Negative electrode active material for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
By using Si-containing composite materials containing amorphous carbon phase and dispersed silicon in nonaqueous electrolyte secondary batteries, the content of metal oxides and silicon is controlled, and the problems of reduced cycle characteristics and high reaction resistance are solved, and high capacity is achieved and a nonaqueous electrolyte secondary battery with excellent circulation characteristics.
Patent Information
- Application Number
- CN202380029049.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-12
AI Technical Summary
The existing Si-containing materials have problems such as lowering circulation characteristics and high reaction resistance in non-aqueous electrolyte secondary batteries, and it is difficult to effectively suppress side reactions with the electrolyte solution.
The Si-containing composite material containing an amorphous carbon phase and silicon and metal oxide dispersed in the carbon phase is used as the negative electrode active material, and the metal oxide content is controlled to be 0.001 to 2 mass%, and the silicon content is less than 60 mass%, so as to be controlled to be less than 60 mass%, so as to be Improve the cycle characteristics of the battery and reduce the reaction resistance.
A nonaqueous electrolyte secondary battery with high capacity and excellent circulation characteristics is realized, effectively suppressing side reactions with the electrolyte, and improving the circulation characteristics and battery performance of the battery.
Smart Images

Figure CN118946983A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a negative electrode active material for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery using the negative electrode active material. Background Art
[0002] In recent years, non-aqueous electrolyte secondary batteries such as lithium-ion batteries have been widely used for applications requiring high capacity, such as vehicle-mounted applications and power storage applications. The negative electrode active material, which is the main component of the negative electrode, is one of the important elements in achieving high capacity of the battery, and therefore various studies are being conducted on the negative electrode active material. Among them, the use of silicon-containing materials (Si-containing materials) as negative electrode active materials with high theoretical capacity density has attracted much attention.
[0003] As the Si-containing material, for example, a composite material containing a carbon material and silicon is disclosed in Patent Document 1. Also, Patent Document 2 discloses a Si-containing material containing a composite body composed of silicon and an oxide surrounding the silicon, and a carbon material.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: U.S. Patent Application Publication No. 2020 / 0107693
[0007] Patent Document 2: Japanese Patent Application No. 2007-500421 Summary of the invention
[0008] Regarding the negative electrode active material used in non-aqueous electrolyte secondary batteries, from the perspective of high capacity and improved battery cycle characteristics, it is best to use a material that is difficult to cause side reactions with the electrolyte and has low reaction resistance. The Si-containing materials of Patent Documents 1 and 2 still have room for improvement in terms of suppressing side reactions with the electrolyte and reducing reaction resistance.
[0009] The negative electrode active material for a non-aqueous electrolyte secondary battery of the present invention is characterized in that it has a Si-containing composite material comprising an amorphous carbon phase and silicon and metal oxides dispersed in the carbon phase, wherein the content of the metal oxide is 0.001 to 2% by mass relative to the mass of the Si-containing composite material, and the content of silicon is less than 60% by mass relative to the mass of the Si-containing composite material.
[0010] The nonaqueous electrolyte secondary battery of the present invention comprises a positive electrode, a negative electrode, and a nonaqueous electrolyte, wherein the negative electrode contains the above-mentioned negative electrode active material.
[0011] According to the negative electrode active material of the present invention, a non-aqueous electrolyte secondary battery with high capacity and excellent cycle characteristics can be realized. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of the embodiment.
[0013] Figure 2 It is a cross-sectional view of a negative electrode active material as an example of an embodiment. DETAILED DESCRIPTION
[0014] As shown below, the theoretical capacity density of Si-containing materials is high, which contributes to the high capacity of batteries when used as negative electrode active materials. On the other hand, in batteries using Si-containing materials, there is a problem of reduced cycle characteristics. Therefore, the inventors of the present invention have conducted in-depth research on high-capacity non-aqueous electrolyte secondary batteries using Si-containing materials in order to improve cycle characteristics. As a result, it was found that in Si-containing materials comprising an amorphous carbon phase and silicon dispersed in the carbon phase, by adding a specified amount of metal oxide to the carbon phase and controlling the content of silicon to be less than a specified amount, the cycle characteristics can be excellently improved.
[0015] According to the negative electrode active material of the present invention, it can be considered that the side reaction with the electrolyte can be effectively suppressed while maintaining a low reaction resistance, and as a result, it is helpful to improve the cycle characteristics of the battery. It should be noted that it can be considered that if the metal oxide contained in the carbon phase is greater than a specified amount, the reaction resistance increases sharply and the cycle characteristics cannot be improved.
[0016] Hereinafter, with reference to the accompanying drawings, an example of an embodiment of a nonaqueous electrolyte secondary battery negative electrode active material and a nonaqueous electrolyte secondary battery using the negative electrode active material of the present invention is described in detail. It should be noted that the configuration formed by selectively combining the various constituent elements of the multiple embodiments and variations described below is included in the scope of the present invention.
[0017] Hereinafter, as a non-aqueous electrolyte secondary battery, a cylindrical battery in which a wound electrode body 14 is contained in an outer packaging can 16 having a bottomed cylindrical shape is exemplified, but the outer packaging body of the battery is not limited to a cylindrical outer packaging can. The non-aqueous electrolyte secondary battery of the present invention may be, for example, a square battery having a square outer packaging can, or a button-shaped battery having a button-shaped outer packaging can, or may be a soft-pack battery having an outer packaging body composed of a laminate sheet including a metal layer and a resin layer. In addition, the electrode body is not limited to a wound type, and may also be a stacked electrode body in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked with a separator.
[0018] Figure 1 FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery 10 as an example of an embodiment. Figure 1As shown, the nonaqueous electrolyte secondary battery 10 includes a wound electrode body 14, a nonaqueous electrolyte (not shown), and an outer can 16 for housing the electrode body 14 and the nonaqueous electrolyte. The electrode body 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a winding structure in which the positive electrode 11 and the negative electrode 12 are wound in a spiral shape with the separator 13 interposed therebetween. The outer can 16 is a metal container in a bottomed cylindrical shape with one end side opened in the axial direction, and the opening of the outer can 16 is sealed by a sealing body 17. In the following, for the convenience of explanation, the sealing body 17 side of the battery is set as the upper side, and the bottom side of the outer can 16 is set as the lower side.
[0019] The non-aqueous electrolyte comprises a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous solvent may be, for example, esters, ethers, nitriles, amides, and mixed solvents of two or more thereof. As an example of a non-aqueous solvent, ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and mixed solvents thereof may be cited. The non-aqueous solvent may also contain a halogen substitute (e.g., fluoroethylene carbonate (FEC), etc.) in which at least a portion of the hydrogen of these solvents is replaced by a halogen atom such as fluorine. When FEC is added, an example of a suitable addition amount is 0.5 to 5% by mass of the mass of the non-aqueous solvent. The electrolyte salt may be, for example, a lithium salt such as LiPF6. In addition, 1 to 5% by mass of vinylene carbonate (VC) may be added relative to the mass of the non-aqueous electrolyte.
[0020] The positive electrode 11, the negative electrode 12, and the separator 13 constituting the electrode body 14 are all long strips, which are alternately stacked in the radial direction of the electrode body 14 by being wound into a spiral shape. In order to prevent the precipitation of lithium, the negative electrode 12 is formed to be one circle larger than the positive electrode 11. That is, the negative electrode 12 is formed longer in the length direction and the width direction (short side direction) than the positive electrode 11. The separator 13 is formed to be at least one circle larger than the positive electrode 11, for example, two sheets are arranged in a manner of sandwiching the positive electrode 11. The electrode body 14 has a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like.
[0021] The positive electrode 11 has a positive electrode core and a positive electrode mixture layer formed on the positive electrode core. The positive electrode core can be made of a foil of a metal such as aluminum or aluminum alloy that is stable in the potential range of the positive electrode 11, or a film having the metal disposed on the surface. The positive electrode mixture layer contains a positive electrode active material, a conductive agent, and a binder, and the positive electrode mixture layer is preferably formed on both sides of the positive electrode core except for the exposed portion where the positive electrode lead 20 is welded. For example, a positive electrode mixture slurry containing a positive electrode active material, a conductive agent, and a binder is applied to the positive electrode core, and after the coating is dried, it is compressed to form a positive electrode mixture layer on both sides of the positive electrode core, thereby making the positive electrode 11.
[0022] The positive electrode mixture layer contains a particulate lithium metal composite oxide as a positive electrode active material. The lithium metal composite oxide is a composite oxide containing metal elements such as Co, Mn, Ni, and Al in addition to Li. The metal element constituting the lithium metal composite oxide is, for example, at least one selected from Mg, Al, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, Y, Zr, Sn, Sb, W, Pb, and Bi. Among them, it is preferred to contain at least one selected from Co, Ni, and Mn. As an example of a suitable composite oxide, a lithium metal composite oxide containing Ni, Co, and Mn and a lithium metal composite oxide containing Ni, Co, and Al can be cited.
[0023] As the conductive agent contained in the positive electrode mixture layer, carbon black such as acetylene black and ketjen black, graphite, carbon nanotubes (CNT), carbon nanofibers, graphene and other carbon materials can be exemplified. As the binder contained in the positive electrode mixture layer, fluorine-containing resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, etc. can be exemplified. In addition, these resins and carboxymethyl cellulose (CMC) or its salt, polyethylene oxide (PEO), etc. can also be used in combination.
[0024] The negative electrode 12 has a negative electrode core and a negative electrode mixture layer formed on the negative electrode core. The negative electrode core can be made of a foil of a metal such as copper or copper alloy that is stable in the potential range of the negative electrode 12, or a film having the metal disposed on the surface. The negative electrode mixture layer contains a negative electrode active material, a binder, and a conductive agent used as needed, and is preferably formed on both sides of the negative electrode core except for the exposed portion where the negative electrode lead 21 is welded. A negative electrode mixture slurry containing a negative electrode active material and a binder is applied to the surface of the negative electrode core, and after the coating is dried, it is compressed to form negative electrode mixture layers on both sides of the negative electrode core, thereby making the negative electrode 12.
[0025] The binder contained in the negative electrode mixture layer can also use fluorine-containing resin, PAN, polyimide, acrylic resin, polyolefin, etc. in the same way as in the case of the positive electrode 11, but preferably styrene-butadiene rubber (SBR) is used. In addition, the negative electrode mixture layer preferably contains CMC or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol (PVA), etc. Among them, it is suitable to use SBR with CMC or its salt, PAA or its salt, etc. A conductive agent such as CNT may also be contained in the negative electrode mixture layer.
[0026] The separator 13 can use a porous sheet with ion permeability and insulation. Specific examples of the porous sheet include microporous films, woven fabrics, non-woven fabrics, etc. The material of the separator 13 is preferably polyolefins such as polyethylene and polypropylene, cellulose, etc. The separator 13 can be a single-layer structure or a multi-layer structure. In addition, a resin layer with high heat resistance such as aromatic polyamide resin can be formed on the surface of the separator 13. A filler layer containing an inorganic filler can be formed at the interface between the separator 13 and at least one selected from the positive electrode 11 and the negative electrode 12.
[0027] Insulating plates 18 and 19 are disposed above and below the electrode body 14 , respectively. Figure 1 In the example shown, the positive electrode lead 20 extends toward the sealing body 17 through the through hole of the insulating plate 18, and the negative electrode lead 21 extends toward the bottom side of the outer can 16 through the outer side of the insulating plate 19. The positive electrode lead 20 is connected to the lower surface of the internal terminal plate 23 of the sealing body 17 by welding or the like, and the cap 27 as the top plate of the sealing body 17 electrically connected to the internal terminal plate 23 serves as the positive terminal. The negative electrode lead 21 is connected to the inner surface of the bottom of the outer can 16 by welding or the like, and the outer can 16 serves as the negative terminal.
[0028] A gasket 28 is provided between the outer can 16 and the sealing body 17 to ensure the airtightness of the battery interior. A groove 22 is formed in the outer can 16, with a portion of the side surface bulging inward to support the sealing body 17. The groove 22 is preferably formed in an annular shape along the circumferential direction of the outer can 16, and the sealing body 17 is supported by its upper surface. The sealing body 17 is fixed to the upper part of the outer can 16 by using the groove 22 and the open end of the outer can 16 that is caulked to the sealing body 17.
[0029] The sealing body 17 has a structure in which an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26 and a cap 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective central portions, and an insulating member 25 is sandwiched between their respective peripheral portions. When the internal pressure of the battery rises due to abnormal heat, the lower valve body 24 is deformed and broken in a manner that pushes the upper valve body 26 toward the cap 27 side, thereby blocking the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure rises further, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.
[0030] Below, in reference Figure 2 At the same time, the negative electrode active material is described in detail.
[0031] Figure 2Schematically showing a particle cross section of a Si-containing composite material 30 as an example of an embodiment. The negative electrode 12 contains at least the Si-containing composite material 30 as a negative electrode active material, preferably the Si-containing composite material 30 and graphite. If the Si-containing composite material 30 and graphite are used as negative electrode active materials, it is easy to achieve both high capacity and excellent cycle characteristics. The content of graphite is, for example, 70 to 99% by mass, preferably 75 to 97% by mass, relative to the total mass of the negative electrode active material.
[0032] Graphite can be any of artificial graphites such as blocky artificial graphite (MAG), graphitized mesophase carbon microbeads (MCMB), and natural graphites such as flaky graphite, blocky graphite, and earthy graphite. The volume-based median particle size of graphite (hereinafter referred to as "D50") is not particularly limited, but is preferably 10 to 30 μm, more preferably 15 to 25 μm. D50 means the particle size at which the accumulation of frequencies in the volume-based particle size distribution reaches 50% from the smaller side of the particle size. The particle size distribution of graphite can be measured using a laser diffraction particle size distribution measuring device (e.g., SALD-2000A manufactured by Shimadzu Corporation) and using water as a dispersion medium.
[0033] like Figure 2 As shown, the Si-containing composite material 30 includes a carbon phase 31 and silicon 32 and a metal oxide 35 dispersed in the carbon phase 31. The Si-containing composite material 30 has a mother particle 33 including a carbon phase 31 and silicon 32, and preferably a conductive layer 34 is formed on the surface of the mother particle 33. The mother particle 33 has a sea island structure in which fine silicon 32 and metal oxide 35 are dispersed in the matrix of the carbon phase 31. It can be considered that by adding a specified amount of metal oxide 35 to the carbon phase 31, the side reaction with the electrolyte can be effectively suppressed while maintaining a low reaction resistance, and the cycle characteristics of the battery are greatly improved. The Si-containing composite material 30 can be composed only of the mother particle 33, but from the viewpoint of preventing the contact between the silicon 32 and the non-aqueous electrolyte, the Si-containing composite material 30 preferably has a conductive layer 34.
[0034] The D50 of the Si-containing composite material 30 is preferably smaller than the D50 of graphite. By mixing the Si-containing composite material 30 with a small particle size and the graphite with a large particle size, the filling density of the negative electrode active material in the negative electrode mixture layer becomes higher, which helps to increase the capacity of the battery. The D50 of the Si-containing composite material 30 can be measured using the same method as the D50 of graphite, preferably 2 to 20 μm, and more preferably 3 to 15 μm. If the D50 is within this range, the surface area of the Si-containing composite material 30 is of an appropriate size, and side reactions with non-aqueous electrolytes are easily suppressed.
[0035] Silicon 32 is dispersed in the amorphous carbon phase 31 with ion conductivity in the state of fine-sized particles described later, and Li ions are repeatedly absorbed and released as the battery is charged and discharged. The Si-containing composite material 30 exhibits capacity through the Faraday reaction in which silicon 32 participates. Silicon 32 is a negative electrode active material with a higher capacity than graphite, and the degree of expansion and contraction accompanying charging and discharging is also large. However, since silicon 32 is dispersed in the carbon phase 31, the stress caused by the volume change of silicon 32 is relieved by the carbon phase 31. In addition, the carbon phase 31 can prevent silicon 32 from contacting with the non-aqueous electrolyte, and can suppress side reactions.
[0036] The content of silicon 32 is limited to 60% by mass or less relative to the mass of the Si-containing composite material 30. If the content of silicon 32 is greater than 60% by mass, the particles are prone to breakage due to, for example, a large volume change of the particles accompanying charge and discharge. It is believed that as a result, a side reaction between the non-aqueous electrolyte and silicon 32 is likely to occur, and the cycle characteristics of the battery are greatly reduced.
[0037] On the other hand, if the content of silicon 32 is too low, the capacity of the Si-containing composite material 30 is reduced, so the content of silicon 32 relative to the mass of the Si-containing composite material 30 is preferably 20% by mass or more, more preferably 30% by mass or more, and particularly preferably 40% by mass or more. The appropriate content of silicon 32 is 30 to 60% by mass, more preferably 40 to 55% by mass.
[0038] Silicon 32 is composed of a plurality of microcrystals, for example. The microcrystal size of silicon 32 is preferably less than 30 nm, more preferably less than 20 nm, and particularly preferably less than 15 nm. In this case, the volume change of the Si-containing composite material 30 caused by the expansion and contraction of silicon 32 accompanying charge and discharge can be reduced, and the improvement effect of the cycle characteristics becomes more significant. The microcrystal size of silicon 32 can be calculated using the Scherrer formula based on the half-value width of the diffraction peak of the Si (iii) plane obtained by X-ray diffraction (XRD) measurement of the Si-containing composite material 30.
[0039] The average particle size of silicon 32 is preferably less than 500 nm, more preferably less than 200 nm, and particularly preferably less than 50 nm at least before the first charge and discharge. By dispersing silicon 32 in a finer manner, the volume change of the Si-containing composite material 30 during charge and discharge becomes smaller, and the stability of the particle structure is further improved. The average particle size of silicon 32 can be obtained by observing the particle cross-section of the Si-containing composite material 30 using a scanning electron microscope (SEM). Specifically, any 100 silicon 32 are selected from the SEM image of the cross-section of the Si-containing composite material 30 and the diameter of the circumscribed circle of each particle is measured, and each measured value is averaged and obtained.
[0040] The carbon phase 31 is a continuous phase of amorphous carbon. The carbon phase 31 has good ion conductivity, and Li ions are supplied to the silicon 32 via the carbon phase 31. The amorphous carbon constituting the carbon phase 31 is, for example, a carbon material having an average plane spacing of the (002) plane obtained by XRD measurement of more than 0.34 nm, which can be obtained by heat treating asphalt having a softening point of 200°C or more at a temperature of 700 to 900°C. The conductive layer 34 is also formed by heat treatment of asphalt, but the carbon phase 31 is preferably formed using asphalt having a higher softening point than the conductive layer 34.
[0041] The carbon phase 31 contains a metal oxide 35 on the basis of containing silicon 32. The metal oxide 35 is preferably not biased around the silicon 32, but is roughly uniformly dispersed in the entire carbon phase 31. The content of the metal oxide 35 is 0.001 to 2% by mass relative to the mass of the Si-containing composite material 30. It can be considered that if the content of the metal oxide 35 is greater than 2% by mass, the reaction resistance rises sharply and the improvement effect of the cycle characteristics cannot be obtained. In addition, if the content is less than 0.001% by mass, the effect of adding the metal oxide 35 cannot be manifested, and the improvement effect of the cycle characteristics cannot be obtained.
[0042] The content of the metal oxide 35 is preferably 0.1 to 2 mass%, more preferably 0.5 to 2 mass%, and particularly preferably 1 to 2 mass% relative to the mass of the Si-containing composite material 30. It is believed that if the content of the metal oxide 35 is within this range, the side reaction between the Si-containing composite material 30 and the electrolyte can be effectively suppressed, and the effect of improving the cycle characteristics becomes more significant, compared with the case where the content is out of this range.
[0043] The metal oxide 35 is dispersed in the carbon phase 31 in the form of particles having a size equal to or smaller than that of the silicon 32, for example. It can be said that the metal oxide 35 is dispersed in the carbon phase 31 in the form of fine particles, similarly to the silicon 32. When the average particle size of the metal oxide 35 is larger than the average particle size of the silicon 32, the dispersibility of the silicon 32 decreases and tends to be concentrated in a part of the carbon phase 31. The average particle size of the metal oxide 35 is preferably 500 nm or less, more preferably 200 nm or less, and particularly preferably 50 nm or less.
[0044] The metal oxide 35 is a metal oxide that does not react with Li. As specific examples, zirconium oxide, aluminum oxide, titanium oxide, nickel oxide, yttrium oxide, etc. can be cited. Among them, it is preferably at least one selected from zirconium oxide (ZrO2), aluminum oxide (Al2O3) and titanium oxide (TiO2). By using ZrO2, Al2O3, or TiO2 as the metal oxide 35, the improvement effect of the cycle characteristics becomes more significant. Particularly suitable metal oxide 35 is ZrO2 or TiO2.
[0045] The content of the elements in the carbon phase 31 can be measured by inductively coupled plasma emission spectrometry (ICP). Specifically, the Si-containing composite material 30 is dissolved in a heated acid solution (a mixed acid of hydrofluoric acid, nitric acid, and sulfuric acid), and the carbon in the solution residue is filtered out. Thereafter, the obtained filtrate is analyzed by ICP to determine the content of the elements in the carbon phase 31. In addition, the carbon content in the Si-containing composite material 30 can be measured using a carbon-sulfur analyzer (e.g., EMIA-520 manufactured by Horiba, Ltd.).
[0046] As shown above, the Si-containing composite material 30 has a conductive layer 34 formed on the surface of the mother particle 33. The conductive layer 34 covers at least a portion of the surface of the mother particle 33, preferably substantially covering the entire surface of the mother particle 33. The conductive layer 34 is a thin film layer containing a conductive material, which improves the conductivity of the Si-containing composite material 30. The thickness of the conductive layer 34 is preferably thin enough not to affect the particle size of the Si-containing composite material 30. Regarding the thickness of the conductive layer 34, if the conductivity and the diffusivity of Li ions are considered, it is preferably 1 to 200 nm, and more preferably 5 to 100 nm. The thickness of the conductive layer 34 can be measured by observing the particle cross-section using SEM. It should be noted that the Si-containing composite material 30 can be composed only of the mother particle 33, but the presence of the conductive layer 34 can more reliably prevent the contact between silicon 32 and the non-aqueous electrolyte.
[0047] The conductive material constituting the conductive layer 34 is preferably a conductive carbon material. As the carbon material, amorphous carbon, graphite (natural graphite, artificial graphite, graphitized mesophase carbon, etc.), soft carbon (easily graphitized carbon), hard carbon, etc. can be used. Among them, amorphous carbon is preferred from the perspective of easily forming a thin conductive layer 34 covering the surface of the mother particle 33. As amorphous carbon, carbon black, a burnt product of asphalt, coke, activated carbon, etc. can be cited. Among them, a burnt product of asphalt is preferred.
[0048] The Si-containing composite material 30 can be made, for example, by mixing silicon powder, metal oxide powder and amorphous carbon such as asphalt, heat treating the mixture and pulverizing it. By heat treating the mixture, a mother particle 33 in which silicon 32 and metal oxide 35 are dispersed in a carbon phase 31 can be obtained. The mixing and heat treatment of the raw materials are preferably carried out in an inert atmosphere (for example, an atmosphere of argon, nitrogen, etc.). The mixing of the raw materials can be carried out using a ball mill, for example. The powders of silicon and metal oxides preferably use materials with an average particle size of less than 1 μm.
[0049] The above-mentioned heat treatment is performed in an inert atmosphere, for example, at a temperature of 450 to 1000° C. If the heat treatment temperature is within this range, it is easy to form a sea island structure in which tiny particles of silicon 32 and metal oxide 35 are dispersed in the carbon phase 31 with low crystallinity. The heat treatment temperature is preferably 600 to 950° C., and more preferably 700 to 900° C. The heat treatment time is, for example, 1 to 10 hours. The heat treatment conditions also affect the crystallites of silicon 32. Generally, the higher the temperature, the larger the crystallite size.
[0050] The manufacturing process of the Si-containing composite material 30 further includes a process of forming a conductive layer 34 on the surface of the mother particle 33. As for the method of forming a carbon film as the conductive layer 34, there can be exemplified a CVD method using hydrocarbon gas such as acetylene and methane as a raw material, a method of mixing coal tar, petroleum asphalt, phenolic resin, etc. with the mother particle 33 and heat-treating it, etc. For example, the mixture of the mother particle 33 and asphalt is heat-treated at 700 to 900° C. in an inert atmosphere, thereby obtaining a Si-containing composite material 30 having a conductive layer 34 of amorphous carbon formed on the surface of the mother particle 33.
[0051] Example
[0052] Hereinafter, the present invention will be further described using experimental examples; however, the present invention is not limited to these experimental examples.
[0053] <Experimental Example 1>
[0054] [Production of positive electrode]
[0055] Use LiCo 0.979 Zr 0.001 Mg 0.01 Al 0.01 The composite oxide represented by O2 is used as the positive electrode active material. The positive electrode active material, acetylene black and PVDF are mixed at a solid content mass ratio of 95:2.5:2.5, and N-methyl-2-pyrrolidone (NMP) is used as a dispersion medium to prepare a positive electrode mixture slurry. Then, the positive electrode mixture slurry is applied to the surface of the positive electrode core made of aluminum foil using a scraper method, and the coating is dried and rolled, and then cut into a given electrode size to obtain a positive electrode with a positive electrode mixture layer formed on both sides of the positive electrode core.
[0056] [Production of negative electrode active material (composite material)]
[0057] In an inert atmosphere, silicon powder (purity ≥ 99.9%, average particle size 100nm), zirconium oxide powder (average particle size 5nm) and pitch (softening point 225-275°C, solid carbon content ≥ 70% by mass) were mixed and mixed for 1 hour using a ball mill. The mixture was heat treated at 800°C for 5 hours in an inert atmosphere, crushed using a roll crusher, and then further crushed using a jet mill to obtain a crushed product with a D50 of 10μm. The crushed product is the mother particle of the composite material.
[0058] Next, the mother particles and asphalt (softening point ≤ 100 ° C, solid carbon content ≥ 55% by mass) are mixed, heat treated at 800 ° C in an inert atmosphere for 5 hours, and then crushed using a roll crusher and a jet mill until D50 is 6 μm, thereby forming a carbon film on the surface of the mother particles to obtain a Si-containing composite material (D50: about 6 μm) in which fine zirconium oxide is dispersed in the carbon phase. The composition (element concentration) of the composite material is confirmed by ICP. Relative to the mass of the Si-containing composite material, the content of silicon is 50% by mass and the content of zirconium oxide is 1% by mass. In addition, the D50 of the composite material is measured using a laser diffraction particle size distribution measuring device (manufactured by Shimadzu Corporation, SALD-2000A) with water as the dispersion medium.
[0059] [Production of negative electrode]
[0060] A material obtained by mixing the above composite material and graphite with a D50 of about 22 μm in a mass ratio of 5:95 is used as a negative electrode active material. A dispersion of the negative electrode active material, CMC Na salt and SBR is mixed in a solid component mass ratio of 97.5:1.5:1.0, and water is used as a dispersion medium to prepare a negative electrode mixture slurry. Then, the negative electrode mixture slurry is applied to the surface of a negative electrode core made of copper foil using a scraper method, and after the coating is dried and rolled, it is cut into a given electrode size to obtain a negative electrode with a negative electrode mixture layer formed on both sides of the negative electrode core.
[0061] [Preparation of non-aqueous electrolyte]
[0062] Lithium hexafluorophosphate (LiPF6) was dissolved at a concentration of 1 mol / L in a solvent obtained by mixing ethylene carbonate (EC) and methyl ethyl carbonate (MEC) in a volume ratio of 3:7 (25°C), and vinylene carbonate (VC) was added at a concentration of 2% by mass to prepare a non-aqueous electrolyte.
[0063] [Fabrication of non-aqueous electrolyte secondary battery]
[0064] After the positive electrode and the negative electrode are wound into a spiral shape with a polyethylene separator sandwiched therebetween, a polypropylene winding fixing tape is attached to the outermost circumference, and the wound body is pressed into a flat shape to obtain an electrode body. A laminate sheet having a five-layer structure of resin layer (polypropylene) / adhesive layer / aluminum alloy layer / adhesive layer / resin layer (polypropylene) is processed to form an outer packaging body, and the electrode body and non-aqueous electrolyte are contained in the outer packaging body in an inactive atmosphere. Thereafter, the interior of the outer packaging body is depressurized to allow the electrolyte to penetrate the separator, and the opening of the outer packaging body is sealed to produce a soft-pack type non-aqueous electrolyte secondary battery with a length of 62 mm, a width of 35 mm, and a thickness of 3.6 mm.
[0065] <Experimental Example 2>
[0066] A nonaqueous electrolyte secondary battery was produced in the same manner as in Experimental Example 1 except that the content of zirconium oxide was changed to 0.001 mass % based on the mass of the Si-containing composite material.
[0067] <Experimental Example 3>
[0068] A nonaqueous electrolyte secondary battery was produced in the same manner as in Experimental Example 1 except that the content of zirconium oxide was changed to 2 mass % based on the mass of the Si-containing composite material.
[0069] <Experimental Example 4>
[0070] A nonaqueous electrolyte secondary battery was produced in the same manner as in Experimental Example 1 except that zirconium oxide was replaced with aluminum oxide (average particle size: 50 nm).
[0071] <Experimental Example 5>
[0072] A nonaqueous electrolyte secondary battery was produced in the same manner as in Experimental Example 1 except that zirconium oxide was replaced with titanium oxide (average particle size: 25 nm).
[0073] <Experimental Example 6>
[0074] A nonaqueous electrolyte secondary battery was produced in the same manner as in Experimental Example 1 except that the silicon content was changed to 60 mass % based on the mass of the Si-containing composite material.
[0075] <Experimental Example 7>
[0076] A nonaqueous electrolyte secondary battery was produced in the same manner as in Experimental Example 1 except that zirconium oxide was not added.
[0077] <Experimental Example 8>
[0078] A nonaqueous electrolyte secondary battery was produced in the same manner as in Experimental Example 1 except that the content of zirconium oxide was changed to 5 mass % based on the mass of the Si-containing composite material.
[0079] <Experimental Example 9>
[0080] A nonaqueous electrolyte secondary battery was produced in the same manner as in Experimental Example 1 except that the silicon content was changed to 70 mass % based on the mass of the Si-containing composite material.
[0081] The capacity retention rate of the battery of each experimental example was evaluated by the following method. The evaluation results are shown in Table 1 together with the composition of the composite material.
[0082] [Evaluation of cycle characteristics]
[0083] The battery to be evaluated was charged at a constant current of 1 It (800 mA) at 25°C until the voltage reached 4.2 V, and then charged at a constant voltage of 4.2 V until the current reached 1 / 20 It (40 mA). Thereafter, the battery was discharged at a constant current of 1 It (800 mA) at 25°C until the voltage reached 2.75 V. This charge and discharge was repeated for 300 cycles, and the ratio of the discharge capacity at the 300th cycle to the discharge capacity at the 1st cycle was calculated as the capacity retention rate.
[0084] [Table 1]
[0085]
[0086] According to the results shown in Table 1, it can be understood that the batteries of Experimental Examples 1 to 6 have a high capacity retention rate in the cycle test and excellent cycle characteristics compared with the previous battery (Experimental Example 7) using a Si-containing composite material that does not contain metal oxides such as ZrO2 in the carbon phase. In addition, even when ZrO2 is contained, when its content is greater than 2% by mass and when the content of silicon is greater than 60% by mass, the improvement effect of the cycle characteristics cannot be obtained.
[0087] When Al2O3 and TiO2 are added instead of ZrO2, good cycle characteristics can also be obtained (refer to Experimental Examples 1, 4, and 5). However, when a Si-containing composite material with added ZrO2 or TiO2 is used as the metal oxide, the improvement in cycle characteristics is more significant.
[0088] Description of Reference Numerals
[0089] 10 non-aqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 16 outer packaging can, 17 sealing body, 18, 19 insulating plates, 20 positive electrode lead, 21 negative electrode lead, 22 slotted portion, 23 internal terminal plate, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cap, 28 gasket, 30 Si-containing composite material, 31 carbon phase, 32 silicon, 33 mother particle, 34 conductive layer, 35 metal oxide.
Claims
1. A negative electrode active material for a non-aqueous electrolyte secondary battery, The invention has a Si-containing composite material including an amorphous carbon phase and silicon and a metal oxide dispersed in the carbon phase. The content of the metal oxide is 0.001 mass % to 2 mass % relative to the mass of the Si-containing composite material. The content of the silicon is 60 mass % or less relative to the mass of the Si-containing composite material.
2. The negative electrode active material according to claim 1, wherein The metal oxide is at least one selected from zirconium oxide, aluminum oxide and titanium oxide.