Modified hydrotalcite for lead ion adsorption as well as preparation method and application thereof
By intercalating the sodium ethylenediaminetetramethylphosphonate into hydrotalcite, modifying hydrotalcite is solved, and the problem of pure LDH lacks the ability to remove heavy metal lead ions is achieved, and the effect of efficiently removing heavy metal lead ions is achieved.
Patent Information
- Application Number
- CN202410955937.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-15
AI Technical Summary
The ability of pure layered double hydroxide (LDH) to remove heavy metal lead ions is limited by the problem of fewer functional groups in its layer and prone to agglomeration, resulting in low heavy metal removal efficiency.
By intercalating sodium ethylenediaminetetramethylphosphonate as anion into the hydrotalcite layer, its adsorption performance is enhanced to form modified hydrotalcite for lead ion adsorption, with the chemical formula Zn2+1-xAl3+x(OH)2( EDTMPS)·H2O, used to remove heavy metal lead ions.
The adsorption performance of hydrotalcite is significantly improved, and the efficient and rapid removal of heavy metal lead ions is achieved. The adsorption capacity is between 107 and 109 mg/g, the removal rate is between 85.60 and 87.20%, and it is easy to operate and low cost.
Smart Images

Figure CN118949915A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrotalcite, and in particular to a modified hydrotalcite for lead ion adsorption, and a preparation method and application thereof. Background Art
[0002] With the rapid development of industry, water pollution has become a global environmental problem, mainly from industrial wastewater discharged by industries such as plastics, electroplating, papermaking, and fertilizers. The most serious harmful substance in wastewater is heavy metal pollution. As we all know, heavy metals cannot be degraded by organisms, are highly toxic and carcinogenic. It has a strong persistence in the ecosystem and can easily accumulate in the human body through daily drinking water, causing serious harm to human health. Lead is one of the common heavy metals in industrial wastewater, which can have harmful effects on the human nervous system, brain, digestive system, and immune system. Therefore, it is urgent to remove lead ion heavy metal pollution in industrial wastewater.
[0003] Among the numerous heavy metal removal technologies, adsorption has the advantages of low cost, low investment, and simple operation, and is widely used because of its efficient and rapid ion removal. At present, common adsorbents mainly include minerals (montmorillonite, layered double hydroxides), biomass materials (wheat straw, algae), carbon-based materials (activated carbon, graphene oxide, carbon nanotubes), etc. Among them, layered double hydroxides (LDHs) have a large specific surface area, a positively charged layer, and exchangeable intercalated anions. They have excellent adsorption properties for anions through interlayer anion exchange and electrostatic attraction, and are a very promising adsorbent. However, pure LDH has the problem of relatively few functional groups in the layer and easy agglomeration, which greatly limits its ability to remove heavy metals. Therefore, it is necessary to overcome the limitations of pure LDH. In this regard, the present invention proposes a modified hydrotalcite for lead ion adsorption and its preparation method and application to increase its potential for adsorbing heavy metals.
[0004] Organic phosphonates are the most promising organic complexing and chelating agents. They can have strong complexing effects with many metal ions. They are non-toxic or low-toxic, environmentally friendly, and can be used to remove heavy metals. At the same time, their structure contains a P=O double bond at 900~1200cm ~1 It has obvious infrared absorption band, which is consistent with the nighttime geothermal radiation band, and has great potential for use in functional films. The present invention further develops the different functionalities of organic phosphonate intercalated hydrotalcite to improve the adsorption capacity of lead ions in sewage. Summary of the invention
[0005] The present invention aims to provide a modified hydrotalcite for lead ion adsorption, a preparation method and an application thereof. Ethylenediaminetetramethylenephosphonate organic phosphonate is selected as an anion to be intercalated between the hydrotalcite layers, thereby enhancing the adsorption performance of the hydrotalcite and removing heavy metal lead ions efficiently and quickly.
[0006] To achieve the above object, the present invention provides an application of a modified hydrotalcite for lead ion adsorption, wherein the chemical formula of the modified hydrotalcite for lead ion adsorption is: Zn 2+ 1-x Al 3+ x (OH)2(EDTMPS)·H2O, wherein EDTMPS represents sodium ethylenediaminetetramethylenephosphonate. The modified hydrotalcite for lead ion adsorption is placed in a wastewater solution containing lead ions, and the concentration of the modified hydrotalcite for lead ion adsorption in the wastewater solution is 0.2-1.2 g / L.
[0007] Preferably, the specific application steps are:
[0008] 1) Weigh a certain amount of modified hydrotalcite for lead ion adsorption and place it in a wastewater solution containing lead ions, and adjust the pH of the lead ion solution to 2-5 with dilute nitric acid;
[0009] 2) The modified hydrotalcite for lead ion adsorption is shaken at room temperature for 20 to 30 hours to reach adsorption equilibrium, and after adsorption is completed, it is filtered through a 0.45 μm microporous filter membrane to obtain a clear and bright filtrate.
[0010] Preferably, the adsorption capacity of the modified hydrotalcite for lead ion adsorption is 107-109 mg / g, and the removal rate is 85.60%-87.20%. Further preferably, the modified hydrotalcite for lead ion adsorption is used for adsorption of lead ions in industrial wastewater, with a maximum adsorption capacity of 108.52 mg / g and a removal rate of 86.82%.
[0011] The present invention also provides a method for preparing a modified hydrotalcite for lead ion adsorption, which is used to prepare the modified hydrotalcite for lead ion adsorption. The modified hydrotalcite for lead ion adsorption is prepared from sodium ethylenediaminetetramethylenephosphonate intercalated hydrotalcite, and the preparation steps are as follows:
[0012] S1: preparing a hydrotalcite precursor;
[0013] S2: preparing a solution of sodium ethylenediaminetetramethylenephosphonate of a predetermined concentration;
[0014] S3: dispersing the hydrotalcite precursor in deionized water to prepare a suspension, slowly titrating the sodium ethylenediaminetetramethylenephosphonate solution into the suspension, crystallizing in nitrogen at a constant temperature for a predetermined time, filtering and washing with deionized water until the pH of the washing solution is about 7, and centrifugally drying to obtain the modified hydrotalcite for lead ion adsorption.
[0015] Preferably, the steps for preparing the hydrotalcite precursor are: dissolving Zn(NO3)2·6H2O and Al(NO3)3·9H2O in deionized water in a predetermined ratio to form a first mixed solution; dissolving NaOH in deionized water to form a NaOH solution of a predetermined concentration, and then slowly adding the NaOH solution dropwise to the first mixed solution until the pH is neutral, crystallizing at 90°C for 66h, and then filtering and washing until the pH of the filtrate is about 7, and drying to obtain the hydrotalcite precursor.
[0016] Preferably, the concentration of the sodium ethylenediaminetetra(methylenephosphonate) solution is 0.05 to 3 mol / L.
[0017] Preferably, the crystallization time at 110° C. in S3 is 16 h.
[0018] The present invention also provides a modified hydrotalcite for lead ion adsorption, and the modified hydrotalcite for lead ion adsorption is prepared by the above preparation method.
[0019] The beneficial effects of the present invention are as follows: the present invention uses sodium ethylenediaminetetramethylenephosphonate to modify the hydrotalcite, which has a higher adsorption capacity than the unmodified hydrotalcite, enhances the adsorption performance of the hydrotalcite, and applies the modified hydrotalcite to adsorb lead ions in wastewater, thereby achieving the purpose of efficiently removing heavy metal lead ions, and has broad application prospects in the field of heavy metal pollution. The present invention can greatly increase the surface area of the modified hydrotalcite by intercalating sodium ethylenediaminetetramethylenephosphonate into the hydrotalcite, thereby providing more binding sites for adsorbing metals, and sodium ethylenediaminetetramethylenephosphonate belongs to organic phosphonates, has a strong chelating effect and electrostatic attraction to lead ions, thus greatly improving the adsorption capacity of the hydrotalcite for heavy metals, and can improve the removal rate of lead ions in the waste liquid. In addition, the application method is simple to operate, has the characteristics of low cost, low investment and high efficiency in removing lead ions, and is easy to promote and use. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The XRD spectra of the modified hydrotalcite for lead ion adsorption in Example 1 and Example 2 and the hydrotalcite precursor in Example 2 are shown.
[0021] Among them, (a) is the hydrotalcite precursor in Example 2; (b) is the modified hydrotalcite for lead ion adsorption in Example 1; (c) is the modified hydrotalcite for lead ion adsorption in Example 2.
[0022] Figure 2 FT-IR spectra of the modified hydrotalcite for lead ion adsorption in Example 5 and the hydrotalcite in Comparative Example 1.
[0023] Figure 3The modified hydrotalcite for lead ion adsorption in Example 5 and the hydrotalcite for Pb adsorption in Comparative Example 1 2+ trend chart. DETAILED DESCRIPTION
[0024] The embodiments described below are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The present invention provides an application of a modified hydrotalcite for lead ion adsorption, wherein the chemical formula of the modified hydrotalcite for lead ion adsorption is: Zn 2+ 1~x Al 3+ x (OH)2(EDTMPS)·H2O, wherein EDTMPS represents sodium ethylenediaminetetramethylenephosphonate. The modified hydrotalcite for lead ion adsorption is placed in a wastewater solution containing lead ions, and the concentration of the modified hydrotalcite for lead ion adsorption in the wastewater solution is 0.2-1.2 g / L.
[0026] The specific application steps are:
[0027] 1) Weigh a certain amount of modified hydrotalcite for lead ion adsorption and place it in a wastewater solution containing lead ions, and adjust the pH of the lead ion solution to 2-5 with dilute nitric acid;
[0028] 2) The modified hydrotalcite for lead ion adsorption is shaken at room temperature for 20 to 30 hours to reach adsorption equilibrium, and after adsorption is completed, it is filtered through a 0.45 μm microporous filter membrane to obtain a clear and bright filtrate.
[0029] The adsorption capacity of the modified hydrotalcite for lead ion adsorption is 107-109 mg / g.
[0030] The present invention also provides a method for preparing a modified hydrotalcite for lead ion adsorption, which is used to prepare the modified hydrotalcite for lead ion adsorption. The modified hydrotalcite for lead ion adsorption is prepared from sodium ethylenediaminetetramethylenephosphonate intercalated hydrotalcite, and the preparation steps are as follows:
[0031] S1: preparing a hydrotalcite precursor;
[0032] S2: preparing a solution of sodium ethylenediaminetetramethylenephosphonate of a predetermined concentration;
[0033] S3: dispersing the hydrotalcite precursor in deionized water to prepare a suspension, slowly titrating the sodium ethylenediaminetetramethylenephosphonate solution into the suspension, crystallizing in nitrogen at a constant temperature for a predetermined time, filtering and washing with deionized water until the pH of the washing solution is about 7, and centrifugally drying to obtain the modified hydrotalcite for lead ion adsorption.
[0034] The steps for preparing the hydrotalcite precursor are as follows: dissolving Zn(NO3)2·6H2O and Al(NO3)3·9H2O in deionized water in a predetermined ratio to form a first mixed solution; dissolving NaOH in deionized water to form a NaOH solution of a predetermined concentration, and then slowly adding the NaOH solution to the first mixed solution until the pH is neutral, crystallizing at 90°C for 66 hours, and then filtering and washing until the pH of the filtrate is about 7, and drying to obtain the hydrotalcite precursor.
[0035] The concentration of the sodium ethylenediaminetetra(methylenephosphonate) solution is 0.05-3 mol / L.
[0036] The crystallization time in S3 at 110°C was 16 h.
[0037] The present invention also provides a modified hydrotalcite for lead ion adsorption, and the modified hydrotalcite for lead ion adsorption is prepared by the above preparation method.
[0038] Example 1
[0039] This embodiment provides a modified hydrotalcite for lead ion adsorption, and the preparation steps of the modified hydrotalcite for lead ion adsorption are as follows:
[0040] (1) 0.04 mol of Zn(NO3)2·6H2O and 0.01 mol of Al(NO3)3·9H2O were dissolved in deionized water to prepare 100 ml of a first mixed solution; 0.1 mol of NaOH was dissolved in deionized water to prepare a NaOH solution, and then the NaOH solution was slowly added dropwise to the first mixed solution to make its pH neutral, crystallized at 90°C for 66 hours, and then filtered and washed until the pH of the filtrate was about 7, and dried to obtain a hydrotalcite precursor.
[0041] (2) The dried hydrotalcite precursor was ultrasonically dispersed in deionized water to prepare a 100 ml hydrotalcite suspension, which was transferred to a three-necked flask and stirred evenly. 0.1 mol of ethylenediaminetetramethylenephosphonic acid sodium (EDTMPSNa) was weighed and dissolved in 100 ml of deionized water, placed in a constant pressure funnel, and slowly dripped into the hydrotalcite suspension. Crystallization was carried out at 110°C for 16 hours, and the filtrate was filtered and washed until the filtrate was neutral. The modified hydrotalcite (EDTMPS-LDH) for lead ion adsorption was obtained by drying.
[0042] The steps of applying the modified hydrotalcite for lead ion adsorption to the wastewater solution are as follows:
[0043] Weigh 0.01g of modified hydrotalcite for lead ion adsorption and place it in 50ml of wastewater solution containing 100mg / L lead ion concentration. Use dilute nitric acid to adjust the pH of the lead ion solution to 5. Oscillate at room temperature for 6h. Use the modified hydrotalcite for lead ion adsorption to adsorb lead ions. After the oscillation and adsorption are completed, filter with a 0.45μm microporous filter membrane to obtain a clear and bright filtrate, and use an atomic absorption spectrophotometer to measure the residual Pb in the filtrate. 2+ Content, calculated Pb 2+ The adsorption capacity is 103.49 mg / g and the removal rate is 20.70%.
[0044] Example 2
[0045] This embodiment provides a modified hydrotalcite for lead ion adsorption, and the preparation steps of the modified hydrotalcite for lead ion adsorption are as follows:
[0046] (1) 0.02 mol of Zn(NO3)2·6H2O and 0.01 mol of Al(NO3)3·9H2O are dissolved in deionized water to prepare 100 ml of a first mixed solution; 0.1 mol of NaOH is dissolved in deionized water to prepare a NaOH solution, and then the NaOH solution is slowly added dropwise to the first mixed solution to make its pH neutral, crystallize at 90°C for 66 hours, and then filter and wash until the filtrate has a pH of about 7, and dry to obtain a hydrotalcite precursor.
[0047] (2) The dried hydrotalcite precursor was ultrasonically dispersed in deionized water to prepare a 100 ml hydrotalcite suspension, which was transferred to a three-necked flask and stirred evenly. 0.2 mol of ethylenediaminetetramethylenephosphonic acid sodium (EDTMPSNa) was weighed and dissolved in 100 ml of deionized water, placed in a constant pressure funnel, and slowly dripped into the hydrotalcite suspension. Crystallization was carried out at 110°C for 16 hours, and the filtrate was filtered and washed until the filtrate was neutral. The modified hydrotalcite (EDTMPS-LDH) for lead ion adsorption was obtained by drying.
[0048] The steps of applying the modified hydrotalcite for lead ion adsorption to the wastewater solution are as follows:
[0049] Weigh 0.01g of modified hydrotalcite for lead ion adsorption and place it in 50ml of wastewater solution containing 100mg / L lead ion concentration. Use dilute nitric acid to adjust the pH of the lead ion solution to 2. Oscillate at room temperature for 6h. Use the modified hydrotalcite for lead ion adsorption to adsorb lead ions. After the oscillation and adsorption are completed, filter with a 0.45μm microporous filter membrane to obtain a clear and bright filtrate, and use an atomic absorption spectrophotometer to measure the residual Pb in the filtrate. 2+ Content, calculated Pb 2+ The adsorption capacity was 23.20 mg / g and the removal rate was 4.64%.
[0050] Example 3
[0051] This embodiment provides a modified hydrotalcite for lead ion adsorption, and the preparation steps of the modified hydrotalcite for lead ion adsorption are as follows:
[0052] (1) 0.02 mol of Zn(NO3)2·6H2O and 0.01 mol of Al(NO3)3·9H2O are dissolved in deionized water to prepare 100 ml of a first mixed solution; 0.1 mol of NaOH is dissolved in deionized water to prepare a NaOH solution, and then the NaOH solution is slowly added dropwise to the first mixed solution to make its pH neutral, crystallize at 90°C for 66 hours, and then filter and wash until the filtrate has a pH of about 7, and dry to obtain a hydrotalcite precursor.
[0053] (2) The dried hydrotalcite precursor was ultrasonically dispersed in deionized water to prepare a 100 ml hydrotalcite suspension, which was transferred to a three-necked flask and stirred evenly. 0.2 mol of ethylenediaminetetramethylenephosphonic acid sodium (EDTMPSNa) was weighed and dissolved in 100 ml of deionized water, placed in a constant pressure funnel, and slowly dripped into the hydrotalcite suspension. Crystallization was carried out at 110°C for 16 hours, and the filtrate was filtered and washed until the filtrate was neutral. The modified hydrotalcite (EDTMPS-LDH) for lead ion adsorption was obtained by drying.
[0054] The steps of applying the modified hydrotalcite for lead ion adsorption to the wastewater solution are as follows:
[0055] Weigh 0.02g of modified hydrotalcite for lead ion adsorption and place it in 50ml of wastewater solution containing 100mg / L lead ion concentration. Use dilute nitric acid to adjust the pH of the lead ion solution to 3. Oscillate at room temperature for 6h. Use the modified hydrotalcite for lead ion adsorption to adsorb lead ions. After the oscillation and adsorption are completed, filter with a 0.45μm microporous filter membrane to obtain a clear and bright filtrate, and use an atomic absorption spectrophotometer to measure the residual Pb in the filtrate. 2+ Content, calculated Pb 2+ The adsorption capacity is 33.43 mg / g, and the removal rate is 13.37%.
[0056] Example 4
[0057] This embodiment provides a modified hydrotalcite for lead ion adsorption, and the preparation steps of the modified hydrotalcite for lead ion adsorption are as follows:
[0058] (1) 0.02 mol of Zn(NO3)2·6H2O and 0.01 mol of Al(NO3)3·9H2O are dissolved in deionized water to prepare 100 ml of a first mixed solution; 0.1 mol of NaOH is dissolved in deionized water to prepare a NaOH solution, and then the NaOH solution is slowly added dropwise to the first mixed solution to make its pH neutral, crystallize at 90°C for 66 hours, and then filter and wash until the filtrate has a pH of about 7, and dry to obtain a hydrotalcite precursor.
[0059] (2) The dried hydrotalcite precursor was ultrasonically dispersed in deionized water to prepare a 100 ml hydrotalcite suspension, which was transferred to a three-necked flask and stirred evenly. 0.2 mol of ethylenediaminetetramethylenephosphonic acid sodium (EDTMPSNa) was weighed and dissolved in 100 ml of deionized water, placed in a constant pressure funnel, and slowly dripped into the hydrotalcite suspension. Crystallization was carried out at 110°C for 16 hours, and the filtrate was filtered and washed until the filtrate was neutral. The modified hydrotalcite (EDTMPS-LDH) for lead ion adsorption was obtained by drying.
[0060] The steps of applying the modified hydrotalcite for lead ion adsorption to the wastewater solution are as follows:
[0061] Weigh 0.03g of modified hydrotalcite for lead ion adsorption and place it in 50ml of wastewater solution containing 100mg / L lead ion concentration. Use dilute nitric acid to adjust the pH of the lead ion solution to 4. Oscillate at room temperature for 6h. Use the modified hydrotalcite for lead ion adsorption to adsorb lead ions. After the oscillation and adsorption are completed, filter with a 0.45μm microporous filter membrane to obtain a clear and bright filtrate, and use an atomic absorption spectrophotometer to measure the residual Pb in the filtrate. 2+ Content, calculated Pb 2+ The adsorption capacity is 40.55 mg / g and the removal rate is 24.33%.
[0062] Example 5
[0063] This embodiment provides a modified hydrotalcite for lead ion adsorption, and the preparation steps of the modified hydrotalcite for lead ion adsorption are as follows:
[0064] (1) 0.02 mol of Zn(NO3)2·6H2O and 0.01 mol of Al(NO3)3·9H2O are dissolved in deionized water to prepare 100 ml of a first mixed solution; 0.1 mol of NaOH is dissolved in deionized water to prepare a NaOH solution, and then the NaOH solution is slowly added dropwise to the first mixed solution to make its pH neutral, crystallize at 90°C for 66 hours, and then filter and wash until the filtrate has a pH of about 7, and dry to obtain a hydrotalcite precursor.
[0065] (2) The dried hydrotalcite precursor was ultrasonically dispersed in deionized water to prepare a 100 ml hydrotalcite suspension, which was transferred to a three-necked flask and stirred evenly. 0.2 mol of ethylenediaminetetramethylenephosphonic acid sodium (EDTMPSNa) was weighed and dissolved in 100 ml of deionized water, placed in a constant pressure funnel, and slowly dripped into the hydrotalcite suspension. Crystallization was carried out at 110°C for 16 hours, and the filtrate was filtered and washed until the filtrate was neutral. The modified hydrotalcite (EDTMPS-LDH) for lead ion adsorption was obtained by drying.
[0066] The steps of applying the modified hydrotalcite for lead ion adsorption to the wastewater solution are as follows:
[0067] Weigh 0.04g of modified hydrotalcite for lead ion adsorption and place it in 50ml of wastewater solution with a lead ion concentration of 100mg / L. Use dilute nitric acid to adjust the pH of the lead ion solution to 5. Oscillate at room temperature for 6h. Use the modified hydrotalcite for lead ion adsorption to adsorb lead ions. After the oscillation and adsorption are completed, filter with a 0.45μm microporous filter membrane to obtain a clear and bright filtrate, and use an atomic absorption spectrophotometer to measure the residual Pb in the filtrate. 2+ Content, calculated Pb 2+ The adsorption capacity is 70.42 mg / g and the removal rate is 56.34%.
[0068] Example 6
[0069] This embodiment provides a modified hydrotalcite for lead ion adsorption, and the preparation steps of the modified hydrotalcite for lead ion adsorption are as follows:
[0070] (1) 0.02 mol of Zn(NO3)2·6H2O and 0.01 mol of Al(NO3)3·9H2O are dissolved in deionized water to prepare 100 ml of a first mixed solution; 0.1 mol of NaOH is dissolved in deionized water to prepare a NaOH solution, and then the NaOH solution is slowly added dropwise to the first mixed solution to make its pH neutral, crystallize at 90°C for 66 hours, and then filter and wash until the filtrate has a pH of about 7, and dry to obtain a hydrotalcite precursor.
[0071] (2) The dried hydrotalcite precursor was ultrasonically dispersed in deionized water to prepare a 100 ml hydrotalcite suspension, which was transferred to a three-necked flask and stirred evenly. 0.2 mol of ethylenediaminetetramethylenephosphonic acid sodium (EDTMPSNa) was weighed and dissolved in 100 ml of deionized water, placed in a constant pressure funnel, and slowly dripped into the hydrotalcite suspension. Crystallization was carried out at 110°C for 16 hours, and the filtrate was filtered and washed until the filtrate was neutral. The modified hydrotalcite (EDTMPS-LDH) for lead ion adsorption was obtained by drying.
[0072] The steps of applying the modified hydrotalcite for lead ion adsorption to the wastewater solution are as follows:
[0073] Weigh 0.04g of modified hydrotalcite for lead ion adsorption and place it in 50ml of wastewater solution with a lead ion concentration of 100mg / L. Use dilute nitric acid to adjust the pH of the lead ion solution to 5, and oscillate at room temperature for 20h. Use the modified hydrotalcite for lead ion adsorption to adsorb lead ions. After the oscillation and adsorption are completed, filter with a 0.45μm microporous filter membrane to obtain a clear and bright filtrate, and use an atomic absorption spectrophotometer to measure the residual Pb in the filtrate. 2+ Content, calculated Pb 2+ The adsorption capacity is 108.52 mg / g, and the removal rate is 86.82%.
[0074] Comparative Example 1
[0075] 0.02 mol of Zn(NO3)2·6H2O and 0.01 mol of Al(NO3)3·9H2O were dissolved in deionized water to prepare 100 ml of a first mixed solution; 0.1 mol of NaOH was dissolved in deionized water to prepare a NaOH solution, and then the NaOH solution was slowly added dropwise to the first mixed solution to make its pH neutral, crystallized at 90°C for 66 hours, and then filtered and washed until the pH of the filtrate was about 7, and dried to obtain hydrotalcite.
[0076] 0.04 g of hydrotalcite was weighed and placed in 50 ml of wastewater solution containing 100 mg / L of lead ion concentration. The pH of the lead ion solution was adjusted to 5 with dilute nitric acid. The organic modified hydrotalcite adsorbed lead ions and oscillated at room temperature for a period of time. After the oscillation and adsorption were completed, a clear and bright filtrate was obtained by filtering with a 0.45 μm microporous filter membrane, and the residual Pb in the filtrate was measured using an atomic absorption spectrophotometer. 2+ Content, calculated Pb 2+ The adsorption capacity was 7.81 mg / g and the removal rate was 6.25%.
[0077] The modified hydrotalcite for lead ion adsorption prepared in Example 1 and Example 2 and the hydrotalcite precursor were subjected to XRD analysis, and the test spectrum is shown in Figure 2 ; The modified hydrotalcite prepared in Example 5 and Comparative Example 1 was subjected to RT-IR analysis and the Pb 2+ Adsorption analysis, test spectra are shown in Figure 3 .
[0078] Spectral analysis:
[0079] from Figure 1 It can be seen that EDTMPS was successfully intercalated into the interlayer of hydrotalcite, but other impurity peaks appeared in Example 1. By comparing with the standard card, it was found that these impurity peaks were ZnO. Figure 2 It is further proved that EDTMPS enters the interlayer of hydrotalcite at 900-1200 cm ~1 The vibration peak of the phosphonate group appeared. Figure 3 The results of Example 5 and Comparative Example 1 on Pb at different adsorption times 2+ The adsorption effect of Figure 3 It can be seen that both of them increase with the increase of adsorption time for Pb 2+ The adsorption capacity of hydrotalcite modified by EDTMPS intercalation is increasing, but the adsorption capacity of hydrotalcite modified by EDTMPS intercalation is much greater than that of hydrotalcite not modified by intercalation. In summary, EDTMPS intercalation modified hydrotalcite has the adsorption performance of heavy metals, and the adsorbent combines the adsorption capacity of EDTMPS and hydrotalcite, and the adsorption performance is enhanced.
[0080] The present invention is described in detail above in conjunction with the embodiments. It should be noted that the various specific technical features described in the above specific embodiments can be combined and changed in any suitable manner without contradiction, and the present invention will not further explain various possible combinations. In addition, other variations and combinations of the various technical features of the present invention should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. An application of modified hydrotalcite for lead ion adsorption, characterized in that: The chemical formula of the modified hydrotalcite for lead ion adsorption is: Zn 2+ 1-x Al 3+ x (OH)2(EDTMPS)·H2O, wherein EDTMPS represents sodium ethylenediaminetetramethylenephosphonate; the modified hydrotalcite for lead ion adsorption is placed in a wastewater solution containing lead ions, and the concentration of the modified hydrotalcite for lead ion adsorption in the wastewater solution is 0.2-1.2 g / L.
2. The use of the modified hydrotalcite for lead ion adsorption according to claim 1, characterized in that: The specific application steps are: 1) Weigh a certain amount of modified hydrotalcite for lead ion adsorption and place it in a wastewater solution containing lead ions, and adjust the pH of the lead ion solution to 2-5 with dilute nitric acid; 2) The modified hydrotalcite for lead ion adsorption is shaken at room temperature for 20 to 30 hours to reach adsorption equilibrium, and after adsorption is completed, it is filtered through a 0.45 μm microporous filter membrane to obtain a clear and bright filtrate.
3. The use of the modified hydrotalcite for lead ion adsorption according to claim 2, characterized in that: The adsorption capacity of the modified hydrotalcite for lead ion adsorption is 107-109 mg / g, and the removal rate is 85.60%-87.20%.
4. A method for preparing a modified hydrotalcite for lead ion adsorption, for preparing the modified hydrotalcite for lead ion adsorption according to any one of claims 1 to 3, characterized in that: The modified hydrotalcite for lead ion adsorption is prepared from sodium ethylenediaminetetramethylenephosphonate intercalated hydrotalcite, and the preparation steps are as follows: S1: preparing a hydrotalcite precursor; S2: preparing a solution of sodium ethylenediaminetetramethylenephosphonate of a predetermined concentration; S3: dispersing the hydrotalcite precursor in deionized water to prepare a suspension, slowly titrating the sodium ethylenediaminetetramethylenephosphonate solution into the suspension, crystallizing in nitrogen at a constant temperature for a predetermined time, filtering and washing with deionized water until the pH of the washing solution is about 7, and centrifugally drying to obtain the modified hydrotalcite for lead ion adsorption.
5. The method for preparing the modified hydrotalcite for lead ion adsorption according to claim 4, characterized in that: The preparation steps of the hydrotalcite precursor are as follows: dissolving Zn(NO3)2·6H2O and Al(NO3)3·9H2O in deionized water according to a predetermined ratio to prepare a first mixed solution; dissolving NaOH in deionized water to prepare a NaOH solution of a predetermined concentration, then slowly adding the NaOH solution dropwise to the first mixed solution until the pH is neutral, crystallizing at 90°C for 66 hours, then filtering and washing until the pH of the filtrate is about 7, and drying to obtain the hydrotalcite precursor.
6. The method for preparing the modified hydrotalcite for lead ion adsorption according to claim 5, characterized in that: The concentration of the sodium ethylenediaminetetra(methylenephosphonate) solution is 0.05-3 mol / L.
7. The method for preparing the modified hydrotalcite for lead ion adsorption according to claim 6, characterized in that: The crystallization time in S3 at 110°C was 16 h.
8. A modified hydrotalcite for lead ion adsorption, characterized in that: The modified hydrotalcite for lead ion adsorption is prepared by the preparation method described in claim 6.
Citation Information
Patent Citations
Modified hydrotalcite-like adsorbent and application thereof
CN106881067A
Novel phosphine-containing hydrotalcite infrared thermal insulation material and preparation method thereof
CN116875279A
Infrared thermal insulation film containing phosphino hydrotalcite
CN117247625A
Cited By
Ethylenediamine tetramethylenephosphonic acid modified starch as well as preparation method and application thereof
CN120865442A