Preparation method of BOPA (Biaxially Oriented Polyamide) film containing graphene oxide-based nano composite material

By loading graphene oxide onto the surface of polyamide films, the problems of weakened bactericidal effect and environmental hazards of nanomaterials are solved, achieving efficient and environmentally friendly bactericidal effect and cost reduction, which is suitable for seawater desalination and wastewater reuse treatment.

CN118949710APending Publication Date: 2024-11-15HESHAN YUNCHENG NEW MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411033281.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The bactericidal effect of nanomaterials doped in existing polyamide films weakens over time and is harmful to the environment, limiting their large-scale application. Graphene oxide is ineffective in the film and is costly.

Method used

Graphene oxide was loaded onto the surface of a polyamide film, and a polyamide-polysulfone hollow fiber composite film was prepared by interfacial polymerization. The composite film was then reacted with a mixed solution of graphene oxide to form a polyamide film loaded with graphene oxide nanosheets.

Benefits of technology

It improves the membrane's inhibitory effect on bacterial growth, which does not weaken over time, reduces the amount of graphene oxide used, lowers costs, maintains permeability and filtration capacity, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949710A_ABST
    Figure CN118949710A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a BOPA film containing a graphene oxide-based nanocomposite, which comprises the following steps: S1, preparing graphene, adding graphite into a mixed solution of sulfuric acid and phosphoric acid, carrying out ultrasonic treatment to obtain a reaction solution, adding potassium permanganate powder into the reaction solution, and stirring; according to the invention, the graphene oxide is loaded on the surface of the polyamide film, so that the inhibition effect of the film on the growth of bacteria is not weakened along with the increase of time, meanwhile, the permeability and filtering capacity of the polyamide film are not influenced, the cleaning times of the film are reduced, and the service life of the film is prolonged; the graphene oxide is loaded on the surface of the polyamide film, so that the usage amount of the graphene oxide is greatly reduced, the production cost is reduced, the raw materials are saved, the environment is protected, the use effect is improved, and the polyamide film can be widely applied to seawater desalination and sewage regeneration treatment and has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thin films, in particular to a method for manufacturing a BOPA film containing a graphene oxide-based nanocomposite material. Background Art

[0002] The commonly used method is to dope the polyamide film with bactericidal nanomaterials, such as silver nanoparticles. However, the bactericidal effect of nanoparticles will gradually decrease over time; at the same time, if they cannot be recycled in time, the nanoparticles will harm the environment, which also limits the large-scale practical application of such materials.

[0003] In addition, graphene is a new type of two-dimensional planar nanomaterial, which is composed of a dense layer of carbon atoms wrapped in a honeycomb crystal lattice. Its thickness is only 0.35nm, and it has extremely high adsorption and permeability; oxidized graphene can also be obtained by chemical oxidation of graphene, and the cost is relatively low. Oxidized graphene can effectively inhibit the growth of bacteria on the surface of polyamide composite film, and this effect will not decrease with the growth of time, and there is no need to repeatedly clean the film, which increases the service life of the film. However, this bactericidal effect of graphene oxide must be through direct contact with bacterial cells. If graphene oxide is placed in the film, it is ineffective in killing microorganisms and bacteria. Moreover, since nanomaterials are expensive, they may also have an impact on the environment.

[0004] To this end, we introduce a method for manufacturing BOPA films containing graphene oxide-based nanocomposites. Summary of the invention

[0005] The object of the present invention is to provide a method for manufacturing a BOPA film containing a graphene oxide-based nanocomposite material to solve the problems raised in the above background technology.

[0006] To achieve the above object, the present invention provides the following technical scheme: A method for manufacturing a BOPA film containing a graphene oxide-based nanocomposite material, comprising: S1, preparing graphene, adding 1.5 g of graphite to 200 mL of a mixed solution of sulfuric acid and phosphoric acid in a volume ratio of 9:1, and simultaneously ultrasonically treating to obtain a reaction solution, adding 5 to 10 g of potassium permanganate powder to the reaction solution, and stirring continuously, slowly heating the solution to a constant temperature of 50° C., and stirring for 12 h to obtain a graphene solution;

[0007] S2. Prepare graphene oxide, restore the graphene solution to room temperature, add 3-5 mL of hydrogen peroxide, and dilute it to 2 L with distilled water, pass the solution through a 44-μm standard metal test sieve, and use a polytetrafluoroethylene syringe filter with a pore size of 5 μm to perform vacuum filtration, and collect the solid components in the filtrate;

[0008] S3, preparing a polyamide and polysulfone hollow fiber composite membrane, using a polysulfone hollow fiber ultrafiltration membrane as a base membrane, m-phenylenediamine as an aqueous phase monomer, and trimesoyl chloride as an organic phase monomer, and preparing a polyamide and polysulfone hollow fiber composite membrane by an interfacial polymerization method;

[0009] First, 12% by mass of polysulfone glass powder is added to 1-methyl-2-pyrrolidone with a purity greater than 99.5%, and stirred until completely dissolved, and the mixed solution is placed in a desiccator and dried overnight to obtain a mixed solution;

[0010] Next, the film support is immersed in a 3.4% by mass m-phenylenediamine aqueous solution for 1 to 5 minutes, and after being taken out and the excess solution is removed, it is immersed in a 0.15% by mass trimesoyl chloride organic phase solution for 1 minute, so that a dense polymer cortex is formed on the film support through the interface reaction between m-phenylenediamine and trimesoyl chloride;

[0011] Then, the polymer skin layer was sequentially immersed in 95°C distilled water for 2 minutes, in 200 ppm sodium hypochlorite aqueous solution for 2 minutes, and in 1000 ppm sodium bisulfite aqueous solution for 30 seconds, and then washed and stored in distilled water at 4°C to obtain a polyamide and polysulfone hollow fiber composite membrane;

[0012] S4, functionalizing the surface of the composite membrane, wrapping and covering the obtained polyamide and polysulfone hollow fiber composite membrane with a frame, exposing only the polymer cortex on the top of the film, so that ethylenediamine is attached to the surface of the composite film, and a treated polyamide and polysulfone hollow fiber composite membrane is obtained;

[0013] Secondly, 10 to 15 mg of graphene oxide is uniformly added into 10 mL of a buffer solution of 10 mmol / L fatty acid methyl ester sulfonate with a pH of 6, and ultrasonic treatment is performed for 10 to 15 minutes to form a stable suspension;

[0014] The suspension was centrifuged, and the supernatant was transferred into 40 mL of 10 mmol / L fatty acid methyl ester sulfonate buffer with a pH of 6 at room temperature for reaction for 15 min to obtain a mixed solution of graphene oxide;

[0015] Then, the treated polyamide and polysulfone hollow fiber composite membrane were contacted with a mixed solution of graphene oxide for reaction, and a mixed solution of 2 mmol / L of dichloroethane and 5 mmol / L of hydroxysuccinimide was added to obtain a reactant. The reactant was rinsed with distilled water, and the graphene oxide that failed to adhere to the surface of the composite film was removed by ultrasonic treatment for 2 minutes to obtain a polyamide film loaded with graphene oxide nanosheets.

[0016] Preferably, according to S2, the collected solid component is washed with 100 mL of distilled water, 100 mL of 1:10 hydrochloric acid solution, 100 mL of distilled water and 100 mL of ethanol in sequence, and the supernatant is removed after centrifugation of the mixed solution each time to obtain a solid material;

[0017] The solid material was subjected to 72 hours of dialysis purification, and then filtered through a polytetrafluoroethylene syringe filter with a pore size of 0.45 micrometers, and dried under vacuum conditions, finally obtaining graphene oxide flakes with a width of 30 to 650 nanometers.

[0018] Preferably, according to S3, the polyester non-woven fabric is bonded to a clean glass plate and moistened with 1-methyl-2-pyrrolidone, 5 to 15 mL of the above-mentioned reaction mixture is poured on one end of the moistened polyester non-woven fabric, and the reaction mixture is evenly applied to the non-woven fabric using a coater to obtain a treated glass plate, and the treated glass plate is placed in a distilled water gel bath for 10 to 15 minutes for phase separation to form a film support.

[0019] Preferably, according to S4, the polymer cortex is contacted with a mixed buffer solution consisting of 4 mmol / L ethylene dichloride with a pH of 5, 10 mmol / L hydroxysuccinimide, 0.5 mol / L sodium chloride, and 10 mmol / L fatty acid methyl ester sulfonate for 1 to 1.5 hours, and then washed twice with distilled water to remove the residual mixed buffer solution on the surface of the composite membrane;

[0020] The polyamide and polysulfone hollow fiber composite membrane is then contacted with a buffer solution consisting of 10 mmol / L ethylenediamine with a pH of 7.5, 0.15 mmol / L sodium chloride and 10 mmol / L hydroxyethylpiperazineethanesulfonic acid for 25 to 35 minutes to obtain a treated polyamide and polysulfone hollow fiber composite membrane.

[0021] Preferably, the mixed solution of S4 hydroxysuccinimide is placed on an orbital shaker and stirred at 70 rpm / min for 10 to 20 min to allow the graphene oxide to adhere to the surface of the polyamide film, and is stored in distilled water at 4°C.

[0022] Compared with the prior art, the present invention has the following beneficial effects: by loading graphene oxide on the surface of a polyamide film, the present invention ensures that the inhibitory effect of the film on bacterial growth will not weaken over time, and will not affect the permeability and filtering capacity of the polyamide film itself, thereby reducing the number of cleaning times of the film and extending the service life of the film.

[0023] Graphene oxide is loaded on the surface of a polyamide film. Compared with the prior art in which graphene oxide is placed inside a polyamide film, the present invention not only greatly reduces the amount of graphene oxide used and reduces production costs, but is also beneficial to saving raw materials and protecting the environment, while also improving the use effect. It can be widely used in seawater desalination and sewage regeneration treatment and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic flow chart of a method for manufacturing a BOPA film containing a graphene oxide-based nanocomposite material according to the present invention;

[0025] Figure 2 This is a schematic diagram of a SEM scanning image of a polyamide film loaded with graphene oxide nanosheets of the present invention;

[0026] Figure 3 The figure is a schematic diagram comparing the bacteria killing effects of the functionalized film modified with graphene oxide of the present invention and the ordinary film without treatment. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] See also Figure 1-3 The present invention provides a technical solution: a method for manufacturing a BOPA film containing a graphene oxide-based nanocomposite material, comprising: S1, preparing graphene, adding 1.5 g of graphite to 200 mL of a mixed solution of sulfuric acid and phosphoric acid in a volume ratio of 9:1, and simultaneously ultrasonically treating to obtain a reaction solution, adding 5 to 10 g of potassium permanganate powder to the reaction solution, and stirring continuously, slowly heating the solution to a constant temperature of 50° C., and stirring for 12 h to obtain a graphene solution;

[0029] S2. Prepare graphene oxide, restore the graphene solution to room temperature, add 3-5 mL of hydrogen peroxide, and dilute it to 2 L with distilled water, pass the solution through a 44-μm standard metal test sieve, and use a polytetrafluoroethylene syringe filter with a pore size of 5 μm to perform vacuum filtration, and collect the solid components in the filtrate;

[0030] S3, preparing a polyamide and polysulfone hollow fiber composite membrane, using a polysulfone hollow fiber ultrafiltration membrane as a base membrane, m-phenylenediamine as an aqueous phase monomer, and trimesoyl chloride as an organic phase monomer, and preparing a polyamide and polysulfone hollow fiber composite membrane by an interfacial polymerization method;

[0031] First, 12% by mass of polysulfone glass powder is added to 1-methyl-2-pyrrolidone with a purity greater than 99.5%, and stirred until completely dissolved, and the mixed solution is placed in a desiccator and dried overnight to obtain a mixed solution;

[0032] Next, the film support is immersed in a 3.4% by mass m-phenylenediamine aqueous solution for 1 to 5 minutes, and after being taken out and the excess solution is removed, it is immersed in a 0.15% by mass trimesoyl chloride organic phase solution for 1 minute, so that a dense polymer cortex is formed on the film support through the interface reaction between m-phenylenediamine and trimesoyl chloride;

[0033] Then, the polymer skin layer was sequentially immersed in 95°C distilled water for 2 minutes, in 200 ppm sodium hypochlorite aqueous solution for 2 minutes, and in 1000 ppm sodium bisulfite aqueous solution for 30 seconds, and then washed and stored in distilled water at 4°C to obtain a polyamide and polysulfone hollow fiber composite membrane;

[0034] S4, functionalizing the surface of the composite membrane, wrapping and covering the obtained polyamide and polysulfone hollow fiber composite membrane with a frame, exposing only the polymer cortex on the top of the film, so that ethylenediamine is attached to the surface of the composite film, and a treated polyamide and polysulfone hollow fiber composite membrane is obtained;

[0035] Secondly, 10 to 15 mg of graphene oxide is uniformly added into 10 mL of a buffer solution of 10 mmol / L fatty acid methyl ester sulfonate with a pH of 6, and ultrasonic treatment is performed for 10 to 15 minutes to form a stable suspension;

[0036] The suspension was centrifuged, and the supernatant was transferred into 40 mL of 10 mmol / L fatty acid methyl ester sulfonate buffer with a pH of 6 at room temperature for reaction for 15 min to obtain a mixed solution of graphene oxide;

[0037] Then, the treated polyamide and polysulfone hollow fiber composite membrane were contacted with a mixed solution of graphene oxide for reaction, and a mixed solution of 2 mmol / L of dichloroethane and 5 mmol / L of hydroxysuccinimide was added to obtain a reactant. The reactant was rinsed with distilled water, and the graphene oxide that failed to adhere to the surface of the composite film was removed by ultrasonic treatment for 2 minutes to obtain a polyamide film loaded with graphene oxide nanosheets.

[0038] According to S2, the collected solid components are washed with 100 mL of distilled water, 100 mL of 1:10 hydrochloric acid solution, 100 mL of distilled water and 100 mL of ethanol in sequence, and the supernatant is removed after centrifugation of the mixed solution each time to obtain a solid material;

[0039] The solid material was subjected to 72 hours of dialysis purification, and then filtered through a polytetrafluoroethylene syringe filter with a pore size of 0.45 micrometers, and dried under vacuum conditions, finally obtaining graphene oxide flakes with a width of 30 to 650 nanometers.

[0040] According to S3, the polyester non-woven fabric is bonded to a clean glass plate and moistened with 1-methyl-2-pyrrolidone, 5 to 15 mL of the above-mentioned reaction mixture is poured on one end of the moistened polyester non-woven fabric, and the reaction mixture is evenly applied to the non-woven fabric using a coater to obtain a treated glass plate, and the treated glass plate is placed in a distilled water gel bath for 10 to 15 minutes for phase separation to form a film support.

[0041] According to S4, the polymer cortex is contacted with a mixed buffer solution consisting of 4 mmol / L ethylene dichloride with a pH of 5, 10 mmol / L hydroxysuccinimide, 0.5 mol / L sodium chloride, and 10 mmol / L fatty acid methyl ester sulfonate for 1 to 1.5 hours, and then washed twice with distilled water to remove the residual mixed buffer solution on the surface of the composite membrane;

[0042] The polyamide and polysulfone hollow fiber composite membrane is then contacted with a buffer solution consisting of 10 mmol / L ethylenediamine with a pH of 7.5, 0.15 mmol / L sodium chloride and 10 mmol / L hydroxyethylpiperazineethanesulfonic acid for 25 to 35 minutes to obtain a treated polyamide and polysulfone hollow fiber composite membrane.

[0043] The mixed solution of S4 hydroxysuccinimide was placed on an orbital shaker and stirred at 70 rpm / min for 10 to 20 min to allow the graphene oxide to adhere to the surface of the polyamide film, and the film was stored in distilled water at 4°C.

[0044] Specifically, when using:

[0045] 1. Preparation of graphene: Add 1.5 g of graphite to 200 mL of a mixed solution of H2SO4 and H3PO4 in a volume ratio of 9:1, and ultrasonically treat for 5 to 10 minutes to obtain a reaction solution, and treat the reaction solution in an ice bath; then, add 5 to 10 g of KMnO4 powder to the reaction solution, and stir continuously. Slowly heat the solution and keep it at 50°C, stir for 12 hours, and obtain a graphene solution.

[0046] 2. Preparation of graphene oxide: First, slowly restore the graphene solution to room temperature, add 3-5 mL of H2O2, and dilute it to 2 L with distilled water. Pass the solution through a 44 μm standard metal test sieve, and use a polytetrafluoroethylene syringe filter with a pore size of 5 μm for vacuum filtration to collect the solid components in the filtrate; then, wash the collected solid components with 100 mL of distilled water, 100 mL of 1:10 hydrochloric acid solution, 100 mL of distilled water, and 100 mL of ethanol in turn, and remove the supernatant after centrifugation of the mixed solution each time to obtain a solid material; finally, the solid material is subjected to 72 h of dialysis purification, and then filtered with a polytetrafluoroethylene syringe filter with a pore size of 0.45 μm, and dried under vacuum conditions to finally obtain graphene oxide flakes with a width of 30 to 650 nm.

[0047] 3. Preparation of polyamide and polysulfone hollow fiber composite membrane: Using polysulfone hollow fiber ultrafiltration membrane as base membrane, m-phenylenediamine as aqueous phase monomer, and trimesoyl chloride as organic phase monomer, polyamide and polysulfone hollow fiber composite membrane were prepared by interfacial polymerization: First, 12% of polysulfone glass powder by mass was added to 1-methyl-2-pyrrolidone with a purity of more than 99.5%, and stirred until completely dissolved. The mixed solution was placed in a dryer and dried overnight to obtain a mixed solution; a polyester non-woven fabric was bonded to a clean glass plate and moistened with 1-methyl-2-pyrrolidone, 5 to 15 mL of the above reaction mixture was poured on one end of the moistened polyester non-woven fabric, and the reaction mixture was evenly applied to the non-woven fabric using a coater to obtain a treated glass plate; the treated glass The plate is placed in a distilled water gel bath for 10 to 15 minutes for phase separation to form a film support; then, the film support is immersed in a 3.4% by mass m-phenylenediamine aqueous solution for 1 to 5 minutes, and after being taken out and the excess solution is removed, it is immersed in a 0.15% by mass trimesoyl chloride organic phase solution for 1 minute to form a dense polymer cortex on the film support through the interface reaction between m-phenylenediamine and trimesoyl chloride; the polymer cortex is sequentially immersed in 95°C distilled water for 2 minutes, 200ppm NaOCl aqueous solution for 2 minutes, and 1000ppm NaHSO3 aqueous solution for 30 seconds, and then it is washed and stored in distilled water at 4°C to obtain a polyamide and polysulfone hollow fiber composite membrane.

[0048] 4. Surface functionalization of the composite membrane: The obtained polyamide and polysulfone hollow fiber composite membrane was wrapped and covered with a frame, exposing only the polymer cortex on the top of the film, and then it was contacted with a mixed buffer solution consisting of 4mmol / L ethylene dichloride, 10mmol / L hydroxysuccinimide, 0.5mol / L NaCl and 10mmol / L fatty acid methyl ester sulfonate at pH 5 for 1 to 1.5 hours, and then washed twice with distilled water to remove the residual mixed buffer solution on the surface of the composite membrane; then the polyamide and polysulfone hollow fiber composite membrane was contacted with a buffer solution consisting of 10mmol / L ethylenediamine, 0.15mmol / L NaCl and 10mmol / L hydroxyethylpiperazine ethanesulfonic acid at pH 7.5 for 25 to 35 minutes, so that ethylenediamine adhered to the surface of the composite film, and the treated polyamide and polysulfone hollow fiber composite membrane was obtained; secondly, 10 to 15mg of graphene oxide was uniformly added to 10mL of 10mmol / L ethylenediamine at pH 6 / L fatty acid methyl ester sulfonate buffer solution, and ultrasonically treat it for 10 to 15 minutes to form a stable suspension; centrifuge the suspension, and transfer the supernatant into 40mL of 10mmol / L fatty acid methyl ester sulfonate buffer solution with a pH of 6 at room temperature for reaction for 15 minutes to obtain a mixed solution of graphene oxide; then, the treated polyamide and polysulfone hollow fiber composite membrane is contacted with the mixed solution of graphene oxide for reaction, and a mixed solution of 2mmol / L ethylene dichloride and 5mmol / L hydroxysuccinimide is added, and placed on an orbital shaker, and stirred at a speed of 70rpm / min for 10 to 20 minutes to allow the graphene oxide to adhere to the surface of the polyamide film to obtain a reactant; rinse the reactant with distilled water, and remove the graphene oxide that cannot be attached to the surface of the composite film by ultrasonic treatment for 2 minutes to obtain a polyamide film loaded with graphene oxide nanosheets, and store it in distilled water at 4°C.

[0049] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for producing a BOPA film containing a graphene oxide-based nanocomposite material, characterized in that: include: S1, preparing graphene, adding graphite to a mixed solution of sulfuric acid and phosphoric acid, and simultaneously ultrasonically treating to obtain a reaction solution, adding potassium permanganate powder to the reaction solution, stirring, and slowly heating the solution to obtain a graphene solution; S2, preparing graphene oxide, after the graphene solution is restored to room temperature, adding hydrogen peroxide, and diluting it with distilled water, passing the solution through a metal test sieve, and vacuum filtering using a polytetrafluoroethylene syringe filter to collect the solid components in the filtrate; S3, preparing a polyamide and polysulfone hollow fiber composite membrane, using a polysulfone hollow fiber ultrafiltration membrane as a base membrane, m-phenylenediamine as an aqueous phase monomer, and trimesoyl chloride as an organic phase monomer, and preparing a polyamide and polysulfone hollow fiber composite membrane by an interfacial polymerization method; S4. Functionalizing the surface of the composite membrane: Wrapping and covering the obtained polyamide and polysulfone hollow fiber composite membrane with a frame, leaving only the polymer cortex on the top of the film exposed, so that ethylenediamine is attached to the surface of the composite film, and a polyamide film loaded with graphene oxide nanosheets is obtained.

2. The method for producing a BOPA film containing a graphene oxide-based nanocomposite material according to claim 1, characterized in that: According to S2, the collected solid components are washed with 100 mL of distilled water, 100 mL of 1:10 hydrochloric acid solution, 100 mL of distilled water and 100 mL of ethanol in sequence, and the supernatant is removed after centrifugation of the mixed solution each time to obtain a solid material; The solid material was subjected to 72 hours of dialysis purification, and then filtered through a polytetrafluoroethylene syringe filter with a pore size of 0.45 micrometers, and dried under vacuum conditions, finally obtaining graphene oxide flakes with a width of 30 to 650 nanometers.

3. The method for producing a BOPA film containing a graphene oxide-based nanocomposite material according to claim 1, characterized in that: According to S3, the polyester non-woven fabric is bonded to a clean glass plate and moistened with 1-methyl-2-pyrrolidone, 5 to 15 mL of the above-mentioned reaction mixture is poured on one end of the moistened polyester non-woven fabric, and the reaction mixture is evenly applied to the non-woven fabric using a coater to obtain a treated glass plate, and the treated glass plate is placed in a distilled water gel bath for 10 to 15 minutes for phase separation to form a film support.

4. The method for producing a BOPA film containing a graphene oxide-based nanocomposite material according to claim 1, characterized in that: According to S4, the polymer cortex is contacted with a mixed buffer solution consisting of 4 mmol / L ethylene dichloride with a pH of 5, 10 mmol / L hydroxysuccinimide, 0.5 mol / L sodium chloride, and 10 mmol / L fatty acid methyl ester sulfonate for 1 to 1.5 hours, and then washed twice with distilled water to remove the residual mixed buffer solution on the surface of the composite membrane; The polyamide and polysulfone hollow fiber composite membrane is then contacted with a buffer solution consisting of 10 mmol / L ethylenediamine, 0.15 mmol / L sodium chloride and 10 mmol / L hydroxyethylpiperazineethanesulfonic acid with a pH of 7.5 for 25 to 35 minutes.

5. The method for producing a BOPA film containing graphene oxide-based nanocomposite material according to claim 1, characterized in that: The mixed solution of S4 hydroxysuccinimide was placed on an orbital shaker and stirred at 70 rpm / min for 10 to 20 min to allow the graphene oxide to adhere to the surface of the polyamide film, and the film was stored in distilled water at 4°C.

6. The method for producing a BOPA film containing graphene oxide-based nanocomposite material according to claim 1, characterized in that: According to S1, 1.5 g of graphite was added to 200 mL of a mixed solution of sulfuric acid and phosphoric acid in a volume ratio of 9:1, and 5 to 10 g of potassium permanganate powder. The solution was slowly heated and kept at a constant temperature of 50°C and stirred for 12 hours.

7. The method for producing a BOPA film containing graphene oxide-based nanocomposite material according to claim 1, characterized in that: According to S3, a mixed solution is obtained by adding 12% by mass of polysulfone glass powder to 1-methyl-2-pyrrolidone with a purity greater than 99.5%, stirring until completely dissolved, and placing the mixed solution in a desiccator to dry overnight; Next, the film support is immersed in a 3.4% by mass m-phenylenediamine aqueous solution for 1 to 5 minutes, and after being taken out and the excess solution is removed, it is immersed in a 0.15% by mass trimesoyl chloride organic phase solution for 1 minute, so that a dense polymer cortex is formed on the film support through the interface reaction between m-phenylenediamine and trimesoyl chloride; Then, the polymer cortex was sequentially soaked in 95°C distilled water for 2 minutes, in 200 ppm sodium hypochlorite aqueous solution for 2 minutes, and in 1000 ppm sodium bisulfite aqueous solution for 30 seconds, and then washed and stored in distilled water at 4°C to prepare a polyamide and polysulfone hollow fiber composite membrane.

8. The method for producing a BOPA film containing graphene oxide-based nanocomposite material according to claim 1, characterized in that: According to S4, 10 to 15 mg of graphene oxide is uniformly added into 10 mL of a buffer solution of 10 mmol / L fatty acid methyl ester sulfonate with a pH of 6, and ultrasonically treated for 10 to 15 min to form a stable suspension; The suspension was centrifuged, and the supernatant was transferred into 40 mL of 10 mmol / L fatty acid methyl ester sulfonate buffer with a pH of 6 at room temperature for reaction for 15 min to obtain a mixed solution of graphene oxide; Then, the treated polyamide and polysulfone hollow fiber composite membrane was contacted with a mixed solution of graphene oxide, and a mixed solution of 2 mmol / L of dichloroethane and 5 mmol / L of hydroxysuccinimide was added to obtain a reactant. The reactant was rinsed with distilled water, and the graphene oxide that failed to adhere to the surface of the composite film was removed by ultrasonic treatment for 2 minutes.

9. The method for producing a BOPA film containing graphene oxide-based nanocomposite material according to claim 1, characterized in that: According to S2, hydrogen peroxide is 3-5mL and diluted to 2L with distilled water.

10. The method for producing a BOPA film containing graphene oxide-based nanocomposite material according to claim 1, characterized in that: The S2 metal test sieve is standardly 44 microns, while the pore size of the PTFE syringe filter is 5 microns.

Citation Information

Cited By

  • Modification and filtration integrated device and reverse osmosis composite membrane preparation method thereof

    CN120081570A