Modified zinc-iron spinel catalyst, preparation method and application
By combining alkali metal or alkaline earth metal on zinc iron spinel catalyst, the surface characteristics of the catalyst are adjusted, and the problems of insufficient CO2 conversion and C5+ selectivity of the existing catalysts are solved, achieving efficient C5+ hydrocarbon yield and low Methane selectivity.
Patent Information
- Application Number
- CN202410997399.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-15
AI Technical Summary
When existing catalysts convert CO2 to C5+ hydrocarbons, the CO2 conversion rate and C5+ hydrocarbon selectivity are insufficient, resulting in a lower C5+ yield.
Using modified zinc-iron spinel catalyst, the electron state and oxygen vacancies of the catalyst are adjusted by combining alkali metal or alkaline earth metal on zinc-iron spinel structure, the CO2 adsorption and activation capacity is improved, and the RWGS and carbon chain growth reaction is promoted. .
It significantly improves CO2 conversion and C5+ selectivity, improves the yield of C5+ hydrocarbons, reaches more than 31%, and reduces methane selectivity.
Smart Images

Figure CN118950003A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts for preparing higher carbon hydrocarbons by hydrogenating carbon dioxide, and in particular to a modified zinc-iron spinel catalyst, a preparation method and an application thereof. Background Art
[0002] Liquid fuel (C 5+ Hydrocarbons, generally including naphtha, gasoline, diesel, lubricating oil and other hydrocarbon substances. These chemicals have a large number of carbon atoms, have the advantages of high energy density, easy storage and transportation, and are often used as fuels or as chemical raw materials for processing and utilization. However, with the reduction of oil resources and the increase of CO2 emissions, economic development has been restricted and serious environmental problems have been brought about. Therefore, the development of targeted catalysis to convert CO2 into C 5+ Hydrocarbon technology is urgent.
[0003] In recent years, research on the conversion of CO2 by means of thermal catalysis, photocatalysis or electrocatalysis has emerged. Among them, the direct conversion of CO2 into high value-added hydrocarbons or fuels by modified Fischer-Tropsch synthesis has attracted widespread attention. Efficient catalysts are an important way to improve the conversion of CO2 into C 5+ The key to conversion and selectivity. Iron-based catalysts are considered to be the most promising catalysts for CO2 hydrogenation due to their low cost and excellent catalytic activity. During the reaction, Fe can be converted into Fe3O4 and iron carbide in situ, which are used for reverse water gas shift (RWGS) and chain growth reactions, respectively. However, pure iron catalysts have two serious problems: low CO2 conversion and high CH4 selectivity.
[0004] At present, most of the existing technologies use oxide / zeolite composite catalysts to catalyze CO2 to produce C 5+ , the carbon chain growth reaction is promoted by modifying zeolite. Specifically, Na-Fe3O4 / HZSM-5 and In2O3 / HZSM-5 composite catalysts have higher C 5+ The selectivity of hydrocarbons is low, but the CO2 conversion rate is only between 10% and 30%. For example, the document Nat. Commun. 2017, 8: 15174 discloses the use of Na-Fe3O4 / HZSM-5 catalyst, and its product C5-C 11 The proportion of total hydrocarbons is about 78%, but the CO2 conversion rate is only 22%. In addition, these composite catalysts usually have high CO selectivity, which also leads to C 5+ The yield is not ideal.
[0005] The invention patent application with publication number CN115155590A, entitled "A preparation method and application of a catalyst suitable for hydrogenation of carbon dioxide to produce liquid hydrocarbons", discloses that an electronic additive is evenly distributed in a MOF skeleton material, fully mixed with nitrogen-containing organic matter, and pyrolyzed under an inert gas atmosphere to obtain a nitrogen-doped carbon-supported iron-based catalyst. The CO2 conversion rate of the optimal embodiment 6K10CuFe-NC (PDA+NH2-BTC) catalyst is 39.54%, and the CO2 conversion rate of the target product C 5+ The selectivity to hydrocarbons is 54.32%, the selectivity to methane is 9.97%, and the selectivity to CO is 6.38%. Although the catalyst effectively improves the CO2 conversion rate, the conversion rate and the selectivity to C 5+ The selectivity of hydrocarbons is still not good enough, so C 5+ The yield is lower.
[0006] The invention patent application with publication number CN112570031A, entitled Catalyst for hydrogenation of carbon dioxide to produce high carbon hydrocarbons and its preparation and application, discloses a method of adding a soluble salt solution of Zn, K, Na, and Mn dropwise to an Fe-based metal organic framework material, performing equal volume impregnation, and drying and calcining to obtain a catalyst product. The CO2 conversion rate of the optimal embodiment MIL-88B-Fe-0.08K catalyst is 37.87%, and the CO2 conversion rate of the target product C 5+ The selectivity to hydrocarbons is as high as 83.78%, and the selectivity to methane is 9.9%. The catalyst greatly improves the selectivity to C 5+ The selectivity of hydrocarbons has been improved, but the CO2 conversion rate has not yet achieved an effective breakthrough.
[0007] In summary, the development of CO2 conversion into C 5+ Hydrocarbon directional catalyst, both CO2 conversion rate and C 5+ The ultimate goal of hydrocarbon selectivity is to 5+ Hydrocarbon yield is a technical problem that everyone is trying to break through. Summary of the invention
[0008] The purpose of the present invention is to provide a modified zinc-iron spinel catalyst, a preparation method and an application thereof, in order to further improve C 5+ The hydrocarbon yield provides new ideas.
[0009] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a modified zinc-iron spinel catalyst, which is a spinel structure or contains a spinel structure, which includes ZnFe2O4 spinel and an alkali metal or alkaline earth metal composited thereon; the molar ratio of Fe and Zn elements in the catalyst is 0.1 to 10, and the mass percentage of the alkali metal or alkaline earth metal in the catalyst is 0.1% to 10%.
[0010] Preferably, the alkali metal or alkaline earth metal is selected from sodium, magnesium, potassium and calcium.
[0011] Preferably, the active components in the catalyst are Fe3O4, Fe5C2 and ZnO.
[0012] A preferred solution of the above catalyst is that the catalyst is composed of ZnFe2O4 spinel and alkali metal Na, the molar ratio of Fe and Zn elements in the catalyst is 2:1, and the mass percentage of Na in the catalyst is 2%.
[0013] Another technical solution provided by the present invention is a method for preparing a modified zinc-iron spinel catalyst, comprising heating and dissolving an Fe precursor and a Zn precursor in a dispersant, then adding Na salt and Li salt or Na salt and K salt, grinding into powder after recrystallization, and calcining to obtain ZnFe2O4 spinel; adding a salt solution of an alkali metal or an alkaline earth metal dropwise to a catalyst precursor containing ZnFe2O4 spinel synthesized by a molten salt-assisted calcination method after recrystallization, fully dispersing and impregnating, and then calcining the product to obtain a modified zinc-iron spinel catalyst.
[0014] Preferably, the alkali metal or alkaline earth metal is selected from sodium, magnesium, potassium, and calcium, and the salt solution is one of carbonate, bicarbonate, nitrate, and sulfate; the solvent in the salt solution of the alkali metal or alkaline earth metal is deionized water, wherein the amount of the alkali metal or alkaline earth metal element is 0.5wt% to 5wt% of the total mass of the catalyst, and when it is added dropwise to the catalyst precursor, it is slowly added dropwise under ultrasonic conditions; the temperature of calcination after impregnation is 400 to 600°C, and the time is 2 to 5h.
[0015] In the above preferred embodiment, the slow dripping is completed in 1 to 2 hours; the alkali metal or alkaline earth metal salt solution uses sodium carbonate, and the amount of Na element is 1wt% to 4wt% of the total mass of the catalyst; the temperature of calcination after impregnation is 450 to 550°C, and the time is 3 to 4 hours.
[0016] Preferably, molten salt assisted calcination synthesis is used to obtain surface oxygen vacancies.
[0017] In the above preferred embodiments, the Fe precursor and the Zn precursor are ferric acetate and zinc acetate, the dispersant is water, and the dissolution is carried out under heating and stirring conditions; the salts of the Na salt and the Li salt or the Na salt and the K salt are NaCl and LiCl or NaCl and KCl; the recrystallization drying temperature is 100-140°C, and the time is 8-15h; the calcination temperature before impregnation is 700-1100°C, the heating rate is 2°C / min, and the insulation time is 0.5-2h.
[0018] Another technical solution provided by the present invention is: a modified zinc-iron spinel catalyst, or a catalyst prepared by the above preparation method, used in catalyzing the direct conversion of carbon dioxide into liquid fuel products, C 5+ The hydrocarbon yield can reach over 31%.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The modified zinc-iron spinel catalyst, preparation method and application thereof, the precursor prepared by molten salt assisted calcination has a single phase and obvious spinel structure characteristics, and the molten salt assisted calcination is conducive to the generation of abundant surface oxygen vacancies. The large amount of oxygen vacancies on the catalyst can significantly improve the adsorption of CO2 and promote the adsorption of oxygen-containing substances (*CO3 2- / *HCO3 - , *HCOO, *CO), and promote the activation of CO2; the appropriate zinc-iron ratio can significantly promote RWGS and carbon chain growth reactions, which is beneficial to improving the CO2 conversion rate, promoting the formation of intermediates, and accelerating subsequent reactions.
[0021] 2. The modified zinc-iron spinel catalyst, preparation method and application adopt an impregnation method to introduce alkali metal or alkaline earth metal elements, which has simple steps, can adjust the surface electronic state of the Fe-based catalyst, modify the alkalinity of the spinel surface, significantly increase the CO2 adsorption capacity, thereby affecting the iron carbonization rate, promoting the formation of iron carbide, and improving the catalytic performance. At the same time, the addition of alkali metal or alkaline earth metal elements inhibits the generation of CH4, significantly improving the CO2 conversion rate and C 5+ Selective.
[0022] 3. The modified zinc-iron spinel catalyst, preparation method and application have excellent C 5+ The high hydrocarbon yield not only opens up a new path for the design and modification of Fe-based catalysts, but also reveals broad prospects for directly converting carbon dioxide into liquid fuels. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The XRD spectra of Fe2O3 and three zinc-iron spinel catalyst precursors obtained in Example 1;
[0024] Figure 2 The XRD spectra of Fe2O3 obtained in Example 1 after reacting with three zinc-iron spinel catalyst precursors;
[0025] Figure 3 The scanning electron microscope images of Fe2O3 and three zinc-iron spinel catalyst precursors obtained in Example 1, in which a is Fe2O3, b is FeZn (4:1), c is FeZn (2:1), and d is FeZn (1:1);
[0026] Figure 4 The scanning electron microscope images of Fe2O3 obtained in Example 1 after the reaction with three zinc-iron spinel catalyst precursors, in which a is Fe2O3 after the reaction, b is FeZn (4:1) after the reaction, c is FeZn (2:1) after the reaction, and d is FeZn (1:1) after the reaction;
[0027] Figure 5 H2-TPR spectra of Fe2O3 and three zinc-iron spinel catalyst precursors obtained in Example 1. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters for implementation. It is particularly important to point out that all similar replacements and modifications are obvious to those skilled in the art, and they all fall within the scope of protection of the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0029] A modified zinc-iron spinel catalyst has a spinel structure or contains a spinel structure, comprising ZnFe2O4 spinel and an alkali metal or alkaline earth metal composited thereon; the molar ratio of Fe and Zn elements in the catalyst is 0.1 to 10, and the mass percentage of the alkali metal or alkaline earth metal in the catalyst is 0.1% to 10%; the alkali metal or alkaline earth metal can be further selected from sodium, magnesium, potassium, and calcium; the active components in the catalyst are preferably Fe3O4, Fe5C2 and ZnO.
[0030] In addition, the catalyst can be expressed as nwt% AM Fe x Zn y , or nwt%AMFeZn(X:Y), wherein AM is an alkali metal or alkaline earth metal element, x / y is the molar ratio of Fe and Zn elements in the catalyst; and nwt% is the mass percentage of the modified metal element in the entire catalyst.
[0031] The preparation method of the above-mentioned catalyst comprises: heating and dissolving an Fe precursor and a Zn precursor in a dispersant, then adding Na salt and Li salt or Na salt and K salt, grinding into powder after recrystallization, and calcining to obtain ZnFe2O4 spinel; dropping an alkali metal or alkaline earth metal salt solution into a catalyst precursor containing ZnFe2O4 spinel synthesized by a molten salt-assisted calcination method after recrystallization, fully dispersing and impregnating, and calcining the product to obtain a modified zinc-iron spinel catalyst;
[0032] For reference, in the above method: the alkali metal or alkaline earth metal is selected from sodium, magnesium, potassium, and calcium, and the salt solution is one of carbonate, bicarbonate, nitrate, and sulfate; the solvent in the salt solution of the alkali metal or alkaline earth metal is deionized water, wherein the amount of the alkali metal or alkaline earth metal element is 0.5wt% to 5wt% of the total mass of the catalyst, and when it is added dropwise to the catalyst precursor, it is slowly added dropwise under ultrasonic conditions; the temperature of calcination after impregnation is 400 to 600°C, and the time is 2 to 5h.
[0033] In a preferred embodiment, the slow addition is completed in 1 to 2 hours; the alkali metal or alkaline earth metal salt solution is sodium carbonate, and the amount of Na element is 1wt% to 4wt% of the total mass of the catalyst; the calcination temperature is 450 to 550°C, and the time is 3 to 4 hours.
[0034] For reference, the above-mentioned molten salt-assisted calcination synthesis is conducive to the generation of abundant surface oxygen vacancies and promotes the activation of CO2; further preferably, the Fe precursor and the Zn precursor are ferric acetate and zinc acetate, the dispersant is water, and the dissolution is carried out under heating and stirring conditions; the salts in the Na salt and the Li salt or the Na salt and the K salt are NaCl and LiCl or NaCl and KCl; the recrystallization drying temperature is 100-140°C, and the time is 8-15h; the calcination temperature before impregnation is 700-1100°C, the heating rate is 2°C / min, and the insulation time is 0.5-2h; the addition of sodium salt and lithium salt or potassium salt, on the one hand, helps to assist recrystallization, on the other hand, can reduce the melting temperature of the system, generally can ensure a certain molar ratio, such as salt: ZnFe2O4 greater than 2:1, too much will cause waste.
[0035] The above catalyst can be used to catalyze the direct conversion of carbon dioxide into liquid fuel products;
[0036] In some of the above preferred schemes, for example, when the catalyst is composed of ZnFe2O4 spinel and alkali metal Na, the molar ratio of Fe to Zn in the catalyst is 2:1, and the mass percentage of Na in the catalyst is 2%, C 5+ The hydrocarbon yield can reach more than 31%, and many other schemes can reach more than 32%, which exceeds the schemes recorded in the background technology; in addition, from the perspective of CH4 selectivity, the catalysts of the present invention are all lower than 15%, and can easily reach less than 12% under slightly controlled conditions. The CH4 selectivity performance under the optimal scheme (2wt% Na FeZn (2:1)) is less than 6%. From the perspective of carbon dioxide conversion rate, the present invention can reach more than 42%, and the highest can reach more than 48%.
[0037] The following examples are only for illustrative purposes, and it is impossible to list all examples. Therefore, the specific numbers in the following examples should not be used as absolute limiting conditions. The specific conditions should be based on the above-mentioned implementation methods and the content of the invention. As for the scope of protection required, the claims should be based on the scope. The content of the present invention is further described in conjunction with the examples below. The experimental raw materials used in the following examples are all general commercial products.
[0038] Embodiment 1:
[0039] This embodiment provides a Fe2O3 and a series of FeZn catalyst precursors, and the specific preparation method is as follows:
[0040] 10 mmol of ferric acetate was dissolved in 20 mL of water by heating. Subsequently, 40 mmol of NaCl and LiCl were added to the above solution and recrystallized at 120°C overnight. After drying, the solid was ground into powder. Then, it was calcined at 900°C for 1 hour at a heating rate of 2°C / min. The calcined sample was thoroughly washed with hot water to remove salts, and the sample was recorded as Fe2O3.
[0041] 10mmol of ferric acetate, 20mmol of ferric acetate, 40mmol of ferric acetate and three portions of 10mmol of zinc acetate were heated and dissolved in 20mL of water. Subsequently, 40mmol of NaCl and LiCl were added to the three solutions and recrystallized at 120°C overnight (12h). After drying, the three solids were ground into powders. Then, they were calcined at 900°C for 1h at a heating rate of 2°C / min. The calcined samples were thoroughly washed with hot water to remove salts, and the three groups of samples were recorded as FeZn (X:1, X=4, 2, 1), where X represents the molar ratio of Fe to Zn.
[0042] XRD analysis was performed on the above four groups of samples, and the results are as follows: Figure 1 As shown. It can be seen that the Fe2O3 catalyst is mainly composed of hematite. After adding Zn, the structure of the iron-based catalyst changed significantly. FeZn (4:1) appears as a solid solution state of Fe2O3 and ZnFe2O4. The FeZn (2:1) catalyst presents a typical ZnFe2O4 spinel structure. When the Fe / Zn ratio is 1:1, some additional diffraction peaks appear in the FeZn (1:1) catalyst, which are attributed to ZnO.
[0043] The above four groups of samples were directly used as catalysts to catalyze the hydrogenation of carbon dioxide under the same conditions, including normal pressure and high pressure (4.0MPa) tests; XRD analysis was performed on the four groups of samples after the reaction. Figure 2It can be seen that the diffraction peaks of Fe3O4 and Fe5C2 can be detected on all the catalysts after the reaction. For the FeZn (2:1) catalyst, the catalyst structure changes from the ZnFe2O4 phase to a mixed phase of Fe3O4, ZnO and Fe5C2. During the reduction process, ZnFe2O4 begins to decompose and the ZnO signal appears. Iron exists in the form of Fe and FeO. When reacting at normal pressure, the crystallinity of the sample further decreases and the signal of Fe5C2 appears. However, after reacting under high pressure (4.0MPa), the crystallinity of Fe and Zn increases. In addition to the Fe5C2 phase, ZnO phase and Fe3O4 phase are also observed. Fe5C2 plays a key role in the CC chain growth reaction because it can increase the C 5+ In the “tandem mechanism”, the Fe3O4 and Fe5C2 active phases are responsible for the conversion of CO2 to CO and the subsequent chain growth reaction.
[0044] The surface morphology of the four groups of samples before reaction was observed using a scanning electron microscope. Figure 3 As shown, the results show that the prepared Fe2O3 is composed of octahedral particles of different sizes, with an average particle size of about 0.68μm. The average particle size of FeZn(4:1) is about 0.42μm, which is smaller than that of Fe2O3. The average particle size of FeZn(2:1) is about 0.61μm, which is larger than that of FeZn(4:1) catalyst. With the increase of Zn content, the average particle size of the prepared FeZn(1:1) sample increases to 0.71μm. For the prepared FeZn(1:1) sample, the separation of ZnO particles from ZnFe2O4 octahedrons is the main reason for the further increase in the average particle size.
[0045] The surface morphology of the four groups of samples after reaction under high pressure (4.0MPa) was observed using a scanning electron microscope. Figure 4 As shown in the figure, for the Fe2O3 catalyst after the reaction, the morphology of the Fe2O3 catalyst has changed significantly, the particle size has decreased sharply, and the outer surface has become rough. After the reaction, the octahedral morphology disappears, and irregular particles and a small amount of rod-like structures are presented. Among them, the particle size of FeZn (2:1) is significantly reduced, and the specific surface area is increased. After the reaction, FeZn (2:1) shows the separation of rod-like ZnO and iron particles.
[0046] H2-TPR spectrum was used to detect the four groups of samples after reaction to study their reduction behavior. Figure 5 As shown, the H2-TPR spectrum of Fe2O3 at 454℃ is Fe 3+ →Fe 2+ At the same time, Fe 2+ →Fe 0 The reduction temperature of FeZn(2:1) is 632℃. Fe3+ →Fe 2+ The excessive introduction of Zn in FeZn (1:1) leads to the independent formation of ZnO, which makes Fe 3+ →Fe 2+ The reduction peak shifted to 400 °C. These results indicate that the addition of an appropriate amount of Zn can promote the reduction of iron-based catalysts.
[0047] Embodiment 2:
[0048] The four pre-reaction samples prepared in Example 1 were divided into multiple groups as precursors, sodium carbonate was used as the modified raw material, and various different masses of sodium carbonate (corresponding to a mass percentage of sodium in the catalyst of 0.1% to 10%) were weighed and dissolved in a small amount of water to prepare solutions;
[0049] Each group respectively slowly added sodium carbonate solution to the catalyst precursor under ultrasonic conditions (to ensure sufficient impregnation), the slow addition time was 1 to 2 hours, and calcined after the addition was completed, the calcination temperature was 400 to 600°C, and the time was 2 to 5 hours; and a variety of nwt% Na FeZn (X:1) catalysts were prepared.
[0050] Embodiment 3:
[0051] The samples of Example 1 and Example 2 were respectively tested for CO2 hydrogenation performance. The various samples were subjected to catalytic hydrogenation reaction under the conditions of 360°C, 4.0MPa and 4000mL gcat-1h-1 space velocity. The following groups of representative experimental results are compared, including unmodified FeZn (2:1), modified (1, 2, 4) wt% Na FeZn (2:1), modified 2wt% Na Fe2O3, and modified 2wt% Na FeZn (1:1, 4:1), representing Na loading 0-4wt%, Fe:Zn at 1:1-4:1 and no Zn addition, respectively. The test results are shown in Table 1:
[0052] Table 1 Effect of Na loading and Fe:Zn ratio in catalyst on catalytic performance of CO2 hydrogenation
[0053]
[0054] It can be seen from the table above that with the increase of Na content, CO2 conversion rate and C 5+ The selectivity increases first and then decreases. When the Na loading is 2 wt%, the CO2 conversion rate and C 5+ The selectivities reached 48.2% and 72.4%, respectively, and the yield reached 31.7%. Further increasing the Na loading to 4 wt%, the CO2 conversion rate slightly decreased to 44.5%, and the C 5+The selectivity dropped significantly to 56.2%. Excessive Na loading reduced the exposure of active sites, promoted the methanogenic reaction, and inhibited the carbon chain growth reaction. Therefore, appropriate Na loading is beneficial to increase the C 5+ The formation of hydrocarbons.
[0055] The CO2 conversion rate of the 2wt% NaFeZn (4:1) catalyst is 45.5%, and the CO selectivity is 11.9%. When the Fe:Zn molar ratio is 2:1, the CO2 conversion rate of the catalyst is 48.2%, and the CO selectivity is 11.9%. 5+ The selectivity is 72.4%, while the undesired CO selectivity is suppressed to 8.9%. Compared with other FeZn catalysts in this example, the 2wt% NaFeZn (1:1) catalyst has a lower CO2 conversion rate and a higher CO selectivity. In addition, too high a zinc content will lead to an increase in CH4 selectivity and a decrease in C 5+ These results show that appropriate zinc content is beneficial to improve CO2 conversion and C 5+ Selective.
[0056] Embodiment 4:
[0057] The method is the same as that in Example 2, but K, Mg, and Ca are used to replace Na element, respectively, to prepare a variety of nwt% AM FeZn (X: Y) catalysts, and the CO2 hydrogenation performance of different catalyst samples is tested. Various samples are subjected to catalytic hydrogenation reaction under the conditions of 360°C, 4.0 MPa and 4000 mL gcat-1 h-1 space velocity. The following groups of representative experimental results are compared, including 1wt% KFeZn (2: 1), 1wt% Mg FeZn (2: 1), and 1wt% Ca FeZn (2: 1); the specific results are shown in Table 2 below:
[0058] Table 2 Effect of modified elements loaded in catalyst on catalytic performance of CO2 hydrogenation
[0059]
[0060] Compared with 1wt% NaFeZn (2:1) in Example 3, it can be seen that potassium has a higher CO2 conversion rate and C 5+ The selectivity is better than that of FeZn (2:1) in Example 3, and the performance of the three catalysts in this example is greatly improved.
[0061] In summary, the results of each embodiment show that the alkali metal modified ZnFe2O4 spinel catalyst synthesized by the molten salt assisted strategy adopted in the present invention shows obvious advantages, which can maintain a high CO2 conversion rate and significantly improve C 5+ Selectivity is beneficial to improve C 5+Yield, providing new ideas for the development of CO2 hydrogenation catalyst field.
[0062] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
[0063] The matters not described in detail in the present invention are all known technologies to those skilled in the art.
Claims
1. A modified zinc-iron spinel catalyst, characterized in that: The catalyst is a spinel structure or contains a spinel structure, which includes ZnFe2O4 spinel and an alkali metal or alkaline earth metal compounded thereon; the molar ratio of Fe and Zn elements in the catalyst is 0.1-10, and the mass percentage of the alkali metal or alkaline earth metal in the catalyst is 0.1%-10%.
2. A modified zinc-iron spinel catalyst according to claim 1, characterized in that: The alkali metal or alkaline earth metal is selected from sodium, magnesium, potassium and calcium.
3. A modified zinc-iron spinel catalyst according to claim 2, characterized in that: The active components in the catalyst are Fe3O4, Fe5C2 and ZnO.
4. A modified zinc-iron spinel catalyst according to claim 1, characterized in that: The catalyst is composed of ZnFe2O4 spinel and alkali metal Na, the molar ratio of Fe and Zn elements in the catalyst is 2:1, and the mass percentage of Na in the catalyst is 2%.
5. A method for preparing a modified zinc-iron spinel catalyst according to any one of claims 1 to 4, characterized in that: The method comprises heating and dissolving an Fe precursor and a Zn precursor in a dispersant, then adding Na salt and Li salt or Na salt and K salt, grinding into powder after recrystallization, and calcining to obtain ZnFe2O4 spinel; dropping an alkali metal or alkaline earth metal salt solution into a catalyst precursor containing ZnFe2O4 spinel synthesized by a molten salt-assisted calcination method after recrystallization, fully dispersing and impregnating, and calcining the product to obtain a modified zinc-iron spinel catalyst.
6. The preparation method according to claim 5, characterized in that: The alkali metal or alkaline earth metal is selected from sodium, magnesium, potassium, and calcium, and the salt solution is one of carbonate, bicarbonate, nitrate, and sulfate; the solvent in the salt solution of the alkali metal or alkaline earth metal is deionized water, wherein the amount of the alkali metal or alkaline earth metal element is 0.5wt% to 5wt% of the total mass of the catalyst, and when it is dripped into the catalyst precursor, it is slowly dripped under ultrasonic conditions; the calcination temperature after impregnation is 400 to 600°C, and the time is 2 to 5h.
7. The preparation method according to claim 6, characterized in that: The slow dripping takes 1 to 2 hours to complete; the alkali metal or alkaline earth metal salt solution uses sodium carbonate, and the amount of Na element is 1wt% to 4wt% of the total mass of the catalyst; the calcination temperature after impregnation is 450 to 550°C and the time is 3 to 4 hours.
8. The preparation method according to claim 5, characterized in that: The molten salt assisted calcination synthesis is used to obtain surface oxygen vacancies.
9. The preparation method according to claim 5, characterized in that: In the synthesis steps of the molten salt-assisted calcination method: Fe precursor and Zn precursor are ferric acetate and zinc acetate, the dispersant is water, and the dissolution is carried out under heating and stirring conditions; the salts of Na salt and Li salt or Na salt and K salt are NaCl and LiCl or NaCl and KCl; the recrystallization drying temperature is 100-140°C, and the time is 8-15h; the calcination temperature before impregnation is 700-1100°C, the heating rate is 2°C / min, and the insulation time is 0.5-2h.
10. Use of the modified zinc-iron spinel catalyst according to any one of claims 1 to 4, or the catalyst prepared by the preparation method according to any one of claims 5 to 9, in catalyzing direct conversion of carbon dioxide into liquid fuel products, characterized in that: C 5+ The hydrocarbon yield can reach more than 31%, and the CH4 selectivity can reach less than 6%.
Citation Information
Patent Citations
Catalyst for preparing olefin by dehydrogenation of low-carbon alkane and preparation and application thereof
CN114588898A
Fe-Zn bimetallic catalyst, preparation method and application
CN118056609A
Iron-zinc catalysts for the conversion of synthesis gas to alpha-olefins
US5185378A
KR20190043869A
Cited By
Preparation method of sodium-promoted zinc-aluminum spinel supported iron-based catalyst and application of catalyst in olefin synthesis
CN119701920A
Preparation method of catalyst for preparing diesel fraction hydrocarbon through carbon dioxide hydrogenation
CN120586885A
K-ZnFe-LDH catalyst and preparation method and application thereof
CN121869369A