supplying step.

[0502] (17) The embodiments and the modified embodiments described in (1) to (16) above may be appropriately modified by replacing each structure with the structure of another modified embodiment or combining them.

[0503] Description of Reference Numerals

[0504] 1: Substrate processing equipment

[0505] 10: Control Department

[0506] 11,11a,11b,11c,11d: Processing unit

[0507] 13: Substrate holding part

[0508] 21a: Supply unit (processing liquid supply unit)

[0509] 21b: Supply unit (drying auxiliary liquid supply unit)

[0510] 31,61,73: Heating unit

[0511] 41: Irradiation Department

[0512] F1: 1st drying auxiliary liquid

[0513] F2: Second drying auxiliary liquid

[0514] G1: 1st liquid film

[0515] G2: Second liquid film

[0516] H1: 1st cured film

[0517] H1b: Lower surface of the first cured film

[0518] H2: Second cured film

[0519] H2b: Lower surface of the second cured film

[0520] L: Treatment liquid

[0521] W: substrate

[0522] WS: Surface of substrate

[0523] WS1: upper surface of substrate

[0524] P: Pattern

[0525] A: convex part

[0526] A2: Top of the convex part (upper end of the convex part)

[0527] A3: The side of the convex part

[0528] AH: height of convex part

[0529] B: concave part

[0530] B1: Bottom of the recess

[0531] BW: Width of the concave part

[0532] T1L: 1st low temperature

[0533] T1H: 1st high temperature

[0534] T2: Second temperature

[0535] T2L: 2nd Low Temperature

[0536] T2H: Second highest temperature

Claims

1. A substrate processing method for processing a substrate having a pattern including a plurality of convex portions and a plurality of concave portions, wherein: Include: A first coating step of coating the substrate with a first drying auxiliary liquid comprising a thermosetting material and a solvent; a first curing step of heating the first drying auxiliary liquid on the substrate to form a first cured film on the substrate; and a first thermal decomposition step of thermally decomposing the first cured film by heating the first cured film to dry the substrate; In the first hardening step, At least a portion of the first cured film is formed above the pattern, The first cured film is in contact with the upper end of the protrusion, The first cured film is entirely located above the bottom of the recessed portion.

2. The substrate processing method according to claim 1, wherein: In the first curing step, the first cured film bridges the upper ends of the protrusions.

3. The substrate processing method according to claim 1 or 2, wherein: In the first curing step, the entire first cured film is located at a position equal to or higher than the upper end of the convex portion.

4. The substrate processing method according to claim 1 or 2, wherein: In the first hardening step, The first cured film has a lower surface, The lower surface of the first cured film is in contact with the upper ends of the projections and is curved convexly upward between the projections adjacent to each other.

5. The substrate processing method according to claim 1 or 2, wherein: In the first curing step, the thermosetting material becomes a polymer. The first cured film includes the polymer. The polymer has a length greater than a width of the recessed portion.

6. The substrate processing method according to claim 1 or 2, wherein: In the first curing step, a heating temperature of the first drying auxiliary liquid is adjusted based on the width of the recess.

7. The substrate processing method according to claim 1 or 2, wherein: In the first curing step, the first drying auxiliary liquid is heated at a first low temperature. In the first thermal decomposition step, the first cured film is heated at a first high temperature higher than the first low temperature.

8. The substrate processing method according to claim 1 or 2, wherein: In the first curing step, the solvent in the first drying auxiliary liquid is evaporated.

9. A substrate processing method for processing a substrate having a pattern including a plurality of convex portions and a plurality of concave portions, wherein: Include: A second coating step of coating the substrate with a second drying auxiliary liquid containing an ultraviolet curable material; a second curing step of irradiating the second drying auxiliary liquid on the substrate with ultraviolet rays to form a second cured film on the substrate; and a second thermal decomposition step of thermally decomposing the second cured film by heating the second cured film to dry the substrate; In the second hardening step, At least a portion of the second cured film is formed above the pattern, The second cured film is in contact with the upper end of the protrusion, and The second cured film is entirely located above the bottom of the recessed portion.

10. The substrate processing method according to claim 9, wherein: In the second curing step, the second cured film bridges the upper ends of the protrusions.

11. The substrate processing method according to claim 9 or 10, wherein: In the second curing step, all of the second cured film is located at a position equal to or higher than the upper end of the convex portion.

12. The substrate processing method according to claim 9 or 10, wherein: In the second hardening step, The second cured film has a lower surface, The lower surface of the second cured film is in contact with the upper ends of the projections and is curved convexly upward between the projections adjacent to each other.

13. The substrate processing method according to claim 9 or 10, wherein: In the second curing step, the ultraviolet curable material becomes a polymer. The second cured film includes the polymer. The polymer has a length greater than a width of the recessed portion.

14. The substrate processing method according to claim 9 or 10, wherein: When the second curing step is completed, a portion of the second drying auxiliary liquid remains on the substrate. In the second thermal decomposition step, the second drying auxiliary liquid remaining on the substrate is also evaporated.

15. The substrate processing method according to claim 14, wherein: In the second thermal decomposition step, the second drying auxiliary liquid remaining on the substrate is evaporated before the second cured film is thermally decomposed.