Welding method for pot-shaped target material assembly

By using a niobium flange ring similar to the tantalum target material in the pot shape for electron beam welding, combined with a two-step welding process, the problem of poor welding caused by the material difference between the pot target material and the support component was solved, achieving a high-efficiency and low-cost welding effect.

CN118951280APending Publication Date: 2024-11-15KONFOONG MATERIALS INTERNATIONAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411360919.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing pot-shaped target material and support component have a large difference in melting point, which leads to a decrease in welding bonding rate, reduced welding strength, and a complex and costly process.

Method used

A niobium flange ring with similar properties and melting point to the tantalum target material in the pot shape is used for electron beam welding. The two-step electron beam welding process, including the first electron beam welding and the second electron beam welding, combined with machining, forms the pot-shaped target material assembly.

Benefits of technology

It significantly improves the welding bonding rate and strength, reduces costs, simplifies the process, and improves processing efficiency; the welding strength can reach 150MPa.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005064916560000081
    Figure BDA0005064916560000081
  • Figure BDA0005064916560000091
    Figure BDA0005064916560000091
Patent Text Reader

Abstract

The invention relates to a welding method of a pot-shaped target material assembly, which comprises the following steps: (1) respectively pretreating the welding surfaces of a pot-shaped tantalum target material and a niobium flange ring piece to obtain a target material to be welded and a ring piece to be welded; and (2) after the to-be-welded target material obtained in the step (1) and the to-be-welded ring piece are assembled, first electron beam welding treatment and second electron beam welding treatment are sequentially conducted, and the pot-shaped target material assembly is obtained after machining. The niobium flange ring piece which is easy to weld with the pot-shaped tantalum target material and has the melting point similar to that of the pot-shaped tantalum target material is adopted for electron beam welding, the machining efficiency can be effectively improved, the cost can be effectively reduced, meanwhile, high welding strength is guaranteed, and the problem of poor welding can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of target material preparation, and in particular to a welding method for a pot-shaped target material assembly. Background Art

[0002] The pot-shaped target is a special-shaped target, which is usually composed of a pot-shaped sputtering body and a flange that supports and fixes the sputtering process, wherein the flange can be assembled with the machine. The pot-shaped sputtering body is usually a high-purity sputtering material, which requires the flange to be well welded with the sputtering body, and has the characteristics of good machinability, not easy to deform and high strength.

[0003] At present, the pot-shaped target is usually made by stamping ingots and welding them with flanges. Since the materials of the flange and the pot-shaped sputtering body are often different, the difference in melting points requires adjustment of appropriate welding methods. Generally, electron beam welding or hot isostatic pressing welding is mixed with electron beam welding, which will also lead to a decrease in the welding bonding rate of the two materials and a decrease in welding strength.

[0004] CN 114603243A discloses a welding method for a pot-shaped target material, which comprises: welding the pot-shaped target material and a support member by electron beam, wherein a bevel is provided on the welding surface with a high melting point of the material during welding; the vertical length of the bevel is 4-7 mm; the height of the bevel is 0.2-0.5 mm; the electron beam welding comprises first welding, second welding, third welding and fourth welding; the first welding is welding the non-bevel welding surface; the second welding is welding the end surface 0.4-0.8 mm away from the bevel; the third welding is welding the end surface 0.6-1.2 mm away from the bevel; and the fourth welding is welding the gap between the pot-shaped target material and the support member. However, due to the large difference in the melting point of the pot-shaped target material and the support member, the welding effect cannot be guaranteed.

[0005] CN 114713960A discloses a welding method for a pot-shaped target, the welding method comprising: welding a support member and a pot-shaped target by electron beam; the support member comprises a first ring and a second ring from the outside to the inside; the material of the second ring is the same as that of the pot-shaped target; the pot-shaped target is provided with an annular step; the inner diameter of the annular step is less than the inner diameter of the second ring. The welding method provided by the invention realizes the welding of the support member and the pot-shaped target by specifically designing the support member, but the different materials of the first ring and the second ring still have the problem of reduced welding bonding rate, and the process flow is relatively complicated and the production cost is high.

[0006] Therefore, in view of the shortcomings of the existing technology, it is urgent to provide a welding method with simple process flow, low cost and good welding effect. Summary of the invention

[0007] The object of the present invention is to provide a welding method for a pot-shaped target assembly, which uses a niobium flange ring to directly perform electron beam welding with a tantalum target, thereby improving processing efficiency and ensuring welding effect.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] The present invention provides a welding method for a pot-shaped target assembly, the welding method comprising the following steps:

[0010] (1) Pre-treating the welding surfaces of the pot-shaped tantalum target and the niobium flange ring respectively to obtain a target to be welded and a ring to be welded;

[0011] (2) Assembling the target material to be welded obtained in step (1) and the ring member to be welded, and sequentially performing a first electron beam welding treatment and a second electron beam welding treatment, and obtaining the pot-shaped target material assembly after machining.

[0012] The welding method of the pot-shaped target assembly provided by the present invention aims at the problems of complex process, poor welding effect and high cost in the traditional welding process of using tantalum-titanium flange rings to form a composite ring and then welding it with a tantalum target. By using niobium flange rings which have similar performance to the pot-shaped tantalum target and are easy to weld and have a similar melting point for electron beam welding, the cost can be effectively reduced, the process flow can be reduced, and a good welding bonding rate and welding strength can be guaranteed. Among them, the two-step welding process of the first electron beam welding treatment and the second electron beam welding treatment can significantly improve the welding effect of the target material to be welded and the ring to be welded, and avoid the problem of poor welding.

[0013] Preferably, the pot-shaped tantalum target in step (1) is a pot-shaped tantalum target obtained by stamping a tantalum ingot.

[0014] Preferably, the pretreatment in step (1) comprises washing and drying performed sequentially.

[0015] The pretreatment can remove stains on the surfaces of the pot-shaped tantalum target and the niobium flange ring, thereby avoiding affecting the effect of subsequent welding.

[0016] Preferably, the cleaning agent comprises acetone.

[0017] Preferably, the cleaning time is 5-10 min, for example, 5 min, 6 min, 8 min, 9 min or 10 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] Preferably, the drying temperature is 70-75°C, for example, 70°C, 71°C, 72°C, 73°C or 75°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, the drying time is 1-2 hours, for example, 1 hour, 1.2 hours, 1.5 hours, 1.8 hours or 2 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0020] Preferably, the assembling step in step (2) includes: sleeve the ring to be welded on the top outer wall of the target material to be welded.

[0021] Preferably, the weld gap of the assembly in step (2) is 0.3-0.8 mm, for example, it can be 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm or 0.8 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0022] The weld gap of the assembly needs to be controlled within a reasonable range. If the weld gap is too large, the welding bonding rate will be reduced, resulting in poor welding. If the weld gap is too small, electron beam welding cannot be effectively performed.

[0023] Preferably, the absolute vacuum degree of the first electron beam welding process and the second electron beam welding process in step (2) is ≤1×10 -3 Pa, for example, can be 1×10 -3 Pa, 0.8×10 -3 Pa, 0.5×10 -3 Pa, 0.2×10 -3 Pa or 1×10 -4 Pa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] Preferably, the beam current of the first electron beam welding process in step (2) is 10-30 mA, for example, 10 mA, 15 mA, 20 mA, 25 mA or 30 mA, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] Preferably, the line speed of the first electron beam welding process in step (2) is 10-15 mm / s, for example, it can be 10 mm / s, 12 mm / s, 13 mm / s, 14 mm / s or 15 mm / s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the beam current of the second electron beam welding process in step (2) is 40-60 mA, for example, 40 mA, 45 mA, 50 mA, 55 mA or 60 mA, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the line speed of the second electron beam welding process in step (2) is 10-15 mm / s, for example, it can be 10 mm / s, 12 mm / s, 13 mm / s, 14 mm / s or 15 mm / s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] Preferably, the machining in step (2) includes turning.

[0029] As a preferred technical solution of the welding method described in the present invention, the welding method comprises the following steps:

[0030] (1) The tantalum ingot is subjected to stamping treatment to obtain a pot-shaped tantalum target, and the welding surfaces of the obtained pot-shaped tantalum target and the niobium flange ring are cleaned with acetone for 5-10 minutes and dried at 70-75° C. for 1-2 hours to obtain a target to be welded and a ring to be welded;

[0031] (2) The ring to be welded in step (1) is placed on the top outer wall of the target material to be welded, with a weld gap of 0.3-0.8 mm, and then the absolute vacuum is ≤1×10 -3 Pa, the first electron beam welding process and the second electron beam welding process are performed in sequence; the beam current of the first electron beam welding process is 10-30mA, and the line speed is 10-15mm / s; the beam current of the second electron beam welding process is 40-60mA, and the line speed is 10-15mm / s; the pot-shaped target assembly is obtained after turning.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The welding method of the pot-shaped target assembly provided by the present invention aims at the problems of complex process, poor welding effect and high cost in the traditional welding process of using tantalum-titanium flange rings to form a composite ring and then welding it with a tantalum target. By using niobium flange rings which have similar performance to the pot-shaped tantalum target and are easy to weld and have a similar melting point for electron beam welding, the cost can be effectively reduced, the process flow can be reduced, the processing efficiency can be improved, and the welding strength can reach 150MPa. Among them, the two-step welding process of the first electron beam welding treatment and the second electron beam welding treatment can significantly improve the welding effect of the target material to be welded and the ring to be welded, and the problem of poor welding can be avoided. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0035] Example 1

[0036] This embodiment provides a welding method for a pot-shaped target assembly, and the welding method comprises the following steps:

[0037] (1) The tantalum ingot is subjected to stamping treatment to obtain a pot-shaped tantalum target, and the welding surfaces of the obtained pot-shaped tantalum target and the niobium flange ring are cleaned with acetone for 8 minutes and dried at 72° C. for 1.5 hours to obtain a target to be welded and a ring to be welded;

[0038] (2) The ring to be welded in step (1) is placed on the top outer wall of the target material to be welded, with a weld gap of 0.5 mm, and then the absolute vacuum is 1×10 -3 Pa, the first electron beam welding process and the second electron beam welding process are performed sequentially; the beam current of the first electron beam welding process is 20mA, and the line speed is 13mm / s; the beam current of the second electron beam welding process is 50mA, and the line speed is 13mm / s; the pot-shaped target assembly is obtained after turning.

[0039] Example 2

[0040] This embodiment provides a welding method for a pot-shaped target assembly, and the welding method comprises the following steps:

[0041] (1) The tantalum ingot is subjected to stamping treatment to obtain a pot-shaped tantalum target, and the welding surfaces of the obtained pot-shaped tantalum target and the niobium flange ring are cleaned with acetone for 5 minutes and dried at 70° C. for 2 hours to obtain a target to be welded and a ring to be welded;

[0042] (2) The ring to be welded in step (1) is placed on the top outer wall of the target material to be welded, with a weld gap of 0.3 mm, and then the absolute vacuum is 0.5×10 -3 Pa, the first electron beam welding process and the second electron beam welding process are performed sequentially; the beam current of the first electron beam welding process is 10mA, and the line speed is 10mm / s; the beam current of the second electron beam welding process is 40mA, and the line speed is 10mm / s; the pot-shaped target assembly is obtained after turning.

[0043] Example 3

[0044] This embodiment provides a welding method for a pot-shaped target assembly, and the welding method comprises the following steps:

[0045] (1) The tantalum ingot is subjected to stamping treatment to obtain a pot-shaped tantalum target, and the welding surfaces of the obtained pot-shaped tantalum target and the niobium flange ring are cleaned with acetone for 10 minutes and dried at 75° C. for 1 hour to obtain a target to be welded and a ring to be welded;

[0046] (2) The ring to be welded in step (1) is placed on the top outer wall of the target material to be welded, with a weld gap of 0.8 mm, and then the absolute vacuum is 1×10 -4 Pa, the first electron beam welding process and the second electron beam welding process are performed sequentially; the beam current of the first electron beam welding process is 30mA, and the line speed is 15mm / s; the beam current of the second electron beam welding process is 60mA, and the line speed is 15mm / s; the pot-shaped target assembly is obtained after turning.

[0047] Example 4

[0048] This embodiment provides a welding method for a pot-shaped target assembly, which is different from Embodiment 1 in that, except that the acetone in step (1) is replaced by a sodium hydroxide solution with a mass concentration of 10%, the rest is the same as Embodiment 1.

[0049] Example 5

[0050] This embodiment provides a welding method for a pot-shaped target assembly, which is different from Embodiment 1 in that, except for adjusting the weld gap in step (2) to 0.2 mm, the rest is the same as Embodiment 1.

[0051] Example 6

[0052] This embodiment provides a welding method for a pot-shaped target assembly, which is different from Embodiment 1 in that, except for adjusting the weld gap in step (2) to 1 mm, the rest is the same as Embodiment 1.

[0053] Example 7

[0054] This embodiment provides a welding method for a pot-shaped target assembly, which is different from Embodiment 1 in that, except for adjusting the beam current of the second electron beam welding process in step (2) to 30 mA, the rest is the same as Embodiment 1.

[0055] Example 8

[0056] This embodiment provides a welding method for a pot-shaped target assembly, which is different from Embodiment 1 in that, except for adjusting the beam current of the second electron beam welding process in step (2) to 70 mA, the rest is the same as Embodiment 1.

[0057] Example 9

[0058] This embodiment provides a welding method for a pot-shaped target assembly, which is different from Embodiment 1 in that, except for adjusting the linear speed of the second electron beam welding process in step (2) to 8 mm / s, the rest is the same as Embodiment 1.

[0059] Example 10

[0060] This embodiment provides a welding method for a pot-shaped target assembly, which is different from Embodiment 1 in that, except for adjusting the linear speed of the second electron beam welding process in step (2) to 17 mm / s, the rest is the same as Embodiment 1.

[0061] Comparative Example 1

[0062] This comparative example provides a welding method for a pot-shaped target assembly, which is different from Example 1 in that, except for replacing the niobium flange ring in step (1) with a titanium flange ring, the rest is the same as Example 1.

[0063] Comparative Example 2

[0064] This comparative example provides a welding method for a pot-shaped target assembly, which differs from Example 1 in that step (1) is not provided, and the rest is the same as Example 1.

[0065] Comparative Example 3

[0066] This comparative example provides a welding method for a pot-shaped target assembly, which differs from Example 1 in that the first electron beam welding process is not provided in step (2), and the rest is the same as Example 1.

[0067] Comparative Example 4

[0068] This comparative example provides a welding method for a pot-shaped target assembly, which differs from Example 1 in that a third electron beam welding process is provided in step (2), the beam current of the third electron beam welding process is 50 mA, the line speed is 13 mm / s, and the rest is the same as Example 1.

[0069] The pot-shaped target assembly was welded using the welding methods provided in Examples 1-10 and Comparative Examples 1-4. The welding strength of the pot-shaped target assembly was tested by a welding tensile test. The results are shown in Table 1.

[0070] Table 1

[0071]

[0072]

[0073] It can be seen from Table 1 that the welding method of the pot-shaped target assembly provided by the present invention can ensure the welding strength of the pot-shaped tantalum target and the niobium flange ring, significantly improve the processing efficiency, shorten the process flow, and improve the economic benefits;

[0074] By comparing Example 1 with Example 4, it can be seen that the oil stains on the surface of the pot-shaped tantalum target and the niobium flange ring cannot be completely removed by using an alkaline agent for cleaning, thereby affecting the subsequent welding process; by comparing Example 1 with Examples 5 and 6, it can be seen that if the weld gap is too large, the welding strength will be reduced, and there will be problems of poor welding; if the welding gap is too small, electron beam welding cannot be effectively performed; by comparing Example 1 with Examples 7-10, it can be seen that the beam current and line speed of the electron beam welding process need to be controlled within a reasonable range. If they are too large or too small, the welding strength of the target assembly will be adversely affected;

[0075] By comparing Example 1 with Comparative Example 1, it can be seen that the use of titanium flange rings has a large difference in melting point with the tantalum target and thus cannot be effectively welded; by comparing Example 1 with Comparative Example 2, it can be seen that without pre-treating the surfaces of the pot-shaped tantalum target and the niobium flange ring, the oil stains on the surfaces of the two cannot be removed, thereby significantly reducing the welding strength of the assembly; by comparing Example 1 with Comparative Examples 3 and 4, it can be seen that performing one or three electron beam welding treatments will reduce the welding strength of the assembly compared to two electron beam welding treatments.

[0076] In summary, the welding method of the pot-shaped target assembly provided by the present invention aims at the problems of complex process, poor welding effect and high cost in the traditional welding process of using tantalum-titanium flange rings to hot isostatically press to weld a composite ring to a tantalum target and then welding it to the composite ring. By using niobium flange rings which have similar performance to the pot-shaped tantalum target and are easy to weld and have a similar melting point for electron beam welding, the cost can be effectively reduced, the process flow can be reduced, the processing efficiency can be improved, and the welding strength can reach 150MPa. Among them, the two-step welding process of the first electron beam welding treatment and the second electron beam welding treatment can significantly improve the welding effect of the target material to be welded and the ring to be welded, and avoid the problem of poor welding.

[0077] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A welding method for a pot-shaped target assembly, characterized in that: The welding method comprises the following steps: (1) Pre-treating the welding surfaces of the pot-shaped tantalum target and the niobium flange ring respectively to obtain a target to be welded and a ring to be welded; (2) Assembling the target material to be welded obtained in step (1) and the ring member to be welded, and sequentially performing a first electron beam welding treatment and a second electron beam welding treatment, and obtaining the pot-shaped target material assembly after machining.

2. The welding method according to claim 1, characterized in that: The pot-shaped tantalum target material in step (1) is a pot-shaped tantalum target material obtained by stamping a tantalum ingot.

3. The welding method according to claim 1 or 2, characterized in that: The pretreatment in step (1) includes washing and drying performed in sequence.

4. The welding method according to claim 3, characterized in that: The cleaning reagent includes acetone; Preferably, the cleaning time is 5-10 minutes.

5. The welding method according to claim 3 or 4, characterized in that: The drying temperature is 70-75°C; Preferably, the drying time is 1-2 hours.

6. The welding method according to any one of claims 1 to 5, characterized in that: The assembling step in step (2) includes: sleeve-arranging the ring to be welded on the top outer wall of the target material to be welded; Preferably, the weld gap of the assembly in step (2) is 0.3-0.8 mm.

7. The welding method according to any one of claims 1 to 6, characterized in that: Step (2) The absolute vacuum degree of the first electron beam welding process and the second electron beam welding process is ≤1×10 -3 Pa; Preferably, in step (2), the beam current of the first electron beam welding process is 10-30 mA; Preferably, the line speed of the first electron beam welding process in step (2) is 10-15 mm / s.

8. The welding method according to any one of claims 1 to 7, characterized in that: Step (2) The beam current of the second electron beam welding process is 40-60 mA; Preferably, the line speed of the second electron beam welding process in step (2) is 10-15 mm / s.

9. The welding method according to any one of claims 1 to 8, characterized in that: The machining in step (2) includes turning.

10. The welding method according to claim 1, characterized in that: The welding method comprises the following steps: (1) The tantalum ingot is subjected to stamping treatment to obtain a pot-shaped tantalum target, and the welding surfaces of the obtained pot-shaped tantalum target and the niobium flange ring are cleaned with acetone for 5-10 minutes and dried at 70-75° C. for 1-2 hours to obtain a target to be welded and a ring to be welded; (2) The ring to be welded in step (1) is placed on the top outer wall of the target material to be welded, with a weld gap of 0.3-0.8 mm, and then the absolute vacuum is ≤1×10 -3 Pa, the first electron beam welding process and the second electron beam welding process are performed in sequence; the beam current of the first electron beam welding process is 10-30mA, and the line speed is 10-15mm / s; the beam current of the second electron beam welding process is 40-60mA, and the line speed is 10-15mm / s; the pot-shaped target assembly is obtained after turning.