Polymer film-forming composition and selective polymer film-forming method
By using a polymer film composition of free radical generator and addition reactive compounds in semiconductor device manufacturing, the accuracy problem of resist masking method in lithography technology is solved, and selective masking of different regions on the substrate surface is achieved and The curability of polymer films is suitable for regionally selective film making by atomic layer deposition method, which improves the fineness of semiconductor devices and the accuracy of mask patterns.
Patent Information
- Application Number
- CN202380030289.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-29
- Publication Date
- 2024-11-12
AI Technical Summary
In semiconductor device manufacturing, the resist masking method using lithography technology has problems with many steps and accuracy, making it difficult to achieve efficient control of the horizontal film thickness of atomic layer and regional selective film formation.
Using a polymer film forming composition containing a free radical generator and a free radical addition reactive compound, a polymer film is formed by heating, and an unnecessary region is removed with a solvent to achieve selective masking of different material areas on the substrate surface. .
The polymer film is selectively formed according to the material on the substrate surface, which improves the curability and regional control of the film, and is suitable for the atomic layer deposition method, which improves the fineness and mask pattern of semiconductor devices. accuracy.
Smart Images

Figure CN118946956A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polymer film-forming composition, for example, a polymer film-forming composition useful in semiconductor integrated circuit manufacturing and capable of selectively forming a film depending on the material of a substrate surface, and further relates to a selective polymer film-forming method using the polymer film-forming composition. Background Art
[0002] In recent years, the trend toward high integration and miniaturization of semiconductor devices has intensified, and the miniaturization of organic patterns of masks used in device manufacturing and inorganic patterns produced by subsequent etching processes has progressed, and this has led to a demand for film thickness control at the atomic layer level.
[0003] As a method for forming a thin film at the atomic layer level on a substrate, the atomic layer deposition method (ALD (Atomic Layer Deposition) method, also known as atomic layer epitaxy method) is known. The ALD method is considered to be a type of general CVD (Chemical Vapor Deposition) method, but it is known to have both high height difference coverage and film thickness controllability compared to the CVD method.
[0004] The ALD method is a thin film forming technology that alternately supplies two gases containing elements constituting the film to be formed as main components onto a substrate to form a thin film on the substrate in atomic layer units, and repeats this operation multiple times to form a film of a desired thickness.
[0005] The ALD method utilizes a self-control function (self-limiting function) of deposition in which only one or a few layers of components of the raw material gas are adsorbed on the substrate surface during the supply of the raw material gas and the excess raw material gas does not contribute to the deposition.
[0006] For example, when forming an Al2O3 film on a substrate, a raw material gas composed of TMA (trimethylaluminum) and an oxidizing gas containing oxygen atoms (O) are used. In addition, when forming a nitride film on a substrate, a nitriding gas is used instead of an oxidizing gas.
[0007] In recent years, a method of selectively depositing a layer on a substrate surface by using the ALD method, that is, performing area-selective film formation has been proposed (for example, Patent Document 1).
[0008] Furthermore, in order to be suitable for a regioselective film-forming method on a substrate using an ALD method, a method of regioselectively modifying a substrate surface has been proposed (eg, Patent Document 2).
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent No. 4043785
[0012] Patent Document 2: Japanese Patent Application Publication No. 2019-121777 Summary of the invention
[0013] Problems to be solved by the invention
[0014] As described above, with the recent miniaturization of semiconductor devices and the accompanying further miniaturization of mask patterns, masking methods using resists and the like using photolithography technology used in semiconductor device manufacturing have many steps and problems in photolithography accuracy.
[0015] The present invention aims to provide a material that can be applied to the area-selective film forming method using the ALD method and can selectively mask the surface of a substrate according to its material.
[0016] Means for solving problems
[0017] The present inventors have found that a polymer film can be selectively formed according to the material of the substrate surface by combining a radical addition-reactive compound with a specific radical generator, thereby completing the present invention.
[0018] That is, as a first aspect, the present invention relates to a composition for forming a polymer film, which is a composition for forming a polymer film, which is used for selectively forming a polymer film on a region (RI) of a substrate having a region (RI) on the surface formed by a metal (I) and a region (R-II) on the surface formed by a material (II) different from the metal (I), wherein the above-mentioned composition for forming a polymer film contains a free radical generator (A) and a free radical addition-reactive compound (B).
[0019] As a second aspect, the present invention relates to a composition for forming a polymer film, which is a composition for forming a polymer film, in a substrate having a region (RI) on the surface formed by a metal (I), and a region (R-II) on the surface formed by a material (II) different from the metal (I), and is used to selectively form a polymer film on a region (RI) of a substrate, wherein the composition for forming a polymer film comprises a free radical generator (A) and a free radical addition-reactive compound (B), and is composed of a component composition whose curing property is higher in the region (RI) than in the region (R-II) when the substrate is heated.
[0020] According to a third aspect, the present invention relates to the polymer film-forming composition according to the first aspect or the second aspect, wherein the radical generator (A) is a radical generator containing a sulfur atom.
[0021] According to a fourth aspect, the present invention relates to the polymer film-forming composition according to any one of the first to third aspects, wherein the radical generator (A) is an oxime ester radical generator.
[0022] According to a fifth aspect, the present invention relates to the polymer film-forming composition according to any one of the first to fourth aspects, wherein the radical generator (A) is a radical generator represented by the following formula (1).
[0023]
[0024] [Wherein,
[0025] R 1 and R 3 Each is independently an optionally substituted phenyl group, an optionally substituted 5- to 10-membered aromatic heterocyclic group, or an optionally substituted alkyl group having 1 to 10 carbon atoms, wherein the substituent in the above phenyl group, aromatic heterocyclic group or alkyl group may contain a sulfur atom,
[0026] R 2 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may be substituted, wherein the substituent in the alkyl group may include a sulfur atom,
[0027] n is 0 or 1,
[0028] The wavy line represents either the E or Z geometric isomer or a mixture thereof.]
[0029] As a sixth aspect, the present invention relates to the polymer film-forming composition according to any one of the first to fifth aspects, wherein the radical addition-reactive compound (B) is at least one polymer selected from polyimides, polyamic acids, and polyamic acid esters having radical addition-reactive double bonds in the molecule.
[0030] According to a seventh aspect, the present invention relates to the polymer film-forming composition according to any one of the first to sixth aspects, wherein the radical addition-reactive compound (B) is at least one selected from polyimide precursors having a unit structure represented by the following formula (2).
[0031]
[0032] [Wherein,
[0033] X 1 is a 4-valent organic group, Y 1 is a divalent organic group,
[0034] R 4 and R 5 are each independently a hydrogen atom or a monovalent organic group, wherein the above R 4 and R 5At least one of them is a group represented by formula (3).]
[0035]
[0036] [Wherein,
[0037] R 6 , R 7 and R 8 Each is independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, m is an integer of 1 to 10, and * represents the bonding position with the oxygen atom in the above formula (2).
[0038] As an eighth aspect, the present invention relates to the polymer film-forming composition according to any one of the first to fifth aspects, wherein the radical addition-reactive compound (B) is at least one selected from the group consisting of a (meth)acrylate compound and a vinyl compound.
[0039] As a ninth aspect, the present invention relates to the polymer film-forming composition according to any one of the first aspect to the eighth aspect, wherein the metal (I) is copper, an alloy containing copper, titanium, or an alloy containing titanium.
[0040] As a tenth aspect, the present invention relates to the polymer film-forming composition according to any one of the first to ninth aspects, wherein the material (II) is at least one selected from SiO2, SiN, SiC, SiOC, SiCN, Ta, TaN, Ti and TiN.
[0041] As an eleventh aspect, the present invention relates to a selective polymer film forming method, which is a method for selectively forming a polymer film on a surface of a substrate.
[0042] The surface has a region (RI) formed of a metal (I), and a region (R-II) adjacent to the region (RI) and formed of a material (II) different from the metal (I),
[0043] The selective polymer film forming method comprises the following steps:
[0044] a polymer film forming step of applying a polymer film-forming composition comprising a radical generator (A) and a radical addition-reactive compound (B) to the surface and heating the composition to form a polymer film; and
[0045] Next, a step is performed in which the substrate surface is brought into contact with a solvent (C) to remove the coating material on the region (R-II).
[0046] As a 12th aspect, the selective polymer film formation method described in the 11th aspect further includes the following step after the step of removing the coating on the above-mentioned area (R-II): a residue removal step of removing the residue on the above-mentioned area (R-II) by dry etching.
[0047] As a thirteenth aspect, the present invention relates to a thin film forming method, which is a method for forming a thin film selectively on a region (R-II) by an atomic layer deposition method in a substrate having a region (RI) formed of a metal (I) and a region (R-II) formed of a material (II) different from the metal (I), the method comprising the following steps:
[0048] A step of forming a thin film by atomic layer deposition on the surface of the substrate having the polymer film formed in the region (RI) by the selective polymer film formation method according to the eleventh aspect or the twelfth aspect.
[0049] As a fourteenth aspect, the thin film forming method according to the thirteenth aspect further comprises the step of removing the polymer film on the region (RI) formed of the metal (I) after the step of forming the thin film.
[0050] As a fifteenth aspect, the present invention relates to a laminated body having a plurality of regions formed on a surface of a substrate,
[0051] The above region includes a region (RI) formed of metal (I), and a region (R-II) adjacent to the region (RI) and formed of a material (II) different from the metal (I).
[0052] A polymer film formed from the polymer film-forming composition according to any one of the first aspect to the tenth aspect is present on the region (RI),
[0053] The region (R-II) does not have the polymer film.
[0054] Effects of the Invention
[0055] According to the present invention, a polymer film-forming composition and a selective film-forming method can be provided that can selectively form a polymer film according to the material of a substrate surface, particularly on a substrate surface having a plurality of regions formed of different materials.
[0056] Furthermore, according to the present invention, it is possible to provide a laminate (substrate) on which a polymer film is regioselectively formed, which can be particularly applied to regioselective film formation on a substrate surface using an atomic layer deposition method (ALD method). BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1This is a diagram showing a scanning electron microscope photograph of a cross section in the vertical direction of the (untreated) substrate used in Film Formation Example 3.
[0058] Figure 2 This is a diagram showing a scanning electron microscope photograph of a cross section in the vertical direction of the substrate produced in Film Formation Example 3. DETAILED DESCRIPTION
[0059] The present invention is directed to a polymer film-forming composition capable of selectively forming a film depending on the material of a substrate surface, and a selective polymer film-forming method using the polymer film-forming composition.
[0060] [Substrate]
[0061] The substrate to which the polymer film-forming composition and the selective polymer film-forming method of the present invention are applied has a region (RI) whose surface is formed of a metal (I) and a region (R-II) whose surface is formed of a material (II) different from the metal (I).
[0062] The metal (I) is preferably copper, an alloy containing copper, titanium, or an alloy containing titanium.
[0063] In addition, the above-mentioned material (II) is preferably at least one selected from SiO2, SiN, SiC, SiOC, SiCN, Ta, TaN, Ti, or TiN.
[0064] The "surface" of the substrate here refers not only to the "surface" of the substrate itself, but also to the "surface" of a layer or pattern formed of the above-mentioned metal (I) or material (II) provided on the substrate.
[0065] In addition, on the same substrate, both the region (RI) and the region (R-II) may have a plurality of regions (RI) and regions (R-II) having different metal types / material types.
[0066] [Polymer film-forming composition]
[0067] The polymer film-forming composition according to the present invention comprises a radical generator (A) and a radical addition-reactive compound (B), and may contain other components as necessary.
[0068] The polymer film-forming composition according to the present invention may be composed of a component composition in which, when heated on the substrate, the curing property is higher in the region (RI) than in the region (R-II).
[0069] 《Free Radical Generator (A)》
[0070] As the radical generator (A) used in the polymer film-forming composition of the present invention, for example, a radical generator containing a sulfur atom can be used.
[0071] As the radical generator (A), for example, an oxime ester radical generator can be used.
[0072] Oxime ester radical generators are generally used as photoradical polymerization initiators in photopolymerization / UV curing. As described later, the present invention is characterized in that the composition is thermally cured to obtain a polymer film, that is, the oxime ester radical generator is used as a thermal radical polymerization initiator.
[0073] As the radical generator (A), for example, a radical generator represented by the following formula (1) can be used.
[0074]
[0075] In the above formula (1), R 1 and R 3 Each is independently an optionally substituted phenyl group, an optionally substituted 5- to 10-membered aromatic heterocyclic group, or an optionally substituted alkyl group having 1 to 10 carbon atoms, wherein the substituent in the above phenyl group, aromatic heterocyclic group or alkyl group may contain a sulfur atom,
[0076] R 2 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may be substituted, wherein the substituent in the alkyl group may include a sulfur atom,
[0077] n is 0 or 1,
[0078] The wavy line represents either E or Z geometric isomers or a mixture thereof.
[0079] Examples of the alkyl group having 1 to 10 carbon atoms include linear or branched alkyl groups having 1 to 10 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, 1-methyl-n-butyl, 2-methyl-n-butyl, 3-methyl-n-butyl, 1,1-dimethyl-n-propyl, 1,2-dimethyl-n-propyl, 2,2-dimethyl-n-propyl, 1-ethyl-n-propyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl -n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl and 1-ethyl-2-methyl-n-propyl, etc.
[0080] In addition, a cyclic alkyl group can also be used. For example, as the cyclic alkyl group having 3 to 10 carbon atoms, there can be mentioned a cyclopropyl group, a cyclobutyl group, a 1-methyl-cyclopropyl group, a 2-methyl-cyclopropyl group, a cyclopentyl group, a 1-methyl-cyclobutyl group, a 2-methyl-cyclobutyl group, a 3-methyl-cyclobutyl group, a 1,2-dimethyl-cyclopropyl group, a 2,3-dimethyl-cyclopropyl group, a 1-ethyl-cyclopropyl group, a 2-ethyl-cyclopropyl group, a cyclohexyl group, a 1-methyl-cyclopentyl group, a 2-methyl-cyclopentyl group, a 3-methyl-cyclopentyl group, a 1-ethyl-cyclobutyl group, a 2-ethyl-cyclobutyl group, a 3-ethyl-cyclobutyl group, a 1,2-dimethyl-cyclobutyl group, a 1,3-dimethyl-cyclobutyl group, a 2,2-dimethyl-cyclobutyl group Cycloalkyl groups such as cyclobutyl, 2,3-dimethyl-cyclobutyl, 2,4-dimethyl-cyclobutyl, 3,3-dimethyl-cyclobutyl, 1-n-propyl-cyclopropyl, 2-n-propyl-cyclopropyl, 1-isopropyl-cyclopropyl, 2-isopropyl-cyclopropyl, 1,2,2-trimethyl-cyclopropyl, 1,2,3-trimethyl-cyclopropyl, 2,2,3-trimethyl-cyclopropyl, 1-ethyl-2-methyl-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, 2-ethyl-2-methyl-cyclopropyl and 2-ethyl-3-methyl-cyclopropyl, and cross-linked cycloalkyl groups such as dicyclobutyl, dicyclopentyl, dicyclohexyl, dicycloheptyl, dicyclooctyl, dicyclononyl and dicyclodecyl.
[0081] Examples of the 5- to 10-membered aromatic heterocyclic group include furyl, pyrrolyl, imidazolyl, imidazolinyl, thienyl, pyrazolyl, Azolyl, iso oxazolyl, thiazolyl, isothiazolyl, pyridinyl, pyrazinyl, pyrimidinyl, pyridazinyl, triazinyl, benzofuranyl, indolyl, indolizinyl, isoindolyl, benzothiophenyl, benzimidazolyl, purinyl, quinolyl, isoquinolyl, quinoxalinyl, quinazolinyl, cinnolinyl, benzopyranyl and the like.
[0082] In addition, as the substituent of the above-mentioned phenyl group, aromatic heterocyclic group, and alkyl group, halogen atoms, alkyl groups, phenyl groups, hydroxyl groups, carboxyl groups, epoxy groups, acryloyl groups, methacryloyl groups, mercapto groups, alkylthio groups, arylthio groups, heterocyclic thio groups, sulfonyl groups, alkylsulfonyl groups, arylsulfonyl groups, heterocyclic sulfonyl groups, amino groups, amide groups, alkoxy groups, cyano groups, etc. can be mentioned. The above-mentioned phenyl group, aromatic heterocyclic group, and alkyl group can have two or more of these substituents. In addition, they can be one substituent in which two or more of these substituents are combined.
[0083] Specific examples of the free radical generator (A) include, but are not limited to, 1-[4-(phenylthio)phenyl]-1,2-octanedione-2-(O-benzoyl oxime) (BASF Japan Co., Ltd., Irgacure (registered trademark) OXE01), 5-(4-isopropylphenylthio)-1,2-indanedione, 2-O-acetyl)oxime (OMNIRAD 1312, IGM RESINS Co., Ltd.), 1-[4-(phenylthio)phenyl]-3-cyclopentylpropane-1,2-dione-2-(O-benzoyl oxime), and a compound represented by the following formula (Adekacure NCI-930, ADEKA Co., Ltd.).
[0084]
[0085] 《Free Radical Addition Reactive Compounds (B)》
[0086] The radical addition-reactive compound (B) used in the polymer film-forming composition of the present invention is, for example, a compound having at least one radical addition-reactive double bond in the molecule, and preferably a compound having two or more radical addition-reactive double bonds in the molecule.
[0087] Examples of the radical addition reactive compound (B) include polymers having a radical addition reactive double bond in the molecule (for example, polyimide, polyamic acid, and polyamic acid ester), (meth)acrylate compounds, and vinyl compounds, but are not limited thereto.
[0088] The radical addition-reactive compound (B) may be used alone or in combination of two or more.
[0089] As an example of the radical addition reactive compound (B), a polyimide precursor including a unit structure represented by the following formula (2) can be mentioned.
[0090]
[0091] In the above formula (2), X 1 is a 4-valent organic group, Y 1 is a divalent organic group,
[0092] R 4 and R 5 Each independently represents a hydrogen atom or a monovalent organic group. 4 and R 5 At least one of them is a group represented by formula (3) described later.
[0093] The above X 1 There are no particular limitations on the tetravalent organic group as long as it is a tetravalent organic group, and examples thereof include tetravalent organic groups having 6 to 40 carbon atoms. More specifically, examples thereof include a tetravalent organic group containing an aromatic ring and / or an aliphatic ring, preferably containing 2 to 8 aromatic rings and / or aliphatic rings, and may contain at least one ether bond (—O—) or ester bond (—COO—, —OCO—) connecting them.
[0094] For example, X 1 Examples include tetravalent organic groups represented by the following formula (4) or (5).
[0095]
[0096] In the above formula, A 1 , A 2 It is a divalent organic group containing a directly bonded aromatic ring and / or aliphatic ring having 6 to 40 carbon atoms, or a divalent organic group containing an aromatic ring and / or aliphatic ring having 6 to 40 carbon atoms which may be interrupted by an alkylene group, -CO-, -COO-, -OCO-, or -O-, wherein the alkylene group may be substituted by a halogen atom and may form a ring.
[0097] More preferably, the above A 1 , A 2 It is a divalent organic group containing a directly bonded aromatic ring and / or aliphatic ring having 6 to 40 carbon atoms, or a divalent organic group containing an aromatic ring and / or aliphatic ring having 6 to 40 carbon atoms interrupted by an alkylene group having 2 to 4 carbon atoms which may be substituted with a halogen atom and can form a ring, and more preferably, it is a divalent organic group containing an aromatic ring having 6 to 40 carbon atoms interrupted by an alkylene group having 2 to 4 carbon atoms.
[0098] As the above X 1Examples include various tetravalent groups represented by the group of the following formula (6) and tetravalent groups represented by formulae (6-1) to (6-14). In each formula, * represents a bond to the carbon atom of the carbonyl group in formula (2).
[0099]
[0100]
[0101] The above X 1 The structure may be one kind or a combination of two or more kinds.
[0102] The above Y 1 There are no particular limitations on the group as long as it is a divalent organic group, and examples thereof include divalent organic groups having 6 to 40 carbon atoms.
[0103] More specifically, there can be mentioned a divalent organic group containing 1 to 8 aromatic rings and / or aliphatic rings, for example, an aromatic ring and / or aliphatic ring which may be substituted, a divalent aliphatic group having no cyclic structure, and a siloxane group.
[0104] As the above Y 1 , various divalent groups represented by the following groups of formulae (7) to (9) can be cited. It should be noted that in the formulae, A each independently represents an alkyl group such as methyl, ethyl, propyl, butyl, etc. In addition, in each formula, * is a bond to the nitrogen atom in formula (2).
[0105]
[0106] The above Y 1 The structure may be one kind or a combination of two or more kinds.
[0107] The above R 4 and R 5 Each independently represents a hydrogen atom or a monovalent organic group, wherein R 5 and R 6 Any one of them is a group represented by formula (3) described later.
[0108] The monovalent organic group is not particularly limited and may be, for example, a monovalent aliphatic group having 1 to 30 carbon atoms or 5 to 22 carbon atoms, a cyclic aliphatic group, a group in which an aromatic group and an aliphatic group are combined, or a group in which these groups are substituted with a halogen atom, a nitro group, an amino group, a cyano group, a methoxy group, an acetoxy group, etc. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0109] As mentioned above, R 4 and R 5 At least one of them is a monovalent organic group represented by the following formula (3), and R4 and R 5 Both are monovalent organic groups represented by formula (3). 4 and R 5 The total amount of the monovalent organic group represented by the formula (3) is such that the amount of the monovalent organic group represented by the formula (3) is 50 mol % or more, or alternatively 80 mol % or more.
[0110]
[0111] In the above formula (3), R 6 , R 7 and R 8 Each independently represents a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, m represents an integer of 1 to 10, and * represents a bonding position to an oxygen atom in formula (2).
[0112] Examples of the monovalent organic group having 1 to 3 carbon atoms include straight-chain alkyl groups such as methyl, ethyl and propyl groups; branched-chain alkyl groups such as isopropyl groups; alicyclic alkyl groups such as cyclopropyl groups; alkenyl groups such as vinyl and allyl groups; alkynyl groups such as ethynyl groups; alkoxy groups such as methoxy, ethoxy and propoxy groups; acyl groups such as acetyl groups; ester groups such as methoxycarbonyl groups; formyl groups; haloformyl groups; carbamoyl groups; cyano groups; heterocyclic groups such as oxiranyl, aziridinyl, thietanyl, triazine, oxathiolanyl, dihydroazetidinyl and dihydrothiazolyl groups, and the like.
[0113] R in formula (3) 6 There are no limitations as long as it is a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, and it may be, for example, a hydrogen atom or a methyl group.
[0114] In addition, R 7 and R 8 There is no limitation as long as each independently represents a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, and the group may be, for example, a hydrogen atom.
[0115] Furthermore, m may preferably be an integer of 2 or more and 4 or less.
[0116] The polyimide precursor including the unit structure represented by the above formula (2) can be converted into a polyimide by subjecting it to a heating cyclization treatment.
[0117] An example of a method for preparing a polyimide precursor including a unit structure represented by the above formula (2) is as follows.
[0118] For example, by making the tetravalent organic group X 1 The tetracarboxylic dianhydride is reacted with an alcohol formed by bonding a monovalent organic group represented by the above formula (3) and a hydroxyl group to prepare a partially esterified tetracarboxylic acid (hereinafter also referred to as an acid / ester), and then reacted with an alcohol containing the above divalent organic group Y1 By polycondensing the diamines, a polyimide precursor having a unit structure represented by the above formula (2) can be obtained.
[0119] (Preparation of acid / ester)
[0120] As the tetravalent organic group X 1 The tetracarboxylic dianhydride includes, for example, pyromellitic anhydride, diphenyl-3,3',4,4'-tetracarboxylic dianhydride (=4,4'-biphenyltetracarboxylic dianhydride), diphenyl ether-3,3',4,4'-tetracarboxylic dianhydride (=4,4'-oxydiphthalic dianhydride), benzophenone-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, diphenyl sulfone-3,3',4,4'-tetracarboxylic dianhydride, diphenylmethane-3,3',4,4'-tetracarboxylic dianhydride, 2,2-bis(3,4-phthalic anhydride)propane, 2,2-bis(3,4-phthalic anhydride)-1,1,1,3,3,3-hexafluoropropane, and the like.
[0121] Moreover, tetracarboxylic dianhydrides represented by the following formula (6-1-a) to formula (6-14-a) are also exemplified.
[0122]
[0123] These can be used alone or in combination of two or more.
[0124] Examples of the alcohol having a structure represented by the above formula (3) include 2-acryloyloxyethyl alcohol, 1-acryloyloxy-3-propyl alcohol, hydroxymethyl vinyl ketone, 2-hydroxyethyl vinyl ketone, 2-hydroxy-3-methoxypropyl acrylate, 2-hydroxy-3-butoxypropyl acrylate, 2-hydroxy-3-butoxypropyl acrylate, 2-methacryloyloxyethyl alcohol, 1-methacryloyloxy-3-propyl alcohol, 2-hydroxy-3-methoxypropyl methacrylate, 2-hydroxy-3-butoxypropyl methacrylate, 2-hydroxy-3-butoxypropyl methacrylate, and 2-hydroxyethyl methacrylate.
[0125] In the preparation of the acid / ester, the alcohol having the structure represented by the above formula (3) is preferably in the form of 4 and R 5 The total content of the precipitate is adjusted to be 80 mol % or more.
[0126] The above-mentioned tetracarboxylic dianhydride and the above-mentioned alcohol are stirred, dissolved and mixed in a reaction solvent at a reaction temperature of 0 to 100° C. for 10 to 40 hours in the presence of a basic catalyst such as pyridine, so that the half-esterification reaction of the acid dianhydride proceeds and the desired acid / ester body can be obtained.
[0127] As the above-mentioned reaction solvent, a reaction solvent that dissolves the acid / ester body and the polyimide precursor that is a polycondensation product of the acid / ester body and diamines is preferred, and examples thereof include N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, tetramethylurea, γ-butyrolactone, ketones, esters, lactones, ethers, halogenated hydrocarbons, hydrocarbons, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, methyl acetate, ethyl acetate, butyl acetate, diethyl oxalate, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, dichloromethane, 1,2-dichloroethane, 1,4-dichlorobutane, chlorobenzene, o-dichlorobenzene, hexane, heptane, benzene, toluene, xylene, etc. These may be used alone or in combination of two or more thereof as required.
[0128] (Preparation of polyimide precursor)
[0129] The acid / ester body is converted into a polyanhydride by adding a known dehydration condensation agent such as dicyclohexylcarbodiimide, N,N'-diisopropylcarbodiimide, 1-ethoxycarbonyl-2-ethoxy-1,2-dihydroquinoline, 1,1-carbonyldioxy-di-1,2,3-benzotriazole, N,N'-disuccinimidyl carbonate, etc. to the above-mentioned acid / ester body (typically a solution in the above-mentioned reaction solvent) under ice cooling, and then adding dropwise a divalent organic group Y 1 A polyimide precursor having a unit structure represented by formula (2) can be obtained by separately dissolving or dispersing a diamine in a solvent and polycondensing the mixture.
[0130] As the divalent organic group Y 1The diamines include, for example, p-phenylenediamine, m-phenylenediamine, 4,4-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 4,4'-diaminobenzophenone, 3,4 '-Diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4-bis(3-aminophenoxy)biphenyl, bis[4-(4 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 9,10-bis(4-aminophenyl)anthracene, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,4-bis(3-aminopropyldimethylsilyl)benzene, o-tolidine sulfone, 9 ,9-bis(4-aminophenyl)fluorene, and substances in which a part of the hydrogen atoms on these benzene rings are substituted with methyl, ethyl, hydroxymethyl, hydroxyethyl, halogen, etc., such as 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 2,2'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 3,3'-dichloro-4,4'-diaminobiphenyl, and mixtures thereof.
[0131] In addition, diamines represented by the group of the following formula (9-1) are also mentioned.
[0132]
[0133] The above-mentioned diamines are not limited to these.
[0134] After the polycondensation reaction is completed, the water-absorbing byproduct of the dehydration condensation agent coexisting in the reaction solution is filtered and separated as needed, and then a poor solvent such as water, aliphatic lower alcohol, or a mixture thereof is added to the reaction solution to precipitate the polymer component, and further, the polymer is repeatedly redissolved and reprecipitated, so that the polymer can be purified and vacuum dried to isolate the polyimide precursor containing the unit structure shown in formula (2). In order to improve the purification degree, the solution of the polymer can be passed through a column filled with an anion and / or cation exchange resin swollen with a suitable organic solvent to remove ionic impurities.
[0135] The molecular weight of the polyimide precursor including the unit structure represented by formula (2) may be, for example, 5,000 to 150,000, or 7,000 to 50,000, when measured as a polystyrene-equivalent weight average molecular weight by gel permeation chromatography.
[0136] In addition, as an example of the radical addition reactive compound (B), a (meth)acrylate compound and a vinyl compound can be cited. It should be noted that the (meth)acrylate compound and the vinyl compound are different from polyimide, polyamic acid, and polyamic acid ester having a radical addition reactive double bond in the molecule, and a polyimide precursor containing a unit structure represented by formula (2).
[0137] These (meth)acrylate compounds and vinyl compounds can be used alone or in combination of two or more. In addition, the above-mentioned (meth)acrylate compounds and vinyl compounds can be used together with the polyimide, polyamic acid, and polyamic acid ester having a free radical addition reactive double bond in the above-mentioned molecule, and a polyimide precursor containing a unit structure represented by the above formula (2).
[0138] In addition, the (meth)acrylate compound in the present invention refers to both acrylate compounds and methacrylate compounds. For example, (meth)acrylic acid refers to acrylic acid and methacrylic acid.
[0139] Among them, as the (meth)acrylate compound and the vinyl compound, a polyfunctional compound, that is, a polyfunctional (meth)acrylate compound and a polyfunctional vinyl compound can be preferably used, and in particular, a polyfunctional (meth)acrylate compound can be preferably used.
[0140] Examples of the polyfunctional (meth)acrylate compound include trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol di(meth)acrylate monostearate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, glycerol tri(meth)acrylate, propoxylated glycerol tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, ethoxylated dipentaerythritol hexa(meth)acrylate, ethoxylated glycerol tri(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, ethoxylated bisphenol F di(meth)acrylate. Acid ester, 1,3-propylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 2-methyl-1,8-octanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, bis(2-hydroxyethyl)isocyanurate di(meth)acrylate, tris(2-hydroxyethyl)isocyanurate di(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, tricyclo[5.2.1.0 2,6 ] decanedimethanol di(meth)acrylate, dioxanediol di(meth)acrylate, 2-hydroxy-1-acryloyloxy-3-methacryloyloxypropane, 2-hydroxy-1,3-di(meth)acryloyloxypropane, 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene, bis[4-(meth)acryloylthiophenyl]sulfide, bis[2-(meth)acryloylthioethyl]sulfide, 1,3-adamantanediol di(meth)acrylate, 1,3-adamantanedimethanol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, tris(2-(meth)acryloyloxyethyl)phosphate, ε-caprolactone-modified tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, etc.
[0141] In addition, as one of the multifunctional (meth) acrylate compounds, a multifunctional carbamate (meth) acrylate compound can be used. The compound is a compound having multiple acryloyl groups or methacryloyl groups in one molecule and having one or more carbamate bonds (-NHCOO-). As the above-mentioned multifunctional carbamate (meth) acrylate, for example, a substance obtained by the reaction of a multifunctional isocyanate with a (meth) acrylate having a hydroxyl group, a substance obtained by the reaction of a multifunctional isocyanate with a (meth) acrylate having a hydroxyl group and a polyol, etc. can be cited, but the multifunctional carbamate (meth) acrylate compound that can be used in the present invention is not limited to such exemplification.
[0142] In addition, as said polyfunctional isocyanate, tolylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hexamethylene diisocyanate, etc. are mentioned, for example.
[0143] Examples of the (meth)acrylate having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, and tripentaerythritol hepta(meth)acrylate.
[0144] Furthermore, examples of the polyol include glycols such as ethylene glycol, propylene glycol, neopentyl glycol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, and dipropylene glycol; polyester polyols which are reaction products of these glycols with aliphatic dicarboxylic acids or dicarboxylic anhydrides such as succinic acid, maleic acid, and adipic acid; polyether polyols; polycarbonate diols, and the like.
[0145] As an example of the vinyl compound, the following polyfunctional vinyl compounds can be mentioned.
[0146] (A1) Vinyl hydrocarbons:
[0147] (A1-1) Aliphatic vinyl hydrocarbons; isoprene, butadiene, 3-methyl-1,2-butadiene, 2,3-dimethyl-1,3-butadiene, 1,2-polybutadiene, pentadiene, hexadiene, octadiene, etc.
[0148] (A1-2) Alicyclic vinyl hydrocarbons; cyclopentadiene, cyclohexadiene, cyclooctadiene, norbornadiene, etc.
[0149] (A1-3) Aromatic vinyl hydrocarbons; divinylbenzene, divinyltoluene, divinylxylene, trivinylbenzene, divinylbiphenyl, divinylnaphthalene, divinylfluorene, divinylcarbazole, divinylpyridine, etc.
[0150] (A2) Vinyl esters, allyl esters, vinyl ethers, allyl ethers, vinyl ketones:
[0151] (A2-1) Vinyl esters; divinyl adipate, divinyl maleate, divinyl phthalate, divinyl isophthalate, divinyl itaconate, vinyl (meth)acrylate, etc.
[0152] (A2-2) Allyl esters; diallyl maleate, diallyl phthalate, diallyl isophthalate, diallyl adipate, allyl (meth)acrylate, etc.
[0153] (A2-3) Vinyl ethers; divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, etc.
[0154] (A2-4) Allyl ethers; diallyl ether, diallyloxyethane, triallyloxyethane, tetraallyloxyethane, tetraallyloxypropane, tetraallyloxybutane, tetramethallyloxyethane, etc.
[0155] (A2-5) Vinyl ketones; divinyl ketone, diallyl ketone, etc.
[0156] (A3) Nitrogen-containing vinyl compounds:
[0157] Diallylamine, diallyl isocyanurate, diallyl cyanurate, ethoxylated isocyanurate di(meth)acrylate, ethoxylated isocyanurate tri(meth)acrylate, methylenebis(meth)acrylamide, bismaleimide, etc.
[0158] (A4) Silicon-containing vinyl compounds:
[0159] Dimethyldivinylsilane, divinyl(methyl)(phenyl)silane, diphenyldivinylsilane, 1,3-divinyl-1,1,3,3-tetramethyldisilazane, 1,3-divinyl-1,1,3,3-tetraphenyldisilazane, diethoxydivinylsilane, etc.
[0160] (A5) Fluorine-containing vinyl compounds:
[0161] 1,4-divinylperfluorobutane, 1,4-divinyloctafluorobutane, 1,6-divinylperfluorohexane, 1,6-divinyldodecafluorohexane, 1,8-divinylperfluorooctane, 1,8-divinylhexafluorooctane, etc.
[0162] Examples of the (meth)acrylate compound and the vinyl compound include the monofunctional (meth)acrylate compounds and vinyl compounds (the (meth)acrylate compounds and vinyl compounds having one radical addition-reactive double bond in the molecule) exemplified below.
[0163] (C1) (Meth) acrylic acid compounds:
[0164] (C1-1) (Meth) acrylic acid; (meth) acrylic acid, itaconic acid, 2-trifluoromethyl acrylic acid, 2-ethyl acrylic acid, 2-propyl acrylic acid, 2-bromomethyl acrylic acid, 2-acetamidoacrylic acid, 2-ethylacryloyl chloride, 3,3-dimethyl (meth)acryloyl chloride, etc.
[0165] (C1-2) (Meth)acrylates; methyl (meth)acrylate, ethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 2-carboxyethyl (meth)acrylate, mono-2-(meth)acryloyloxyethyl succinate, bis[2-(meth)acryloyloxyethyl]phosphate, 2-(meth)acryloyloxyethyl acetoacetate, 2-dimethylaminoethyl (meth)acrylate, 2-diethylaminoethyl (meth)acrylate, [2-(meth)acryloyloxyethyl]trimethylammonium chloride, 2-isocyanate ethyl (meth)acrylate, 2-[9H-carbazol-9-yl]ethyl (meth)acrylate, vinyl (meth)acrylate, 3-dimethylaminopropyl (meth)acrylate, allyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, octadecyl (meth)acrylate, Isobornyl ester, tetrahydrofurfuryl (meth)acrylate, (R)-α-(meth)acryloyloxy-β,β-dimethyl-γ-butyrolactone, 2-naphthyl (meth)acrylate, ethylene glycol methyl ether (meth)acrylate, ethylene glycol cyclopentenyl ether (meth)acrylate, ethylene glycol phenyl ether (meth)acrylate, ethylene glycol (meth)acrylate phosphate, diethylene glycol ethyl ether (meth)acrylate, diethylene glycol 2-ethylhexyl ether (meth)acrylate, dipropylene glycol allyl ether (meth)acrylate, neopentyl glycol methyl ether propoxylated (meth)acrylate, polyethylene glycol methyl ether (meth)acrylate ) acrylate, polyethylene glycol phenyl ether (meth) acrylate, polypropylene glycol methyl ether (meth) acrylate, polypropylene glycol 4-nonylphenyl ether (meth) acrylate, 2-ethyl acrylate, 2-ethyl benzyl acrylate, 2-propyl acrylate, 2-propyl benzyl acrylate, 2-acetamido methyl acrylate, cis-2-cyanoacrylate, vinyl crotonate, vinyl cinnamate, isopropyl cinnamate, isobutyl cinnamate, tert-butyl cinnamate, isopentyl cinnamate, 2-cyano-3,3-diphenyl ethyl acrylate, 2-ethylhexyl 2-cyano-3,3-diphenyl acrylate, etc.
[0166] (C1-3) (Meth)acrylates containing epoxy groups; glycidyl (meth)acrylate, etc.
[0167] (C1-4) (meth)acrylates containing hydroxyl groups; 2-hydroxyethyl (meth)acrylate, 2-(4-benzoyl-3-hydroxyphenoxy)ethyl (meth)acrylate, 2-hydroxypropyl 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxyethyl caprolactone, hydroxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 3-acryloyloxy-2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, 3-hydroxy-2-methylenebutyric acid methyl ester, etc.
[0168] (C1-5) Halogen-containing (meth)acrylates; pentabromobenzyl (meth)acrylate, pentabromophenyl (meth)acrylate, methyl 2-bromoacrylate, tert-butyl 2-bromoacrylate, methyl 2-bromomethylacrylate, ethyl 2-bromomethylacrylate, etc.
[0169] (C1-6) Silicon-containing (meth)acrylates; 2-trimethylsilylethyl methacrylate, 3-trimethoxysilylpropyl (meth)acrylate, 2-trimethylsilyloxyethyl (meth)acrylate, 3-[tris(trimethylsiloxy)silyl]propyl (meth)acrylate, trimethylsilyl (meth)acrylate, etc.
[0170] (C1-7) Sulfur-containing (meth)acrylates; 2-methylthioethyl (meth)acrylate, etc.
[0171] (C2) Vinyl compounds:
[0172] (C2-1) Styrenes; styrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 2,4,6-trimethylstyrene, 3,4-dimethoxystyrene, 4-benzyloxy-3-methoxystyrene, 4-ethoxystyrene, 4-tert-butylstyrene, 4-tert-butoxystyrene, 4-acetoxystyrene, 2-trifluoromethylstyrene, 3-trifluoromethylstyrene, 4-trifluoromethylstyrene, 3,5-bis(trifluoromethyl)styrene, 4-vinylaniline, 4-vinylanisole, N,N-dimethylvinylbenzylamine, 4-vinylbiphenyl, 2-fluorostyrene, 3-fluorostyrene, 4-fluorostyrene, 2,6-difluorostyrene, 2,3,4,5 ,6-pentafluorostyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 2,6-dichlorostyrene, 2-bromostyrene, 3-bromostyrene, 4-bromostyrene, 3-nitrostyrene, 3-vinylbenzoic acid, 4-vinylbenzoic acid, 4-vinylphenyl tert-butyl carbonate, 4-styrenesulfonic acid, 4-vinylphenylboronic acid, α-methylstyrene, α,2-dimethylstyrene, 1,3-diisopropenylbenzene, 4-chloro-α-methylstyrene, 2,4-diphenyl-4-methyl-1-pentene, 2-isopropenylaniline, 3-isopropenyl-α,α-dimethylbenzyl isocyanate, 1-phenyl-1-trimethylsiloxyethylene, α-bromostyrene, 1-vinylnaphthalene, 2-vinylnaphthalene, 9-vinylanthracene, etc.
[0173] (C2-2) Nitrogen-containing heterocyclic vinyl compounds; N-vinylimidazole, 2-vinylpyridine, 4-vinylpyridine, 9-vinylcarbazole, 1-vinyl-2-pyrrolidone, N-vinylphthalimide, N-vinylcaprolactone, etc.
[0174] (C2-3) Vinyl esters; vinyl acetate, vinyl trifluoroacetate, vinyl propionate, vinyl pivalate, vinyl decanoate, vinyl neodecanoate, vinyl stearate, vinyl benzoate, etc.
[0175] (C2-4) vinyl ethers; 4-vinyloxymethyl cyclohexyl methyl benzoate, ethyl vinyl ether, 2-chloroethyl vinyl ether, propyl vinyl ether, butyl vinyl ether, 4-vinyloxy butyl benzoate, isobutyl vinyl ether, tert-butyl vinyl ether, tert-amyl vinyl ether, cyclohexyl vinyl ether, 2-ethylhexyl vinyl ether, octadecyl vinyl ether, dodecyl vinyl ether, vinyloxytrimethylsilane, 1,4-butanediol vinyl ether, 1,4-cyclohexanedimethanol vinyl ether, ethylene glycol vinyl ether, ethylene glycol butyl vinyl ether, diethylene glycol vinyl ether, ethyl 1-propenyl ether, etc.
[0176] (C2-5) Other vinyl compounds; 1,1-dichloroethylene, cis-1,3-dichloro-1-propylene, 2-methyl-2-vinyl oxirane, vinyl cyclopentane, vinyl cyclohexane, 4-vinyl-1-cyclohexanone, 5-vinyl-2-norbornene, vinyl ferrocene, vinyl trimethylsilane, vinyl trimethoxysilane, N-vinyl formamide, N-methyl-N-vinylacetamide, vinyl bromide, ethyl vinyl sulfide, methyl vinyl sulfone, vinyl sulfonic acid, vinyl phosphonic acid, trans-4,4'-difluorochalcone, etc.
[0177] Furthermore, as the radical addition-reactive compound (B), other addition-reactive compounds having one radical addition-reactive double bond in the molecule, such as those exemplified below, may be included.
[0178] (C3) (Meth)acrylamides:
[0179] (Meth)acrylamide, diacetone (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, N-tris (hydroxymethyl)methyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, N-isobutyloxymethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-[3-dimethylaminopropyl] (meth)acrylamide, 3-((meth)acryloylamino)propyltrimethylammonium chloride, N-tert-butyl (meth)acrylamide, 4-(meth)acryloylmorpholine, N-phenyl (meth)acrylamide, 2-acrylamidoglycolic acid, 2-acrylamido-2-methyl-1-propanesulfonic acid, etc.
[0180] (C4) (Meth) acrylonitrile: (meth) acrylonitrile, 2-chloroacrylonitrile, 1-cyanovinyl acetate, etc.
[0181] As the above-mentioned free radical addition reactive compound (B), it is preferred to use at least one selected from a polyimide precursor containing a unit structure represented by the above-mentioned formula (2), the above-mentioned multifunctional (meth)acrylate compound and a multifunctional vinyl compound. In addition, it is possible to use at least one selected from a polyimide precursor containing a unit structure represented by the above-mentioned formula (2) and a multifunctional (meth)acrylate compound. It is particularly preferred to use a polyimide precursor containing a unit structure represented by the formula (2).
[0182] In addition, in the above-mentioned free radical addition reactive compound (B), the blending amount of the above-mentioned monofunctional (meth)acrylate compound, vinyl compound ((meth)acrylate compound, vinyl compound having one free radical addition reactive double bond in the molecule), and the above-mentioned other addition reactive compounds can be 0% by mass to 30% by mass of the total mass of the above-mentioned free radical addition reactive compound (B) in terms of their total amount.
[0183] In the polymer film-forming composition according to the present invention, the blending amounts of the radical generator (A) and the radical addition-reactive compound (B) may be, for example, 0.1 to 20 parts by mass, or 0.5 to 10 parts by mass, relative to 100 parts by mass of the radical addition-reactive compound (B).
[0184] 《Other ingredients》
[0185] The polymer film-forming composition according to the present invention may further contain other components in addition to the above-mentioned components (A) and (B) within a range not impairing the effects of the present invention.
[0186] Examples of other components include hindered phenol compounds, carboxylic acid compounds or anhydrides thereof, solvents, other resin components, crosslinking compounds, thermal crosslinking agents, adhesion promoters, polymerization inhibitors, azole compounds, fillers, etc., but are not limited thereto.
[0187] 〈Hindered phenol compounds〉
[0188] Examples of the hindered phenol compound include 2,6-di-tert-butyl-4-methylphenol, 2,5-di-tert-butyl-hydroquinone, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, isooctyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 4,4'-methylenebis(2,6-di-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 4,4'-butylenebis(3-methyl-6-tert-butylphenol), triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl) propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], 2,2-thiobis -Diethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-benzenepropionamide), 2,2'-methylene-bis(4-methyl-6-tert-butylphenol), 2,2'-methylene-bis(4-ethyl-6-tert-butylphenol), pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tris-(3,5-di-tert-butyl-4-hydroxybenzyl)-isocyanurate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-isopropylbenzyl)-1,3,5-triazine- 2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-sec-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-(1-ethylpropyl)-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-triethylmethyl-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-( 1H,3H,5H)-trione, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-phenylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,5,6-trimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-5-ethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione5H)-trione, 1,3,5-tris(4-tert-butyl-6-ethyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-5,6-diethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, ,3,5-tris(4-tert-butyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-tert-butyl-5-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[(3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl)methyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, etc., but not limited to these. ,
[0189] When the hindered phenol compound is used, the amount thereof blended may be, for example, 0.1 to 20 parts by mass based on 100 parts by mass of the radical addition-reactive compound (B).
[0190] <Carboxylic acid compound or anhydride thereof>
[0191] By blending the carboxylic acid compound or its anhydride, it is expected that the polyimide precursor having a unit structure represented by the formula (2) in the radical addition-reactive compound (B) in the polymer film-forming composition can be stabilized.
[0192] Specific examples of the carboxylic acid compound are given below, but the present invention is not limited thereto. In addition, the carboxylic acid compound exemplified below may also be an anhydride thereof.
[0193]
[0194] When the carboxylic acid compound or its anhydride is used, it can be blended in an amount of, for example, 0.1 to 10 parts by mass based on 100 parts by mass of the radical addition reactive compound (B).
[0195] The carboxylic acid compound or its anhydride may be present by chemically bonding with the radical addition reactive compound (B) and / or other resin components other than the radical addition reactive compound (B) described later.
[0196] 〈Solvent〉
[0197] As the above-mentioned solvent, an organic solvent is preferably used from the aspect of solubility in the free radical addition reactive compound (B). Specifically, N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, dimethyl sulfoxide, diethylene glycol dimethyl ether, cyclopentanone, cyclohexanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, tetramethylurea, 1,3-dimethyl-2-imidazolidinone, N-cyclohexyl-2-pyrrolidone, ethyl lactate, etc. can be mentioned, and they can be used alone or in combination of two or more.
[0198] The solvent can be used in an amount of, for example, 30 to 1500 parts by mass, or 100 to 1000 parts by mass, based on 100 parts by mass of the radical addition-reactive compound (B), depending on the desired coating film thickness and viscosity of the polymer film-forming composition.
[0199] 〈Other resin components〉
[0200] As other resin components, for example, poly Azoles, poly Azole precursors, phenolic resins, polyamides, epoxy resins, silicone resins, acrylic resins, and polyimides other than the above-mentioned (B) radical addition-reactive compounds.
[0201] When using these other resin components, the compounding amount thereof can be in the range of, for example, 0.01 to 20 parts by mass based on 100 parts by mass of the radical addition-reactive compound (B).
[0202] 〈Cross-linking compound〉
[0203] As the crosslinking compound, for example, an isocyanate compound can be used.
[0204] Examples of the isocyanate compound include an isocyanate compound represented by formula (20).
[0205]
[0206] In the formula, R 23 represents a hydrogen atom or a methyl group, R 24 represents an alkylene group having 1 to 5 carbon atoms which may have a substituent and may be interrupted by an oxygen atom, R 25 It represents an isocyanate group or a blocked isocyanate group.
[0207] In R 24In the above, examples of the alkylene group having 1 to 5 carbon atoms include substituted or unsubstituted methylene, ethylene, propylene, butylene, etc. Examples of the alkylene group interrupted by an oxygen atom include -CH2-O-CH2-, -C2H4-O-CH2-, -CH2-O-C2H4-, etc. Examples of the substituent include halogen atoms, acryloyl, methacryloyl, nitro, amino, cyano, methoxy, acetoxy, etc.
[0208] R 25 It represents an isocyanate group (-NCO) or a blocked isocyanate group. The blocked isocyanate group refers to a group in which the isocyanate group is blocked by a thermally removable protective group, that is, a group obtained by reacting an isocyanate blocking compound (blocking agent) with an isocyanate group.
[0209] The so-called isocyanate blocking agent generally refers to a substance that reacts with isocyanate groups to prevent them from reacting with functional groups in other molecules (e.g., acid functional groups, etc.) at room temperature, but dissociates at high temperatures to regenerate the isocyanate groups and enable subsequent reactions (e.g., with acid functional groups).
[0210] Examples of the blocking agent include alcohols such as methanol, ethanol, isopropanol, n-butanol, 2-ethoxyhexanol, 2-N,N-dimethylaminoethanol, 2-ethoxyethanol, and cyclohexanol, phenols such as phenol, o-nitrophenol, p-chlorophenol, o-cresol, m-cresol, and p-cresol, lactams such as ε-caprolactam, acetone oxime, methyl ethyl ketone oxime, methyl isobutyl ketone oxime, cyclohexanone oxime, acetophenone oxime, diphenylmethane oxime, and the like. Oxime such as ketoxime, amines, amides, nitrogen-containing heteroaryl compounds such as pyrazole, 3,5-dimethylpyrazole, and 3-methylpyrazole, thiols such as dodecanethiol and benzenethiol, malonic acid diesters, acetoacetic acid esters, malonic acid dinitrile, acetylacetone, methylene disulfone, dibenzoylmethane, dipivaloylmethane, active methylene compounds such as acetone dicarboxylic acid diester, hydroxamate, etc.
[0211] It is advantageous for the blocking agent to be volatile so as to evaporate from the composition after release.
[0212] The blocked isocyanate group is represented by, for example, the following formula.
[0213]
[0214] In the formula, Bloc represents a residue of an isocyanate-blocking compound selected from the group consisting of alcohols, amines, amides, active methylene compounds, nitrogen-containing heteroaryl compounds, oximes, ketoximes, and hydroxamates.
[0215] Specific examples of the isocyanate compound represented by the above formula (20) include isocyanate-containing (meth)acrylates such as 2-isocyanate ethyl methacrylate and 2-isocyanate ethyl acrylate, and compounds obtained by adding blocking agents such as methyl ethyl ketoxime, ε-caprolactam, 3,5-dimethylpyrazole, and diethyl malonate to these compounds. It should be noted that these compounds may be used alone or in combination of two or more.
[0216] In addition to being synthesized by a known method, the isocyanate compound may also be the following commercially available products: Calends (registered trademark) AOI (2-isocyanate ethyl acrylate), Calends AOI-VM (registered trademark) (2-isocyanate ethyl acrylate), Calends (registered trademark) MOI (2-isocyanate ethyl methacrylate), Calends (registered trademark) MOI-BM (methacrylate 2-(O-[1'-methylpropyleneamino]carboxyamino)ethyl ester), Calends Calends (registered trademark) MOI-BP (2-[(3,5-dimethylpyrazolyl)carbonylamino]ethyl methacrylate), Calends (registered trademark) MOI-EG (2-(2-methacryloyloxyethyloxy)ethyl isocyanate), Calends (registered trademark) BEI (1,1-(bisacryloyloxymethyl)ethyl isocyanate), Calends (registered trademark) AOI-BM (2-(O-[1'-methylpropyleneamino]carboxyamino)ethyl acrylate) (all manufactured by Showa Denko K.K.), etc.
[0217] Furthermore, an isocyanate compound having a blocked isocyanate group having the following structure may be used.
[0218]
[0219] When using an isocyanate compound, the compounding amount thereof can be, for example, 1 to 50 parts by mass based on 100 parts by mass of the radical addition-reactive compound (B).
[0220] 〈Thermal crosslinking agent〉
[0221] Examples of the thermal crosslinking agent include hexamethoxymethylmelamine, tetramethoxymethyl glycoluril, tetramethoxymethyl benzoguanamine, 1,3,4,6-tetrakis(methoxymethyl) glycoluril, 1,3,4,6-tetrakis(butoxymethyl) glycoluril, 1,3,4,6-tetrakis(hydroxymethyl) glycoluril, 1,3-bis(hydroxymethyl)urea, 1,1,3,3-tetrakis(butoxymethyl)urea, and 1,1,3,3-tetrakis(methoxymethyl)urea.
[0222] 〈Adhesive additives〉
[0223] Examples of the bonding aid include γ-aminopropyl dimethoxysilane, N-(β-aminoethyl)-γ-aminopropyl methyl dimethoxysilane, γ-glycidoxypropyl methyl dimethoxysilane, γ-mercaptopropyl methyl dimethoxysilane, 3-methacryloxypropyl dimethoxymethyl silane, 3-methacryloxypropyl trimethoxysilane, dimethoxymethyl-3-piperidinopropyl silane, diethoxy-3-glycidoxypropyl methyl silane, and N-(3-diethoxymethylsilylpropyl) succinimide. , N-〔3-(triethoxysilyl)propyl〕o-aminobenzoic acid, benzophenone-3,3'-bis(N-〔3-triethoxysilyl〕propylamide)-4,4'-dicarboxylic acid, benzene-1,4-bis(N-〔3-triethoxysilyl〕propylamide)-2,5-dicarboxylic acid, 3-(triethoxysilyl)propylsuccinic anhydride, N-phenylaminopropyltrimethoxysilane and other silane coupling agents, and tri(ethylacetoacetate)aluminum, tri(acetylacetonate)aluminum, ethylacetoacetate aluminum diisopropylate and other aluminum-based adhesive additives, etc.
[0224] When the above-mentioned adhesion promoter is used, the blending amount thereof can be, for example, in the range of 0.5 to 25 parts by mass based on 100 parts by mass of the radical addition reactive compound (B).
[0225] 〈Polymerization Inhibitor〉
[0226] As the above-mentioned thermal polymerization inhibitor, for example, hydroquinone, N-nitrosodiphenylamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt, N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt, etc. are used.
[0227] When the thermal polymerization inhibitor is used, the amount thereof may be in the range of 0.005 to 12 parts by mass relative to 100 parts by mass of the radical addition reactive compound (B).
[0228] 〈Azole compounds〉
[0229] Examples of the azole compound include 1H-triazole, 5-methyl-1H-triazole, 5-ethyl-1H-triazole, 4,5-dimethyl-1H-triazole, 5-phenyl-1H-triazole, 4-tert-butyl-5-phenyl-1H-triazole, 5-hydroxyphenyl-1H-triazole, phenyltriazole, p-ethoxyphenyltriazole, 5-phenyl-1-(2-dimethylaminoethyl)triazole, 5-benzyl-1H-triazole, hydroxyphenyltriazole, 1,5-dimethyltriazole, 4,5-diethyl-1H-triazole, 1H-benzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]
[0063] -benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-tert-butyl-5-methyl-2-hydroxyphenyl)-benzotriazole, 2-(3,5-di-tert-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, hydroxyphenylbenzotriazole, methylbenzotriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 4-carboxyl-1H-benzotriazole, 5-carboxyl-1H-benzotriazole, 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole, 1-methyl-1H-tetrazole, etc. These azole compounds may be used alone or as a mixture of two or more.
[0230] When an azole compound is used, the amount thereof blended may be, for example, 0.1 to 20 parts by mass, or 0.5 to 5 parts by mass, based on 100 parts by mass of the radical addition-reactive compound (B).
[0231] <filler>
[0232] Examples of the filler include inorganic fillers, and specific examples include sols of silica, aluminum nitride, boron nitride, zirconium oxide, aluminum oxide, and the like.
[0233] [Selective polymer film formation method]
[0234] The selective polymer film forming method of the present invention is a method for forming a polymer film using the above-mentioned polymer film forming composition on a substrate having a region (RI) formed of a metal (I) and a region (R-II) adjacent to the above-mentioned region (RI) and formed of a material (II) different from the above-mentioned metal (I) on the surface. Specific examples of the substrate and the polymer film forming composition used in this method are as described above.
[0235] In detail, the method includes the following steps: a polymer film forming step of coating a polymer film forming composition comprising a free radical generator (A) and a free radical addition reactive compound (B) onto the surface of the above-mentioned substrate and heating the composition to form a polymer film; and a step of subsequently contacting the above-mentioned substrate surface with a solvent (C) to remove the coating on the above-mentioned area (R-II).
[0236] 〈Polymer film forming process〉
[0237] In this step, the polymer film is formed by applying the polymer film-forming composition of the present invention onto the substrate, and then drying and heating the composition as necessary.
[0238] Examples of a method for applying the polymer film-forming composition to a substrate include a method of applying the composition using a spin coater, a bar coater, a knife coater, a curtain coater, a screen printer, or the like, and a method of spraying the composition using a spray coater.
[0239] As a drying method which can be carried out as needed after coating, for example, air drying, heating drying using an oven or a hot plate, vacuum drying, etc. are used.
[0240] The heating conditions can be appropriately selected from, for example, a temperature of 50° C. to 200° C. and a time of 10 seconds to 600 seconds.
[0241] By heating, free radicals are generated by the free radical generator (A), and the free radicals react with the free radical addition reactive compound (B) so that the free radical addition reaction proceeds, and the free radical addition reactive compound (B) is cross-linked. By cross-linking, the coating film is cured. In the present invention, the so-called curability is the property of curing, and the so-called high curability means easy curing (easy to cross-link). As mentioned above, in the present invention, the curability of the polymer film-forming composition on the region (RI) and the region (R-II) is different, that is, in one embodiment, the polymer film-forming composition is composed of components with higher curability in the above-mentioned region (RI) than in the region (R-II) when heated on the substrate. According to the difference in such curability, in the process of removing the polymer film described later, only the coating on the region (R-II) can be selectively removed.
[0242] The thickness of the polymer film obtained in this step is not particularly limited, and may be, for example, 1 nm to 50 μm, 50 nm to 10 μm, or 100 nm to 5 μm.
[0243] <Step of removing the polymer film on the region (R-II)>
[0244] This step is a step of bringing the surface of the substrate on which the polymer film is formed into contact with the solvent (C) to remove the coating material on the region (R-II).
[0245] The method for bringing the substrate surface into contact with the solvent (C) is not particularly limited, and the contact may be carried out by any method selected from a spin jet method, a slurry method, a dipping method, and the like.
[0246] As the solvent (C) used here, for example, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylacetamide, cyclopentanone, cyclohexanone, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, γ-butyrolactone, α-acetyl-γ-butyrolactone, methyl 2-hydroxyisobutyrate, etc., which are generally used as solvents in the manufacturing process of semiconductors, can be used. In addition, two or more solvents, for example, a plurality of them can be used in combination.
[0247] 〈Residue Removal Process〉
[0248] Furthermore, after the step of removing the coating material on the region (R-II), the method may further include a residue removal step of removing the residue on the region (R-II) by dry etching.
[0249] The dry etching in this step can be performed using, for example, an oxygen-based gas (oxygen gas, oxygen / carbonyl sulfide (COS) mixed gas, etc.), and nitrogen gas or argon gas can also be used as a diluent gas.
[0250] By implementing the selective polymer film forming method of the present invention, a polymer film formed from the above polymer film forming composition is formed on a region (RI) of a substrate whose surface is formed only of a metal (I), that is, a laminate (substrate) having a polymer film only on the region (RI) and not having a polymer film on the region (R-II) can be obtained. This laminate is also the object of the present invention.
[0251] [Thin film formation method]
[0252] The substrate having the polymer film only in the region (RI) obtained by the above-mentioned [selective polymer film formation method] can be suitably used for region-selective film formation on the substrate surface using the atomic layer deposition method (ALD method).
[0253] That is, the present invention is aimed at a thin film forming method, wherein the thin film forming method is a method for selectively forming a thin film on a region (R-II) by an atomic layer deposition method in a substrate having a region (RI) formed of a metal (I) and a region (R-II) formed of a material (II) different from the metal (I), and the method comprises the following steps: a step of forming a thin film by an atomic layer deposition method on the surface of the substrate having a polymer film formed on the region (RI) by the selective polymer film forming method.
[0254] Furthermore, the thin film forming method may further include the step of removing the polymer film on the region (RI) formed of the metal (I) after the step of forming the thin film.
[0255] As for the steps, the types of gases used, and the like in the film forming method using the atomic layer deposition method (ALD method), those known in the ALD method can be used.
[0256] Example
[0257] Hereinafter, the present invention will be described in further detail based on Examples and Comparative Examples, but the present invention is not limited to these Examples at all.
[0258] The weight average molecular weights shown in the following synthesis examples of this specification are the measurement results obtained by gel permeation chromatography (hereinafter referred to as GPC in this specification). A GPC apparatus (HLC-8320GPC) manufactured by Tosoh Corporation was used for the measurement, and the measurement conditions and the like were as follows.
[0259] GPC column: KD-803, KD-805 (Shodex)
[0260] Column temperature: 50°C
[0261] Solvent: N,N-dimethylformamide (Kanto Chemical Co., Ltd., special grade), lithium bromide monohydrate (Kanto Chemical Co., Ltd., special grade) (30 mM) / phosphoric acid (Aldrich) (30 mM) / tetrahydrofuran (Kanto Chemical Co., Ltd., special grade) (1%)
[0262] Flow rate: 1.0mL / min
[0263] Standard sample: Polystyrene (manufactured by Dielsions Co., Ltd.)
[0264] <Production Example 1> Synthesis of dicarboxylic acid diester (1)
[0265] 200.00 g (0.68 mol) of 4,4'-biphenyltetracarboxylic dianhydride (Tokyo Chemical Industry Co., Ltd.) was added to a 2-liter four-necked flask, and 176.92 g (1.366 mol) of 2-hydroxyethyl methacrylate (Aldrich), 0.74 g (0.007 mol) of hydroquinone (Tokyo Chemical Industry Co., Ltd.) and 600 g of γ-butyrolactone (Kanto Chemical Co., Ltd., deer special grade) were added, and stirred at 23°C. After adding 108.63 g (1.36 mol) of pyridine (Kanto Chemical Co., Ltd., dehydrated), the temperature was raised to 50°C and stirred at 50°C for 2 hours, thereby obtaining a solution containing the compound represented by the following formula (A).
[0266]
[0267] <Production Example 2> Synthesis of polymer (2) as polyimide precursor
[0268] 82.46 g of the solution containing the compound prepared in Preparation Example 1 and 19.45 g of γ-butyrolactone were added to a 500 ml four-necked flask, and a solution prepared by dissolving 13.13 g of N,N'-diisopropylcarbodiimide (DIC) (Tokyo Chemical Industry Co., Ltd.) in 30 g of γ-butyrolactone was added dropwise to the reaction solution over 0.5 hours at about 5°C while stirring the solution. After the addition, the mixture was further stirred for 0.5 hours. Subsequently, a solution prepared by dissolving 19.68 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (Tokyo Chemical Industry Co., Ltd.) in 30 g of N-methyl-2-pyrrolidone (Kanto Chemical Co., Ltd., deer special grade) was added dropwise over 2 hours while stirring the mixture. Then, the temperature was raised to about 25° C. and the mixture was further stirred for 6 hours, and then 4.5 g of ethanol (Kanto Chemical Co., Ltd., special grade) was added and stirred for 1 hour.
[0269] The obtained reaction mixture was added to 1,500 g of methanol (Kanto Chemical, special grade) to generate a precipitate formed by a crude polymer. After the supernatant was separated from the crude polymer by decantation, 150.0 g of N-methyl-2-pyrrolidone was added to dissolve the precipitate to obtain a crude polymer solution. The obtained crude polymer solution was added dropwise to 2,250 g of water to precipitate the polymer. After the obtained precipitate was filtered and separated, the filtrate was washed twice with 600 g of methanol and vacuum dried to obtain a powdery polymer. The molecular weight of the polymer was measured by GPC (standard polystyrene conversion), and the weight average molecular weight (Mw) was 8,016. The yield was 73.6%. The polymer has a repeating unit structure shown in the following formula (B).
[0270]
[0271] <Example 1>
[0272] 0.73 g of the polymer obtained in Preparation Example 2, 0.04 g of IRGACURE [registered trademark] OXE01 (manufactured by BASF, photopolymerization initiator), 0.22 g of A-DPH-12E (manufactured by Shin-Nakamura Chemical Industry Co., Ltd., ethoxylated dipentaerythritol polyacrylate), 0.01 g of IRGANOX [registered trademark] 3114 (manufactured by BASF, hindered phenol antioxidant), and 0.007 g of phthalic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) were dissolved in a mixed solvent of 1.79 g of N-ethyl-2-pyrrolidone, 5.40 g of cyclopentanone, and 1.80 g of ethyl lactate to prepare a composition. Then, the mixture was filtered using a polypropylene microfilter having a pore size of 5 μm to prepare a polymer film-forming composition 1.
[0273] <Example 2>
[0274] A composition was prepared by dissolving 0.94 g of trimethylolpropane triacrylate [registered trademark] A-TMPT (manufactured by Shin-Nakamura Chemical Industry Co., Ltd., multifunctional acrylate) and 0.06 g of IRGACURE [registered trademark] OXE01 (manufactured by BASF, photopolymerization initiator) in a mixed solvent of 6.30 g of N-ethyl-2-pyrrolidone and 2.70 g of cyclopentanone. The mixture was then filtered using a polypropylene microfilter having a pore size of 5 μm to prepare a polymer film-forming composition 2.
[0275] <Comparative Example 1>
[0276] A composition was prepared by dissolving 0.94 g of trimethylolpropane triacrylate [registered trademark] A-TMPT (manufactured by Shin-Nakamura Chemical Industry Co., Ltd., multifunctional acrylate) in a mixed solvent of 6.30 g of N-ethyl-2-pyrrolidone and 2.70 g of cyclopentanone. The mixture was then filtered using a polypropylene microfilter having a pore size of 5 μm to prepare a polymer film-forming composition 3.
[0277] <Film production example 1>
[0278] A substrate having a SiO2 surface was immersed in a 10% sulfuric acid aqueous solution at room temperature for 1 minute. The substrate was then washed with pure water and ethanol and dried by nitrogen purge. Next, the polymer film-forming composition 1 prepared in Example 1 was applied to the substrate using a spin coater and baked at 130°C for 1 minute.
[0279] <Film production example 2>
[0280] A substrate having a Cu substrate surface was immersed in a 10% sulfuric acid aqueous solution at room temperature for 1 minute. Then, the substrate was washed with pure water and ethanol and dried by nitrogen purge. Next, the polymer film-forming composition 1 prepared in Example 1 was applied to the substrate using a spin coater and baked at 130°C for 1 minute.
[0281] <Film production example 3>
[0282] A substrate on which 0.5 μm and 10 μm Cu and SiO2 lines were alternately arranged was immersed in a 10% sulfuric acid aqueous solution at room temperature for 1 minute. Then, the substrate was washed with pure water and ethanol and dried by nitrogen purge. Next, the polymer film-forming composition 1 prepared in Example 1 was applied to the substrate using a spin coater and baked at 130°C for 1 minute.
[0283] Then, the substrate was washed with cyclopentanone (CYP), and finally, residue was removed by dry etching. The etcher and etching conditions used for dry etching are as follows.
[0284] RIE-200NL (manufactured by Samco Co., Ltd.), etching gas: O2, flow rate: 5 sccm, RF output: 100 W, pressure: 5 Pa, discharge time: 10 Pa
[0285] <Film production example 4>
[0286] A substrate having a SiO2 surface was immersed in a 10% sulfuric acid aqueous solution at room temperature for 1 minute. The substrate was then washed with pure water and ethanol and dried by nitrogen purge. Next, the polymer film-forming composition 2 prepared in Example 2 was applied to the substrate using a spin coater and baked at 130°C for 1 minute.
[0287] <Film production example 5>
[0288] A substrate having a Cu substrate surface was immersed in a 10% sulfuric acid aqueous solution at room temperature for 1 minute. Then, the substrate was washed with pure water and ethanol and dried by nitrogen purge. Next, the polymer film-forming composition 2 prepared in Example 2 was applied to the substrate using a spin coater and baked at 130°C for 1 minute.
[0289] <Film production example 6>
[0290] A substrate having a SiO2 surface was immersed in a 10% sulfuric acid aqueous solution at room temperature for 1 minute. The substrate was then washed with pure water and ethanol and dried by nitrogen purge. Next, the polymer film-forming composition 3 prepared in Comparative Example 1 was applied to the substrate using a spin coater and baked at 130°C for 1 minute.
[0291] <Film production example 7>
[0292] A substrate having a Cu substrate surface was immersed in a 10% sulfuric acid aqueous solution at room temperature for 1 minute. Then, the substrate was washed with pure water and ethanol and dried by nitrogen purge. Next, the polymer film-forming composition 3 prepared in Comparative Example 1 was applied to the substrate using a spin coater and baked at 130°C for 1 minute.
[0293] 〔Substrate selectivity evaluation 1〕
[0294] The substrates prepared in Film Formation Examples 1 and 2 were washed with cyclopentanone (CYP), and then visually inspected to check whether or not a film remained on the substrate.
[0295] 〔Substrate selectivity evaluation 2〕
[0296] The contact angle of a water droplet was determined by a droplet method using a contact angle meter [manufactured by Kyowa Interface Science Co., Ltd., No.: CA-W150] for the substrates prepared in Film Formation Examples 1 and 2 and the substrate used in Substrate Selectivity Evaluation 1 (a substrate prepared by washing the substrates prepared in Film Formation Examples 1 and 2 with cyclopentanone (CYP)). The results are shown in Table 1.
[0297] In the droplet method, a 3 μL water droplet was brought into contact with the substrate at room temperature, and the contact angle was measured after 3 seconds, 5 seconds, and 7 seconds. Each measurement was performed three times, and the average value was used.
[0298] [Table 1]
[0299]
[0300] As shown in Table 1, in the substrate on which the polymer film-forming composition 1 prepared in Example 1 was coated / baked, when the substrate surface was Cu (Film Forming Example 2), it was visually confirmed that the film remained even after washing with cyclopentanone (CYP), but when the substrate surface was SiO2 (Film Forming Example 1), it was visually confirmed that the film did not remain after washing with cyclopentanone (CYP).
[0301] In addition, when the substrate surface is SiO2 (film forming example 1), the contact angle changes significantly before and after washing with cyclopentanone (CYP). This can be said to reflect that the surface state of the substrate changes significantly by washing with CYP, that is, the film formed by the polymer film-forming composition 1 disappears by washing with CYP.
[0302] On the other hand, when the substrate surface is Cu (film forming example 2), the contact angle hardly changes before and after washing with cyclopentanone (CYP), and a high contact angle is shown. This can be said to reflect that the surface state of the substrate does not change after washing with CYP, that is, the film formed by the polymer film-forming composition 1 remains.
[0303] From these results, it can be confirmed that, as for the contact angle measurement results, the film was formed using the polymer film-forming composition 1 prepared in Example 1, so that when the substrate surface was Cu, the film remained after CYP washing, and when the substrate surface was SiO2, the film disappeared.
[0304] 〔Substrate selectivity evaluation 3〕
[0305] The untreated substrate on which the Cu and SiO2 lines used in Film Formation Example 3 were alternately arranged and the substrate prepared in Film Formation Example 3 (the substrate treated with coating / baking, CYP washing and dry etching of the polymer film-forming composition 1) were observed with a scanning electron microscope (SEM, manufactured by Hitachi High-Tech, Regulus (registered trademark) 8240) in a cross section perpendicular to the substrate. The observation results for the untreated substrate are shown in FIG. Figure 1 The observation results of the substrate prepared in Film Formation Example 3 are shown in Figure 2 middle.
[0306] like Figure 1 As shown in FIG. 1 , it can be confirmed that the top of the Cu portion of the untreated substrate is lower than the top of the adjacent SiO2 portion. Figure 2 As shown, it can be confirmed that for the substrate treated using the polymer film-forming composition 1 prepared in Example 1 (substrate produced in Film Formation Example 3), a film is formed on the Cu portion and is higher (bulging) than the top of the adjacent SiO2 portion.
[0307] 〔Substrate selectivity evaluation 4〕
[0308] The substrates prepared in Film Formation Examples 4 to 7 were washed with propylene glycol monomethyl ether acetate (PGMEA), and then visually checked for appearance to confirm whether or not a film remained on the substrate.
[0309] [Table 2]
[0310]
[0311] As shown in Table 2, in the substrate on which the polymer film-forming composition 2 prepared in Example 2 was coated / baked, when the substrate surface was Cu (Film Forming Example 5), it was visually confirmed that the film remained even after washing with propylene glycol monomethyl ether acetate (PGMEA), but when the substrate surface was SiO2 (Film Forming Example 4), it was visually confirmed that the film did not remain after washing with propylene glycol monomethyl ether acetate (PGMEA).
[0312] On the other hand, in the substrate on which the polymer film-forming composition 3 prepared in Comparative Example 1 was coated / baked, even when the substrate surface was Cu (Film Forming Example 7), it was visually confirmed that no film remained after washing with propylene glycol monomethyl ether acetate (PGMEA). In addition, when the substrate surface was SiO2 (Film Forming Example 6), it was also visually confirmed that no film remained after washing with propylene glycol monomethyl ether acetate (PGMEA).
[0313] As described above, the results of substrate selectivity evaluations 1 to 4 confirm that by using polymer film forming composition 1 and polymer film forming composition 2 prepared in Example 1 and Example 2, a film can be selectively formed according to the type (material) of the substrate surface on which the film is formed, that is, a film can be positionally selectively formed according to the material of the underlying substrate surface.
[0314] Industrial Availability
[0315] According to the polymer film-forming composition of the present invention, a polymer film can be selectively formed according to the material of the substrate surface.
Claims
1. A composition for forming a polymer film, which is used for selectively forming a polymer film on region RI of a substrate having a region RI whose surface is formed of a metal (I) and a region R-II whose surface is formed of a material (II) different from the metal (I), The polymer film-forming composition includes a radical generator (A) and a radical addition-reactive compound (B).
2. A composition for forming a polymer film, which is used for selectively forming a polymer film on region RI of a substrate having a region RI whose surface is formed of a metal (I) and a region R-II whose surface is formed of a material (II) different from the metal (I), The polymer film-forming composition comprises a radical generator (A) and a radical addition-reactive compound (B), and The substrate is heated and is composed of a component composition whose curing property is higher in the region RI than in the region R-II. 3 . The polymer film-forming composition according to claim 1 , wherein the radical generator (A) is a radical generator containing a sulfur atom. 4 . The polymer film-forming composition according to claim 1 , wherein the radical generator (A) is an oxime ester radical generator.
5. The polymer film-forming composition according to any one of claims 1 to 4, wherein the radical generator (A) is a radical generator represented by the following formula (1): In the formula, R 1 and R 3 Each is independently a phenyl group which may be substituted, an aromatic heterocyclic group which may be substituted with 5 to 10 members, or an alkyl group which may be substituted with 1 to 10 carbon atoms, wherein the substituent in the phenyl group, the aromatic heterocyclic group or the alkyl group may contain a sulfur atom, R 2 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may be substituted, wherein the substituent in the alkyl group may include a sulfur atom, n is 0 or 1, The wavy line represents either E or Z geometric isomers or a mixture thereof. The polymer film-forming composition according to any one of claims 1 to 5, wherein the radical addition-reactive compound (B) is at least one polymer selected from the group consisting of polyimide, polyamic acid, and polyamic acid ester having a radical addition-reactive double bond in a molecule.
7. The polymer film-forming composition according to any one of claims 1 to 6, wherein the radical addition-reactive compound (B) is at least one selected from polyimide precursors having a unit structure represented by the following formula (2), In the formula, X 1 is a 4-valent organic group, Y 1 is a divalent organic group, R 4 and R 5 are each independently a hydrogen atom or a monovalent organic group, wherein The R 4 and R 5 At least one of them is a group represented by formula (3); In the formula, R 6 , R 7 and R 8 Each is independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, m is an integer of 1 to 10, and * represents a bonding position to the oxygen atom in the above formula (2). 8 . The polymer film-forming composition according to claim 1 , wherein the radical addition-reactive compound (B) is at least one selected from the group consisting of a (meth)acrylate compound and a vinyl compound. 9 . The polymer film-forming composition according to claim 1 , wherein the metal (I) is copper, an alloy containing copper, titanium, or an alloy containing titanium.
10. The polymer film-forming composition according to any one of claims 1 to 9, wherein the material (II) is at least one selected from the group consisting of SiO2, SiN, SiC, SiOC, SiCN, Ta, TaN, Ti and TiN.
11. A method for selectively forming a polymer film on a surface of a substrate, The surface has a region RI formed of a metal (I), and a region R-II adjacent to the region RI and formed of a material (II) different from the metal (I), The selective polymer film forming method comprises the following steps: a polymer film forming step of applying a polymer film-forming composition comprising a radical generator (A) and a radical addition-reactive compound (B) to the surface and heating the composition to form a polymer film; and Next, a step is performed in which the substrate surface is brought into contact with a solvent (C) to remove the coating material on the region R-II.
12. The selective polymer film forming method according to claim 11, further comprising the step of removing residues on the region R-II by dry etching after the step of removing the coating material on the region R-II.
13. A method for forming a thin film, comprising: selectively forming a thin film on a region R-II in a substrate having a region RI formed of a metal (I) and a region R-II formed of a material (II) different from the metal (I) by an atomic layer deposition method, the method comprising the following steps: A step of forming a thin film by atomic layer deposition on the surface of the substrate having the polymer film formed in the region RI by the selective polymer film forming method according to claim 11 or 12. 14 . The thin film forming method according to claim 13 , further comprising, after the step of forming the thin film, a step of removing the polymer film on the region RI formed of the metal (I).
15. A laminate having a plurality of regions formed on a surface of a substrate, The region includes a region RI formed of metal (I), and a region R-II adjacent to the region RI and formed of a material (II) different from the metal (I). A polymer film formed from the polymer film-forming composition according to any one of claims 1 to 10 is present on the region RI, The region R-II does not have the polymer film.