Positive electrode composition and method for producing same, positive electrode and method for producing same, and battery

By using a composition of carbon black and carbon nanotubes in the positive electrode of a lithium-ion secondary battery and by selecting appropriate dispersant, the problems of high internal resistance and insufficient performance are solved, and better discharge rate and cycling characteristics are achieved. , improving the overall performance of the battery.

CN118946981APending Publication Date: 2024-11-12DENKA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030551.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-01-17
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The positive electrode of the existing lithium-ion secondary battery has problems such as high internal resistance, insufficient discharge rate characteristics and cycle characteristics in terms of improving performance.

Method used

Using a positive electrode composition containing carbon black and carbon nanotubes, the ideal dispersion state of carbon black and carbon nanotubes in the positive electrode composition is ensured by selecting a suitable dispersant for conductive materials at different SP values, thereby improving conductivity. and battery performance.

Benefits of technology

The internal resistance reduction, discharge rate characteristics and cycle characteristics of lithium-ion secondary batteries are achieved, extending the service life of the battery and improving the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005060617830000501
    Figure BDA0005060617830000501
  • Figure BDA0005060617830000502
    Figure BDA0005060617830000502
  • Figure BDA0005060617830000511
    Figure BDA0005060617830000511
Patent Text Reader

Abstract

A positive electrode composition containing a conductive material, an active material, a binder, a dispersant for the conductive material, and a liquid medium, the conductive material containing carbon black and carbon nanotubes, the dispersant for the conductive material containing two or more types of dispersants having different SP values, and the carbon black having a BET specific surface area of 100-500 m2 / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive electrode composition and a method for producing the same, a positive electrode and a method for producing the same, and a battery. Background Art

[0002] As environmental and energy issues intensify, the development of technologies to reduce dependence on fossil fuels and realize a low-carbon society is being actively promoted. Such technological developments include the development of low-emission vehicles such as hybrid electric vehicles and electric vehicles, the development of natural energy power generation and storage systems such as solar power generation and wind power generation, and the development of a next-generation power transmission network that efficiently supplies electricity and reduces transmission losses.

[0003] One of the key devices that is common and necessary in these technologies is a battery. For such a battery, a high energy density is required in order to miniaturize the system. In addition, a high output characteristic is required in order to be able to provide a stable power supply without being affected by the ambient temperature of use. In addition, good cycle characteristics that can withstand long-term use are also required. Therefore, the replacement of the previous lead-acid batteries, nickel-cadmium batteries, and nickel-hydrogen batteries to lithium-ion secondary batteries with higher energy density, output characteristics, and cycle characteristics is being rapidly carried out.

[0004] In the past, the positive electrode of a lithium-ion secondary battery was manufactured by applying a positive electrode paste containing a positive electrode active material, a conductive material, and a binding material (also referred to as a binder) to a current collector. As the positive electrode active material, lithium-containing composite oxides such as lithium cobalt oxide and lithium manganese oxide are used. In addition, the conductivity of the positive electrode active material is insufficient, so in order to impart conductivity, an operation of adding a conductive material such as carbon black to the positive electrode paste is implemented (for example, Patent Document 1).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2008-227481 Summary of the invention

[0008] Problems to be solved by the invention

[0009] In recent years, further improvement in the performance of lithium ion secondary batteries has been required.

[0010] The object of the present invention is to provide a positive electrode composition of a lithium ion secondary battery having a small internal resistance and excellent discharge rate characteristics and cycle characteristics, and a method for manufacturing the positive electrode composition. In addition, the object of the present invention is to provide a positive electrode of a lithium ion secondary battery having a small internal resistance and excellent discharge rate characteristics and cycle characteristics, and a method for manufacturing the positive electrode. In addition, the object of the present invention is to provide a battery having the above-mentioned positive electrode.

[0011] Means for solving problems

[0012] The present invention relates to, for example, the following <1> ~ <15> .

[0013] <1> A positive electrode composition comprising a conductive material, an active material, a binder, a conductive material dispersant and a liquid medium, wherein the conductive material comprises carbon black and carbon nanotubes, the conductive material dispersant comprises two or more dispersants having different SP values, and the carbon black has a BET specific surface area of ​​100 to 500 m 2 / g.

[0014] <2> like <1> In the positive electrode composition, the ratio (mass ratio) of the content of the carbon nanotubes to the total content of the carbon black and the carbon nanotubes is 0.1 to 0.7.

[0015] <3> like <1> or <2> In the positive electrode composition, the conductive material dispersant is selected from the group consisting of polyvinyl alcohol, polyvinyl pyrrolidone, polyvinyl butyral, carboxymethyl cellulose and its salts, polyvinyl acetal, polyvinyl acetate, polyvinyl amine and polyvinyl formal.

[0016] <4> like <1> ~ <3> The positive electrode composition according to any one of the preceding claims, wherein the carbon black has 100 to 400 m 2 / g BET specific surface area, and The crystallite size (Lc).

[0017] <5> like <1> ~ <4> The positive electrode composition described in any one of the preceding claims, wherein the carbon nanotubes have an average diameter of 5 to 15 nm.

[0018] <6> A method for manufacturing a positive electrode composition comprises the following steps: a first step of mixing a first agent containing a binding material and a first liquid medium, a second agent containing carbon black, a dispersant for a first conductive material and a second liquid medium, and a third agent containing carbon nanotubes, a dispersant for a second conductive material and a third liquid medium to obtain a mixed liquid; and a second step of mixing the mixed liquid and an active material to obtain a positive electrode composition, wherein the dispersant for the first conductive material has an SP value different from the SP value of the dispersant for the second conductive material.

[0019] <7> A method for manufacturing a positive electrode composition, comprising the following steps: a first step of mixing a first agent containing a binding material and a first liquid medium and a second agent containing carbon black, a dispersant for a first conductive material and a second liquid medium to obtain a first mixed liquid; a second step of mixing the first mixed liquid and a third agent containing carbon nanotubes, a dispersant for a second conductive material and a third liquid medium to obtain a second mixed liquid; and a third step of mixing the second mixed liquid and an active material to obtain a positive electrode composition, wherein the dispersant for the first conductive material has an SP value different from the SP value of the dispersant for the second conductive material.

[0020] <8> like <6> or <7> In the manufacturing method, the SP value of the first conductive material dispersant is higher than the SP value of the second conductive material dispersant.

[0021] <9> like <6> ~ <8> The production method according to any one of the preceding claims, wherein the ratio (mass ratio) of the content of the carbon nanotubes to the total content of the carbon black and the carbon nanotubes is 0.1 to 0.7.

[0022] <10> like <6> ~ <9> The manufacturing method described in any one of the above, wherein the first conductive material dispersant and the second conductive material dispersant are respectively selected from the group consisting of polyvinyl alcohol, polyvinyl pyrrolidone, polyvinyl butyral, carboxymethyl cellulose and its salts, polyvinyl acetal, polyvinyl acetate, polyvinyl amine and polyvinyl formal.

[0023] <11> A method for manufacturing a positive electrode, comprising the following steps: <1> ~ <5> The positive electrode composition described in any one of the above is applied on a current collector to form a composite material layer containing the conductive material, the active material, the binder, and the conductive material dispersant on the current collector.

[0024] <12> A positive electrode comprising a composite material layer, wherein the composite material layer comprises a conductive material, an active material, a binder and a conductive material dispersant, wherein the conductive material comprises carbon black and carbon nanotubes, the conductive material dispersant comprises two or more dispersants having different SP values, and the carbon black has a BET specific surface area of ​​100 to 500 m 2 / g.

[0025] <13> like <12> In the positive electrode, the ratio (mass ratio) of the content of the carbon nanotubes to the total content of the carbon black and the carbon nanotubes is 0.1 to 0.7.

[0026] <14> like <12> or <13> In the positive electrode, the conductive material dispersant is selected from the group consisting of polyvinyl alcohol, polyvinyl pyrrolidone, polyvinyl butyral, carboxymethyl cellulose and its salts, polyvinyl acetal, polyvinyl acetate, polyvinyl amine and polyvinyl formal.

[0027] <15> A battery having <12> ~ <14> The positive electrode according to any one of the above.

[0028] Effects of the Invention

[0029] According to the present invention, a positive electrode composition of a lithium ion secondary battery having a small internal resistance and excellent discharge rate characteristics and cycle characteristics, and a method for manufacturing the positive electrode composition can be provided. In addition, according to the present invention, a positive electrode of a lithium ion secondary battery having a small internal resistance and excellent discharge rate characteristics and cycle characteristics, and a method for manufacturing the positive electrode can be provided. In addition, according to the present invention, a battery having the above-mentioned positive electrode can be provided. DETAILED DESCRIPTION

[0030] Hereinafter, preferred embodiments of the present invention will be described in detail.

[0031] (Positive Electrode Composition)

[0032] The positive electrode composition of this embodiment contains a conductive material, an active material, a binder, a dispersant for a conductive material, and a liquid medium. The positive electrode composition of this embodiment is a dispersion liquid for forming a positive electrode, and may also be referred to as a positive electrode forming composition, a positive electrode forming dispersion liquid, or a positive electrode forming coating liquid.

[0033] In the positive electrode composition of this embodiment, the conductive material contains a BET specific surface area of ​​100 to 500 m 2 / g of carbon black, and carbon nanotubes. In the positive electrode composition of the present embodiment, the conductive material dispersant contains two or more dispersants having different SP values.

[0034] According to the positive electrode composition of this embodiment, a lithium ion secondary battery having low internal resistance and excellent discharge rate characteristics and cycle characteristics can be realized.

[0035] In this embodiment, carbon black and carbon nanotubes are conductive materials. The basic function of conductive materials is to impart conductivity to active materials with insufficient conductivity. In addition, lithium-ion secondary batteries expand and contract active materials due to repeated charge and discharge, thereby gradually losing the contact points between active materials. The conductive material also has the function of connecting active materials that have lost their contact points to each other and preventing the conductivity from being damaged.

[0036] According to the opinion of the inventors of the present application, it is believed that by containing two or more conductive material dispersants with different SP values ​​in the positive electrode composition of the present embodiment, carbon black and carbon nanotubes as conductive materials are dispersed in an ideal dispersed state in the positive electrode composition. It should be noted that in the case of poor dispersion of the conductive material, the active material and the conductive material cannot be fully contacted, it becomes difficult to form a conductive path, and the performance of the active material cannot be fully utilized. As a result, it is believed that a portion with poor conductivity appears locally in the positive electrode, so the active material cannot be fully utilized, the discharge capacity is reduced, and the life of the battery is shortened. In contrast, it is believed that in the positive electrode composition of the present embodiment, since the conductive material is dispersed in an ideal dispersed state, the above-mentioned problems will not occur, and excellent discharge rate characteristics and cycle characteristics can be achieved.

[0037] The carbon black may be carbon black used as a common conductive material for batteries, and may be acetylene black, furnace black, channel black, etc. The carbon black is preferably acetylene black from the viewpoint of excellent purity and easy acquisition of excellent battery characteristics.

[0038] The BET specific surface area of ​​carbon black is 100 m 2 / g or more. By making the BET specific surface area of ​​carbon black 100m 2 / g or more, so that the electrical contact points with the active material and the conductive material are increased, the conductivity imparting effect becomes better, and thus more excellent battery characteristics can be obtained. From the viewpoint of making the internal resistance smaller and the discharge rate characteristics and cycle characteristics better, the BET specific surface area of ​​carbon black is preferably 120m 2 / g or more, more preferably 140m 2 / g or more, more preferably 160m 2 / g or more, can also be 180m 2 / g or more, 200m 2 / g or above or 220m 2 / g or above.

[0039] In addition, the BET specific surface area of ​​carbon black is 500 m 2 / g or less. If the BET specific surface area of ​​carbon black is 500m 2 / g or less, the interaction between the liquid medium and the conductive material, and the interaction between the conductive materials become smaller, and it is easy to disperse evenly in the active material. As a result, it is easy to form a conductive path and obtain better battery characteristics. From the perspective of making the internal resistance smaller and the discharge rate characteristics and cycle characteristics better, the BET specific surface area of ​​carbon black is preferably 450m 2 / g or less, more preferably 400m 2 / g or less, can also be 350m 2 / g or less, 300m 2 / g or below or 250m 2 / g or less.

[0040] That is, the BET specific surface area of ​​carbon black may be, for example, 100 to 500 m 2 / g, 100~450m 2 / g, 100~400m 2 / g, 100~350m 2 / g, 100~300m 2 / g, 100~250m 2 / g, 120~500m 2 / g, 120~450m 2 / g, 120~400m 2 / g, 120~350m 2 / g, 120~300m 2 / g, 120~250m 2 / g, 140~500m 2 / g, 140~450m 2 / g, 140~400m 2 / g, 140~350m 2 / g, 140~300m 2 / g, 140~250m 2 / g, 160~500m 2 / g, 160~450m 2 / g, 160~400m 2 / g, 160~350m 2 / g, 160~300m 2 / g, 160~250m 2 / g, 180~500m 2 / g, 180~450m 2 / g, 180~400m 2 / g, 180~350m 2 / g, 180~300m 2 / g, 180~250m 2 / g, 200~500m 2 / g, 200~450m 2 / g, 200~400m 2 / g, 200~350m 2 / g, 200~300m 2 / g, 200~250m 2 / g, 220~500m 2 / g, 220~450m 2 / g, 220~400m 2 / g, 220~350m 2 / g, 220~300m 2 / g or 220~250m 2 / g.

[0041] The BET specific surface area of ​​carbon black can be measured by a static volumetric method using nitrogen as an adsorbent in accordance with JIS Z8830.

[0042] The crystallite size (Lc) of carbon black is preferably By making the crystallite size (Lc) As a result, the π electrons become easier to move in the crystal layer, and it is easier to form a conductive path for the electrons flowing out of the collector to be transported to the active material, thereby obtaining better battery characteristics. The crystallite size (Lc) of carbon black can also be above, Above or above.

[0043] In addition, the crystallite size (Lc) of carbon black is preferably By making the crystallite size (Lc) The carbon black particles are more likely to be rounded, so the interaction between particles is reduced, and the particles are more easily dispersed in the active material, thereby forming a conductive path more easily and obtaining better battery characteristics. From the perspective of making the internal resistance smaller and the discharge rate characteristics and cycle characteristics better, the crystallite size (Lc) of the carbon black is preferably The following can also be Below or the following.

[0044] That is, the crystallite size (Lc) of carbon black can be, for example,

[0045] or

[0046] The crystallite size (Lc) of carbon black can be measured in accordance with JIS R 7651. The crystallite size (Lc) of carbon black refers to the crystallite size in the c-axis direction of the carbon black crystal layer.

[0047] The average primary particle size of carbon black is preferably 15 nm or more. By making the average primary particle size of carbon black 15 nm or more, the interaction between the liquid medium and the conductive material, and the interaction between the conductive materials become smaller, thereby making it easier to disperse more evenly in the active material, forming a conductive path, and more easily obtaining excellent battery characteristics. The average primary particle size of carbon black can also be 16 nm or more, 17 nm or more, 18 nm or more, 19 nm or more, or 20 nm or more.

[0048] In addition, the average primary particle size of carbon black is preferably 30 nm or less. By making the average primary particle size of carbon black 30 nm or less, the electrical contacts with the active material and the conductive material are increased, and the effect of imparting conductivity becomes good, so it is easier to obtain excellent battery characteristics. From the viewpoint of making the internal resistance smaller, and the viewpoint of making the discharge rate characteristics and cycle characteristics better, the average primary particle size of carbon black is preferably 28 nm or less, and may also be 26 nm or less, 24 nm or less, 22 nm or less, or 20 nm or less.

[0049] That is, the average primary particle size of carbon black can be, for example, 15 to 30 nm, 15 to 28 nm, 15 to 26 nm, 15 to 24 nm, 15 to 22 nm, 15 to 20 nm, 16 to 30 nm, 16 to 28 nm, 16 to 26 nm, 16 to 24 nm, 16 to 22 nm, 16 to 20 nm, 17 to 30 nm, 17 to 28 nm, 17 to 26 nm, 17 to 24 nm, 17 to 2 2nm, 17-20nm, 18-30nm, 18-28nm, 18-26nm, 18-24nm, 18-22nm, 18-20nm, 19-30nm, 19-28nm, 19-26nm, 19-24nm, 19-22nm, 19-20nm, 20-30nm, 20-28nm, 20-26nm, 20-24nm or 20-22nm.

[0050] The average primary particle size of carbon black refers to the average value of the equivalent circle diameters measured based on the images of carbon black observed using a transmission electron microscope (TEM). Specifically, it can be obtained in the following manner: using a transmission electron microscope JEM-2000FX (manufactured by JEOL Ltd.), 10 images of carbon black are taken at a magnification of 100,000 times, and for the obtained images, the equivalent circle diameters of 200 randomly selected primary particles of carbon black are measured by image analysis, and the arithmetic average is taken.

[0051] When the peak area of ​​the peak with mass number m / z57 detected by the temperature rise desorption gas analysis method of carbon black is set as S1, and the peak area of ​​the peak with mass number m / z128 is set as S2, the ratio of peak area S2 to peak area S1 (S2 / S1) is preferably 0.2 to 1.9. The ratio (S2 / S1) represents the proportion of organic components adsorbed on the surface of carbon black. By making the ratio (S2 / S1) less than 1.9, the organic components adsorbed on the surface of carbon black are sufficiently reduced, and the reduction in conductivity caused by the organic components capturing π electrons can be significantly suppressed. In addition, by making the ratio (S2 / S1) more than 0.2, the organic components adsorbed on the surface of carbon black act as dispersants, and the dispersibility in the liquid medium is improved, so the slurry viscosity can be further reduced. The peak area S1 of the peak with mass number m / z57 and the peak area S2 of the peak with mass number m / z128 can be measured by evolved gas mass spectrometry (EGA-MS). For example, carbon black can be placed in a gas chromatograph-mass spectrometer with a pyrolysis device, maintained at 50°C for 5 minutes in a He gas flow under atmospheric pressure, and then heated to 800°C at a rate of 80°C / min. Mass spectrometry analysis of the components released by the temperature increase can be performed to measure the peak area S1 of the peak with a mass number m / z 57 and the peak area S2 of the peak with a mass number m / z 128.

[0052] From the viewpoint of making the internal resistance smaller and the viewpoint of making the discharge rate characteristics and the cycle characteristics better, the ratio (S2 / S1) may be 1.5 or less, 1.0 or less, 0.8 or less, 0.6 or less, 0.5 or less, 0.4 or less, or 0.3 or less. In addition, the ratio (S2 / S1) may be 0.25 or more or 0.3 or more.

[0053] That is, the ratio (S2 / S1) may be, for example, 0.2 to 1.9, 0.2 to 1.5, 0.2 to 1.0, 0.2 to 0.8, 0.2 to 0.6, 0.2 to 0.5, 0.2 to 0.4, 0.2 to 0.3, 0.25 to 1.9, 0.25 to 1.5, 0.25 to 1.0, 0.25 to 0.8, 0.25 to 0.6, 0.25 to 0.5, 0.25 to 0.4, 0.25 to 0.3, 0.3 to 1.9, 0.3 to 1.5, 0.3 to 1.0, 0.3 to 0.8, 0.3 to 0.6, 0.3 to 0.5 or 0.3 to 0.4.

[0054] From the viewpoint of excellent conductivity, the volume resistivity of carbon black may be 0.30 Ω·cm or less or 0.25 Ω·cm or less. The volume resistivity of carbon black is measured, for example, in a state where the carbon black is compressed under a load of 7.5 MPa.

[0055] The ash content and water content of carbon black are not particularly limited. The ash content of carbon black may be, for example, 0.04% by mass or less, and the water content of carbon black may be, for example, 0.10% by mass or less.

[0056] The method for producing carbon black is not particularly limited. For example, carbon black may be produced by a production method including the following steps: a synthesis step of treating a raw gas containing hydrocarbons in a cylindrical decomposition furnace to obtain carbon black; and a high purification step of removing magnetic foreign matter from the carbon black obtained in the synthesis step using a magnet.

[0057] In the synthesis process, the raw gas is processed by a cylindrical decomposition furnace. The cylindrical decomposition furnace may include, for example, a pyrolysis section for performing a pyrolysis reaction of hydrocarbons and a maturation section for modifying the pyrolysis reaction product. The cylindrical decomposition furnace may also include a supply port for supplying the raw gas to the pyrolysis section and a recovery port for recovering the generated carbon black from the maturation section.

[0058] In the pyrolysis section, the supplied raw gas is preferably retained at a temperature of 1900°C or higher for 30 to 150 seconds. By setting the retention time of the raw gas to 30 seconds or more, the formation of carbon aerosol by the completion of the pyrolysis reaction and the growth of the chain structure can be more reliably implemented. In addition, by setting the retention time of the raw gas to 150 seconds or less, the agglomeration of the carbon aerosol can be suppressed, so that it is easier to remove magnetic foreign matter in the high-purification process, and it is easy to obtain high-purity carbon black.

[0059] In the aging section, the pyrolysis reaction product supplied from the pyrolysis section is preferably retained at a temperature of 1700°C or higher for 20 to 90 seconds. By making the retention time of the pyrolysis reaction product 20 seconds or more, it is easy to obtain higher quality carbon black by utilizing the modification of the carbon aerosol and the promotion of aggregate growth. In addition, by making the retention time of the pyrolysis reaction product 90 seconds or less, the agglomeration of the carbon aerosol can be suppressed, so that it is easier to remove magnetic foreign matter in the high purification process, and it is easy to obtain high-purity carbon black.

[0060] The residence time in the pyrolysis section and the ripening section can be appropriately adjusted by adjusting the gas linear velocity of the circulating gas. Preferably, the residence time in the ripening section is shorter than the residence time in the pyrolysis section. That is, preferably, the gas linear velocity in the ripening section is faster than the gas linear velocity in the pyrolysis section.

[0061] In the present embodiment, the raw gas preferably contains acetylene as a carbon source. The content of the carbon source (e.g., acetylene) in the raw gas is, for example, 10% by volume or more, preferably 20% by volume or more, more preferably 30% by volume or more, and may also be 100% by volume. It should be noted that the content of each component in the raw gas is expressed as a volume ratio based on the volume at 100° C. and 1 atmosphere.

[0062] The raw material gas may further contain other hydrocarbons other than the carbon source (e.g., acetylene). As other hydrocarbons, for example, methane, ethane, propane, ethylene, propylene, butadiene, benzene, toluene, xylene, gasoline, kerosene, light oil, heavy oil, etc. can be cited. By adding these other hydrocarbons, the reaction temperature can be changed to increase or decrease the specific surface area of ​​carbon black. Other hydrocarbons are preferably selected from the group consisting of aromatic hydrocarbons such as benzene and toluene and unsaturated hydrocarbons such as ethylene and propylene.

[0063] When the raw material gas contains acetylene and other hydrocarbons, the content of the other hydrocarbons is, for example, 0.1 to 99 parts by volume, preferably 0.2 to 50 parts by volume, and more preferably 0.3 to 30 parts by volume relative to 100 parts by volume of acetylene.

[0064] That is, the content of other hydrocarbons relative to 100 parts by volume of acetylene can be, for example, 0.1 to 99 parts by volume, 0.1 to 50 parts by volume, 0.1 to 30 parts by volume, 0.2 to 99 parts by volume, 0.2 to 50 parts by volume, 0.2 to 30 parts by volume, 0.3 to 99 parts by volume, 0.3 to 50 parts by volume, or 0.3 to 30 parts by volume.

[0065] The raw material gas may further include water vapor gas, oxygen, hydrogen, carbon dioxide gas, etc. As these gases, it is preferred to use high-purity gases of 99.9% by volume or more. By using such high-purity gases, there is a tendency that there are few magnetic foreign matters and carbon black with stable BET specific surface area and oil absorption can be easily manufactured.

[0066] The content of water vapor gas can be, for example, 0 to 80 parts by volume, preferably 0.1 to 70 parts by volume, more preferably 1 to 60 parts by volume, and further preferably 3 to 55 parts by volume, relative to 100 parts by volume of the carbon source (e.g., acetylene) in the raw gas. If the content of water vapor gas is within the above range, the BET specific surface area of ​​carbon black tends to become larger.

[0067] That is, relative to 100 parts by volume of the carbon source (e.g., acetylene) in the raw gas, the content of water vapor gas can be, for example, 0 to 80 parts by volume, 0 to 70 parts by volume, 0 to 60 parts by volume, 0 to 55 parts by volume, 0.1 to 80 parts by volume, 0.1 to 70 parts by volume, 0.1 to 60 parts by volume, 0.1 to 55 parts by volume, 1 to 80 parts by volume, 1 to 70 parts by volume, 1 to 60 parts by volume, 1 to 55 parts by volume, 3 to 80 parts by volume, 3 to 70 parts by volume, 3 to 60 parts by volume, or 3 to 55 parts by volume.

[0068] In the synthesis step, oxygen is preferably supplied to the pyrolysis section together with the raw material gas, and more preferably supplied to the pyrolysis section by spraying oxygen from around a supply port for supplying the raw material gas to the pyrolysis section.

[0069] The cylindrical decomposition furnace preferably has an oxygen injection port near the raw gas supply port, and preferably has a plurality of injection ports arranged at equal intervals to surround the supply port. The number of injection ports is preferably 3 or more, more preferably 3 to 8.

[0070] In addition, the cylindrical decomposition furnace may also be provided with a nozzle of a multi-layer tube structure (e.g., a double-layer tube structure, a triple-layer tube structure, etc.) having a supply port for the raw gas and a nozzle for injecting oxygen from the periphery thereof. In the case of a double-layer tube structure, for example, the raw gas may be injected from the gap portion on the inner tube side, and the oxygen may be injected from the gap portion on the outer tube side. In the case of a triple-layer tube structure formed of an inner tube, a middle tube, and an outer tube, for example, oxygen may be injected from the gap portion formed by the outer wall of the middle tube and the inner wall of the outer tube, and the raw gas may be injected from the remaining gap portion.

[0071] There is no particular restriction on the amount of oxygen injected, if the yield of carbon black is not considered. Carbon black can be produced even if more oxygen is injected than necessary. For example, the amount of oxygen injected can be 0 to 300 parts by volume, 0 to 250 parts by volume, 0 to 220 parts by volume, or 0 to 200 parts by volume, relative to 100 parts by volume of the carbon source (e.g., acetylene) in the raw gas, preferably 0.1 to 190 parts by volume, more preferably 0.5 to 180 parts by volume, and further preferably 1 to 160 parts by volume. If the amount of oxygen injected increases, the BET specific surface area of ​​carbon black and the above-mentioned ratio (S1 / S2) tend to become larger, and if the amount of oxygen injected decreases, the primary particle size of carbon black tends to become larger.

[0072] That is, the injection amount of oxygen gas relative to 100 parts by volume of the carbon source (e.g., acetylene) in the raw material gas may be, for example, 0 to 300 parts by volume, 0 to 250 parts by volume, 0 to 220 parts by volume, 0 to 200 parts by volume, 0 to 190 parts by volume, 0 to 180 parts by volume, 0 to 160 parts by volume, 0.1 to 300 parts by volume, 0.1 to 250 parts by volume, 0.1 to 220 parts by volume, 0.1 to 200 parts by volume, 0.1 to 190 parts by volume, 0. 1-180 parts by volume, 0.1-160 parts by volume, 0.5-300 parts by volume, 0.5-250 parts by volume, 0.5-220 parts by volume, 0.5-200 parts by volume, 0.5-190 parts by volume, 0.5-180 parts by volume, 0.5-160 parts by volume, 1-300 parts by volume, 1-250 parts by volume, 1-220 parts by volume, 1-200 parts by volume, 1-190 parts by volume, 1-180 parts by volume or 1-160 parts by volume.

[0073] In the synthesis step, for example, the addition rate of hydrocarbons other than acetylene, the amount of oxygen injected, etc. can be adjusted to adjust the primary particle size, BET specific surface area, and crystallite size (Lc) of the obtained carbon black.

[0074] The high-purification step is a step of removing magnetic foreign matter from the carbon black obtained in the synthesis step using a magnet. The high-purification step may be, for example, a step of contacting the carbon black obtained in the synthesis step with a magnet, or placing the carbon black obtained in the synthesis step near a magnet (for example, passing the carbon black near a magnet) to remove magnetic foreign matter from the carbon black.

[0075] The maximum surface flux density of the magnet is not particularly limited, and may be, for example, 700 mT or more, preferably 1000 mT or more, and more preferably 1200 mT or more. As a result, the fine magnetic foreign matter attached to the carbon black can be more strongly adsorbed, so it is easy to obtain carbon black with a lower nickel content. The upper limit of the maximum surface flux density of the magnet is not particularly limited, and may be, for example, 1400 mT or less.

[0076] That is, the maximum surface magnetic flux density of the magnet may be, for example, 700 to 1400 mT, 1000 to 1400 mT, or 1200 to 1400 mT.

[0077] The high purification step may be a step of removing magnetic foreign matter from carbon black in such a manner that the nickel content is 50 ppb or less (preferably 40 ppb or less, more preferably 30 ppb or less, and further preferably 20 ppb or less). The lower limit of the nickel content is not particularly limited, and the nickel content in carbon black may be, for example, 1 ppb or more, and from the viewpoint of cost and productivity, may be 10 ppb or more, or 15 ppb or more.

[0078] That is, the nickel content in the carbon black after the high purification process can be, for example, 1 to 50 ppb, 1 to 40 ppb, 1 to 30 ppb, 1 to 20 ppb, 10 to 50 ppb, 10 to 40 ppb, 10 to 30 ppb, 10 to 20 ppb, 15 to 50 ppb, 15 to 40 ppb, 15 to 30 ppb or 15 to 20 ppb.

[0079] Based on the total mass of the solid components in the positive electrode composition, the content of carbon black (C1) can be, for example, 0.01% by mass or more, 0.05% by mass or more, 0.1% by mass or more, 0.2% by mass or more, 0.3% by mass or more, 0.4% by mass or more, or 0.5% by mass or more. Based on the total mass of the solid components in the positive electrode composition, the content of carbon black (C1) can be, for example, 10% by mass or less, 7% by mass or less, 5% by mass or less, 4% by mass or less, 3% by mass or less, or 2% by mass or less.

[0080] That is, based on the total mass of the solid components in the positive electrode composition, the content of carbon black (C1) can be, for example, 0.01 to 10 mass%, 0.01 to 7 mass%, 0.01 to 5 mass%, 0.01 to 4 mass%, 0.01 to 3 mass%, 0.01 to 2 mass%, 0.05 to 10 mass%, 0.05 to 7 mass%, 0.05 to 5 mass%, 0.05 to 4 mass%, 0.05 to 3 mass%, 0.05 to 2 mass%, 0.1 to 10 mass%, 0.1 to 7 mass%, 0.1 to 5 mass%, 0.1 to 4 mass%, 0.1 to 3 mass%, 0.1 to 2 mass%, 0.2 % by mass, 0.4-10% by mass, 0.4-7% by mass, 0.4-5% by mass, 0.4-4% by mass, 0.4-3% by mass, 0.4-2% by mass, 0.5-10% by mass, 0.5-7% by mass, 0.5-5% by mass, 0.5-4% by mass, 0.5-3% by mass or 0.5-2% by mass.

[0081] The carbon nanotubes preferably have an average diameter of 5 to 15 nm and a ratio of the average diameter to the BET specific surface area (average diameter / BET specific surface area) of 0.01 to 0.068 nm / (m 2 / g) of carbon nanotubes. If the average diameter of the carbon nanotubes is as small as 5 to 15 nm, and the ratio of the average diameter to the BET specific surface area is 0.01 to 0.068 nm / (m 2 / g), more conductive paths can be formed in the positive electrode.

[0082] The average diameter of the carbon nanotubes is preferably 5 nm or more. By making the average diameter of the carbon nanotubes 5 nm or more, the interaction between the liquid medium and the conductive material, and the interaction between the conductive materials become smaller, and it is easy to disperse more evenly in the active material. Thus, it is easy to form a conductive path, and more excellent battery characteristics can be obtained. The average diameter of the carbon nanotubes can also be 6 nm or more.

[0083] In addition, the average diameter of the carbon nanotubes is preferably 15 nm or less. By making the average diameter of the carbon nanotubes 15 nm or less, the electrical contacts between the active material and the conductive material become more, the effect of imparting conductivity becomes good, and it is easy to obtain more excellent battery characteristics. From the viewpoint of making the internal resistance smaller, and the viewpoint of making the discharge rate characteristics and cycle characteristics better, the average diameter of the carbon nanotubes is preferably 12 nm or less, more preferably 10 nm or less, and can also be 9 nm or less, 8 nm or less, or 7 nm or less.

[0084] That is, the average diameter of the carbon nanotubes may be 5-15 nm, 5-12 nm, 5-10 nm, 5-9 nm, 5-8 nm, 5-7 nm, 6-15 nm, 6-12 nm, 6-10 nm, 6-9 nm, 6-8 nm, or 6-7 nm.

[0085] The average diameter of carbon nanotubes refers to the average value of the diameters measured based on images of carbon nanotubes observed using a transmission electron microscope (TEM). Specifically, it can be obtained in the following manner: using a transmission electron microscope JEM-2000FX (manufactured by JEOL Ltd.), 10 images of carbon nanotubes are taken at a magnification of 200,000 times, and the diameters of 100 randomly selected carbon nanotubes are measured by image analysis of the obtained images, and the arithmetic average is taken.

[0086] The BET specific surface area of ​​the carbon nanotubes is preferably 170 to 320 m 2 / g. By making the BET specific surface area of ​​carbon nanotubes 170m 2 / g or more, the number of electrical contacts with the active material and the conductive material increases, and the effect of imparting conductivity becomes good, so it is easier to obtain excellent battery characteristics. By making the BET specific surface area of ​​carbon nanotubes 320m 2 / g or less, the carbon nanotubes are more uniformly dispersed, a conductive path is easily formed, and more excellent battery characteristics are easily obtained. The BET specific surface area of ​​the carbon nanotubes can be measured by a static capacity method using nitrogen as an adsorbent in accordance with JIS Z8830.

[0087] From the perspective of lowering the internal resistance and improving the discharge rate characteristics and cycle characteristics, the BET specific surface area of ​​carbon nanotubes can be 180 m 2 / g or more, 200m 2 / g or more, 230m 2 / g or more, 250m 2 / g or more, 280m 2 / g or above or 300m 2 From the perspective of making the internal resistance smaller and the discharge rate characteristics and cycle characteristics more excellent, the BET specific surface area of ​​the carbon nanotubes can be 300 m 2 / g or less.

[0088] That is, the BET specific surface area of ​​carbon nanotubes can be, for example, 170 to 320 m 2 / g, 170~300m 2 / g, 180~320m 2 / g, 180~300m 2 / g, 200~320m 2 / g, 200~300m 2 / g, 230~320m 2 / g, 230~300m 2 / g, 250~320m 2 / g, 250~300m 2 / g, 280~320m 2 / g, 280~300m 2 / g or 300~320m 2 / g.

[0089] The ratio of the average diameter of carbon nanotubes to the BET specific surface area (average diameter / BET specific surface area) is preferably 0.01 to 0.068 nm / (m 2 / g). The above ratio (average diameter / BET specific surface area) is the value obtained by dividing the average diameter of the carbon nanotubes by the BET specific surface area of ​​the carbon nanotubes. By setting the ratio (average diameter / BET specific surface area) to 0.01nm / (m 2 / g) or more, so that the carbon nanotubes are less entangled with each other and are more easily dispersed in the active material. As a result, it is easy to form a conductive path and obtain better battery characteristics. By making the ratio (average diameter / BET specific surface area) 0.068nm / (m 2 / g) or less, the number of carbon nanotubes per unit weight increases, and electricity can be more efficiently conducted in the entire active material, thereby obtaining more excellent battery characteristics.

[0090] From the viewpoint of making the internal resistance smaller and the discharge rate characteristics and cycle characteristics more excellent, the ratio (average diameter / BET specific surface area) can be 0.06 nm / (m 2 / g) or less, 0.04nm / (m 2 / g) or less, 0.03nm / (m 2 / g) or less than 0.02nm / (m 2 From the perspective of making the internal resistance smaller and the discharge rate characteristics and cycle characteristics more excellent, the ratio (average diameter / BET specific surface area) can be 0.02nm / (m 2 / g) or above.

[0091] That is, the ratio (average diameter / BET specific surface area) may be, for example, 0.01 to 0.068 nm / (m 2 / g)、0.01~0.06nm / (m 2 / g)、0.01~0.04nm / (m 2 / g)、0.01~0.03nm / (m 2 / g)、0.01~0.02nm / (m2 / g)、0.02~0.068nm / (m 2 / g)、0.02~0.06nm / (m 2 / g)、0.02~0.04nm / (m 2 / g) or 0.02~0.03nm / (m 2 / g).

[0092] The method for producing carbon nanotubes is not particularly limited. The carbon nanotubes may be produced, for example, by a conventionally known method for producing carbon nanotubes.

[0093] Carbon nanotubes can be produced, for example, by allowing a powdered catalyst obtained by supporting iron on magnesium oxide to be present on the entire horizontal cross-sectional surface of a vertical reactor, allowing methane to flow vertically in the reactor, allowing methane to contact the catalyst at 500 to 1200° C., and then subjecting the obtained product (unoxidized carbon nanotubes) to oxidation treatment. By such a method for producing carbon nanotubes, it is easy to obtain carbon nanotubes composed of multiple graphene layers, having an average diameter of 5 to 15 nm and a BET specific surface area of ​​160 to 300 m 2 / g of carbon nanotubes.

[0094] The oxidation treatment of the above-mentioned product can be, for example, a calcination treatment. The temperature of the calcination treatment is not particularly limited, and can be, for example, 300 to 1000°C. The temperature of the calcination treatment is affected by the atmosphere gas. Therefore, when the oxygen concentration is high, it is preferred to carry out the calcination treatment at a lower temperature, and when the oxygen concentration is low, it is preferred to carry out the calcination treatment at a higher temperature. Specifically, as the calcination treatment of the product, there can be cited a method of calcining in the atmosphere within the range of ±50°C of the combustion peak temperature of the carbon nanotubes before the oxidation treatment, and when the oxygen concentration is higher than the atmosphere, the calcination is carried out in a temperature range slightly lower than the calcination peak temperature, and when the oxygen concentration is lower than the atmosphere, a temperature range slightly higher than the calcination peak temperature is selected. In particular, when the calcination treatment of the carbon nanotubes before the oxidation treatment is carried out in the atmosphere, it is preferably carried out within the range of ±15°C of the combustion peak temperature of the carbon nanotubes before the oxidation treatment.

[0095] The oxidation treatment of the above-mentioned product may also be a treatment based on hydrogen peroxide, mixed acid, nitric acid, etc. As a method for treating the above-mentioned product with hydrogen peroxide, for example, the method of mixing the above-mentioned product in a 34.5% hydrogen peroxide aqueous solution in a manner of 0.01 to 10% by mass, and reacting at a temperature of 0 to 100° C. for 0.5 to 48 hours can be cited. In addition, as a method for treating the above-mentioned product with a mixed acid, for example, the method of mixing the above-mentioned product in a mixed solution of concentrated sulfuric acid and concentrated nitric acid (concentrated sulfuric acid: concentrated nitric acid = 3:1) in a manner of 0.01 to 10% by mass, and reacting at a temperature of 0 to 100° C. for 0.5 to 48 hours can be cited. The mixing ratio of the mixed acid (concentrated sulfuric acid: concentrated nitric acid) can be adjusted in the range of 1:10 to 10:1 according to the amount of single-walled carbon nanotubes in the above-mentioned product. Examples of the method for treating the product with nitric acid include mixing the product in nitric acid having a concentration of 40 to 80% by mass so as to give 0.01 to 10% by mass and reacting the mixture at 60 to 150° C. for 0.5 to 48 hours.

[0096] By subjecting the above product to oxidation treatment, impurities such as amorphous carbon and single-layer carbon nanotubes with low heat resistance in the product can be selectively removed, and the purity of multi-layer graphene layers, especially 2-5-layer carbon nanotubes, can be improved. At the same time, by subjecting the product to oxidation treatment, functional groups can be added to the surface of the carbon nanotubes, thereby improving the affinity with the liquid medium and additives and improving the dispersibility. Among the above oxidation treatments, treatment using nitric acid is preferred.

[0097] The above oxidation treatment may be performed immediately after obtaining the carbon nanotubes before oxidation treatment, or after other purification treatments. For example, when iron / magnesium oxide is used as a catalyst, purification treatment using an acid such as hydrochloric acid may be performed to remove the catalyst before oxidation treatment, and then oxidation treatment may be performed; purification treatment may also be performed after oxidation treatment to remove the catalyst.

[0098] Based on the total mass of the solid components in the positive electrode composition, the content of carbon nanotubes (C2) can be, for example, 0.01% by mass or more, and from the viewpoint of making the internal resistance of the battery lower, and the viewpoint of making the discharge rate characteristics and cycle characteristics better, it can be 0.03% by mass or more, 0.05% by mass or more, 0.07% by mass or more, 0.1% by mass or more, or 0.2% by mass or more. In addition, based on the total mass of the solid components in the positive electrode composition, the content of carbon nanotubes (C2) can be, for example, 5% by mass or less, or 3% by mass or less, 2% by mass or less, 1% by mass or less, 0.9% by mass or less, 0.8% by mass or less, or 0.7% by mass or less.

[0099] That is, based on the total mass of the solid components in the positive electrode composition, the content (C2) of the carbon nanotubes can be, for example, 0.01 to 5 mass%, 0.01 to 3 mass%, 0.01 to 2 mass%, 0.01 to 1 mass%, 0.01 to 0.9 mass%, 0.01 to 0.8 mass%, 0.01 to 0.7 mass%, 0.03 to 5 mass%, 0.03 to 3 mass%, 0.03 to 2 mass%, 0.03 to 1 mass%, 0.03 to 0.9 mass%, 0.03 to 0.8 mass%, 0.03 to 0.7 mass%, 0.05 to 5 mass%, 0.05 to 3 mass%, 0.05 to 2 mass%, 0.05 to 1 mass%, 0.05 to 0.9 mass%, %, 0.05-0.8 mass%, 0.05-0.7 mass%, 0.07-5 mass%, 0.07-3 mass%, 0.07-2 mass%, 0.07-1 mass%, 0.07-0.9 mass%, 0.07-0.8 mass%, 0.07-0.7 mass%, 0.1-5 mass%, 0.1-3 mass%, 0.1-2 mass%, 0.1-1 mass%, 0.1-0.9 mass%, 0.1-0.8 mass%, 0.1-0.7 mass%, 0.2-5 mass%, 0.2-3 mass%, 0.2-2 mass%, 0.2-1 mass%, 0.2-0.9 mass%, 0.2-0.8 mass% or 0.2-0.7 mass%.

[0100] Based on the total mass of the solid components in the positive electrode composition, the total content of carbon black and carbon nanotubes (C1+C2) can be, for example, 0.5% by mass or more, and from the viewpoint of lowering the internal resistance of the battery, and from the viewpoint of better discharge rate characteristics and cycle characteristics, it can be 0.75% by mass or more, 1.0% by mass or more, or 2.0% by mass or more. In addition, based on the total mass of the solid components in the positive electrode composition, the total content of carbon black and carbon nanotubes (C1+C2) can be, for example, 5.0% by mass or less, and from the viewpoint of improving the dispersibility of the conductive material in the positive electrode composition, it can be 4.5% by mass or less, 3.5% by mass or less, or 3.0% by mass or less.

[0101] That is, based on the total mass of the solid components in the positive electrode composition, the total content of carbon black and carbon nanotubes (C1+C2) can be, for example, 0.5-5.0 mass%, 0.5-4.5 mass%, 0.5-3.5 mass%, 0.5-3.0 mass%, 0.75-5.0 mass%, 0.75-4.5 mass%, 0.75-3.5 mass%, 0.75-3.0 mass%, 1.0-5.0 mass%, 1.0-4.5 mass%, 1.0-3.5 mass%, 1.0-3.0 mass%, 2.0-5.0 mass%, 2.0-4.5 mass%, 2.0-3.5 mass% or 2.0-3.0 mass%.

[0102] The ratio (C2 / (C1+C2)) of the carbon nanotube content (C2) to the total content of carbon black and carbon nanotubes (C1+C2) can be, for example, greater than 0.05. From the viewpoint of lowering the internal resistance of the battery and improving the discharge rate characteristics and cycle characteristics, it can be greater than 0.07, greater than 0.1, greater than 0.2 or greater than 0.3.

[0103] In addition, the ratio of the carbon nanotube content (C2) to the total content of carbon black and carbon nanotubes (C1+C2) (C2 / (C1+C2)) can be, for example, less than 0.8, and from the viewpoint of improving the dispersibility of the conductive material in the positive electrode composition, can be less than 0.75, less than 0.7, less than 0.6 or less than 0.5.

[0104] That is, the ratio of the content of carbon nanotubes (C2) to the total content of carbon black and carbon nanotubes (C1+C2) (C2 / (C1+C2)) can be, for example, 0.05 to 0.8, 0.05 to 0.75, 0.05 to 0.7, 0.05 to 0.6, 0.05 to 0.5, 0.07 to 0.8, 0.07 to 0.75, 0.07 to 0.7, 0.07 to 0.6 , 0.07~0.5, 0.1~0.8, 0.1~0.75, 0.1~0.7, 0.1~0.6, 0.1~0.5, 0.2~0.8, 0.2~0.75, 0.2~0.7, 0.2~0.6, 0.2~0.5, 0.3~0.8, 0.3~0.75, 0.3~0.7, 0.3~0.6 or 0.3~0.5.

[0105] The positive electrode composition of the present embodiment may further contain other conductive materials in addition to carbon black and carbon nanotubes. Examples of other conductive materials include Ketjen black, graphite, graphene, activated carbon, and fullerene.

[0106] Based on the total amount of the conductive material, the content of other conductive materials may be, for example, 10% by mass or less, 5% by mass or less, 3% by mass or less, 1% by mass or less, or 0% by mass. That is, based on the total amount of the conductive material, the total amount of carbon black and carbon nanotubes may account for, for example, 90% by mass or more, 95% by mass or more, 97% by mass or more, 99% by mass or more, 99.5% by mass or more, or 100% by mass in the conductive material.

[0107] The active material may be a material that can reversibly absorb and release cations. The active material may also be called a positive electrode active material. For example, the active material may have a volume resistivity of 1×10 4Ω·cm or more, a lithium-containing composite oxide containing manganese, or a polyanion compound containing lithium. Examples of lithium-containing composite oxides containing manganese include LiMnO2, LiMnO3, LiMn2O3, Li 1+x Mn 2-x O4 (where x = 0 to 0.33) and other lithium manganese oxides; LiMn x Ni y Co z O2 (where x+y+z=1, 0≤y<1, 0≤z<1, 0≤x<1), Li 1+x Mn 2-x-y M y O4 (where x = 0 to 0.33, y = 0 to 1.0, 2-xy>0), LiMn 2- x M x O2 (where x = 0.01 to 0.1), Li2Mn3MO8 and other composite oxides containing one or more transition metal elements. Examples of polyanionic compounds containing lithium include polyanionic compounds such as LiFePO4, LiMnPO4, and Li2MPO4F (where M is at least one metal selected from Co, Ni, Fe, Cr, and Zn). M in each composition formula is at least one selected from the group consisting of Fe, Co, Ni, Al, Cu, Mg, Cr, Zn, and Ta.

[0108] From the viewpoint that the bonding between the conductive material and the binder is sufficiently excellent and a battery with better cycle characteristics can be easily obtained, the average particle size (D 50 ) can be 20 μm or less or 10 μm or less. The average particle size (D 50 ) can also be 100 nm or more. The average particle size (D 50 ) can be measured using laser scattering.

[0109] Based on the total mass of the solid components in the positive electrode composition, the content of the active material can be, for example, 80% by mass or more, and from the viewpoint of further improving the battery characteristics, it is preferably 85% by mass or more, and can also be 87% by mass or more, 90% by mass or more, 92% by mass or more, or 95% by mass. In addition, based on the total mass of the solid components in the positive electrode composition, the content of the active material can be, for example, 99.9% by mass or less, and can also be 99.5% by mass or less, 99% by mass or less, or 98% by mass or less.

[0110] That is, based on the total mass of the solid components in the positive electrode composition, the content of the active material can be, for example, 80-99.9 mass%, 80-99.5 mass%, 80-99 mass%, 80-98 mass%, 85-99.9 mass%, 85-99.5 mass%, 85-99 mass%, 85-98 mass%, 87-99.9 mass%, 87-99.5 mass%, 87-99 mass%, 87-98 mass%, 90-99.9 mass%, 90-99.5 mass%, 90-99 mass%, 90-98 mass%, 92-99.9 mass%, 92-99.5 mass%, 92-99 mass%, 92-98 mass%, 95-99.9 mass%, 95-99.5 mass%, 95-99 mass% or 95-98 mass%.

[0111] As the bonding material, for example, polyvinylidene fluoride, polytetrafluoroethylene, styrene butadiene copolymer, (meth) acrylate copolymer can be cited. The structure of the polymer of the bonding material can be, for example, a random copolymer, an alternating copolymer, a graft copolymer, a block copolymer, etc. As the bonding material, from the viewpoint of excellent voltage resistance, polyvinylidene fluoride is preferably used.

[0112] Based on the total mass of the solid components in the positive electrode composition, the content of the binding material can be, for example, 0.3% by mass or more, and from the viewpoint of further improving the bonding property of the positive electrode plate and better cycle characteristics, it can also be 0.5% by mass or more, 1.0% by mass or more, or 1.5% by mass or more. Based on the total mass of the solid components in the positive electrode composition, the content of the binding material can be, for example, 5.0% by mass or less, and from the viewpoint of making the resistance of the positive electrode plate smaller and the discharge rate characteristics further improved, it can also be 4.5% by mass or less, 4.0% by mass or less, or 3.5% by mass or less.

[0113] That is, based on the total mass of the solid components in the positive electrode composition, the content of the binding material can be, for example, 0.3-5.0 mass%, 0.3-4.5 mass%, 0.3-4.0 mass%, 0.3-3.5 mass%, 0.5-5.0 mass%, 0.5-4.5 mass%, 0.5-4.0 mass%, 0.5-3.5 mass%, 1.0-5.0 mass%, 1.0-4.5 mass%, 1.0-4.0 mass%, 1.0-3.5 mass%, 1.5-5.0 mass%, 1.5-4.5 mass%, 1.5-4.0 mass% or 1.5-3.5 mass%.

[0114] Examples of the liquid medium include water, N-methyl-2-pyrrolidone (hereinafter also referred to as "NMP"), cyclohexane, methyl ethyl ketone, methyl isobutyl ketone, etc. Among them, N-methyl-2-pyrrolidone is preferred from the viewpoint of dispersibility.

[0115] The dispersant for the conductive material may be any component having a function of assisting the dispersion of the conductive material (carbon black and carbon nanotubes) in the liquid medium.

[0116] Examples of the dispersant for the conductive material include polymer dispersants and low molecular weight dispersants. From the viewpoint of long-term dispersion stability of the conductive material, polymer dispersants are preferred.

[0117] The positive electrode composition of this embodiment contains two or more dispersants having different SP values ​​as the conductive material dispersant, that is, the positive electrode composition of this embodiment contains a first conductive material dispersant and a second conductive material dispersant having an SP value different from that of the first conductive material dispersant.

[0118] For example, the first conductive material dispersant may be a carbon black dispersant, and the second conductive material dispersant may be a carbon nanotube dispersant. In this case, carbon black has a lower affinity with the liquid medium than carbon nanotubes, and therefore, the first conductive material dispersant preferably has a higher SP value than the second conductive material dispersant. Thus, it is also possible to achieve an effect of suppressing the aggregation between carbon black and carbon nanotubes. From the viewpoint of lowering the internal resistance of the battery, and of achieving better discharge rate characteristics and cycle characteristics, the difference between the SP value of the first conductive material dispersant and the SP value of the second conductive material dispersant is preferably 1 J / cm 3 More preferably 3J / cm 3 More preferably, 5 J / cm 3 The difference between the SP value of the first conductive material dispersant and the SP value of the second conductive material dispersant is preferably 30 J / cm 3 Below, more preferably 20 J / cm 3 Below, more preferably 15 J / cm 3 That is, it can be 1 to 30 J / cm 3 , 1~20J / cm 3 , 1~15J / cm 3 , 3~30J / cm 3 , 3~20J / cm 3 , 3~15J / cm 3 , 5~30J / cm 3 , 5~20J / cm 3 or 5~15J / cm 3 .

[0119] In addition, in this specification, the SP value of the conductive material dispersant indicates a value calculated based on Fedor's estimation method described on page 66 of "SP Value Fundamentals, Application and Calculation Method, Published in 2006, Information Science Co., Ltd."

[0120] The conductive material dispersant may be selected from polyvinyl alcohol (SP value: 35 J / cm 3 ), polyvinyl pyrrolidone (SP value: 25J / cm 3 )、Polyvinyl butyral (SP value: 24J / cm 3 ), carboxymethyl cellulose (SP value: 21J / cm 3 ) and its salts (SP value: 29 J / cm 3 ), polyvinyl acetal (SP value: 25J / cm 3 ), polyvinyl acetate (SP value: 18J / cm 3 )、Polyvinylamine (SP value: 16J / cm 3 ) and polyvinyl formal (SP value: 26J / cm 3 ) in the group consisting of a dispersant.

[0121] Based on the total amount of the solid content of the positive electrode composition, the total content of the conductive material dispersant can be, for example, 0.03% by mass or more, and from the viewpoint of further improving the dispersibility of the conductive material, it is preferably 0.04% by mass or more, more preferably 0.05% by mass or more, and it can also be 0.06% by mass or more, 0.07% by mass or more, or 0.08% by mass or more. In addition, based on the total amount of the solid content of the positive electrode composition, the total content of the conductive material dispersant can be, for example, 1.5% by mass or less, and from the viewpoint of suppressing the decrease in conductivity caused by the insulating dispersant, it is preferably 1.0% by mass or less, more preferably 0.8% by mass or less, and it can also be 0.5% by mass or less, 0.3% by mass or less, or 0.2% by mass or less.

[0122] That is, based on the total amount of the solid content of the positive electrode composition, the total content of the dispersant for conductive material can be, for example, 0.03 to 1.5 mass%, 0.03 to 1.0 mass%, 0.03 to 0.8 mass%, 0.03 to 0.5 mass%, 0.03 to 0.3 mass%, 0.03 to 0.2 mass%, 0.04 to 1.5 mass%, 0.04 to 1.0 mass%, 0.04 to 0.8 mass%, 0.04 to 0.5 mass%, 0.04 to 0.3 mass%, 0.04 to 0.2 mass%, 0.05 to 1.5 mass%, 0.05 to 1.0 mass%, 0.05 to 0.8 mass%, 0.05 to 0.5 mass%, 0.05 to 0.3 mass%, 0.05 to 0.2 mass%, % by mass, 0.05-0.2% by mass, 0.06-1.5% by mass, 0.06-1.0% by mass, 0.06-0.8% by mass, 0.06-0.5% by mass, 0.06-0.3% by mass, 0.06-0.2% by mass, 0.07-1.5% by mass, 0.07-1.0% by mass, 0.07-0.8% by mass, 0.07-0.5% by mass, 0.07-0.3% by mass, 0.07-0.2% by mass, 0.08-1.5% by mass, 0.08-1.0% by mass, 0.08-0.8% by mass, 0.08-0.5% by mass, 0.08-0.3% by mass or 0.08-0.2% by mass.

[0123] Based on the total amount of the solid content of the positive electrode composition, the total content of the first conductive material dispersant can be, for example, 0.01% by mass or more, preferably 0.02% by mass or more, more preferably 0.025% by mass or more, and can also be 0.03% by mass or more, 0.035% by mass or more, or 0.05% by mass or more. In addition, based on the total amount of the solid content of the positive electrode composition, the total content of the first conductive material dispersant can be, for example, 1.0% by mass or less, preferably 0.8% by mass or less, more preferably 0.6% by mass or less, and can also be 0.4% by mass or less, 0.2% by mass or less, or 0.1% by mass or less from the perspective of suppressing the decrease in conductivity caused by the insulating dispersant.

[0124] That is, based on the total amount of the solid content of the positive electrode composition, the total content of the first conductive material dispersant can be, for example, 0.01 to 1.0 mass%, 0.01 to 0.8 mass%, 0.01 to 0.6 mass%, 0.01 to 0.4 mass%, 0.01 to 0.2 mass%, 0.01 to 0.1 mass%, 0.02 to 1.0 mass%, 0.02 to 0.8 mass%, 0.02 to 0.6 mass%, 0.02 to 0.4 mass%, 0.02 to 0.2 mass%, 0.02 to 0.1 mass%, 0.025 to 1.0 mass%, 0.025 to 0.8 mass%, 0.025 to 0.6 mass%, 0.025 to 0.4 mass%, 0.025 % by mass, 0.035-0.8% by mass, 0.035-0.6% by mass, 0.035-0.4% by mass, 0.035-0.2% by mass, 0.035-0.1% by mass, 0.035-1.0% by mass, 0.035-0.8% by mass, 0.035-0.6% by mass, 0.035-0.4% by mass, 0.035-0.2% by mass, 0.035-0.1% by mass, 0.05-1.0% by mass, 0.05-0.8% by mass, 0.05-0.6% by mass, 0.05-0.4% by mass, 0.05-0.2% by mass or 0.05-0.1% by mass.

[0125] Based on the total amount of the solid content of the positive electrode composition, the total content of the second conductive material dispersant can be, for example, 0.01% by mass or more, preferably 0.02% by mass or more, more preferably 0.025% by mass or more, and can also be 0.03% by mass or more, 0.035% by mass or more, or 0.05% by mass or more, based on the total amount of the solid content of the positive electrode composition. The total content of the second conductive material dispersant can be, for example, 1.0% by mass or less, and from the perspective of suppressing the decrease in conductivity caused by the insulating dispersant, preferably 0.8% by mass or less, more preferably 0.6% by mass or less, and can also be 0.4% by mass or less, 0.2% by mass or less, or 0.1% by mass or less.

[0126] That is, based on the total amount of the solid content of the positive electrode composition, the total content of the second conductive material dispersant can be, for example, 0.01 to 1.0 mass%, 0.01 to 0.8 mass%, 0.01 to 0.6 mass%, 0.01 to 0.4 mass%, 0.01 to 0.2 mass%, 0.01 to 0.1 mass%, 0.02 to 1.0 mass%, 0.02 to 0.8 mass%, 0.02 to 0.6 mass%, 0.02 to 0.4 mass%, 0.02 to 0.2 mass%, 0.02 to 0.1 mass%, 0.025 to 1.0 mass%, 0.025 to 0.8 mass%, 0.025 to 0.6 mass%, 0.025 to 0.4 mass%, 0.025 % by mass, 0.035-0.8% by mass, 0.035-0.6% by mass, 0.035-0.4% by mass, 0.035-0.2% by mass, 0.035-0.1% by mass, 0.035-1.0% by mass, 0.035-0.8% by mass, 0.035-0.6% by mass, 0.035-0.4% by mass, 0.035-0.2% by mass, 0.035-0.1% by mass, 0.05-1.0% by mass, 0.05-0.8% by mass, 0.05-0.6% by mass, 0.05-0.4% by mass, 0.05-0.2% by mass or 0.05-0.1% by mass.

[0127] The content of the liquid medium is not particularly limited and can be appropriately changed so that the solid content concentration of the positive electrode composition falls within a desired range.

[0128] The solid content concentration of the positive electrode composition is, for example, 63% by mass or more, and can be 65% by mass or more, 66% by mass or more, or 67% by mass or more from the viewpoint of shortening the time for drying the liquid medium when manufacturing the positive electrode and inhibiting the migration of the conductive material when drying the liquid medium.

[0129] In addition, the solid content concentration of the positive electrode composition is, for example, less than 82 mass %, and can be less than 80 mass %, less than 78 mass %, less than 76 mass %, less than 74 mass %, less than 72 mass % or less than 70 mass % from the viewpoint of being able to smooth the coating film when manufacturing the positive electrode and being able to reduce the deviation of the internal resistance of the battery.

[0130] That is, the solid content concentration of the positive electrode composition can be, for example, 63-82 mass%, 63-80 mass%, 63-78 mass%, 63-76 mass%, 63-74 mass%, 63-72 mass%, 63-70 mass%, 65-82 mass%, 65-80 mass%, 65-78 mass%, 65-76 mass%, 65-74 mass%, 65-72 mass%, 65-70 mass%, 66-82 mass%, 66-80 mass%, 66-78 mass%, 66-76 mass%, 66-74 mass%, 66-72 mass%, 66-70 mass%, 67-82 mass%, 67-80 mass%, 67-78 mass%, 67-76 mass%, 67-74 mass%, 67-72 mass% or 67-70 mass%.

[0131] (Method for producing positive electrode composition)

[0132] The method for producing the positive electrode composition of the present embodiment is not particularly limited, but the following production method is preferred from the viewpoint that the dispersion state of the conductive material becomes more ideal and the battery characteristics are further improved.

[0133] The manufacturing method of the positive electrode composition of this embodiment is the following method: a first agent containing a binding material and a first liquid medium, a second agent containing carbon black, a dispersant for a first conductive material and a second liquid medium, a third agent containing carbon nanotubes, a dispersant for a second conductive material and a third liquid medium, and an active material are mixed in a prescribed order to obtain a positive electrode composition.

[0134] According to the method for manufacturing the positive electrode composition of the present embodiment, compared with the case where carbon black, carbon nanotubes, a dispersant for a conductive material, a binding material and an active material are mixed simultaneously, carbon black and carbon nanotubes as conductive materials are in an ideal dispersed state, and a positive electrode composition that can achieve excellent discharge rate characteristics and cycle characteristics can be easily obtained.

[0135] The method for producing the positive electrode composition of the present embodiment may be, for example, the following first aspect or the following second aspect.

[0136] In the first mode, the method for manufacturing a positive electrode composition includes the following steps: a first step of mixing a first agent containing a binding material and a first liquid medium, a second agent containing carbon black, a dispersant for a first conductive material and a second liquid medium, and a third agent containing carbon nanotubes, a dispersant for a second conductive material and a third liquid medium to obtain a mixed liquid; and a second step of mixing the above-mentioned mixed liquid and an active material to obtain a positive electrode composition.

[0137] According to the first embodiment, compared with the case where carbon black, carbon nanotubes, a dispersant for a conductive material, a binder and an active material are mixed at the same time, the conductive material (carbon black and carbon nanotubes) is easily in an ideal dispersed state, and a positive electrode composition that can achieve excellent discharge rate characteristics and cycle characteristics is easily obtained. Regarding the reason why the manufacturing method of the first embodiment achieves the above effect, it is believed that one reason is that in the first step, the interaction between the binder, carbon black and the dispersant for a conductive material can achieve a dispersed state that is not easy to agglomerate and is not easy to entangle with the carbon nanotubes, and the non-uniformity caused by the agglomeration of carbon black or the entanglement of carbon black and carbon nanotubes can be suppressed.

[0138] The first step of the first method is a step of mixing a first agent containing a binder and a first liquid medium, a second agent containing carbon black, a first conductive material dispersant and a second liquid medium, and a third agent containing carbon nanotubes, a second conductive material dispersant and a third liquid medium to obtain a mixed solution.

[0139] In the first step of the first embodiment, the method of mixing the first agent, the second agent and the third agent is not particularly limited, and can be implemented by a known method (for example, stirring and mixing based on a ball mill, a sand mill, a twin-screw mixer, a self-rotating revolution mixer, a planetary mixer, a disperser, etc.). The first step of the first embodiment can be, for example, a step of mixing the first agent, the second agent and the third agent in a mixing container to obtain a mixed solution.

[0140] The second step of the first embodiment is a step of mixing the mixed solution obtained in the first step with an active material to obtain a positive electrode composition.

[0141] In the second step of the first mode, the method for mixing the mixed solution and the active material is not particularly limited, and can be implemented using a known method (for example, based on stirring and mixing of a ball mill, a sand mill, a twin-screw mixer, a self-rotating revolution mixer, a planetary mixer, a disperser, etc.). The second step of the first mode can be, for example, a step of stirring to obtain a positive electrode composition after adding an active material to a mixing container containing a mixed solution.

[0142] In the second embodiment, the method for manufacturing a positive electrode composition includes the following steps: a first step of mixing a first agent containing a binding material and a first liquid medium and a second agent containing carbon black, a dispersant for a first conductive material and a second liquid medium to obtain a first mixed liquid; a second step of mixing the first mixed liquid and a third agent containing carbon nanotubes, a dispersant for a second conductive material and a third liquid medium to obtain a second mixed liquid; and a third step of mixing the second mixed liquid and an active material to obtain a positive electrode composition.

[0143] According to the second embodiment, compared with the case where carbon black, carbon nanotubes, a dispersant for a conductive material, a binder and an active material are mixed at the same time, the conductive material (carbon black and carbon nanotubes) is easily in an ideal dispersed state, and a positive electrode composition that can achieve excellent discharge rate characteristics and cycle characteristics is easily obtained. Regarding the reason why the manufacturing method of the second embodiment achieves the above effect, it is believed that one reason is that in the first step, the interaction between the binder, carbon black and the dispersant for a conductive material can achieve a dispersed state that is not easy to agglomerate and is not easy to entangle with the carbon nanotubes, and the inhomogeneity of the electrode structure caused by the agglomeration of carbon black or the entanglement of carbon black and carbon nanotubes can be suppressed.

[0144] The first step of the second aspect is a step of mixing a first agent containing a binder and a first liquid medium and a second agent containing carbon black, a first conductive material dispersant, and a second liquid medium to obtain a first mixed liquid.

[0145] In the first step of the second mode, the method for mixing the first agent and the second agent is not particularly limited, and can be implemented by a known method (for example, stirring and mixing based on a ball mill, a sand mill, a twin-screw mixer, a self-rotating revolution mixer, a planetary mixer, a dispersing mixer, etc.). The first step of the second mode can be, for example, a step of mixing the first agent and the second agent after being put into a mixing container to obtain a first mixed solution.

[0146] The second step of the second embodiment is a step of mixing the first mixed liquid obtained in the first step with a third agent containing carbon nanotubes, a second conductive material dispersant, and a third liquid medium to obtain a second mixed liquid.

[0147] In the second step of the second mode, the method for mixing the first mixed solution and the third agent is not particularly limited, and can be implemented by a known method (for example, stirring and mixing based on a ball mill, a sand mill, a twin-screw mixer, a self-rotating revolution mixer, a planetary mixer, a disperser, etc.). The second step of the second mode can be, for example, a step of adding the third agent to a mixing container containing the first mixed solution and stirring to obtain the second mixed solution.

[0148] The third step of the second embodiment is a step of mixing the second mixed solution obtained in the second step with an active material to obtain a positive electrode composition.

[0149] In the third step of the second mode, the method for mixing the second mixed solution and the active material is not particularly limited, and can be implemented using a known method (for example, based on stirring and mixing of a ball mill, a sand mill, a twin-screw mixer, a self-rotating revolution mixer, a planetary mixer, a disperser, etc.). The third step of the second mode can be, for example, a step of stirring to obtain a positive electrode composition after adding an active material to a mixing container containing the second mixed solution.

[0150] Hereinafter, the first agent, the second agent, and the third agent used in the method for producing the positive electrode composition of the present embodiment will be described in detail.

[0151] The first agent contains a bonding material and a first liquid medium.

[0152] The first liquid medium is not particularly limited as long as it can dissolve the binding material and has compatibility with the second liquid medium and the third liquid medium. Examples of the first liquid medium include water, N-methyl-2-pyrrolidone, cyclohexane, methyl ethyl ketone, methyl isobutyl ketone, etc. Among them, N-methyl-2-pyrrolidone is preferred from the viewpoint of solubility.

[0153] The content of the first liquid medium in the first agent is not particularly limited as long as it is in a range that can dissolve the binder, and can be appropriately changed so that the solid content concentration of the positive electrode composition is within a desired range.

[0154] The solid content concentration of the first dose is not particularly limited, and may be, for example, 1.0 mass % or more, 2.0 mass % or more, 3.0 mass % or more, or 4.0 mass % or more. In addition, the solid content concentration of the first dose may be, for example, 11.0 mass % or less, 10.0 mass % or less, or 9.0 mass % or less.

[0155] That is, the solid content concentration of the first dose can be, for example, 1.0 to 11.0 mass%, 1.0 to 10.0 mass%, 1.0 to 9.0 mass%, 2.0 to 11.0 mass%, 2.0 to 10.0 mass%, 2.0 to 9.0 mass%, 3.0 to 11.0 mass%, 3.0 to 10.0 mass%, 3.0 to 9.0 mass%, 4.0 to 11.0 mass%, 4.0 to 10.0 mass% or 4.0 to 9.0 mass%.

[0156] The first agent may further contain ingredients other than the binder and the first liquid medium, such as polyvinyl pyrrolidone, polyvinyl imidazole, polyethylene glycol, polyvinyl alcohol, polyvinyl butyral, carboxymethyl cellulose, acetyl cellulose or carboxylic acid-modified (meth)acrylate copolymer.

[0157] The second agent contains carbon black, a dispersant for the first conductive material, and a second liquid medium.

[0158] The content of carbon black in the second agent is not particularly limited and can be appropriately changed so that the content of carbon black in the positive electrode composition falls within a desired range.

[0159] The first conductive material dispersant may be a component having a function of assisting the dispersion of carbon black in the second liquid medium, and may also be referred to as a carbon black dispersant.

[0160] The content of the first conductive material dispersant in the second agent is not particularly limited and can be appropriately changed so that the content of the conductive material dispersant in the positive electrode composition falls within a desired range.

[0161] The content of the first conductive material dispersant in the second agent may be, for example, 1 part by mass or more relative to 100 parts by mass of carbon black, and is preferably 2 parts by mass or more from the viewpoint of improving the dispersibility of carbon black, more preferably 3 parts by mass or more, and may be 4 parts by mass or more or 5 parts by mass or more. In addition, the content of the first conductive material dispersant in the second agent may be, for example, 50 parts by mass or less relative to 100 parts by mass of carbon black, and is preferably 45 parts by mass or less, more preferably 40 parts by mass or less, and may be 35 parts by mass or less or 30 parts by mass or less from the viewpoint of suppressing the decrease in conductivity caused by the insulating dispersant.

[0162] That is, the content of the first conductive material dispersant in the second agent relative to 100 parts by mass of carbon black can be, for example, 1 to 50 parts by mass, 1 to 45 parts by mass, 1 to 40 parts by mass, 1 to 35 parts by mass, 1 to 30 parts by mass, 2 to 50 parts by mass, 2 to 45 parts by mass, 2 to 40 parts by mass, 2 to 35 parts by mass, 2 to 30 parts by mass, 3 to 50 parts by mass, 3 to 45 parts by mass, 3 to 40 parts by mass, 3 to 35 parts by mass, 3 to 30 parts by mass, 4 to 50 parts by mass, 4 to 45 parts by mass, 4 to 40 parts by mass, 4 to 35 parts by mass, 4 to 30 parts by mass, 5 to 50 parts by mass, 5 to 45 parts by mass, 5 to 40 parts by mass, 5 to 35 parts by mass or 5 to 30 parts by mass.

[0163] The second liquid medium is not particularly limited as long as it can disperse the carbon black and has compatibility with the first liquid medium and the third liquid medium. As the second liquid medium, for example, water, N-methyl-2-pyrrolidone, cyclohexane, methyl ethyl ketone, methyl isobutyl ketone, etc. can be cited. Among them, N-methyl-2-pyrrolidone is preferred from the perspective of the easy dispersibility of carbon black. The second liquid medium may be the same as the first liquid medium and the third liquid medium, or different, but preferably the same.

[0164] The content of the second liquid medium in the second agent is not particularly limited as long as it is within a range capable of dispersing carbon black, and can be appropriately changed so that the solid content concentration of the positive electrode composition is within a desired range.

[0165] The solid content concentration of the second dose is not particularly limited, and may be, for example, 1.5% by mass or more, 2.5% by mass or more, 3.5% by mass or more, or 5.0% by mass or more. In addition, the solid content concentration of the second dose may be, for example, 25.0% by mass or less, 22.0% by mass or less, 20.0% by mass or less, or 18.0% by mass or less.

[0166] That is, the solid content concentration of the second agent can be, for example, 1.5 to 25.0 mass%, 1.5 to 22.0 mass%, 1.5 to 20.0 mass%, 1.5 to 18.0 mass%, 2.5 to 25.0 mass%, 2.5 to 22.0 mass%, 2.5 to 20.0 mass%, 2.5 to 18.0 mass%, 3.5 to 25.0 mass%, 3.5 to 22.0 mass%, 3.5 to 20.0 mass%, 3.5 to 18.0 mass%, 5.0 to 25.0 mass%, 5.0 to 22.0 mass%, 5.0 to 20.0 mass% or 5.0 to 18.0 mass%.

[0167] The third agent includes carbon nanotubes, a dispersant for a second conductive material and a third liquid medium.

[0168] The content of the carbon nanotubes in the third agent is not particularly limited and can be appropriately changed so that the content of the carbon nanotubes in the positive electrode composition falls within a desired range.

[0169] The second conductive material dispersant may be a component having a function of assisting the dispersion of the carbon nanotubes in the third liquid medium, and may also be referred to as a carbon nanotube dispersant.

[0170] The content of the second conductive material dispersant in the third agent is not particularly limited and can be appropriately changed so that the content of the conductive material dispersant in the positive electrode composition falls within a desired range.

[0171] The content of the second conductive material dispersant in the third agent may be, for example, 1 part by mass or more relative to 100 parts by mass of the carbon nanotubes, and is preferably 2 parts by mass or more, more preferably 3 parts by mass or more, and may be 4 parts by mass or more or 5 parts by mass or more from the viewpoint of improving the dispersibility of the carbon nanotubes. In addition, the content of the second conductive material dispersant in the third agent may be, for example, 50 parts by mass or less relative to 100 parts by mass of the carbon nanotubes, and is preferably 45 parts by mass or less, more preferably 40 parts by mass or less, and may be 35 parts by mass or less or 30 parts by mass or less from the viewpoint of suppressing the decrease in conductivity caused by the insulating dispersant.

[0172] That is, the content of the second conductive material dispersant in the third agent relative to 100 parts by mass of carbon nanotubes may be, for example, 1 to 50 parts by mass, 1 to 45 parts by mass, 1 to 40 parts by mass, 1 to 35 parts by mass, 1 to 30 parts by mass, 2 to 50 parts by mass, 2 to 45 parts by mass, 2 to 40 parts by mass, 2 to 35 parts by mass, 2 to 30 parts by mass, 3 to 50 parts by mass, 3 to 45 parts by mass, 3 to 40 parts by mass, 3 to 35 parts by mass, 3 to 30 parts by mass, 4 to 50 parts by mass, 4 to 45 parts by mass, 4 to 40 parts by mass, 4 to 35 parts by mass, 4 to 30 parts by mass, 5 to 50 parts by mass, 5 to 45 parts by mass, 5 to 40 parts by mass, 5 to 35 parts by mass or 5 to 30 parts by mass.

[0173] The third liquid medium is not particularly limited as long as it can disperse the carbon nanotubes and has compatibility with the first liquid medium and the second liquid medium. As the third liquid medium, for example, water, N-methyl-2-pyrrolidone, cyclohexane, methyl ethyl ketone, methyl isobutyl ketone, etc. can be cited. Among them, N-methyl-2-pyrrolidone is preferred from the perspective of the easy dispersibility of the carbon nanotubes. The third liquid medium may be the same as the first liquid medium and the second liquid medium, or different, but preferably the same.

[0174] The content of the third liquid medium in the third agent is not particularly limited as long as it is within a range capable of dispersing the carbon nanotubes, and can be appropriately changed so that the solid content concentration of the positive electrode composition is within a desired range.

[0175] The solid content concentration of the third agent is not particularly limited, and may be, for example, 0.2 mass % or more, 0.8 mass % or more, 1.5 mass % or more, or 2.5 mass % or more. In addition, the solid content concentration of the third agent may be, for example, 15.0 mass % or less, 12.5 mass % or less, 10.0 mass % or less, or 7.5 mass % or less.

[0176] That is, the solid content concentration of the third agent can be, for example, 0.2-15.0 mass%, 0.2-12.5 mass%, 0.2-10.0 mass%, 0.2-7.5 mass%, 0.8-15.0 mass%, 0.8-12.5 mass%, 0.8-10.0 mass%, 0.8-7.5 mass%, 1.5-15.0 mass%, 1.5-12.5 mass%, 1.5-10.0 mass%, 1.5-7.5 mass%, 2.5-15.0 mass%, 2.5-12.5 mass%, 2.5-10.0 mass% or 2.5-7.5 mass%.

[0177] (Manufacturing method of positive electrode)

[0178] The method for producing the positive electrode of the present embodiment includes the step of applying the above-mentioned positive electrode composition on a current collector to form a composite material layer containing a conductive material, a binder, an active material, and a conductive material dispersant on the current collector.

[0179] In the forming process, the positive electrode composition is coated on the collector to form a composite material layer on the collector. The composite material layer is a layer containing solid components (at least conductive material, binder, active material and conductive material dispersant) in the positive electrode composition, and can be a layer formed by removing at least a portion of the liquid medium from the positive electrode composition.

[0180] The current collector is not particularly limited, and known current collectors can be used without particular limitation. As the current collector, for example, metal foil (metals such as gold, silver, copper, platinum, aluminum, iron, nickel, chromium, manganese, lead, tungsten and titanium, and alloys containing any of them as the main component) can be used. Among them, aluminum is preferably used in the positive electrode, and copper is preferably used in the negative electrode. The current collector is usually provided in the form of foil, but is not limited thereto, and a perforated foil-shaped and mesh-shaped current collector can also be used.

[0181] The method for coating the positive electrode composition on the collector is not particularly limited, and may be, for example, die coating, dip coating, roll coating, doctor blade coating, spray coating, gravure coating, screen printing, or electrostatic coating.

[0182] The amount of the positive electrode composition applied is not particularly limited and can be appropriately adjusted so that the thickness of the composite material layer falls within a desired range.

[0183] The composite material layer can be formed by removing at least a portion of the liquid medium from the coating of the positive electrode composition formed on the collector. The method for removing the liquid medium is not particularly limited, and for example, as a method for removing at least a portion of the liquid medium by heating and / or reducing pressure to vaporize it, there can be cited drying, air drying machine, warm air drying machine, infrared heating machine, far infrared heating machine, etc.

[0184] The method for manufacturing the positive electrode of the present embodiment may further include a pressurizing step of pressurizing the composite material layer and the current collector formed in the forming step in a stacking direction. The pressurizing step can bring the composite material layer and the current collector into close contact.

[0185] The pressing method in the pressing step is not particularly limited, and for example, it may be a method such as roll pressing, die pressing, or calendar pressing.

[0186] The thickness of the composite material layer in the positive electrode is not particularly limited, and can be, for example, 50 μm or more, preferably 55 μm or more, more preferably 60 μm or more, and can also be 65 μm or more or 70 μm or more from the viewpoint of high capacity of the battery. In addition, the thickness of the composite material layer in the positive electrode can be, for example, 150 μm or less, and from the viewpoint of further improving the discharge rate characteristics, preferably 140 μm or less, more preferably 130 μm or less, and can also be 120 μm or less or 110 μm or less.

[0187] That is, the thickness of the composite material layer in the positive electrode can be, for example, 50 to 150 μm, 50 to 140 μm, 50 to 130 μm, 50 to 120 μm, 50 to 110 μm, 55 to 150 μm, 55 to 140 μm, 55 to 130 μm, 55 to 120 μm, 55 to 110 μm, 60 to 150 μm, 60 to 140 μm, 60 to 130 μm, 60 to 120 μm, 60 to 110 μm, 65 to 150 μm, 65 to 140 μm, 65 to 130 μm, 65 to 120 μm, 65 to 110 μm, 70 to 150 μm, 70 to 140 μm, 70 to 130 μm, 70 to 120 μm or 70 to 110 μm.

[0188] The positive electrode produced by the production method of this embodiment can be suitably used as a positive electrode of a battery, particularly a secondary battery (lithium ion secondary battery).

[0189] (positive electrode)

[0190] The positive electrode of this embodiment is a positive electrode including a composite material layer containing a conductive material, an active material, a binder, and a dispersant for a conductive material. The positive electrode of this embodiment may be, for example, a positive electrode manufactured by the above-mentioned manufacturing method.

[0191] The positive electrode of this embodiment can be suitably used as a positive electrode of a battery, particularly a secondary battery (lithium ion secondary battery).

[0192] The battery in this embodiment (preferably a secondary battery, more preferably a lithium ion secondary battery) includes a positive electrode manufactured by the above-mentioned manufacturing method. The battery in this embodiment may have the same structure as a known battery except for the positive electrode.

[0193] The use of the battery in this embodiment is not particularly limited, and it can be used in a wide range of fields such as portable AV devices such as digital cameras, camcorders, portable audio players, portable LCD TVs, portable information terminals such as laptops, smart phones, mobile PCs, as well as portable gaming devices, power tools, electric bicycles, hybrid vehicles, electric vehicles, power storage systems, etc.

[0194] As mentioned above, although the preferred embodiment of the present invention was described, the present invention is not limited to the above-mentioned embodiment.

[0195] Example

[0196] Hereinafter, the present invention will be described in more detail using examples, but the present invention is not limited to these examples.

[0197] <Example 1>

[0198] (Carbon Black)

[0199] Acetylene (12 Nm) as a raw material was supplied from a nozzle installed in the upstream part of the carbon black reaction furnace (furnace length 6 m, furnace diameter 0.65 m). 3 / h, toluene 32kg / h, oxygen 22Nm 3 / h, to produce carbon black, which is captured by a bag filter installed in the downstream part of the reactor. Then, it is passed through a dry cyclone separator device and a magnet for removing iron and recovered in a tank. It should be noted that acetylene, toluene and oxygen are heated to 115°C and supplied to the reactor to obtain carbon black A. The BET specific surface area of ​​the obtained carbon black A is 240m 2 / g, the average primary particle size is 20nm, and the crystallite size (Lc) is

[0200] (Carbon black dispersion)

[0201] Carbon black A, NMP as a liquid medium, and polyvinyl alcohol (POVAL DR-1137, SP value: 35 J / cm2, manufactured by Denka Co., Ltd.) as a dispersant were prepared. 3 ). 1.0 mass % of polyvinyl alcohol and 10.0 mass % of carbon black A were added to 89.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 type) to prepare a slurry containing carbon black A. The obtained slurry was added to a bead mill (manufactured by Ashizawa Finetech, MUGEN FLOW MGF2-ZA) equipped with zirconium oxide beads (diameter 0.5 mm) and dispersed. After the dispersion treatment, the zirconium oxide beads were removed by filtration to obtain a carbon black dispersion.

[0202] (Carbon Nanotube Dispersion Liquid)

[0203] Carbon nanotubes (manufactured by CNano, “Flotube 6000”, with an average diameter of 6 nm and a BET specific surface area of ​​300 m 2 / g), NMP as a liquid medium, polyvinyl pyrrolidone (PITZCOL K90 manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., SP value: 25 J / cm3 ). 1.0 mass % of polyvinyl pyrrolidone and 4.0 mass % of carbon nanotubes were added to 95.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 model) to prepare a slurry containing carbon nanotubes. The obtained slurry was put into a bead mill (manufactured by Ashizawa Finetech, MUGEN FLOW MGF2-ZA) equipped with zirconia beads (diameter 0.5 mm) and dispersed. After the dispersion treatment, the zirconia beads were removed by filtration to obtain a carbon nanotube dispersion.

[0204] (Manufacturing of positive electrode composition)

[0205] As an active material, a particle size D 50 12μm lithium nickel manganese cobalt oxide (produced by Beijing Dangsheng Company, "ME6A").

[0206] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.7 parts by mass, the carbon nanotube becomes 0.3 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a rotation speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0207] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 69% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0208] (Manufacturing of positive electrode)

[0209] The positive electrode composition was formed into a film on one side of an aluminum foil (UACJ company) having a thickness of 15 μm using an applicator, thereby producing a laminate, which was left to stand in a dryer and pre-dried at 105°C for 1 hour to completely remove the NMP. Next, the dried laminate was pressurized with a linear pressure of 200 kg / cm using a roller press to prepare a laminate having a thickness of 80 μm as a whole. Next, vacuum drying was performed at 170°C for 3 hours to completely remove the residual moisture and obtain a positive electrode having a current collector and a composite material layer.

[0210] (Manufacturing of negative electrode)

[0211] Prepare pure water (manufactured by Kanto Chemical Co., Ltd.) as a solvent, artificial graphite (manufactured by Hitachi Chemical Co., Ltd., "MAG-D") as a negative electrode active material, styrene butadiene rubber (manufactured by Zeon Co., Ltd., "BM-400B", hereinafter referred to as SBR) as a binder, and carboxymethyl cellulose (manufactured by Daicel Co., Ltd., "D2200", hereinafter referred to as CMC) as a dispersant. Then, weigh and mix CMC in a solid content of 1% by mass and artificial graphite in a solid content of 97% by mass, add pure water to the mixture, and use a rotation-revolution mixer (manufactured by Thinky Co., Ltd., Degassing Rentaro ARV-310) to mix until it becomes uniform, and obtain a mixture. Then, weigh SBR in a solid content of 2% by mass, add it to the obtained mixture, and use a rotation-revolution mixer (manufactured by Thinky Co., Ltd., Degassing Rentaro ARV-310) to mix until it becomes uniform, and obtain a negative electrode composition. Next, the negative electrode composition was formed into a film on a copper foil (manufactured by UACJ) having a thickness of 10 μm using an applicator to prepare a laminate, which was then placed in a dryer and pre-dried at 60°C for 1 hour. Next, a roller press was used to press the laminate at a linear pressure of 50 kg / cm to prepare a laminate having a thickness of 60 μm. Next, vacuum drying was performed at 120°C for 3 hours to completely remove the residual moisture, thereby obtaining a negative electrode having a current collector and a composite material layer.

[0212] (Battery manufacturing)

[0213] In a drying room where the dew point has been controlled to be below -50°C, the produced positive electrode is processed into 40×40mm, and the produced negative electrode is processed into 44×44mm. Then, an aluminum tab is welded to the positive electrode, and a nickel tab is welded to the negative electrode. The composite material coated surfaces of the positive electrode and the negative electrode are respectively placed opposite each other in the center, and a polyolefin microporous membrane processed into 45×45mm is arranged between the positive electrode and the negative electrode. Next, the sheet-shaped outer package cut and processed into a 70×140mm square is folded in half along the center of the long side. Next, the outer package is arranged in a manner that the aluminum tab for the positive electrode and the nickel tab for the negative electrode are exposed on the outside of the outer package, while the folded outer package is used to clamp the positive electrode / polyolefin microporous membrane / negative electrode laminate. Next, a heat sealer is used to heat and weld two sides of the outer package, including the sides where the aluminum tabs for the positive electrode and the nickel tabs for the negative electrode are exposed. Then, 2 g of electrolyte (manufactured by KISHIDA CHEMICAL, a solution containing ethylene carbonate / diethyl carbonate = 1 / 2 (volume ratio) and 1M LiPF6 solution) is injected from the side that has not been heated and welded. After the electrolyte is fully infiltrated into the positive electrode, the negative electrode and the polyolefin microporous membrane, a vacuum heat sealer is used to reduce the internal pressure while heating and welding the remaining side of the outer package to obtain a lithium-ion secondary battery.

[0214] (Battery Evaluation)

[0215] [Internal resistance]

[0216] The produced battery was charged at 4.3V and 0.2C at a constant current and constant voltage at 25°C, and then discharged at a constant current of 0.2C to 3.0V. Then, 5 cycles of charge / discharge were performed under the same conditions, and then charged to a depth of charge of 50%. Then, impedance measurement was performed under the conditions of a frequency range of 10MHz to 0.001Hz and a vibration voltage of 5mV to measure the internal resistance. The results of the internal resistance measurement are shown in Table 1.

[0217] [Discharge rate characteristics (rate capacity maintenance ratio)]

[0218] For the manufactured battery, after constant current and constant voltage charging limited to 4.3V and 0.2C at 25°C, it was discharged to 3.0V at a constant current of 0.2C. Then, after recovery charging was performed again at a constant current and constant voltage limited to 4.3V and 0.2C, it was discharged to 3.0V at a constant current of 0.2C, and the discharge capacity at this time was measured. Next, the recovery charging condition was set to charge at a constant current and constant voltage limited to 4.3V and 0.2C. On the other hand, while the discharge current was changed stepwise to 0.5C, 1C, 2C, and 3C, recovery charging and discharging were repeated, and the discharge capacity relative to each discharge current was measured. As an indicator of the discharge rate characteristics of the battery, the capacity retention rate at 3C discharge relative to 0.2C discharge was calculated as the rate capacity retention rate. The calculation results of the rate capacity retention rate are shown in Table 1.

[0219] [Cycle characteristics (cycle capacity maintenance rate)]

[0220] For the manufactured battery, after constant current and constant voltage charging limited to 4.3V and 1C at 25°C, it was discharged to 3.0V at a constant current of 1C. The above-mentioned charge and discharge were repeated for 500 cycles, and the discharge capacity in each cycle was measured. As an indicator of the cycle characteristics of the battery, the capacity retention rate after 500 cycles relative to the capacity retention rate after 1 cycle was calculated as the cycle capacity retention rate. The calculation results of the cycle capacity retention rate are shown in Table 1.

[0221] <Example 2>

[0222] (Carbon Nanotube Dispersion)

[0223] Prepare carbon nanotubes (manufactured by CNano, "Flotube 6000", with an average diameter of 6 nm and a BET specific surface area of ​​300 m 2 / g), NMP as a liquid medium, polyvinyl butyral (manufactured by Sekisui Chemical Co., Ltd., BL-1, SP value: 24 J / cm 3 ). 1.0 mass % of polyvinyl butyral and 4.0 mass % of carbon nanotubes were added to 95.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 model) to prepare a slurry containing carbon nanotubes. The obtained slurry was put into a bead mill (manufactured by Ashizawa Finetech, MUGEN FLOW MGF2-ZA) equipped with zirconia beads (diameter 0.5 mm) and dispersed. After the dispersion treatment, the zirconia beads were removed by filtration to obtain a carbon nanotube dispersion.

[0224] (Manufacturing of positive electrode and battery)

[0225] In addition to the above carbon nanotube dispersion, the same carbon black dispersion, binder, and active material as in Example 1 were prepared.

[0226] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.7 parts by mass, the carbon nanotube becomes 0.3 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a rotation speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0227] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 69% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0228] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0229] <Example 3>

[0230] (Carbon black dispersion)

[0231] Carbon black A, NMP as a liquid medium, and sodium carboxymethyl cellulose (D2200 manufactured by Daicel, SP value: 29 J / cm) as a dispersant were prepared. 3). 1.0 mass % of sodium carboxymethyl cellulose and 10.0 mass % of carbon black A were added to 89.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 model) to prepare a slurry containing carbon black A. The obtained slurry was added to a bead mill (manufactured by Ashizawa Finetech, MUGEN FLO W MGF2-ZA) equipped with zirconium oxide beads (diameter 0.5 mm) and dispersed. After the dispersion treatment, the zirconium oxide beads were removed by filtration to obtain a carbon black dispersion.

[0232] (Manufacturing of positive electrode and battery)

[0233] In addition to the above carbon black dispersion, the same carbon nanotube dispersion, binder, and active material as in Example 1 were prepared.

[0234] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.7 parts by mass, the carbon nanotube becomes 0.3 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a rotation speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0235] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 69% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0236] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0237] <Example 4>

[0238] (Carbon black dispersion)

[0239] Carbon black A, NMP as a liquid medium, and polyvinyl pyrrolidone (PITZCOL K90 manufactured by Daiichi Kogyo Seiyaku Co., Ltd., SP value: 25 J / cm) as a dispersant were prepared. 3). 1.0 mass % of polyvinyl pyrrolidone and 10.0 mass % of carbon black A were added to 89.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 type) to prepare a slurry containing carbon black A. The obtained slurry was put into a bead mill (manufactured by Ashizawa Finetech, MUG EN FLOW MGF2-ZA) equipped with zirconium oxide beads (diameter 0.5 mm) for dispersion treatment. After the dispersion treatment, the zirconium oxide beads were removed by filtration to obtain a carbon black dispersion.

[0240] (Carbon Nanotube Dispersion Liquid)

[0241] Carbon nanotubes (manufactured by CNano, “Flotube 6000”, with an average diameter of 6 nm and a BET specific surface area of ​​300 m 2 / g), NMP as a liquid medium, polyvinyl butyral (manufactured by Sekisui Chemical Co., Ltd., BL-1, SP value: 24 J / cm 3 ). 1.0 mass % of polyvinyl butyral and 4.0 mass % of carbon nanotubes were added to 95.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 model) to prepare a slurry containing carbon nanotubes. The obtained slurry was put into a bead mill (manufactured by Ashizawa Finetech, MUGEN FLOW MGF2-ZA) equipped with zirconia beads (diameter 0.5 mm) and dispersed. After the dispersion treatment, the zirconia beads were removed by filtration to obtain a carbon nanotube dispersion.

[0242] (Manufacturing of positive electrode and battery)

[0243] In addition to the carbon black dispersion and the carbon nanotube dispersion, the same binder and active material as in Example 1 were prepared.

[0244] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.7 parts by mass, the carbon nanotube becomes 0.3 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a rotation speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0245] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 69% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0246] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0247] <Example 5>

[0248] (Carbon Nanotube Dispersion Liquid)

[0249] Carbon nanotubes (manufactured by CNano, “Flotube 6000”, with an average diameter of 6 nm and a BET specific surface area of ​​300 m 2 / g), NMP as a liquid medium, carboxymethyl cellulose sodium salt (manufactured by Daicel, D2200, SP value: 29 J / cm 3 ). 1.0 mass % of sodium carboxymethyl cellulose and 4.0 mass % of carbon nanotubes were added to 95.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 model) to prepare a slurry containing carbon nanotubes. The obtained slurry was put into a bead mill (manufactured by Ashizawa Finetech, MUGEN FLOW MGF2-ZA) equipped with zirconium oxide beads (diameter 0.5 mm) and dispersed. After the dispersion treatment, the zirconium oxide beads were removed by filtration to obtain a carbon nanotube dispersion.

[0250] (Manufacturing of positive electrode and battery)

[0251] In addition to the above carbon nanotube dispersion, the same carbon black dispersion, binder, and active material as in Example 1 were prepared.

[0252] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.7 parts by mass, the carbon nanotube becomes 0.3 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a rotation speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0253] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 69% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0254] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0255] <Example 6>

[0256] (Manufacturing of positive electrode and battery)

[0257] The same carbon black dispersion, carbon nanotube dispersion, binder and active material as in Example 1 were prepared.

[0258] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.4 parts by mass, the carbon nanotube becomes 0.6 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0259] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 69% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0260] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0261] <Example 7>

[0262] (Carbon Black)

[0263] Acetylene (12 Nm) as a raw material was supplied from a nozzle installed in the upstream part of the carbon black reaction furnace (furnace length 6 m, furnace diameter 0.65 m). 3 / h, toluene 32kg / h, oxygen 19Nm 3 / h, to produce carbon black, which is captured by a bag filter installed in the downstream part of the reactor. Then, it is passed through a dry cyclone separator device and a magnet for removing iron and recovered in a tank. It should be noted that acetylene, toluene and oxygen are heated to 115°C and supplied to the reactor to obtain carbon black B. The BET specific surface area of ​​the obtained carbon black B is 178m 2 / g, the average primary particle size is 22nm, and the crystallite size (Lc) is

[0264] (Carbon black dispersion)

[0265] Carbon black B, NMP as a liquid medium, and polyvinyl alcohol (POVAL DR-1137 manufactured by Denka Co., Ltd., SP value: 35 J / cm) as a dispersant were prepared. 3 ). 1.0 mass % of polyvinyl alcohol and 10.0 mass % of carbon black B were added to 89.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 type) to prepare a slurry containing carbon black B. The obtained slurry was put into a bead mill (manufactured by Ashizawa Finetech, MUGEN FLOW MGF2-ZA) equipped with zirconium oxide beads (diameter 0.5 mm) and dispersed. After the dispersion treatment, the zirconium oxide beads were removed by filtration to obtain a carbon black dispersion.

[0266] (Manufacturing of positive electrode and battery)

[0267] In addition to the above carbon black dispersion, the same carbon nanotube dispersion, binder, and active material as in Example 1 were prepared.

[0268] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.7 parts by mass, the carbon nanotube becomes 0.3 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a rotation speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0269] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 78% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0270] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0271] <Example 8>

[0272] (Carbon Black)

[0273] Acetylene (12 Nm) as a raw material was supplied from a nozzle installed in the upstream part of the carbon black reaction furnace (furnace length 6 m, furnace diameter 0.65 m). 3 / h, toluene 32kg / h, oxygen 26Nm 3 / h, carbon black is produced and captured by a bag filter installed in the downstream part of the reactor. Then, it is passed through a dry cyclone separator device and a magnet for removing iron and recovered in a tank. It should be noted that acetylene, toluene and oxygen are heated to 115°C and supplied to the reactor to obtain carbon black C. The BET specific surface area of ​​the obtained carbon black C is 370m 2 / g, the average primary particle size is 18nm, and the crystallite size (Lc) is

[0274] (Carbon black dispersion)

[0275] Carbon black C, NMP as a liquid medium, and polyvinyl alcohol (POVAL DR-1137, SP value: 35 J / cm2, manufactured by Denka Co., Ltd.) as a dispersant were prepared. 3 ). 1.0 mass % of polyvinyl alcohol and 10.0 mass % of carbon black C were added to 89.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 type) to prepare a slurry containing carbon black C. The obtained slurry was added to a bead mill (manufactured by Ashizawa Finetech, MUGEN FLOW MGF2-ZA) equipped with zirconium oxide beads (diameter 0.5 mm) for dispersion treatment. After the dispersion treatment, the zirconium oxide beads were removed by filtration to obtain a carbon black dispersion.

[0276] (Manufacturing of positive electrode and battery)

[0277] In addition to the above carbon black dispersion, the same carbon nanotube dispersion, binder, and active material as in Example 1 were prepared.

[0278] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.7 parts by mass, the carbon nanotube becomes 0.3 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a rotation speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0279] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 67% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0280] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0281] <Example 9>

[0282] (Manufacturing of positive electrode and battery)

[0283] The same carbon black dispersion, carbon nanotube dispersion, binder and active material as in Example 1 were prepared.

[0284] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.2 parts by mass, the carbon nanotube becomes 0.8 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0285] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 69% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0286] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0287] <Example 10>

[0288] (Manufacturing of positive electrode and battery)

[0289] The same carbon black dispersion, carbon nanotube dispersion, binder and active material as in Example 1 were prepared.

[0290] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.95 parts by mass, the carbon nanotube becomes 0.05 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a rotation speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0291] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 69% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0292] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 3.

[0293] <Comparative Example 1>

[0294] (Carbon Nanotube Dispersion)

[0295] Prepare carbon nanotubes (manufactured by CNano, "Flotube 6000", with an average diameter of 6 nm and a BET specific surface area of ​​300 m 2 / g), NMP as a liquid medium, polyvinyl alcohol (POVAL DR-1137 manufactured by Denka Co., Ltd., SP value: 35 J / cm 3 ). 1.0 mass % of polyvinyl alcohol and 4.0 mass % of carbon nanotubes were added to 95.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 model) to prepare a slurry containing carbon nanotubes. The obtained slurry was put into a bead mill (manufactured by Ashizawa Finetech, MUGEN FLOW MGF 2-ZA) equipped with zirconia beads (diameter 0.5 mm) and dispersed. After the dispersion treatment, the zirconia beads were removed by filtration to obtain a carbon nanotube dispersion.

[0296] (Manufacturing of positive electrode and battery)

[0297] In addition to the above carbon nanotube dispersion, the same carbon black dispersion, binder, and active material as in Example 1 were prepared.

[0298] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.7 parts by mass, the carbon nanotube becomes 0.3 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a rotation speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0299] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 69% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0300] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 4.

[0301] <Comparative Example 2>

[0302] (Carbon black dispersion)

[0303] Carbon black A, NMP as a liquid medium, and polyvinyl pyrrolidone (PITZCOL K90 manufactured by Daiichi Kogyo Seiyaku Co., Ltd., SP value: 25 J / cm) as a dispersant were prepared. 3 ). 1.0 mass % of polyvinyl pyrrolidone and 10.0 mass % of carbon black A were added to 89.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 type) to prepare a slurry containing carbon black A. The obtained slurry was put into a bead mill (manufactured by Ashizawa Finetech, MUG EN FLOW MGF2-ZA) equipped with zirconium oxide beads (diameter 0.5 mm) for dispersion treatment. After the dispersion treatment, the zirconium oxide beads were removed by filtration to obtain a carbon black dispersion.

[0304] In addition to the above carbon black dispersion, the same carbon nanotube dispersion, binder, and active material as in Example 1 were prepared.

[0305] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.7 parts by mass, the carbon nanotube becomes 0.3 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a rotation speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0306] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 69% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0307] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 4.

[0308] <Comparative Example 3>

[0309] (Carbon black dispersion)

[0310] Carbon black A, NMP as a liquid medium, and polyvinyl butyral (manufactured by Sekisui Chemical Co., Ltd., BL-1, SP value: 24 J / cm) as a dispersant were prepared. 3 ). 1.0 mass % of polyvinyl butyral and 10.0 mass % of carbon black A were added to 89.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 type) to prepare a slurry containing carbon black A. The obtained slurry was added to a bead mill (manufactured by Ashizawa Finetech, MUGEN FLOW MGF2-ZA) equipped with zirconium oxide beads (diameter 0.5 mm) for dispersion treatment. After the dispersion treatment, the zirconium oxide beads were removed by filtration to obtain a carbon black dispersion.

[0311] (Carbon Nanotube Dispersion Liquid)

[0312] Carbon nanotubes (manufactured by CNano, “Flotube 6000”, with an average diameter of 6 nm and a BET specific surface area of ​​300 m 2 / g), NMP as a liquid medium, polyvinyl butyral (manufactured by Sekisui Chemical Co., Ltd., BL-1, SP value: 24 J / cm 3). 1.0 mass % of polyvinyl butyral and 4.0 mass % of carbon nanotubes were added to 95.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 model) to prepare a slurry containing carbon nanotubes. The obtained slurry was put into a bead mill (manufactured by Ashizawa Finetech, MUGEN FLOW MGF2-ZA) equipped with zirconia beads (diameter 0.5 mm) and dispersed. After the dispersion treatment, the zirconia beads were removed by filtration to obtain a carbon nanotube dispersion.

[0313] (Manufacturing of positive electrode and battery)

[0314] In addition to the carbon black dispersion and the carbon nanotube dispersion, the same binder and active material as in Example 1 were prepared.

[0315] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.7 parts by mass, the carbon nanotube becomes 0.3 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a rotation speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0316] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 69% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0317] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 4.

[0318] <Comparative Example 4>

[0319] (Carbon black dispersion)

[0320] Carbon black A, NMP as a liquid medium, and sodium carboxymethyl cellulose (D2200, manufactured by Daicel, SP value: 29 J / cm) as a dispersant were prepared. 3). 1.0 mass % of sodium carboxymethyl cellulose and 10.0 mass % of carbon black A were added to 89.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 type) to prepare a slurry containing carbon black A. The obtained slurry was added to a bead mill (manufactured by Ashizawa Finetech, MUGEN FLOW MGF2-ZA) equipped with zirconium oxide beads (diameter 0.5 mm) for dispersion treatment. After the dispersion treatment, the zirconium oxide beads were removed by filtration to obtain a carbon black dispersion.

[0321] (Carbon Nanotube Dispersion)

[0322] Prepare carbon nanotubes (manufactured by CNano, "Flotube 6000", with an average diameter of 6 nm and a BET specific surface area of ​​300 m 2 / g), NMP as a liquid medium, carboxymethyl cellulose sodium salt (manufactured by Daicel, D2200, SP value: 29 J / cm 3 ). 1.0 mass % of sodium carboxymethyl cellulose and 4.0 mass % of carbon nanotubes were added to 95.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 model) to prepare a slurry containing carbon nanotubes. The obtained slurry was put into a bead mill (manufactured by Ashizawa Finetech, MUGEN FLOW MGF2-ZA) equipped with zirconium oxide beads (diameter 0.5 mm) and dispersed. After the dispersion treatment, the zirconium oxide beads were removed by filtration to obtain a carbon nanotube dispersion.

[0323] (Manufacturing of positive electrode and battery)

[0324] In addition to the carbon black dispersion and the carbon nanotube dispersion, the same binder and active material as in Example 1 were prepared.

[0325] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.7 parts by mass, the carbon nanotube becomes 0.3 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a rotation speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0326] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 69% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0327] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 4.

[0328] <Comparative Example 5>

[0329] (Carbon black dispersion)

[0330] The BET specific surface area of ​​carbon black prepared is 87 m 2 / g, an average primary particle size of 25nm and a crystallite size (Lc) of Carbon black (Cabot Corporation, "LiTX-HP"), NMP as a liquid medium, polyvinyl alcohol as a dispersant (Denka Corporation, POVAL DR-1137, SP value: 35 J / cm 3 ). 1.0 mass % of polyvinyl alcohol and 10.0 mass % of LiTX-HP were added to 89.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 type) to prepare a slurry containing LiTX-HP. The obtained slurry was put into a bead mill (manufactured by Ashizawa Finetech, MUGEN FLOW MGF2-ZA) equipped with zirconia beads (diameter 0.5 mm) for dispersion treatment. After the dispersion treatment, the zirconia beads were removed by filtration to obtain a carbon black dispersion.

[0331] In addition to the above carbon black dispersion, the same carbon nanotube dispersion, binder, and active material as in Example 1 were prepared.

[0332] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.7 parts by mass, the carbon nanotube becomes 0.3 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a rotation speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0333] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 70% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0334] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 5.

[0335] <Comparative Example 6>

[0336] (Carbon black dispersion)

[0337] The BET specific surface area of ​​carbon black prepared was 820 m 2 / g, an average primary particle size of 40nm and a crystallite size (Lc) of Carbon black (manufactured by Lion Corporation, “ECP”), NMP as a liquid medium, polyvinyl alcohol as a dispersant (manufactured by Denka Corporation, POVAL DR-1137, SP value: 35 J / cm 3 ). 1.0 mass % of polyvinyl alcohol and 10.0 mass % of ECP were added to 89.0 mass % of NMP, and stirred for 120 minutes using a planetary mixer (manufactured by PRIMIX, Hivis Disper Mix 3D-5 model) to prepare a slurry containing ECP. The obtained slurry was added to a bead mill (manufactured by Ashizawa Finetech, MUGEN FLOW MGF2-ZA) equipped with zirconia beads (diameter 0.5 mm) for dispersion treatment. After the dispersion treatment, the zirconia beads were removed by filtration to obtain a carbon black dispersion.

[0338] In addition to the above carbon black dispersion, the same carbon nanotube dispersion, binder, and active material as in Example 1 were prepared.

[0339] As the first stage, an NMP solution of polyvinylidene fluoride as a binding material (manufactured by KUREHA, "L#7208"), a carbon black dispersion and a carbon nanotube dispersion are measured in a plastic container so that the carbon black becomes 0.7 parts by mass, the carbon nanotube becomes 0.3 parts by mass and the binding material becomes 2 parts by mass. A rotation-revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) is used to mix at a rotation speed of 2000 rpm for 5 minutes to obtain a mixed solution.

[0340] As the second stage, 97 parts by weight of active material and NMP solution were added to the mixed solution obtained in the first stage to prepare a total solid content concentration of 66% by weight. A self-rotating revolution mixer (manufactured by Thinky, Degassing Rentaro ARV-310) was used to mix at a revolution speed of 2000 rpm for 5 minutes to obtain a positive electrode composition.

[0341] Using the obtained positive electrode composition, a positive electrode and a battery were produced and evaluated in the same manner as in Example 1. The results are shown in Table 5.

[0342] [Table 1]

[0343]

[0344] [Table 2]

[0345]

[0346] [Table 3]

[0347]

[0348] [Table 4]

[0349]

[0350] [Table 5]

[0351]

Claims

1. A positive electrode composition comprising a conductive material, an active material, a binder, a dispersant for a conductive material and a liquid medium, The conductive material contains carbon black and carbon nanotubes. The conductive material dispersant contains two or more dispersants with different SP values. The BET specific surface area of ​​the carbon black is 100 to 500 m 2 / g.

2. The positive electrode composition according to claim 1, wherein The ratio (mass ratio) of the content of the carbon nanotubes to the total content of the carbon black and the carbon nanotubes is 0.1 to 0.

7.

3. The positive electrode composition according to claim 1, wherein The conductive material dispersant is selected from the group consisting of polyvinyl alcohol, polyvinyl pyrrolidone, polyvinyl butyral, carboxymethyl cellulose and its salt, polyvinyl acetal, polyvinyl acetate, polyvinyl amine and polyvinyl formal.

4. The positive electrode composition according to claim 1, wherein The carbon black has 100 to 400 m 2 / g BET specific surface area, and The crystallite size (Lc).

5. The positive electrode composition according to claim 1, wherein The carbon nanotubes have an average diameter of 5 to 15 nm.

6. A method for producing a positive electrode composition, comprising the following steps: In a first step, a first agent containing a binder and a first liquid medium, a second agent containing carbon black, a dispersant for a first conductive material, and a second liquid medium, and a third agent containing carbon nanotubes, a dispersant for a second conductive material, and a third liquid medium are mixed to obtain a mixed liquid; and The second step is to mix the mixed solution and the active material to obtain a positive electrode composition. The first conductive material dispersant has an SP value different from an SP value of the second conductive material dispersant.

7. A method for producing a positive electrode composition, comprising the following steps: In the first step, a first agent containing a binder and a first liquid medium is mixed with a second agent containing carbon black, a first conductive material dispersant and a second liquid medium to obtain a first mixed liquid; In a second step, the first mixed solution is mixed with a third agent containing carbon nanotubes, a second conductive material dispersant, and a third liquid medium to obtain a second mixed solution; and The third step is to mix the second mixed solution with an active material to obtain a positive electrode composition. The first conductive material dispersant has an SP value different from an SP value of the second conductive material dispersant.

8. The manufacturing method according to claim 6 or 7, wherein: The SP value of the first conductive material dispersant is higher than the SP value of the second conductive material dispersant.

9. The manufacturing method according to claim 6 or 7, wherein: The ratio (mass ratio) of the content of the carbon nanotubes to the total content of the carbon black and the carbon nanotubes is 0.1 to 0.

7.

10. The manufacturing method according to claim 6 or 7, wherein: The first conductive material dispersant and the second conductive material dispersant are each selected from the group consisting of polyvinyl alcohol, polyvinyl pyrrolidone, polyvinyl butyral, carboxymethyl cellulose and its salt, polyvinyl acetal, polyvinyl acetate, polyvinyl amine, and polyvinyl formal.

11. A method for manufacturing a positive electrode, comprising the steps of: applying the positive electrode composition according to any one of claims 1 to 5 on a current collector, and forming a composite material layer containing the conductive material, the active material, the binder and the conductive material dispersant on the current collector.

12. A positive electrode comprising a composite material layer, wherein the composite material layer contains a conductive material, an active material, a binding material and a dispersant for the conductive material, The conductive material contains carbon black and carbon nanotubes. The conductive material dispersant contains two or more dispersants with different SP values. The BET specific surface area of ​​the carbon black is 100 to 500 m 2 / g.

13. The positive electrode according to claim 12, wherein The ratio (mass ratio) of the content of the carbon nanotubes to the total content of the carbon black and the carbon nanotubes is 0.1 to 0.

7.

14. The positive electrode according to claim 12, wherein The conductive material dispersant is selected from the group consisting of polyvinyl alcohol, polyvinyl pyrrolidone, polyvinyl butyral, carboxymethyl cellulose and its salt, polyvinyl acetal, polyvinyl acetate, polyvinyl amine and polyvinyl formal. 15 . A battery comprising the positive electrode according to claim 12 .