A method for flotation of tungsten ore
The existing tungsten ore is solved by using the two-site chelation of lead and sulfur-nitrogen functional groups in flotation using the combination of lead and sulfur-nitrogen-hydroxamic acid or sulfur-nitrogen ester-hydroxamic acid in tungsten ore flotation. The problem of unsatisfactory flotation performance has achieved efficient tungsten ore recovery and good sorting of tungsten ore and calcium-containing gangue, which has reduced the dosage of drugs and improved economic benefits.
Patent Information
- Application Number
- CN202110887073.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-03
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-08-03
AI Technical Summary
The existing tungsten ore flotation methods have the problem of poor flotation performance, especially the flotation effect of sedraelite, and the dose of the agent is large and the economic benefits are not high.
Using lead ion activator and sulfur-nitrogen-hydroxamic acid or sulfur-nitrogen ester-hydroxamic acid as collectors, the flotation activation effect of tungsten ore is enhanced through the two-site chelation of lead and sulfur-nitrogen functional groups, and the flotation activation effect of tungsten ore is enhanced. Sorting selectivity of ore and calcium-containing ganglite.
It significantly improves the flotation recovery rate of tungsten ore, reduces the amount of flotation agent, improves the sorting selectivity of tungsten ore and calcium-containing gangue, and has good industrial application prospects.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure BDA0003194534650000021
Abstract
Description
Technical Field
[0001] The invention relates to a flotation mineral separation method and belongs to the technical field of mineral flotation. Background Art
[0002] Tungsten ore mainly includes wolframite and scheelite, of which scheelite is the main tungsten mineral, accounting for about 70% of tungsten ore resources, wolframite accounts for about 20%, and mixed black and white tungsten ore accounts for about 10%. Flotation is the main beneficiation method for separating and enriching tungsten ore.
[0003] There are currently two main processes for tungsten flotation (Wei Zhao, Sun Wei, Han Haisheng, Wang Jianjun, Wang Ruolin, Kang Jianhua. Progress and Practice of Tungsten Flotation Technology. Metal Mines, 2021, 540(06): 60-72). One flotation process mainly uses fatty acid collectors, which is divided into room temperature flotation and "Petrov" heated flotation, and is mainly used for the flotation recovery of scheelite. Among them, heated flotation helps the flotation separation of scheelite and calcium-containing gangue minerals. The other flotation process mainly uses hydroxamic acid collectors, which is mainly divided into GY (hydroxamic acid and fatty acid) method and benzohydroxamic acid method. The GY method uses lead nitrate as an activator and uses the synergy of benzohydroxamic acid and fatty acids to achieve mixed flotation of black and white tungsten ores. The benzohydroxamic acid method uses lead nitrate as an activator and benzohydroxamic acid as a collector to float black and white wolframite, which can achieve high-efficiency short-process flotation separation of black and white wolframite at room temperature, and by pre-mixing lead nitrate and benzohydroxamic acid (which may generate lead benzohydroxamic acid complexes or complex ions), the flotation indicators of black and white wolframite can be improved.
[0004] At the same time, a Chinese patent (Liu Guangyi, Qi Jing, Fan Hongli, Liu Sheng. A sulfur-nitrogen-hydroxamic acid bifunctional collector and its application, ZL2018111291418, 2018-9-26) discloses a sulfur-nitrogen-hydroxamic acid collector applied to tungsten ore flotation; and a Chinese patent (Liu Guangyi, Liu Sheng, Zhong Hong, Cao Zhanfang, Wang Shuai. An N-alkyl hydroxamic acid-dithiocarbamate collector and its preparation and flotation method, ZL201710230937.1, 2017-4-10) discloses a sulfur-nitrogen-hydroxamic acid collector applied to tungsten ore flotation. Since the sulfur-nitrogen and sulfur-nitrogen ester functional groups have weak reaction ability to calcium ions (Jing Qi, Guangyi Liu, Yan Dong. Probing the hydrophobic mechanism of N-[(3-hydroxyamino)-propoxy]-N-octyl dithiocarbamate toward bastnaesite flotation by in situ AFM, FTIR and XPS. Journal of Colloid and Interface Science 572 (2020) 179-189), sulfur-nitrogen-hydroxamic acid or sulfur-nitrogen ester-hydroxamic acid is used in the flotation of tungsten ore, especially in the flotation of scheelite, and sulfur-nitrogen or sulfur-nitrogen ester functional groups mainly play a role in regulating the solubility or hydrophilicity of the collector. However, the existing flotation method of tungsten ore still has the problem of unsatisfactory flotation performance. Summary of the invention
[0005] In order to solve the problem of unsatisfactory flotation performance of existing tungsten ore flotation methods, the present invention aims to provide a new tungsten ore flotation method, aiming to improve the flotation effect of tungsten ore and improve the separation selectivity of tungsten ore and gangue.
[0006] A tungsten ore flotation method, wherein a pulp containing tungsten ore and a flotation agent is subjected to flotation to obtain tungsten concentrate; wherein the flotation agent contains at least a lead ion activator and a collector;
[0007] The collector comprises at least one of the sulfur nitrogen-hydroxamic acid collector shown in formula I and the sulfur nitrogen ester-hydroxamic acid collector shown in formula II;
[0008]
[0009] M 1 is sodium, potassium or hydrogen; M 2 is sodium or potassium;
[0010] R 1 C2~C 16 A hydrocarbon group or an oxygen-containing hydrocarbon group;
[0011] R 2 and R 3 Hydrogen, C1~C 16 A hydrocarbon group or an oxygen-containing hydrocarbon group, but R 2 and R 3 Not all are hydrogen; n is 1-4.
[0012] The present invention has found that the sulfur-nitrogen functional group has a strong complexing ability with Pb(Ⅱ), and the hydroxamic acid functional group also has a complexing effect with Pb(Ⅱ). Therefore, sulfur-nitrogen-hydroxamic acid and sulfur-nitrogen ester-hydroxamic acid have a dual-site chelating effect on Pb(Ⅱ), which can enhance the activation flotation of tungsten ore. The tungsten ore flotation method of the present invention has the characteristics of strong capture ability and good selectivity, especially for calcium-containing gangue minerals. Compared with the existing lead ion activation + benzohydroxamic acid flotation or the use of sulfur-nitrogen-hydroxamic acid or sulfur-nitrogen ester-hydroxamic acid alone, the tungsten ore flotation method of the present invention can greatly improve the flotation recovery rate of tungsten ore, with significant economic benefits and good industrial application prospects.
[0013] In the present invention, the synergy of the intramolecular double chelation mechanism of lead and sulfur nitrogen (sulfur nitrogen ester) and hydroxamic acid is the key to improving the tungsten ore capture performance.
[0014] The above tungsten ore flotation method, R 1 C2~C 16 alkyl or oxaalkyl (ether group); preferably butyl, isobutyl, pentyl, isopentyl, n-hexyl, n-octyl or isooctyl.
[0015] The above tungsten ore flotation method, R 2 and R 3 Each is independently H or hydrogen, C1~C 16 An alkyl group or an oxaalkyl group (ether group).
[0016] The above tungsten ore flotation method, R 3 Preferably, hydrogen, R 2 Preferably, R is butyl, isobutyl, pentyl, isopentyl, n-hexyl, n-octyl, isooctyl or dodecyl. 2 and R 3 The same, preferably ethyl, propyl, ethylpropyl or butyl.
[0017] In the above tungsten ore flotation method, n is preferably 2.
[0018] In the present invention, the lead ion activator is a lead ion activator that can ionize Pb in water. 2+ A water-soluble salt thereof; preferably at least one of lead nitrate and lead acetate;
[0019] Preferably, the molar ratio of the collector to the lead ions in the lead ion activator is 1:1 to 10; more preferably 1:2 to 4.
[0020] In the above tungsten ore flotation method, there is no special requirement for the dosage of the flotation agent. For example, based on the weight of the metal ore (tungsten ore), the dosage of the collector is 10 to 1200 g / t, preferably 50 to 500 g / t; more preferably 150 to 350 g / t.
[0021] In the above-mentioned tungsten ore flotation method, there is no special requirement for the pH of the ore pulp during flotation, for example, it can be 6.0 to 10.0, preferably 7.5 to 8.5.
[0022] In the above-mentioned tungsten ore flotation method, the tungsten ore includes at least one of scheelite and wolframite.
[0023] The flotation agent is added in the tungsten ore grinding process, the slurry mixing process or the slurry after slurry mixing.
[0024] Preferably, in the flotation reagent, the lead ion activator and collector are added separately, or pre-mixed and reacted before adding; preferably, they are pre-mixed and reacted before adding. Studies have found that pre-mixing the lead ion activator and the collector before participating in the flotation of tungsten ore can help further improve the flotation performance of tungsten ore.
[0025] In the present invention, the flotation is, for example, froth flotation.
[0026] In the present invention, other agents that are helpful for flotation, such as frothers, pH adjusters, water glass dispersants, etc., are allowed to be added to the flotation agents.
[0027] A preferred tungsten ore flotation method of the present invention comprises the following steps:
[0028] Step (1): tungsten ore is crushed and slurried to obtain slurry;
[0029] Step (2): adding a flotation agent to the ore pulp of step (1) to carry out flotation, and collecting the flotation concentrate; the flotation agent at least comprises the lead ion activator and the sulfur nitrogen-hydroxamic acid (Formula I) collector or the lead ion activator and the sulfur nitrogen ester-hydroxamic acid (Formula II) collector; other flotation agents may also include a frother, a pH adjuster, a water glass dispersant, etc.; the lead ion activator is mainly lead nitrate.
[0030] Compared with the prior art, the advantages of the present invention are:
[0031] 1. The tungsten ore flotation method provided by the present invention has the advantages of low flotation reagent dosage and high tungsten ore recovery rate. Compared with benzohydroxamic acid, the tungsten flotation recovery rate can be increased by more than 40 percentage points; compared with lead nitrate activation and benzohydroxamic acid capture, the tungsten flotation recovery rate can be increased by more than 20 percentage points; compared with the use of sulfur-nitrogen-hydroxamic acid (Formula I) or sulfur-nitrogen ester-hydroxamic acid (Formula II) alone, the tungsten flotation recovery rate can be increased by more than 20 percentage points. Lead nitrate and sulfur-nitrogen-hydroxamic acid (Formula I) or sulfur-nitrogen ester-hydroxamic acid (Formula II) are used in combination, and the sulfur-nitrogen or sulfur-nitrogen ester functional group and the hydroxamic acid functional group can react with Pb 2+ Complexation forms a dual-site action mechanism, which strengthens the activation flotation of tungsten ore and reduces the dosage of reagents.
[0032] 2. The tungsten ore flotation method provided by the present invention has good selectivity for calcium / magnesium-containing gangue minerals (such as calcite and dolomite), and can achieve efficient flotation separation of tungsten ore and calcium / magnesium-containing gangue minerals.
[0033] 3. The tungsten ore flotation method provided by the present invention has the advantages of simple process and high flotation efficiency. The present invention uses sulfur nitrogen-hydroxamic acid or sulfur nitrogen ester-hydroxamic acid and lead nitrate as the main flotation reagents, has a fast flotation speed and high efficiency, does not require changes to on-site process equipment and processes, and is easy for industrial application. DETAILED DESCRIPTION
[0034] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.
[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0036] Comparative Example 1: Flotation of Scheelite with Benzohydroxamic Acid
[0037] The concentration of benzohydroxamic acid was 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, and the flotation recovery rate of scheelite with a particle size of 0.037mm-0.074mm was 7.2%.
[0038] Comparative Example 2: Flotation of Scheelite with Lead Nitrate and Benzohydroxamic Acid
[0039] The concentration of lead nitrate is 1.0×10-4 mol / L, the concentration of benzohydroxamic acid was 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, activated flotation of scheelite with a particle size of 0.037mm to 0.074mm, the recovery rate of scheelite was 53.3%
[0040] Comparative Example 3: Flotation of Scheelite with Potassium N-[(3-Hydroxamic Acid)-Propyl]-N-butyldithiocarbamate
[0041] The concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-butyldithiocarbamate was 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, direct flotation of scheelite with a particle size of 0.037mm-0.074mm was carried out, and the flotation recovery rate of scheelite was 21.1%.
[0042] Example 1: Flotation of Scheelite with Lead Nitrate and Potassium N-[(3-Hydroxamic Acid)-Propyl]-N-Butyldithiocarbamate
[0043] The concentration of lead nitrate is 1.0×10 -4 mol / L, the concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-butyldithiocarbamate was 4×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, activated scheelite with a particle size of 0.037mm-0.074mm was flotated, and the flotation recovery rate of scheelite reached 79.3%.
[0044] Therefore, compared with the single addition of potassium N-[(3-hydroxamic acid)-propyl]-N-butyldithiocarbamate or the combined use of lead nitrate and benzohydroxamic acid, the combined use of lead nitrate and potassium N-[(3-hydroxamic acid)-propyl]-N-butyldithiocarbamate significantly improves the flotation recovery rate of scheelite.
[0045] Comparative Example 4: Flotation of wolframite with benzohydroxamic acid
[0046] The concentration of benzohydroxamic acid was 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, and the wolframite with a particle size of 0.037mm-0.074mm was directly floated, and the flotation recovery rate of the wolframite was 2.6%.
[0047] Comparative Example 5: Flotation of wolframite with lead nitrate and benzohydroxamic acid
[0048] The concentration of lead nitrate is 1.0×10 -4 mol / L, the concentration of benzohydroxamic acid was 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, activated flotation of wolframite with a particle size of 0.037mm-0.074mm was carried out, and the flotation recovery rate of wolframite was 23.8%.
[0049] Comparative Example 6: Flotation of Wolframite with Potassium N-[(3-Hydroxamic Acid)-Propyl]-N-butyldithiocarbamate
[0050] The concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-butyldithiocarbamate was 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, and the wolframite with a particle size of 0.037mm-0.074mm was directly floated, and the flotation recovery rate of the wolframite was 25.2%.
[0051] Example 2: Flotation of wolframite with lead nitrate and potassium N-[(3-hydroxamic acid)-propyl]-N-butyldithiocarbamate
[0052] The concentration of lead nitrate is 1.0×10 -4 mol / L, the concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-butyldithiocarbamate was 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 - 4 mol / L, activated flotation of wolframite with a particle size of 0.037mm-0.074mm was carried out, and the flotation recovery rate of wolframite was 75.9%.
[0053] Therefore, compared with the single addition of potassium N-[(3-hydroxamic acid)-propyl]-N-butyldithiocarbamate or the combined use of lead nitrate and benzohydroxamic acid, the combined use of lead nitrate and potassium N-[(3-hydroxamic acid)-propyl]-N-butyldithiocarbamate significantly improves the flotation recovery rate of wolframite.
[0054] Comparative Example 7: Flotation of Scheelite with Sodium N,N-Diethyldithiocarbamate
[0055] The concentration of sodium N,N-diethyldithiocarbamate is 4.0×10-5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, direct flotation of scheelite with a particle size of 0.037mm-0.074mm was carried out, and the flotation recovery rate of scheelite was 9.9%.
[0056] Comparative Example 8: Flotation of Scheelite with Lead Nitrate and Sodium N,N-Diethyldithiocarbamate
[0057] The concentration of sodium N,N-diethyldithiocarbamate is 4.0×10 -5 mol / L, the concentration of lead nitrate is 1.0×10 - 4 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, activated flotation of scheelite with a particle size of 0.037mm-0.074mm was carried out, and the flotation recovery rate of scheelite was 20.6%.
[0058] Comparative Example 9: Flotation of Scheelite with Potassium N-[(3-Hydroxamic Acid)-Propyl]-N-Hexyldithiocarbamate
[0059] The concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-hexyl dithiocarbamate was 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, direct flotation of scheelite with a particle size of 0.037mm-0.074mm was carried out, and the flotation recovery rate of scheelite was 22.3%.
[0060] Example 3: Flotation of Scheelite with Lead Nitrate and Potassium N-[(3-Hydroxamic Acid)-Propyl]-N-Hexyldithiocarbamate
[0061] The concentration of lead nitrate is 1.0×10 -4 mol / L, the concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-hexyl dithiocarbamate was 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 - 4 mol / L, activated flotation of scheelite with a particle size of 0.037mm-0.074mm was carried out, and the recovery rate of scheelite was 88.7%.
[0062] Therefore, compared with the single addition of sodium N,N-diethyldithiocarbamate or potassium N-[(3-hydroxyxamic acid)-propyl]-N-hexyldithiocarbamate and the combined use of lead nitrate and sodium N,N-diethyldithiocarbamate, the combined use of lead nitrate and potassium N-[(3-hydroxyxamic acid)-propyl]-N-hexyldithiocarbamate significantly improves the flotation recovery rate of scheelite.
[0063] Comparative Example 10: Flotation of wolframite with sodium N,N-diethyldithiocarbamate
[0064] The concentration of sodium N,N-diethyldithiocarbamate is 3.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, and the wolframite with a particle size of 0.037mm-0.074mm was directly floated, and the flotation recovery rate of wolframite was 1.6%.
[0065] Comparative Example 11: Flotation of wolframite with lead nitrate and sodium N,N-diethyldithiocarbamate
[0066] The concentration of sodium N,N-diethyldithiocarbamate is 3.0×10 -5 mol / L, the concentration of lead nitrate is 1.0×10 - 4 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, activated flotation of wolframite with a particle size of 0.037mm-0.074mm was carried out, and the flotation recovery rate of wolframite was 7.7%.
[0067] Comparative Example 12: Flotation of wolframite with potassium N-[(3-hydroxamic acid)-propyl]-N-hexyldithiocarbamate
[0068] The concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-hexyl dithiocarbamate was 3.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, and the wolframite with a particle size of 0.037mm-0.074mm was directly floated, and the flotation recovery rate of the wolframite was 51.9%.
[0069] Example 4: Flotation of wolframite with lead nitrate and potassium N-[(3-hydroxamic acid)-propyl]-N-n-hexyldithiocarbamate
[0070] The concentration of lead nitrate is 1.0×10 -4mol / L, the concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-hexyl dithiocarbamate was 3.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 - 4 mol / L, wolframite with a particle size of 0.037mm-0.074mm was floated, and the flotation recovery rate of wolframite was 89.5%.
[0071] Therefore, compared with the single addition of sodium N,N-diethyldithiocarbamate or potassium N-[(3-hydroxyxamic acid)-propyl]-N-hexyldithiocarbamate and the combined use of lead nitrate and sodium N,N-diethyldithiocarbamate, the combined use of lead nitrate and potassium N-[(3-hydroxyxamic acid)-propyl]-N-hexyldithiocarbamate significantly improves the flotation recovery rate of wolframite.
[0072] Example 5: Flotation of Calcite with Lead Nitrate and Potassium N-[(3-Hydroxamic Acid)-Propyl]-N-Hexyldithiocarbamate
[0073] The concentration of lead nitrate is 1.0×10 -4 mol / L, the pulp pH was 8.0, and the concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-n-hexyl dithiocarbamate was 4.0×10 -5 mol / L, the concentration of methyl isobutyl carbinol (MIBC) was 1.0×10 - 4 mol / L, calcite with a particle size of 0.037mm-0.074mm was floated, and the flotation recovery rate of calcite was 36.5%.
[0074] This shows that, compared with Examples 3 and 4, the collection ability of the combination of lead nitrate and potassium N-[(3-hydroxyxamic acid)-propyl]-N-hexyl dithiocarbamate for wolframite and scheelite is significantly stronger than that of calcite. Compared with calcite, the flotation recovery rate of wolframite or scheelite is more than 50 percentage points higher, indicating that the combination of lead nitrate and potassium N-[(3-hydroxyxamic acid)-propyl]-N-hexyl dithiocarbamate has excellent selectivity for wolframite and scheelite.
[0075] Comparative Example 13: Flotation of Scheelite with Potassium N-[(3-Hydroxamic Acid)-Propyl]-N-Octyldithiocarbamate
[0076] The concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-octyl dithiocarbamate was 1.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4mol / L, direct flotation of scheelite with a particle size of 0.037mm-0.074mm was carried out, and the flotation recovery rate of scheelite was 35.4%.
[0077] Example 6: Flotation of Scheelite with Lead Nitrate and Potassium N-[(3-Hydroxamic Acid)-Propyl]-N-Octyldithiocarbamate
[0078] The concentration of lead nitrate is 1.0×10 -4 mol / L, the concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-octyl dithiocarbamate was 1.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 - 4 mol / L, the scheelite with a particle size of 0.037mm-0.074mm was floated, and the flotation recovery rate of scheelite was 71.9%.
[0079] Therefore, the combined use of lead nitrate and potassium N-[(3-hydroxamic acid)-propyl]-N-octyldithiocarbamate significantly improved the flotation recovery of scheelite compared with the single addition of potassium N-[(3-hydroxamic acid)-propyl]-N-octyldithiocarbamate.
[0080] Comparative Example 14: Flotation of Scheelite with S-[(3-Hydroxamic Acid)-Propyl]-N,N-Dipropyl Dithiocarbamate The concentration of S-[(3-Hydroxamic Acid)-Propyl]-N,N-Dipropyl Dithiocarbamate is 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, and the flotation recovery rate of scheelite with a particle size of 0.037mm-0.074mm was 20.1%.
[0081] Example 7: Flotation of Scheelite with Lead Nitrate and S-[(3-Hydroxamic Acid)-Propyl]-N,N-Dipropyl Dithiocarbamate
[0082] The concentration of lead nitrate is 1.0×10 -4 mol / L, the concentration of S-[(3-hydroxamic acid)-propyl]-N,N-dipropyl dithiocarbamate was 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 - 4 mol / L, the flotation recovery rate of scheelite with a particle size of 0.037mm-0.074mm was 85.7%.
[0083] Therefore, the combined use of lead nitrate and S-[(3-hydroxamic acid)-propyl]-N,N-dipropyl dithiocarbamate significantly improved the flotation recovery of scheelite compared to the single addition of S-[(3-hydroxamic acid)-propyl]-N,N-dipropyl dithiocarbamate.
[0084] Comparative Example 15: S-[(3-Hydroxamic Acid)-Propyl]-N,N-Dipropyl Dithiocarbamate Flotation of Wolframite The concentration of S-[(3-Hydroxamic Acid)-Propyl]-N,N-Dipropyl Dithiocarbamate is 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, and the black tungsten with a particle size of 0.037mm-0.074mm was directly floated, and the flotation recovery rate of black tungsten was 30.7%.
[0085] Example 8: Flotation of wolframite with lead nitrate and S-[(3-hydroxamic acid)-propyl]-N,N-dipropyl dithiocarbamate
[0086] The concentration of lead nitrate is 1.0×10 -4 mol / L, the concentration of S-[(3-hydroxamic acid)-propyl]-N,N-dipropyl dithiocarbamate was 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 - 4 mol / L, wolframite with a particle size of 0.037mm-0.074mm was floated, and the flotation recovery rate of wolframite was 87.1%.
[0087] Therefore, the combined use of lead nitrate and S-[(3-hydroxamic acid)-propyl]-N,N-dipropyl dithiocarbamate significantly improved the flotation recovery of wolframite compared to the single addition of S-[(3-hydroxamic acid)-propyl]-N,N-dipropyl dithiocarbamate.
[0088] Example 9: Mixing lead nitrate and potassium N-[(3-hydroxyxamic acid)-propyl]-N-hexyl dithiocarbamate and adding floating scheelite
[0089] The concentration of lead nitrate is 1.0×10 -4 mol / L, the concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-hexyl dithiocarbamate was 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 - 4mol / L, the particle size of scheelite is 0.037mm~0.074mm. During flotation, potassium N-[(3-hydroxyxamic acid)-propyl]-N-n-hexyl dithiocarbamate and lead nitrate are first mixed and stirred for 20s before being added to the pulp, and then a frother is added for flotation, and the recovery rate of scheelite is 91.9%.
[0090] Compared with first adding lead nitrate and then adding potassium N-[(3-hydroxyxamic acid)-propyl]-N-hexyl dithiocarbamate in Example 3, the mineral processing method of first mixing potassium N-[(3-hydroxyxamic acid)-propyl]-N-hexyl dithiocarbamate and lead nitrate and then adding the slurry in the embodiment of the present invention slightly improves the flotation recovery rate of scheelite.
[0091] Example 10: Mixing lead nitrate and potassium N-[(3-hydroxyxamic acid)-propyl]-N-hexyl dithiocarbamate and adding floating wolframite
[0092] The concentration of lead nitrate is 1.0×10 -4 mol / L, the concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-hexyl dithiocarbamate was 3.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 - 4 mol / L, the particle size of black tungsten is 0.037mm~0.074mm. During flotation, N-[(3-hydroxamic acid)-propyl]-N-n-hexyl dithiocarbamate potassium is mixed with lead nitrate for 20s before adding to the pulp, and then a frother is added for flotation, and the recovery rate of black tungsten is 92.8%.
[0093] Compared with first adding lead nitrate and then adding potassium N-[(3-hydroxyxamic acid)-propyl]-N-hexyl dithiocarbamate in Example 4, the mineral processing method of first mixing potassium N-[(3-hydroxyxamic acid)-propyl]-N-hexyl dithiocarbamate with lead nitrate and then adding the slurry in the embodiment of the present invention slightly improves the flotation recovery rate of wolframite.
[0094] Comparative Example 16: Flotation of artificial mixed scheelite-calcite ore (mass ratio 1:1) by lead nitrate and benzohydroxamic acid
[0095] The concentration of benzohydroxamic acid was 4.0×10 -5 mol / L, the concentration of lead nitrate is 1.0×10 -4 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4mol / L, activated flotation separation was carried out on artificial mixed scheelite-calcite ore with a particle size of 0.037mm-0.074mm, the recovery rate of scheelite was 46.4%, and the recovery rate of calcite was 11.3%.
[0096] Example 11: Flotation of artificial mixed scheelite-calcite ore (mass ratio 1:1) with lead nitrate and potassium N-[(3-hydroxamic acid)-propyl]-N-n-hexyldithiocarbamate
[0097] The concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-hexyl dithiocarbamate was 4.0×10 -5 mol / L, the concentration of lead nitrate is 1.0×10 -4 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 - 4 mol / L, activated flotation separation was carried out on artificial mixed scheelite-calcite ore with a particle size of 0.037mm-0.074mm, the recovery rate of scheelite was 83.2%, and the recovery rate of calcite was 28.4%.
[0098] Therefore, compared with the combined use of lead nitrate and benzohydroxamic acid, the combined use of lead nitrate and potassium N-[(3-hydroxamic acid)-propyl]-N-hexyldithiocarbamate can effectively separate scheelite from its artificial mixed ore with calcite.
[0099] Comparative Example 17: Flotation of Scheelite and Wolframite Mixed Ore (Mass Ratio of Scheelite to Wolframite 7:3) by Potassium N-[(3-Hydroxamic Acid)-Propyl]-N-Hexyldithiocarbamate
[0100] The concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-hexyl dithiocarbamate was 4.0×10 -5 mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 -4 mol / L, activated flotation was carried out on the mixed black and white tungsten ore with a particle size of 0.037mm-0.074mm, and the comprehensive recovery rate of tungsten ore was 33.3%.
[0101] Example 12: Flotation of Scheelite and Wolframite Mixed Ore (Mass Ratio of Scheelite to Wolframite 7:3) Using Lead Nitrate and Potassium N-[(3-Hydroxamic Acid)-Propyl]-N-Hexyldithiocarbamate
[0102] The concentration of potassium N-[(3-hydroxamic acid)-propyl]-N-hexyl dithiocarbamate was 4.0×10 -5 mol / L, the concentration of lead nitrate is 1.0×10 -4mol / L, the pulp pH was 8.0, and the concentration of frother methyl isobutyl carbinol (MIBC) was 1.0×10 - 4 mol / L, activated flotation was carried out on the mixed black and white tungsten ore with a particle size of 0.037mm-0.074mm, and the comprehensive recovery rate of tungsten ore was 85.5%.
[0103] Therefore, compared with the single addition of potassium N-[(3-hydroxyxamic acid)-propyl]-N-hexyldithiocarbamate, the combined use of lead nitrate and potassium N-[(3-hydroxyxamic acid)-propyl]-N-hexyldithiocarbamate significantly improved the comprehensive recovery rate of tungsten ore.
[0104] Example 13: Actual ore flotation test
[0105] A certain scheelite ore contains WO30.26%. The main minerals are scheelite, calcite (about 8%), fluorite (about 2%), and garnet (about 60%). The grinding fineness is -200 mesh 50%, the flotation concentration is 40%, and the flotation process is a primary roughing: the amount of sodium carbonate is 750g / t, the amount of water glass is 1500g / t, the amount of lead nitrate is 250g / t, the amount of N-[(3-hydroxyxamic acid)-propyl]-N-n-hexyl dithiocarbamate potassium is 100g / t, the frother No. 2 oil is 20g / t, and the tungsten rough concentrate is obtained by flotation for 4 minutes, of which the WO3 grade is 3.46% and the tungsten recovery rate is 76.2%. If the same amount of benzohydroxamic acid is used to replace N-[(3-hydroxamic acid)-propyl]-N-hexyl potassium dithiocarbamate, and other conditions are the same, the WO3 grade in the obtained tungsten crude concentrate is 2.64% and the tungsten recovery rate is 50.3%.
[0106] In summary, the method for flotation of tungsten ore by combining lead nitrate and sulfuric acid-hydroxamic acid (Formula I) or sulfuric acid ester-hydroxamic acid (Formula II) provided by the present invention has the advantages of low flotation agent dosage and high tungsten ore recovery rate. Compared with benzohydroxamic acid, the tungsten flotation recovery rate can be increased by more than 40 percentage points; compared with lead nitrate activation and benzohydroxamic acid capture, the tungsten flotation recovery rate can be increased by more than 20 percentage points; compared with the use of sulfuric acid-hydroxamic acid (Formula I) or sulfuric acid ester-hydroxamic acid (Formula II) alone, the tungsten flotation recovery rate can be increased by more than 20 percentage points.
Claims
1. A tungsten ore flotation method, wherein a pulp containing tungsten ore and a flotation agent is subjected to flotation to obtain a tungsten concentrate; characterized in that: The flotation reagent at least comprises a lead ion activator and a collector; The collector comprises a sulfur nitrogen ester-hydroxamic acid collector shown in formula II, or a combined collector comprising a sulfur nitrogen-hydroxamic acid collector shown in formula I and a sulfur nitrogen ester-hydroxamic acid collector shown in formula II; M 1 is sodium, potassium or hydrogen; M 2 is sodium or potassium; R 1 C2~C 16 A hydrocarbon group or an oxygen-containing hydrocarbon group; R 2 and R 3 Hydrogen, C1~C 16 A hydrocarbon group or an oxygen-containing hydrocarbon group, but R 2 and R 3 are not hydrogen at the same time; n is 1-4; The added molar ratio of lead ions in the collector and the lead ion activator is 1:1-10.
2. The tungsten ore flotation method according to claim 1, characterized in that: R 1 C2~C 16 An alkyl group or an oxaalkyl group.
3. The tungsten ore flotation method according to claim 2, characterized in that: R 1 It is butyl, isobutyl, pentyl, isopentyl, n-hexyl, n-octyl or isooctyl.
4. The tungsten ore flotation method according to claim 1, characterized in that: R 2 and R 3 In the above, C1~C 16 The hydrocarbon group is C1~C 16 The oxygen-containing hydrocarbon group is an oxaalkyl group.
5. The tungsten ore flotation method according to claim 1, characterized in that: R 3 is hydrogen; R 2 is butyl, isobutyl, pentyl, isopentyl, n-hexyl, n-octyl, isooctyl or dodecyl; Or, R 2 and R 3 Together they are ethyl, propyl, ethylpropyl or butyl.
6. The tungsten ore flotation method according to claim 1, characterized in that: n is 2.
7. The tungsten ore flotation method according to claim 1, characterized in that: Lead ion activator is a kind of lead ion activator that can ionize Pb in water. 2 + water-soluble salts.
8. The tungsten ore flotation method according to claim 7, characterized in that: The lead ion activator is at least one of lead nitrate and lead acetate.
9. The tungsten ore flotation method according to claim 1, characterized in that: Based on the weight of the tungsten ore, the dosage of the collector is 10-1200 g / t.
10. The tungsten ore flotation method according to claim 1, characterized in that: Based on the weight of the tungsten ore, the dosage of the collector is 50-500 g / t.
11. The tungsten ore flotation method according to claim 1, characterized in that: The pH of the slurry during flotation is 6.0~10.
0.
12. The tungsten ore flotation method according to claim 1, characterized in that: The tungsten ore includes at least one of scheelite and wolframite.
13. The tungsten ore flotation method according to any one of claims 1 to 12, characterized in that: The flotation agent is added in the tungsten ore grinding process, the slurry mixing process or the slurry after slurry mixing.
14. The tungsten ore flotation method according to claim 13, characterized in that: In the flotation reagent, the lead ion activator and the collector are added separately, or mixed in advance and then added.
15. The tungsten ore flotation method according to claim 1, characterized in that: The slurry during flotation also contains a frother.