Titanium dioxide nanosheet loaded with cobalt monatomic and application of titanium dioxide nanosheet in degrading organic pollutants by activating peroxymonosulfate
By stably loading cobalt single atoms on titanium dioxide nanosheets, forming Co/TiO2NS catalysts, the problem of easy shedding and inactivation of metal single atoms is solved, and efficient activation of persulfate degradation of organic pollutants is achieved, reducing wastewater treatment costs, and showing that Good catalytic cycle stability and application prospects.
Patent Information
- Application Number
- CN202411022837.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
Metal single-atom catalysts are prone to shedding and inactivation in wastewater treatment, resulting in a decline in catalytic performance and an increase in environmental risks. It is difficult for the prior art to effectively and stably load on the surface of titanium dioxide, which increases the treatment cost.
The preparation method of titanium dioxide nanosheets with cobalt-loaded single atoms is adopted to synthesize titanium dioxide nanosheets by hydrothermal anatase phase titanium dioxide powder and sodium hydroxide, and the cobalt-loaded single atoms are stably loaded on its surface, and the Co/ is formed by calcining and acid solution treatment. TiO2NS catalyst.
It achieves high stability and dispersion of cobalt single atoms, maintains catalytic performance, reduces the frequency of catalyst replacement, reduces wastewater treatment costs, and maintains excellent catalytic activity in multiple cycles, making it suitable for large-scale continuous production.
Smart Images

Figure CN118949990A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of advanced oxidation wastewater treatment in environmental engineering, and in particular to titanium dioxide nanosheets loaded with cobalt single atoms and applications thereof in activating peroxymonosulfate to degrade organic pollutants. Background Art
[0002] With the rapid development of industry and the rapid advancement of urbanization in recent years, the treatment of highly toxic new organic pollutants in wastewater has gradually become a hot topic in the environmental field. At present, advanced oxidation methods represented by peroxymonosulfate activation are often used for the degradation of organic pollutants. Its most notable feature is the activation of peroxymonosulfate by transition metal catalysts to produce active oxygen species to achieve oxidative degradation of organic pollutants. Single-atom catalysts have received widespread attention in recent years because of their maximized atomic exposure and utilization rates, which can reduce the use of metal raw materials and thus optimize treatment costs. However, metal single atoms are easily attacked by active oxygen species and fall off from the base material, which not only reduces the activity of single-atom catalysts, but also causes potential environmental risks and significantly increases the cost of wastewater treatment.
[0003] Selecting a suitable carrier can stabilize the dispersion of metal single atoms. Metal oxides are abundant in resources, and the charge transfer between them and metal single atoms can affect the charge state of single atoms, thereby affecting their catalytic performance, making metal oxides ideal single-atom support materials. The strong metal-support interaction formed based on this charge transfer helps stabilize the loading of single atoms and prevent the formation of clusters between single atoms, thereby maintaining their catalytic activity and structural stability.
[0004] Titanium dioxide is an abundant, low-cost, green and environmentally friendly metal oxide with tunable structural characteristics. Common titanium dioxide nanoparticles have a small specific surface area and high surface energy, which is not conducive to the loading of metal single atoms. How to develop a simple and low-cost method to load metal single atoms on the surface of titanium dioxide has become the key to solving the problem of easy detachment and deactivation of metal single atoms. The synthesis of stable single-atom catalysts is expected to efficiently activate persulfate and be used in the treatment of new organic pollutants in the water environment. Summary of the invention
[0005] In order to overcome the deficiencies of the above-mentioned prior art, the first object of the present invention is to provide a method for preparing a titanium dioxide nanosheet loaded with a single cobalt atom to prevent the aggregation and shedding of the metal cobalt single atom in the catalytic reaction. Furthermore, the second object of the present invention is to provide the application of the titanium dioxide nanosheet loaded with a single cobalt atom in the activation of persulfate to degrade new antibiotic pollutants. Due to the high stability of the cobalt single atom loaded on the titanium dioxide nanosheet, there is almost no leakage of metal ions during the reaction process, and the catalytic performance can be maintained during a long-term wastewater treatment process, thereby reducing the replacement of the catalyst and reducing the cost of wastewater treatment.
[0006] In order to achieve the purpose, the present invention adopts the following technical scheme:
[0007] The present invention first provides a method for preparing a titanium dioxide nanosheet loaded with a single cobalt atom, comprising the following steps:
[0008] Step 1: Place anatase phase titanium dioxide powder, sodium hydroxide and water in a reactor and stir them thoroughly. Then keep the reactor warm in an oven and cool it naturally to room temperature. The obtained product is washed and vacuum dried to obtain titanium dioxide nanosheets, which are recorded as TiO 2 NS;
[0009] Step 2: TiO obtained in step 1 2 Add cobalt salt solution to NS, shake thoroughly and centrifuge, wash the obtained product thoroughly and dry it in vacuum;
[0010] Step 3: The sample obtained in step 2 is placed in a muffle furnace and calcined in an air atmosphere. The calcined sample is then placed in an inorganic acid solution and shaken thoroughly. After centrifugation, the obtained product is washed and vacuum dried to obtain titanium dioxide nanosheets loaded with cobalt single atoms, which are recorded as Co / TiO 2 NS.
[0011] Preferably, in step 1, the mass ratio of titanium dioxide powder to sodium hydroxide is 1:16-48.
[0012] Preferably, in step 1, the insulation time in the oven is 6-24 hours and the oven temperature is 110-150°C.
[0013] Preferably, in step 2, the cobalt salt is one of cobalt sulfate, cobalt nitrate, cobalt chloride hexahydrate and cobalt carbonate, the concentration of the cobalt salt solution is 1-10 mM, and the mass ratio of titanium dioxide nanosheets to cobalt salt is 1:0.01-0.5.
[0014] Preferably, in step 3, the calcination temperature is 150-250°C, the calcination time is 1-4 hours, and the heating rate is 2-10°C.
[0015] Preferably, in step 3, the inorganic acid solution is one of hydrochloric acid solution, sulfuric acid solution and nitric acid solution, and the concentration of the inorganic acid solution is 0.5-1.5M.
[0016] The present invention also provides the use of the titanium dioxide nanosheets loaded with single cobalt atoms prepared according to the above preparation method as a catalyst in activating permonosulfate to degrade organic pollutants, which can be specifically as follows: adding the titanium dioxide nanosheets loaded with single cobalt atoms and permonosulfate as catalysts to the aqueous solution of organic pollutants to be treated, and the permonosulfate generates strongly oxidizing hydroxyl radicals under the activation of the catalyst to achieve the degradation of organic pollutants.
[0017] Preferably, the mass ratio of the organic pollutant, the catalyst and the peroxymonosulfate is 1:1-5:3-10.
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0019] The present invention uses titanium dioxide as a raw material to synthesize titanium dioxide nanosheets, and utilizes the strong metal-carrier interaction between titanium dioxide nanosheets and cobalt single atoms to achieve stable loading and dispersion of cobalt single atoms. This method has the characteristics of easy raw material availability, low cost, simple operation, etc., and is suitable for large-scale continuous production. The Co / TiO synthesized by the present invention 2 The single cobalt atom in NS as a catalytic site can efficiently activate peroxymonosulfate to produce highly oxidizing hydroxyl radicals, achieve efficient oxidative degradation of new antibiotic pollutants, and maintain excellent catalytic performance in multiple degradation cycles, which has good practical application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The Co / TiO synthesized in Example 1 2 Transmission electron microscopy (TEM) image of NS;
[0021] Figure 2 The Co / TiO synthesized in Example 1 2 Hard-line X-ray synchrotron radiation spectra (EXAFs) of NS;
[0022] Figure 3 The transmission electron microscope (TEM) image of the synthetic product in Example 2 is shown in FIG.
[0023] Figure 4 The transmission electron microscope (TEM) image of the product synthesized in Example 3;
[0024] Figure 5 is a transmission electron microscopy (TEM) image of the synthetic product in Example 4;
[0025] Figure 6is a transmission electron microscopy (TEM) image of the synthetic product in Example 5;
[0026] Figure 7 The Co / TiO 2 NS and TiO 2 Degradation rate diagram of sulfamethoxazole SMX degraded by NS activated peroxymonosulfate;
[0027] Figure 8 The Co / TiO 2 Electron paramagnetic resonance spectrum in NS system (the trapping agent is 5,5-dimethyl-1-pyrroline N-oxide);
[0028] Fig. 9 The Co / TiO 2 Characterization of cyclic stability of NS;
[0029] Fig.10 The Co / TiO 2 Graph of cobalt ion leaching from NS during 5 cycles;
[0030] Fig.11 The Co / TiO 2 Degradation of SMX by NS at different pH values;
[0031] Fig.12 The Co / TiO 2 Degradation diagram of NS on new pollutants of different antibiotics. DETAILED DESCRIPTION
[0032] The following will be combined with the accompanying drawings of the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0033] 1. Preparation of Titanium Dioxide Nanosheets Loaded with Cobalt Single Atoms
[0034] Example 1
[0035] In this example, titanium dioxide nanosheets loaded with cobalt single atoms were prepared according to the following steps:
[0036] Step 1: 500 mg of commercial anatase TiO 2The powder, 12.8 g of sodium hydroxide and 40 mL of water were added to a 100 mL polytetrafluoroethylene reactor liner and stirred thoroughly. The reactor was then transferred to an oven and kept at 140 ° C for 12 h, and then naturally cooled to room temperature slowly. After centrifugal separation, the obtained solid product was washed with deionized water until neutral, and dried in a vacuum drying oven at 60 ° C for 24 hours to obtain titanium dioxide nanosheets TiO 2 NS.
[0037] Step 2: Prepare 10 mM cobalt sulfate solution and add the product TiO2 from step 1 into a 100 mL conical flask. 2 NS and 40 mL of cobalt sulfate solution were shaken thoroughly for 2 hours. After the reaction was completed, the solid product was centrifuged and washed twice with water and dried in a vacuum drying oven at 60°C for 24 hours.
[0038] Step 3: The dried product was placed in a porcelain boat, and then calcined in a muffle furnace at 200 ° C for 2 hours. After cooling naturally to room temperature, the product was placed in 50 mL of sulfuric acid solution (1M) and shaken for 2 hours. After centrifugation, it was washed with deionized water until neutral, dried at 60 ° C in vacuum for 24 hours, and ground to obtain titanium dioxide nanosheets Co / TiO loaded with cobalt single atoms. 2 NS.
[0039] The present invention is to obtain the final Co / TiO 2 NS conducted TEM and EXAFs tests. Figure 1 This is a transmission electron microscope image of the material, which shows the prepared Co / TiO 2 The NS catalyst is in the form of two-dimensional nanosheets, with no obvious Co single-element nanoparticles or clusters on the surface, indicating the atomic-level dispersion state of Co; Figure 2 This is the X-ray absorption fine structure spectrum of the material. There is no Co-Co bond in the figure, which strongly proves the atomic-level dispersion of Co.
[0040] Example 2
[0041] Titanium dioxide material was prepared in the same manner as in step 1 of Example 1, except that the amount of sodium hydroxide used was 8 g. TEM image ( Figure 3 ) shows that although a lower dosage of sodium hydroxide can also be used to synthesize titanium dioxide nanosheets, there will be more raw titanium dioxide (the small dot-like particles in the figure) remaining.
[0042] Example 3
[0043] Titanium dioxide material was prepared in the same manner as in step 1 of Example 1, except that the amount of sodium hydroxide used was 24 g. TEM image ( Figure 4 ) showed that a distinct tubular titanium dioxide structure was produced under this amount of sodium hydroxide.
[0044] Example 4
[0045] Titanium dioxide material was prepared in the same manner as in step 1 of Example 1, except that the hydrothermal temperature was 180°C. TEM image ( Figure 5 ) showed that a distinct tubular titanium dioxide structure was produced under this condition.
[0046] Example 5
[0047] Titanium dioxide material was prepared in the same manner as in step 1 of Example 1, except that the hydrothermal time was 24 hours. TEM image ( Figure 6 ) showed that the structure of titanium dioxide nanosheets was obviously destroyed under this condition, indicating that a longer hydrothermal time is not conducive to the formation of titanium dioxide nanosheets.
[0048] In combination with Examples 1-5, the final preferred hydrothermal synthesis conditions are: the amount of sodium hydroxide used is 8-24 g, the hydrothermal temperature is 140° C., and the hydrothermal time is 12 hours.
[0049] 2. Co / TiO 2 Application of NS catalyst in the degradation of organic pollutants by activating peroxymonosulfate
[0050] Example 6, Co / TiO 2 NS catalyst and TiO without cobalt atoms 2 Comparison of catalytic performance of NS
[0051] Take 3 mg of Co / TiO prepared in Example 1 2 NS materials or TiO 2 NS material was added to 100 mL of sulfamethoxazole solution (C 0 =10 mg / L), stir rapidly for 3 minutes to fully disperse the catalyst in the solution, and then add 10 mg PMS (KHSO 5 0.5KHSO 4 0.5K 2 SO 4 ), start timing; 1 minute later, take 500 μL of the reaction solution and mix it with 500 μL of methanol solution, filter it through a 0.45 μM water filter membrane, and then test the concentration of residual pollutants by high performance liquid chromatography C t , the degradation rate is recorded as 1-C t / C 0 .
[0052] Figure 7 Co / TiO 2 NS and TiO 2 The degradation rate diagram of sulfamethoxazole SMX by NS-activated persulfate is shown in the figure: Co / TiO 2NS exhibits an extremely high SMX degradation rate, which can remove 100% of 10 mg / L SMX within 1 minute. 2 NS can only remove about 20% of SMX in 1 minute. This reflects the 2 NS has excellent catalytic activity and proves that Co / TiO 2 The catalytic active sites in NS are mainly Co single atoms.
[0053] Figure 8 Co / TiO 2 Electron paramagnetic resonance spectrum in NS / PMS system (the trapping agent is 5,5-dimethyl-1-pyrroline N-oxide). The obvious quartet signal in the figure (intensity ratio is 1:2:2:1) reveals the generation of hydroxyl radicals, indicating that Co / TiO 2 NS can activate PMS to produce highly oxidative hydroxyl radicals, thereby achieving efficient oxidative degradation of organic pollutants.
[0054] Example 7, Co / TiO 2 Stability test of NS catalyst
[0055] If the heterogeneous catalyst has good recyclability, the cost of wastewater treatment can be significantly reduced. In this embodiment, the catalyst used in the method of Example 6 is centrifuged, washed twice with water and ethanol respectively, placed in a vacuum drying oven for 24 hours, and reused in the next degradation experiment. The specific implementation conditions of the degradation experiment are the same as those of Example 6. Fig. 9 The catalytic efficiency changes of the catalyst in 5 cycles are given. It can be found that after 5 cycles, Co / TiO 2 The catalytic activity of the NS material showed almost no decay, indicating its excellent catalytic cycling stability. Fig.10 Reflects the Co / TiO 2 The leaching of Co metal ions from NS materials in 5 cycles showed that the leaching amount of metal ions in 5 cycles was zero, reflecting that titanium dioxide nanosheets can stably load cobalt single atoms, and this structurally stable single-atom material can resist the destruction of its structure by strong oxidizing free radicals in the catalytic system, showing good practical application prospects.
[0056] Example 8: Degradation of sulfamethoxazole at different pH values
[0057] Same as Example 6, except that the pH of the initial sulfamethoxazole contaminant solution was adjusted to 3, 5, 7, and 9, respectively. Fig.11 It shows that Co / TiO 2 NS can remove SMX 100% within 1 minute at different initial solution pH, reflecting the wide pH applicability range of the catalyst.
[0058] Example 9: Degradation of high concentration sulfamethoxazole solution
[0059] Same as Example 6, except that the concentration of sulfamethoxazole solution was increased from 10 mg / L to 15 mg / L. The results showed that Co / TiO 2 The degradation rate of SMX by NS was still 100% within 1 min, reflecting the x The material has extremely high catalytic activity.
[0060] Example 10: Degradation of new pollutants from different antibiotics
[0061] To test Co / TiO 2 The degradation effect of NS catalyst on different highly toxic organic new pollutants is the same as that in Example 6, except that the pollutant is changed to one of tetracycline (TTC), ciprofloxacin (CIP), and sulfadimethoxine (SMZ), and the concentration of the pollutant solution is 10 mg / L. Under the same experimental conditions as in Example 6, Fig.12 The results show that Co / TiO 2 The degradation rate of TTC and CIP by NS was 100% within 1 minute, and the removal rate of SMZ was 83%, indicating that Co / TiO 2 NS has excellent removal effect on various toxic antibiotic new pollutants in wastewater.
[0062] The above are merely exemplary embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing titanium dioxide nanosheets loaded with cobalt single atoms, characterized in that: The following steps are involved: Step 1: Anatase phase titanium dioxide powder, sodium hydroxide and water are placed in a reactor and stirred thoroughly, and then the reactor is kept warm in an oven and then naturally cooled to room temperature. The obtained product is washed and vacuum dried to obtain titanium dioxide nanosheets, which are recorded as TiO2 NS. Step 2: Add the cobalt salt solution to the TiO2 NS obtained in step 1, shake thoroughly and centrifuge to separate, wash the obtained product thoroughly and dry it in vacuum; Step 3: The sample obtained in step 2 is placed in a muffle furnace and calcined in an air atmosphere, and then the calcined sample is placed in an inorganic acid solution and shaken thoroughly. After centrifugal separation, the obtained product is washed and vacuum dried to obtain titanium dioxide nanosheets loaded with cobalt single atoms, which are recorded as Co / TiO2NS.
2. The preparation method according to claim 1, characterized in that: In step 1, the mass ratio of titanium dioxide powder to sodium hydroxide is 1:16-48.
3. The preparation method according to claim 1, characterized in that: In step 1, the heat preservation time in the oven is 6-24 hours, and the oven temperature is 110-150°C.
4. The preparation method according to claim 1, characterized in that: In step 2, the cobalt salt is one of cobalt sulfate, cobalt nitrate, cobalt chloride hexahydrate and cobalt carbonate, the concentration of the cobalt salt solution is 1-10mM, and the mass ratio of titanium dioxide nanosheets to cobalt salt is 1:0.01-0.
5.
5. The preparation method according to claim 1, characterized in that: In step 3, the calcination temperature is 150-250°C, the calcination time is 1-4 hours, and the heating rate is 2-10°C.
6. The preparation method according to claim 1, characterized in that: In step 3, the inorganic acid solution is one of hydrochloric acid solution, sulfuric acid solution and nitric acid solution, and the concentration of the inorganic acid solution is 0.5-1.5M.
7. A titanium dioxide nanosheet loaded with single cobalt atoms obtained by the preparation method according to any one of claims 1 to 6.
8. Use of the titanium dioxide nanosheet loaded with cobalt single atoms as claimed in claim 7 as a catalyst in activating peroxymonosulfate to degrade organic pollutants.
9. The use according to claim 8, characterized in that: Titanium dioxide nanosheets loaded with single cobalt atoms and permonosulfate as catalysts are added to the aqueous solution of organic pollutants to be treated. The permonosulfate generates strongly oxidizing hydroxyl radicals under the activation of the catalyst, thereby achieving the degradation of organic pollutants.
10. The use according to claim 9, characterized in that: The mass ratio of organic pollutants, catalyst and peroxymonosulfate is 1:1-5:3-10.
Citation Information
Patent Citations
Preparation method of titanium dioxide nano-sheet supported nickel titanate composite photocatalyst
CN108380217A
Preparation method and application of TiO2-loaded monatomic Co catalyst
CN109908899A
Gram-grade supported monatomic catalyst as well as preparation method and application thereof
CN115805071A
Ultrathin titanium dioxide nanowire loaded Co monatomic heterogeneous catalytic material as well as preparation and application thereof
CN118304886A