Flotation separation combined inhibitor for low-grade siliceous phosphorite and application of flotation separation combined inhibitor

By using a combination of copper ions, water glass, and hydroxyethylidene diphosphonic acid as inhibitors, the selective inhibition problem in the flotation separation of low-grade siliceous phosphate rock was solved, improving the grade and recovery rate of phosphate rock, simplifying wastewater treatment, and achieving efficient separation of siliceous gangue minerals.

CN118950264APending Publication Date: 2024-11-15KUNMING UNIV OF SCI & TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411057595.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In existing technologies, flotation separation of low-grade siliceous phosphate rock is difficult, especially the selective inhibition effect of siliceous gangue minerals is poor, which leads to great difficulty in treating mineral processing wastewater. In addition, traditional inhibitors such as water glass require large amounts and have poor selectivity.

Method used

A combination of copper ions, water glass, and hydroxyethylidene diphosphonic acid was used as inhibitors to achieve efficient separation of phosphate rock and siliceous gangue minerals through a flotation process consisting of one roughing, two scavenging, and three cleaning stages.

Benefits of technology

It improves the grade and recovery rate of phosphate rock, reduces the amount of reagents used, simplifies wastewater treatment, avoids the settling difficulties when water glass is used alone, and achieves efficient selective inhibition of siliceous gangue minerals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950264A_ABST
    Figure CN118950264A_ABST
Patent Text Reader

Abstract

The invention discloses a flotation separation combined inhibitor for low-grade siliceous phosphorite and application of the flotation separation combined inhibitor, and belongs to the technical field of mineral processing flotation. The combined inhibitor is composed of copper ions, water glass and 1-hydroxyethylidene-1, 1-diphosphonic acid in a mass ratio of (0.5-2): (5-20): (1.5-5). The invention further provides application of the siliceous gangue mineral combined inhibitor. The application specifically comprises the following steps that firstly, an ore sample is ground; the ore pulp is adjusted to the needed ore pulp concentration and pH value, a combined inhibitor is added, rough flotation is conducted once, and phosphorite rough concentrate and siliceous gangue tailings are obtained; and carrying out concentration for three times to obtain a final phosphorite concentrate product. And scavenging twice to obtain the phosphate flotation tailings. The combined inhibitor is high in selectivity, green, economical and environmentally friendly, the dosage of a water glass agent is effectively reduced, flotation separation of phosphorite and siliceous gangue minerals is achieved, and the application prospect is wide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a flotation separation combined inhibitor for low-grade siliceous phosphate ore and application thereof, belonging to the technical field of mineral processing and flotation. Background Art

[0002] Phosphorus is one of the elements necessary for the growth of life on Earth. It is widely used in agricultural production, chemical pharmaceuticals, building materials and other fields. Phosphate rock is the main source of phosphorus resources. It refers to the general term for phosphate minerals that can be used economically, mainly apatite and phosphorite. Phosphate rock is an important non-metallic strategic resource that is irreplaceable and non-renewable. my country has a large basic reserve of phosphate resources and rich types of phosphate mines, but the grade of the original ore is low, the rich ore resources are few, the embedded particle size is fine, the impurity content is high, and the mining is difficult. Most of the medium and low-grade phosphate ores need to be processed before further use.

[0003] According to the type and content of gangue components in phosphate ore, phosphate ore can be divided into calcareous, siliceous and mixed (silicon-calcium / calcium-siliceous) phosphate ore. The gangue minerals of siliceous phosphate ore are mainly quartz, feldspar and mica, etc., and also contain a small amount of calcite and dolomite. The processing and treatment of this type of phosphate ore focuses on the efficient removal of siliceous minerals in phosphate ore. Since the natural hydrophobicity of silicate minerals such as quartz is poorer than that of useful mineral phosphate minerals, positive flotation process can be used for desiliconization. Fatty acid collectors are often selected in the removal process, so the selection and application of efficient selective inhibitors for siliceous gangue minerals is crucial.

[0004] At present, the most widely used inhibitor in the industry is still the traditional inhibitor water glass. In the flotation process, the amount of water glass used is large, and the selective inhibition effect is poor. Adding a large amount of water glass will also make the tailings highly dispersed, difficult to settle, and difficult to treat the mineral processing wastewater. Therefore, the development of green, low-cost and efficient inhibitors for siliceous gangue minerals in phosphate ore flotation is the development trend of mineral processing in the future, which is of great significance to improving the utilization rate of phosphorus resources in my country. Summary of the invention

[0005] In order to solve the problem of difficulty in flotation separation of existing phosphate ore and siliceous gangue minerals such as quartz and feldspar, the purpose of the present invention is to provide a flotation separation combined inhibitor for low-grade siliceous phosphate ore and its application, which is used to solve the problem of difficulty in flotation separation of phosphate ore and siliceous gangue minerals such as quartz in positive flotation.

[0006] The combined inhibitor includes copper ions, water glass and hydroxyethylidene diphosphonic acid.

[0007] Preferably, the mass ratio of copper ion, water glass and hydroxyethylidene diphosphonic acid in the combined inhibitor is (0.5-2):(5-20):(1.5-5).

[0008] Preferably, the copper ion is a compound containing copper ions.

[0009] Preferably, the copper ion compound is copper sulfate.

[0010] The present invention also provides an application of a combined depressant in the flotation separation of low-grade siliceous phosphate ore.

[0011] Preferably, phosphate concentrate and phosphate tailings are obtained from low-grade siliceous phosphate ore through a flotation process of one roughing selection, two scavenging selections and three concentrating selections.

[0012] Preferably, the combined inhibitor is added during the roughing, the first cleaning (cleaning I) and the second cleaning (cleaning II) processes, and the combined inhibitor is not added in other processes.

[0013] Preferably, the amount of combined inhibitor added during the roughing process is 250-500 g / t; the amount of combined inhibitor added during the first concentration is 80-180 g / t, and the amount of combined inhibitor added during the second concentration is 30-60 g / t.

[0014] Preferably, the combined inhibitor is first dissolved with deionized water when used. The specific process is: first dissolve copper sulfate with deionized water, then add water glass, stir, and finally add hydroxyethylidene diphosphonic acid, stir evenly, and stir each agent for 3 to 5 minutes.

[0015] Preferably, the specific process flow of flotation separation is as follows:

[0016] (1) Grind the ore sample and adjust the slurry to the required slurry concentration and pH value.

[0017] (2) Rough selection of phosphate ore: adding a combined depressant to the slurry obtained in step (1), stirring, adding a collector, stirring, and flotation to obtain a rough phosphate ore concentrate and siliceous gangue tailings.

[0018] (3) Phosphate ore scavenging: The gangue tailings obtained in step (2) are subjected to phosphate ore scavenging. In the first scavenging (scavenging I), a collector is added, stirred, and flotated; in the second scavenging (scavenging II), a collector is added, stirred, and flotated to obtain the final floating phosphorus tailings.

[0019] (4) Phosphate ore concentration: The rough concentrate obtained in step (2) is subjected to phosphate ore concentration. In the first concentration (concentration I), a combined depressant is added, stirred, and floated; in the second concentration (concentration II), a combined depressant is added, stirred, and floated; in the third concentration (concentration III), no combined depressant is added, stirred, and floated to obtain a final phosphate concentrate.

[0020] Preferably, in step (1), the grinding fineness satisfies -0.074 mm, accounting for 70% to 85%.

[0021] Preferably, in step (1), the slurry concentration is 15% to 25%, the slurry pH is 8 to 11, the adjusting agent is one or a combination of two of sodium hydroxide and sodium carbonate in any proportion, and the slurry adjustment time is 2 to 3 minutes.

[0022] Preferably, in step (2), the addition amount of the combined inhibitor is 250-500 g / t, the addition amount of the collector sodium oleate is 200-450 g / t; the stirring time is 2-3 min, and the flotation time is 4-5 min.

[0023] Preferably, in step (3), the amount of collector added in the first scavenging (scavenging I) is 60-150 g / t; the amount of collector added in the second scavenging (scavenging II) is 20-50 g / t; the stirring time of the first scavenging (scavenging I) and the second scavenging (scavenging II) is 2-3 min, the flotation time of the first scavenging (scavenging I) is 3-4 min, and the flotation time of the second scavenging (scavenging II) is 2.5-3.5 min.

[0024] Preferably, in step (4), the amount of the combined depressant added in the first concentration (concentration I) is 80-180 g / t, the stirring time is 2-3 min, and the flotation time is 2-3 min; in the second concentration (concentration II), the amount of the combined depressant added is 30-60 g / t, the stirring time is 2-3 min, and the flotation time is 2-3 min.

[0025] The collector used in the flotation separation process can be any conventional collector.

[0026] The principle of the present invention is as follows: water glass is a commonly used flotation inhibitor for siliceous gangue minerals in the flotation of phosphate-containing ores, but the inhibitory ability of water glass is greatly affected by the slurry environment and its poor selectivity restricts its wide application; copper ions will undergo hydroxylation reactions to varying degrees in an alkaline slurry solution, and the generated different copper hydroxy compounds will selectively adsorb on the surface of siliceous gangue minerals such as calcite and dolomite, and because of the large amount of hydrophilic polar groups (hydroxyl groups, etc.) contained in them, they have a selective inhibitory effect on siliceous minerals; hydroxyethylidene diphosphonic acid is an organic phosphoric acid with a molecular formula of Its molecules contain polar groups such as phosphate and hydroxyl groups, which can be selectively adsorbed on the surface of silicon-containing minerals to play a selective inhibitory role. At the same time, copper ions will also coordinate with these polar functional groups and co-adsorb on the surface of silicon-containing gangue minerals to produce a selective inhibitory effect. The addition of water glass has the effect of dispersing the slurry, which can effectively reduce the viscosity of the slurry and increase the adsorption of the agent on the mineral surface. Therefore, the coordination and co-adsorption behavior of copper ions and hydroxyethylidene diphosphonic acid on the surface of silicon-containing gangue minerals promote the selective inhibition of water glass on silicon-containing gangue minerals, effectively increase the selectivity of water glass, and reduce the impact of single water glass on the environment.

[0027] Beneficial effects of the present invention

[0028] (1) The present invention proposes for the first time to use a combination of metal ion copper ion with an organic inhibitor hydroxyethylidene diphosphonic acid and an inorganic inhibitor water glass as a flotation inhibitor for siliceous gangue minerals in phosphate ore flotation. Its application in phosphate ore flotation has not been reported yet.

[0029] (2) The combined inhibition in the present invention is applied to phosphate ore flotation, aiming to achieve efficient flotation separation of phosphate ore and siliceous gangue minerals, and obtain high-grade phosphate ore concentrate, which has the characteristics of small dosage, strong selective inhibition and good separation index.

[0030] (3) The active ingredients of the combined inhibitors of the present invention are all conventional drugs, which are widely available, non-toxic, water-soluble, easily degradable, and inexpensive.

[0031] (4) The combined inhibitor of the present invention has a simple formulation and is easy to implement in industry, thus successfully avoiding the problems of wastewater being difficult to settle and reuse when using only water glass as an inhibitor. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The phosphate rock flotation process flow diagram of the embodiment and the comparative example. DETAILED DESCRIPTION

[0033] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0034] Example 1

[0035] In the composition of the combined inhibitor in this embodiment, the mass ratio of copper sulfate, water glass and hydroxyethylidene diphosphonic acid is 0.5:20:1.5, and the collector is a sodium oleate aqueous solution.

[0036] A low-grade siliceous collophosphate ore in Yunnan has a P2O5 grade of 14.37% in the original ore. The gangue minerals are mainly quartz, feldspar and dolomite, with a SiO2 content of 28.59%, followed by andradite, calcite, mica and a small amount of fine-grained clay minerals such as kaolin. The mineral mud is relatively serious, and it belongs to a low-grade siliceous phosphate ore. The flotation separation process of this embodiment is as follows Figure 1 The results are shown in Table 1. The specific steps are as follows:

[0037] (1) The raw ore is ground to a grinding fineness of -0.074 mm, accounting for 75%, and a pulp concentration of 20%; the pH adjuster is sodium carbonate, and the pH of the pulp is adjusted to 9.5.

[0038] (2) The qualified raw ore pulp in step (1) is subjected to rough phosphate ore selection: first, a combined inhibitor is added in an amount of 450 g / t, and stirred for 2 min, and then a collector sodium oleate is added in an amount of 360 g / t, and stirred for 2 min; flotation is performed for 4 min; and finally, a rougher concentrate and a rougher tailing are obtained.

[0039] (3) The rougher tailings obtained in step (2) are subjected to phosphate ore scavenging: in the first scavenging (scavenging I), a collector sodium oleate is added in an amount of 120 g / t, stirred for 2 min, and floated for 3 min; in the second scavenging (scavenging II), a collector is added in an amount of 40 g / t, stirred for 2 min, and floated for 2.5 min; and the final phosphate tailings are obtained.

[0040] (4) The rougher concentrate obtained in step (2) is subjected to phosphate ore concentration: in the first concentration (concentration I), a combined depressant is added in an amount of 150 g / t, stirred for 2 min, and floated for 2 min; in the second concentration (concentration II), a combined depressant is added in an amount of 50 g / t, stirred for 2 min, and floated for 2 min; in the third concentration (concentration III), no depressant is added, blank concentration is performed, and floatation is performed for 2 min to obtain the final phosphate concentrate.

[0041] Comparative Example 1

[0042] The process flow of this comparative example is the same as that of Example 1. For comparison, the difference between this comparative example and Example 1 is that the inhibitor uses a single water glass. The flotation results are shown in Table 1. The specific operation steps are as follows (the steps not mentioned are the same as those in Example 1):

[0043] In step (2), during the roughing process of phosphate ore, water glass is selected as the inhibitor, and the dosage is 450 g / t;

[0044] In step (4) phosphate ore concentration: in the first concentration (concentration I), the amount of inhibitor water glass used is 150 g / t; in the second concentration (concentration II), the amount of inhibitor water glass used is 50 g / t, and the types of other reagents added, the amounts of reagents used and the flotation time are the same as those in Example 1.

[0045] Comparative Example 2

[0046] The process flow of this comparative example is the same as that of the embodiment. As a comparison, the difference between this comparative example and embodiment 1 is that the inhibitor adopts a single organic inhibitor hydroxyethylidene diphosphonic acid. The flotation results are shown in Table 1. The specific operation steps are as follows (the steps not mentioned are the same as those in embodiment 1):

[0047] In the step (2) of phosphate roughing, the inhibitor is hydroxyethylidene diphosphonic acid, and the dosage is 450 g / t;

[0048] In step (4) phosphate ore concentration: in the first concentration (concentration I), the amount of inhibitor hydroxyethylidene diphosphonic acid is 150 g / t; in the second concentration (concentration II), the amount of inhibitor hydroxyethylidene diphosphonic acid is 50 g / t. The other reagents added, the amount of reagents used and the flotation time are the same as those in Example 1.

[0049] Table 1 Full process closed circuit test results of Example 1 and Comparative Examples 1-2

[0050]

[0051] As shown in Table 1, under the same flotation collector and flotation process conditions, compared with single flotation inorganic depressant water glass and single flotation organic depressant hydroxyethylidene diphosphonic acid, the combined depressor (mass ratio of copper ion, water glass, hydroxyethylidene diphosphonic acid is 10%, 50% and 40%) can obtain higher P2O5 grade and P2O5 recovery rate, which are 34.62% and 86.58% respectively. This shows that the combined depressor under this mass ratio condition is an excellent depressor for low-grade siliceous phosphate ore.

[0052] Example 2

[0053] The composition of the combined inhibitor in this embodiment includes copper sulfate (copper ions), water glass, and hydroxyethylidene diphosphonic acid in a mass ratio of 2:5:5, and the collector is a sodium oleate aqueous solution.

[0054] A low-grade collophanite in Hubei has a complex mineral composition. The P2O5 grade in the ore is 11.36%, the SiO2 content is 25.49%, the CaO content is 28.62%, the MgO content is 5.74%, the Fe2O3 content is 2.38%, the main gangue minerals are quartz, mica, calcite and dolomite, and the main phosphorus-containing mineral in the ore is collophanite, and the occupancy rate of phosphorus in the gangue minerals is very low. The flotation process of this embodiment is as follows: Figure 1 As shown, the specific steps are as follows:

[0055] (1) The raw ore is ground to a grinding fineness of -0.074 mm, accounting for 78%, and a pulp concentration of 18%; the pH adjuster is sodium carbonate, and the pH of the pulp is adjusted to 10.5.

[0056] (2) The qualified raw ore pulp in step (1) is subjected to rough phosphate ore selection: first, a combined inhibitor is added in an amount of 420 g / t, and stirred for 2 min, and then a collector sodium oleate is added in an amount of 400 g / t, and stirred for 2 min; flotation is performed for 4 min; and finally, a rougher concentrate and a rougher tailing are obtained.

[0057] (3) The roughing tailings obtained in step (2) are subjected to phosphate ore scavenging: scavenging I: adding a collector sodium oleate in an amount of 130 g / t, stirring for 2 min, and flotation for 3 min; scavenging II: adding a collector in an amount of 45 g / t, stirring for 2 min, and flotation for 2.5 min; and obtaining the final phosphate tailings.

[0058] (4) The rougher concentrate obtained in step (2) is subjected to phosphate ore concentration: Concentration I: adding a combined depressant in an amount of 140 g / t, stirring for 2 min, and flotation for 2 min; Concentration II: adding a combined depressant in an amount of 48 g / t, stirring for 2 min, and flotation for 2 min; Concentration III: without adding depressants, blank concentration, flotation for 2 min, to obtain the final phosphate concentrate.

[0059] Comparative Example 3

[0060] The process flow of this comparative example is the same as that of Example 2. For comparison, the difference between this comparative example and Example 2 is that the inhibitor is water glass + copper ion, and the mass ratio of copper ion to water glass is 20% and 80%. The pH of the ore pulp is adjusted to 10.5. The flotation results are shown in Table 2. The specific operation steps are as follows (the steps not mentioned are the same as those in Example 2):

[0061] In step (2), during the roughing process of phosphate ore, water glass + copper ions are selected as the inhibitor, and the dosage is 420 g / t;

[0062] Step (4) Phosphate ore concentration: In the first concentration (concentration I), the amount of inhibitor water glass + copper ion is 140 g / t; In the second concentration (concentration II), the amount of inhibitor water glass + copper ion is 48 g / t. The other reagents added, the amount of reagents used and the flotation time are the same as those in Example 1.

[0063] Comparative Example 4

[0064] The process flow of this comparative example is the same as that of Example 2. For comparison, the difference between this comparative example and Example 2 is that the inhibitor uses water glass + hydroxyethylidene diphosphonic acid, the mass ratio of water glass and hydroxyethylidene diphosphonic acid is 70% and 30%, the pH of the slurry is adjusted to 10.5, and the flotation results are shown in Table 2. The specific operation steps are as follows (the steps not mentioned are the same as those in Example 2):

[0065] In the step (2) of phosphate ore roughing, water glass + hydroxyethylidene diphosphonic acid are selected as the inhibitor, and the dosage is 420 g / t;

[0066] Step (4) phosphate ore concentration: in the first concentration (concentration I), the amount of inhibitor water glass + hydroxyethylidene diphosphonic acid is 140 g / t; in the second concentration (concentration II), the amount of inhibitor water glass + hydroxyethylidene diphosphonic acid is 48 g / t. The other reagents added, the amount of reagents used and the flotation time are the same as those in Example 1.

[0067] Comparative Example 5

[0068] The process flow of this comparative example is the same as that of Example 2. For comparison, the difference between this comparative example and Example 2 is that the inhibitor uses a single water glass, the pH of the pulp is adjusted to 10.5, and the flotation results are shown in Table 2. The specific operation steps are as follows (the steps not mentioned are the same as those in Example 2):

[0069] In step (2), during the roughing process of phosphate ore, water glass is selected as the inhibitor, and the dosage is 420 g / t;

[0070] Step (4) Phosphate ore concentration: In the first concentration (concentration I), the amount of water glass as an inhibitor is 140 g / t; In the second concentration (concentration II), the amount of water glass as an inhibitor is 48 g / t. The other reagents added, the amount of reagents used and the flotation time are the same as those in Example 1.

[0071] Comparative Example 6

[0072] The process flow of this comparative example is the same as that of Example 2. For comparison, the difference between this comparative example and Example 2 is that the inhibitor uses a single organic inhibitor, hydroxyethylidene diphosphonic acid, the pulp pH is adjusted to 10.5, and the flotation results are shown in Table 2. The specific operation steps are as follows (the steps not mentioned are the same as those in Example 2):

[0073] In the step (2) of phosphate ore roughing, the inhibitor is hydroxyethylidene diphosphonic acid, and the dosage is 420 g / t;

[0074] In step (4) phosphate ore concentration: in the first concentration (concentration I), the amount of inhibitor hydroxyethylidene diphosphonic acid is 140 g / t; in the second concentration (concentration II), the amount of inhibitor hydroxyethylidene diphosphonic acid is 48 g / t. The other reagents added, the reagent amounts and the flotation time are the same as those in Example 2.

[0075] Table 2 Full process closed circuit test results of Example 2 and Comparative Examples 3 to 6

[0076]

[0077] By analyzing comparative examples 3 to 6, it can be seen that, compared with Example 2, when pH = 10.5, the index of phosphate ore flotation is the best when the combined collector is used. At this time, the grade of P2O5 in the phosphate concentrate is 31.29%, and the recovery rate of P2O5 is 82.76%. Therefore, from the effect of the reagent, the effect of the combined inhibitor is better than that of water glass + copper ions, water glass + hydroxyethylidene diphosphonic acid, a single inorganic inhibitor water glass and a single organic inhibitor hydroxyethylidene diphosphonic acid.

Claims

1. A combined depressant for flotation separation of low-grade siliceous phosphate ore, characterized in that: The combined inhibitor includes copper ions, water glass and hydroxyethylidene diphosphonic acid.

2. The combined depressant for flotation separation of low-grade siliceous phosphate ore according to claim 1, characterized in that: The mass ratio of copper ion, water glass and hydroxyethylidene diphosphonic acid in the combined inhibitor is (0.5-2):(5-20):(1.5-5).

3. The combined depressant for flotation separation of low-grade siliceous phosphate ore according to claim 1, characterized in that: The copper ion is a compound containing copper ions.

4. The combined depressant for flotation separation of low-grade siliceous phosphate ore according to claim 3, characterized in that: The compound containing copper ions is copper sulfate.

5. Use of the combined depressant for flotation separation of low-grade siliceous phosphate ore according to any one of claims 1 to 3 in the flotation separation of low-grade siliceous phosphate ore.

6. The use according to claim 5, characterized in that: Phosphate concentrate and tailings are obtained from low-grade siliceous phosphate ore through a flotation process of one roughing selection, two scavenging selections and three concentrating selections.

7. The use according to claim 6, characterized in that: Combined inhibitors are added in the first roughing, first cleaning and second cleaning processes, and are not added in other processes.

8. The use according to claim 5, characterized in that: The amount of combined inhibitor added during the roughing process is 250-500 g / t; the amount of combined inhibitor added during the first concentration is 80-180 g / t, and the amount of combined inhibitor added during the second concentration is 30-60 g / t.

Citation Information

Patent Citations

  • Positive flotation method of low grade refractory phosphate ores

    CN101791592A

  • Composite inhibitor and direct flotation method for low-grade refractory phosphate

    CN104259012A

  • Application of organic phosphoric acid type compound to mineral flotation

    CN108654844A

  • Beneficiation method for silicate and carbonate type fluorite ores

    CN111632747A

  • Magnesium silicate gangue combined inhibitor and high-efficiency sorting method for low-grade magnesium silicate-containing copper sulphide ore

    CN117900035A